Electronic component with adhesive sheet and transfer sheet
By using a UV-curable adhesive layer containing (meth)acrylic resin, the problem of inconsistent adhesion between the insulating and conductive areas of the adhesive layer is solved, achieving residue-free peeling in the processing of electronic components, and applicable to multiple processes of semiconductor components.
Patent Information
- Application Number
- CN202580029994.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-23
- Filing Date
- 2025-02-18
- Publication Date
- 2026-11-20
AI Technical Summary
In the prior art, adhesive layers tend to leave residue when peeled off from the adhered object, making it difficult to exhibit excellent adhesion and peelability between areas containing insulating materials such as resin and conductive materials. This is especially problematic in the processing of electronic components due to inconsistent adhesive layer behavior.
The UV-curable adhesive layer, containing (meth)acrylic resin, is used for electronic components and transfer sheets. UV irradiation enables the adhesive layer to exhibit excellent adhesion in both insulating and conductive areas, and leaves no residue upon peeling.
It achieves high adhesion between insulating and conductive areas with no residue after peeling, making it suitable for the processing of electronic components, especially for reducing adhesive residue in back-grinding of semiconductor elements, fan-out packaging, semiconductor chip sealing and mounting processes.
Smart Images

Figure CN123147291A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to electronic components with adhesive sheets and transfer sheets. Background Technology
[0002] For a long time, as a wiring board used to mount electronic components such as semiconductor elements, it has been known to be an insulating layer made by heat curing an insulating sheet obtained by impregnating a thermosetting resin composition into a heat-resistant fiber substrate such as glass cloth, and a wiring conductor made of a metal foil such as copper foil, which is alternately laminated, and the wiring conductors sandwiched between the insulating layers are electrically connected to each other by a through conductor made by curing a conductive paste filled in the through holes formed in the insulating layer.
[0003] For example, Patent Document 1 describes a method for manufacturing a wiring substrate, which includes the following steps: overlapping a transfer sheet, in which a wiring conductor made of metal foil is peelably held on an adhesive layer adhered to a main surface of a transfer substrate film, with the wiring conductor in contact with the main surface of an insulating sheet containing an uncured thermosetting resin composition, and pressing the insulating sheet at a specified temperature to embed the wiring conductor into the main surface of the insulating sheet; and then peeling the transfer substrate film and the adhesive layer together from the main surface of the insulating sheet to transfer the wiring conductor onto the main surface of the insulating sheet.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2010-129910 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] As an example of the performance required for transfer sheets, one can be the ability to remove the adhesive layer without leaving any residue on the substrate when peeling the transfer substrate film and adhesive layer together from the substrate.
[0009] In recent years, with the miniaturization of wiring patterns, there has been a growing demand for adhesive layers that possess both high levels of adhesion and peel strength, as well as the ability to prevent the adhesive layer from transferring to the substrate. In particular, the behavior of adhesives can sometimes differ between surfaces containing insulating materials such as resins and areas containing conductive materials such as wiring conductors. For surfaces with such mixed areas exhibiting different adhesive properties, adhesive layers that exhibit superior properties are highly desirable from the viewpoints of adhesion, peel strength, and prevention of transfer.
[0010] As a type of tape used for applications requiring adhesive strength and peelability of sheets with adhesive layers, it is also used in the processing of electronic components such as semiconductor elements.
[0011] This disclosure provides an electronic component with an adhesive sheet, which has an adhesive sheet that is adhered with excellent adhesive strength to the surface of an object having insulating and conductive regions. The adhesive sheet can be peeled off without leaving adhesive residue on the electronic component after it is no longer needed. This disclosure further provides a transfer sheet with an adhesive layer that has sufficiently excellent adhesion to retain the conductor layer during wiring conductor formation, and can be peeled off without being transferred to the object after the wiring conductor has been transferred to it.
[0012] Methods for solving problems
[0013] The contents of this disclosure include the following schemes.
[0014] [1]
[0015] An electronic component with an adhesive sheet, comprising: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and Electronic components disposed on the aforementioned UV-curable adhesive layer of the aforementioned adhesive sheet, The surface of the aforementioned electronic component that is in contact with the aforementioned UV-curable adhesive layer has an insulating region and a conductive region. The aforementioned UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition described above comprises a (meth)acrylic resin (A), which contains structural units of formulas (1) to (3) and optionally contains structural units of formula (4).
[0016]
[0017] (In equation (1), R) 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
[0018] [2]
[0019] A transfer film having: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and Wiring conductors are locally disposed on the aforementioned UV-curable adhesive layer. The aforementioned UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition described above comprises a (meth)acrylic resin (A), which contains structural units of formulas (1) to (3) and optionally contains structural units of formula (4).
[0020]
[0021] (In equation (1), R) 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
[0022] [3]
[0023] A transfer sheet with a conductive layer has the following characteristics: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and The conductor layer disposed on the aforementioned UV-curable adhesive layer, The aforementioned UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition described above comprises a (meth)acrylic resin (A), which contains structural units of formulas (1) to (3) and optionally contains structural units of formula (4).
[0024]
[0025] (In equation (1), R) 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
[0026] [4]
[0027] According to the electronic component with adhesive sheet described in [1], the transfer sheet described in [2], or the transfer sheet described in [3], a sheet with a conductor layer is used. The thickness of the aforementioned substrate layer is 5–500 μm. The thickness of the above-mentioned UV-curable adhesive layer is 1 to 300 μm.
[0028] [5]
[0029] According to the transfer sheet described in [2] or the transfer sheet described in [3], the thickness of the wiring conductor or the conductor layer is 0.5 to 100 μm, and is in the range of 0.01 to 1.20 times the thickness of the UV-curable adhesive layer.
[0030] [6]
[0031] Electronic components with adhesive sheets, transfer sheets, or sheets with conductive layers for transfer sheets according to any one of [1] to [5] The above adhesive composition contains The above-mentioned (meth)acrylic resin (A), Photopolymerization initiator (B), and Crosslinking agent (C).
[0032] [7]
[0033] The method for manufacturing a transfer sheet with a conductor layer as described in any one of [3] to [6] comprises the following steps: A process for providing an adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and The process of setting a conductor layer on the exposed surface of the above-mentioned UV-curable adhesive layer.
[0034] [8]
[0035] A method for manufacturing a transfer film, comprising the following steps: A process for forming a pattern of a resist layer in which a resist layer is provided on the exposed surface of the conductor layer of a transfer sheet having a conductor layer as described in any one of [3] to [6], the resist layer is exposed by a photomask and developed with a developer. An etching process that removes the exposed areas of the conductor layer formed by the above patterning process to form a wiring conductor; and The removal process is a process of removing the resist layer on the wiring conductor formed by the above etching process.
[0036] [9]
[0037] A method for manufacturing a wiring board includes the following steps: A transfer process in which the surface of the wiring conductor is in contact with the insulating sheet by means of any one of [2] and [4] to [6], thereby transferring the wiring conductor to the insulating sheet.
[0038]
[10]
[0039] A method for manufacturing a wiring substrate includes: providing a sealing layer on the surface of a transfer sheet provided with the wiring conductor as described in any one of [2] and [4] to [6].
[0040]
[11]
[0041] The method for manufacturing a wiring substrate according to
[10] includes: providing a conductive path through the sealing layer in such a way that a portion of the wiring conductor is connected to the conductive path.
[0042]
[12]
[0043] A method for manufacturing an electronic device, comprising the following steps: Preparation process for a substrate having insulating and conductive areas on its surface; A bonding process of bonding an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer to the surface of the substrate. The processing step of processing the substrate to which the adhesive sheet is attached; The ultraviolet irradiation process involves subjecting the aforementioned adhesive sheet to ultraviolet light irradiation to cure the aforementioned ultraviolet-curable adhesive layer; and The peeling process of removing the adhesive sheet from the substrate. The aforementioned UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition described above comprises a (meth)acrylic resin (A), which contains structural units of formulas (1) to (3) and optionally contains structural units of formula (4).
[0044]
[0045] (In equation (1), R) 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
[0046] The effects of the invention
[0047] According to this disclosure, an electronic component with an adhesive sheet can be provided, which has an adhesive sheet that is adhered with excellent adhesive force to the surface of an object having an insulating region and a conductive region. The adhesive sheet can be peeled off from the electronic component without leaving adhesive residue after it is no longer needed. Furthermore, according to this disclosure, a transfer sheet with an adhesive layer can be provided. This adhesive layer has sufficiently excellent adhesive force for maintaining the conductor layer during wiring conductor formation, and can be peeled off from the object without being transferred to it after the wiring conductor has been transferred to the object. Attached Figure Description
[0048] Figure 1 A schematic diagram illustrating an exemplary manufacturing method of a fan-out package.
[0049] Figure 2 This is a schematic diagram of an electronic device according to one embodiment.
[0050] Figure 3 A schematic diagram illustrating an exemplary manufacturing method of an electronic device according to one embodiment.
[0051] Figure 4 A schematic diagram illustrating an exemplary manufacturing method of an electronic device according to one embodiment.
[0052] Figure 5 A schematic diagram illustrating an exemplary manufacturing method of an electronic device according to one embodiment. Detailed Implementation
[0053] The embodiments of the present invention will now be described in detail. However, the present invention is not limited to the embodiments shown below.
[0054] In this specification, when "~" is used to indicate a range of values, the values at both ends are the upper and lower limits, respectively, and are included within the range. When multiple upper or lower limits are specified, a range can be created from all combinations of the upper and lower limits. Similarly, when multiple ranges are specified, additional ranges can be created by individually selecting and combining the upper and lower limits from these ranges.
[0055] In this specification, the term "(meth)acrylic" refers to "acrylic" or "methacrylic". The term "(meth)acrylate" refers to "acrylate" or "methacrylate", and the term "(meth)acryloyloxy" refers to "acryloyloxy" or "methacryloyloxy".
[0056] Electronic components with adhesive tabs
[0057] One embodiment of the electronic component with an adhesive sheet includes: an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer; and an electronic component disposed on the ultraviolet-curable adhesive layer of the adhesive sheet. By using the electronic component with the adhesive sheet as an intermediate, an article with less adhesive residue caused by the adhesive layer can be obtained.
[0058] <Electronic Components>
[0059] An electronic component according to one embodiment has an insulating region and a conductive region on the adhesion surface of an adhesive sheet. The insulating region is formed of an electrical insulator such as resin. The conductive region is formed of a conductor such as metal. Because the adhesive sheet has excellent adhesion to multiple regions containing different materials, such as insulating and conductive regions, it can be peeled off in any region without adhesive residue after ultraviolet irradiation. Therefore, it is preferably used in electronic components having insulating and conductive regions. The adhesive sheet is attached to the adhesion surface of the electronic component as a protective strip or as a temporary fixing strip for the electronic component during processing. Specifically, the adhesive sheet can be used, for example, in the back-side grinding process of semiconductor wafers, the sealing process of semiconductor chips during the manufacture of fan-out wafer level packages (FO-WLP), 2.xD SiP, and the cutting process of semiconductor element interconnects, as well as the mounting process of semiconductor elements, electronic components, etc., onto substrates such as interposers. Examples of electronic components include semiconductor wafers, semiconductor chips, semiconductor element interconnects, semiconductor elements, electronic components, and substrates.
[0060] The adhesive strength of an adhesive sheet can be reduced by irradiation with ultraviolet light (also known as UV). UV irradiation of the adhesive sheet can be performed, for example, as follows: UV light is irradiated onto the adhesive sheet bonded to the adhesive surface. This irradiation penetrates the substrate of the adhesive sheet into the UV-curable adhesive layer, causing the unsaturated bonds in the adhesive layer to form a three-dimensional cross-linked structure and cure. As a result, the adhesive strength of the adhesive layer is reduced. It should be noted that if the adhered object is translucent, UV light can be irradiated from the adhered object side towards the adhesive sheet.
[0061] Examples of light sources used for UV irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, chemical lamps, and black lamps.
[0062] The preferred UV irradiation dose applied to the adhesive sheet is 50–3,000 mJ / cm². 2 More preferably 100–600 mJ / cm 2 If the UV irradiation dose applied to the adhesive sheet is 50 mJ / cm 2The above demonstrates how UV-curable adhesive layers can be cured at a sufficiently fast rate through UV irradiation, resulting in minimal adhesion after UV irradiation. Even when the UV irradiation dose to the adhesive sheet exceeds 3000 mJ / cm², this is still possible. 2 However, this method also fails to achieve the desired effect. Therefore, the UV irradiation dose applied to the adhesive sheet is increased to 3,000 mJ / cm². 2 This allows for the economical removal of the adhesive sheet while mitigating the effects of UV radiation on the adhered material.
[0063] One embodiment of a semiconductor device manufacturing method includes the following steps: a preparation step of preparing a semiconductor wafer having insulating and conductive regions on its surface; a bonding step of bonding an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer to the surface of the semiconductor wafer; a processing step of processing the semiconductor wafer with the adhesive sheet bonded thereto; an ultraviolet irradiation step of photocuring the adhesive sheet with ultraviolet light to cure the ultraviolet-curable adhesive layer; and a peeling step of removing the adhesive sheet from the semiconductor wafer. In this embodiment, a back-side grinding step can be cited as an example of a processing step.
[0064] One embodiment of a semiconductor device manufacturing method includes the following steps: a preparation step of preparing a semiconductor chip having an insulating region and a conductive region on its surface; a bonding step of bonding an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer onto the surface of the semiconductor chip; a sealing step of sealing the semiconductor chip with the adhesive sheet bonded thereto; an ultraviolet irradiation step of irradiating the adhesive sheet with ultraviolet light to photocur the ultraviolet-curable adhesive layer; and a peeling step of peeling the adhesive sheet off the semiconductor chip.
[0065] One embodiment of the semiconductor element manufacturing method includes the following steps: a preparation step of preparing a semiconductor element connector having an insulating region and a conductive region on its surface; a pasting step of pasting an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer onto the surface of the semiconductor element connector; a cutting step of cutting the semiconductor element connector with the adhesive sheet pasted thereon into semiconductor elements; an ultraviolet irradiation step of irradiating the adhesive sheet with ultraviolet light to photocur the ultraviolet-curable adhesive layer; and a peeling step of peeling the adhesive sheet off from the semiconductor elements.
[0066] The following is for reference Figure 1 The manufacturing method of semiconductor devices is explained. Figure 1 The following is a process flow diagram illustrating an exemplary manufacturing method for a fan-out package, with each step explained below.
[0067] (a): An adhesive sheet 15 having a substrate layer 12 and an ultraviolet-curable adhesive layer 14 disposed on the substrate layer 12 is attached to the surface of a semiconductor chip 20 having an insulating region 16 and a conductor region 18, thereby obtaining an electronic component 100 with an adhesive sheet.
[0068] (b): The semiconductor chip 20 is sealed with sealing resin 22 to form a semiconductor element connector 200.
[0069] (c): After the adhesive sheet 15 is irradiated with ultraviolet light to light-cur the ultraviolet-curable adhesive layer 14 and the adhesive force is reduced, the adhesive sheet 15 is peeled off from the semiconductor device interconnect 200.
[0070] (d): A redistribution layer 24 is formed on the semiconductor element interconnect 200.
[0071] (e): Conductor pillars 26 and bumps 28 are formed in the redistribution layer 24.
[0072] (f): An adhesive sheet 15 having a substrate layer 12 and an ultraviolet-curable adhesive layer 14 disposed on the substrate layer 12 is bonded to the redistribution layer 24 of the semiconductor element interconnect 200 to obtain an electronic component 110 with an adhesive sheet.
[0073] (g): Cut the semiconductor element connector 200 with the adhesive sheet 15 attached to it into semiconductor elements 300.
[0074] (h): After the adhesive sheet 15 is irradiated with ultraviolet light to light-cur the ultraviolet-curable adhesive layer 14 and the adhesive force is reduced, the adhesive sheet 15 is peeled off from each semiconductor element 300.
[0075] exist Figure 1 In this approach, a single chip is sealed within a single semiconductor element, but the number of sealed chips is not limited. By sealing multiple chips within a single semiconductor element, 2.xD SiP (System-in-Package) structures can be fabricated. Figure 1 In steps (a) and (f), adhesive sheet 15 is applied, but in any step, adhesive sheet with other adhesive layers can be used instead of adhesive sheet 15. From the viewpoint of reducing adhesive residue on the adhered object, it is preferable to use adhesive sheet 15 in both steps.
[0076] One embodiment of the electronic device manufacturing method includes the following steps: a preparation step of preparing a substrate having insulating and conductive regions on its surface; a bonding step of bonding an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate surface; a processing step of processing the substrate with the adhesive sheet bonded thereto; an ultraviolet irradiation step of irradiating the adhesive sheet with ultraviolet light to cure the ultraviolet-curable adhesive layer; and a peeling step of peeling the adhesive sheet from the substrate. In this embodiment, examples of processing steps include, for example, an mounting step, a sealing step, a noise suppression layer formation step, a cutting step, and a monolithization step.
[0077] Figure 2 This is a longitudinal cross-sectional view showing an example of an electronic device that can be manufactured by a manufacturing method of an electronic device according to one embodiment. It should be noted that in the following description, [the following will be used to describe...]. Figure 2 The upper side is called "upper", and the lower side is called "lower".
[0078] Figure 2 The illustrated electronic device 400 includes a substrate 32 having conductor pillars 26 arranged through the thickness direction, semiconductor elements 34 and electronic components 36 such as capacitors and coils disposed on the substrate 32, a sealing portion 42 sealing the semiconductor elements 34 and electronic components 36, wiring 30 formed on the lower surface of the substrate 32 and electrically connected to the conductor pillars, bumps 28 electrically connected to the wiring 30, and an opening 41 covering the wiring 30 and exposing the bumps 28. Figure 2 The noise suppression layer 38 (not shown in the image) covers the upper and side surfaces of the covered portion 40 and the covered sealing portion 42, the side surface of the substrate 32, and a portion of the side surface of the covered portion 40.
[0079] The substrate 32 is a substrate that supports the semiconductor element 34 and the electronic element 36. The top view of the substrate 32 is usually a quadrilateral such as a square or rectangle. A plurality of through holes are formed in the substrate 32 along its thickness direction, and conductor pillars 26 are provided corresponding to the through holes.
[0080] Semiconductor element 34 and electronic element 36 are disposed on substrate 32 such that the electrode pads (not shown) on the lower surface side of semiconductor element 34 and electronic element 36 correspond to conductor pillar 26. With semiconductor element 34 and electronic element 36 disposed in this position, sealing portion 42 is formed to cover semiconductor element 34, electronic element 36 and upper surface side of substrate 32.
[0081] The conductor post 26, which is formed corresponding to the through hole of the substrate 32, is electrically connected at its upper end to the electrode pad of the semiconductor element 34 or electronic element 36. A wiring 30 formed in a predetermined shape is provided on the lower surface of the substrate 32, a portion of which is electrically connected to the lower end of the conductor post 26.
[0082] A bump 28 is electrically connected to the lower surface of the wiring 30, thereby electrically connecting the semiconductor element 34 or electronic element 36 to the bump 28 via electrode pads, conductor posts 26 and wiring 30. Furthermore, a cover portion 40 is provided to cover the wiring 30, and the cover portion 40 has an opening 41 for exposing the bump 28 from its lower side.
[0083] A noise suppression layer 38 is provided covering the upper surface of the sealing portion 42, the side surface of the sealing portion 42, the side surface of the substrate 32, and a portion of the side surface of the covered portion 40. Through this noise suppression layer 38, electromagnetic waves generated by at least one of the semiconductor elements 34 and electronic components 36 disposed on the substrate 32 are blocked from passing through other electronic components located outside the electronic device 400, thereby suppressing noise caused by electromagnetic waves. It should be noted that a portion of the wiring 30 is exposed on the side surface of the covered portion 40 of the noise suppression layer 38. This wiring 30 is electrically connected to the noise suppression layer 38, thereby grounding the noise suppression layer 38 via the wiring 30.
[0084] It should be noted that, Figure 2 The electronic device 400 includes one semiconductor element 34 and two electronic elements 36, but the number of semiconductor elements 34 and electronic elements 36 is not limited thereto. The electronic device may also include either a semiconductor element or an electronic element. Figure 2 The electronic device 400 has a noise suppression layer 38, but the electronic device may also not have a noise suppression layer 38.
[0085] (Manufacturing method of electronic device 400)
[0086] Electronic device 400 can be manufactured using adhesive sheets. The adhesive sheets are attached to the adhesive surface of the substrate as a protective strip for the substrate's adhesion surface or as a temporary fixing strip for the substrate during processing. By using electronic components with adhesive sheets as intermediates, electronic devices with minimal adhesive residue caused by adhesive layers can be obtained.
[0087] The electronic device 400 with the configuration described above can be manufactured, for example, by the following method. One embodiment of the method for manufacturing an electronic device includes the following steps: a preparation step for preparing an electronic component sealing connector, wherein the electronic component sealing connector has a substrate, at least one selected from semiconductor elements and electronic elements disposed on a first surface of the substrate, and a sealing portion formed on the first surface of the substrate to seal the substrate and at least one selected from semiconductor elements and electronic elements, and is provided with wiring formed on a second surface of the substrate, a cover portion formed on the second surface of the substrate and covering the substrate and wiring and having an opening that exposes a portion of the wiring, and a bump electrically connected to the wiring exposed in the opening; a cutting step for forming an electronic component sealing connector by cutting along the thickness direction in a manner corresponding to each electronic component sealing connector to be formed, thereby providing a recess exposed on the side of the electronic component sealing connector; a noise suppression layer forming step for forming a noise suppression layer covering the upper surface and side surface of the electronic component sealing connector; and a monolithic step for obtaining multiple electronic devices at the same time by monolithicizing the recess until it penetrates the cover portion. The method for manufacturing an electronic device further includes the following steps: a bonding step of bonding an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer to the surface of a substrate having insulating and conductive regions; an ultraviolet irradiation step of irradiating the adhesive sheet with ultraviolet light to cure the ultraviolet-curable adhesive layer; and a peeling step of peeling the adhesive sheet off the substrate. It should be noted that the term "surface of the substrate" does not refer only to the surface of the substrate itself; when wiring, coatings, bumps, etc., are formed on the surface of the substrate, it refers to the surface of its outermost layer.
[0088] The following is for reference Figures 3-5 The specific methods for manufacturing electronic devices with these processes are described in detail. Figures 3-5 This is a process flow diagram illustrating an exemplary manufacturing method for producing multiple electronic devices 400 simultaneously. It should be noted that in the following description, [the following will be used to describe...]. Figures 3-5 The upper side is called "upper", and the lower side is called "lower".
[0089] (Preparation process)
[0090] Prepare Figure 4 (a) shows an electronic component sealing connector 500 with wiring 30, cover 40 and bump 28. The electronic component sealing connector 500 is prepared, for example, by going through the following processes [1-1] to [1-7].
[0091] [1-1]
[0092] Prepare Figure 3The substrate 32 is as shown in (a). The substrate 32 has a plurality of pre-formed through-holes and further has conductor posts 26 embedded corresponding to these through-holes. The conductor posts 26 are formed in subsequent steps [1-5] at positions corresponding to the electrode pads of the semiconductor elements 34 and electronic components 36 when the semiconductor elements 34 and electronic components 36 are disposed on the substrate 32. That is, the number of conductor posts 26 on the substrate 32 is the same as the total number of terminals of the plurality of semiconductor elements 34 and electronic components 36 disposed on the substrate 32. For protection or temporary fixation, adhesive sheets can be attached to the lower or upper surface of the substrate 32.
[0093] It should be noted that the substrate 32 is monolithically cut along its thickness direction, thereby serving as an intermediary layer to support the semiconductor element 34 and the electronic element 36.
[0094] The substrate 32 is not particularly limited as long as it has sufficient rigidity to support the semiconductor element 34 and the electronic element 36. Specific examples include rigid substrates such as core substrates made of core material and multilayer substrates made of multilayer material, as well as flexible substrates. Among these, multilayer substrates are preferred for their superior processability.
[0095] There are no particular limitations on the laminate material; examples include a cured product of a resin composition containing thermosetting resins such as phenolic resin, urea resin, melamine resin, and epoxy resin, a curing agent, and an inorganic filler, as the main material. From the viewpoint of the adhesive properties of the laminate and its peelability during the peeling process, the presence of epoxy resin is preferred.
[0096] There are no particular limitations on the core material; examples include substances mainly composed of thermosetting resins such as cyanate ester resin, epoxy resin, and bismaleimide-triazine resin. From the viewpoint of the adhesive properties of the adhesive sheet and its peelability during the peeling process, the inclusion of epoxy resin is preferred.
[0097] Examples of flexible substrates include polyimide, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyethersulfone (PES), polytetrafluoroethylene (PTFE), and polyimide benzo[a]. Substances composed primarily of thermoplastic resins such as PIBO and liquid crystal polymers.
[0098] From the perspective of providing flexibility, the material of the flexible substrate can contain a rubber component. Examples of rubber components include, for instance, at least one selected from acrylic rubber, isoprene rubber, butyl rubber, styrene-butadiene rubber, butadiene rubber, nitrile rubber, silicone rubber, urethane rubber, chloroprene rubber, ethylene propylene rubber, fluororubber, vulcanized rubber, epichlorohydrin rubber, and chlorinated butyl rubber. The rubber component can be used alone or in combination with two or more components.
[0099] From the viewpoint of imparting thermosetting properties, rubber components can have crosslinking groups. Crosslinking groups are simply reactive groups capable of initiating a reaction that crosslinks the molecular chains. Examples include (meth)acryloyl, vinyl, epoxy, styrene, amino, isocyanurate, urea, cyanate, isocyanate, mercapto, hydroxyl, carboxyl, and anhydride groups. Preferably, the rubber component contains at least one group selected from anhydride and carboxyl groups. Examples of rubber components containing anhydride groups include rubber partially modified with maleic anhydride.
[0100] The flexible substrate material can be a cured product of a resin composition containing a rubber component. This resin composition may contain a crosslinking component. Examples of crosslinking components include compounds having at least one reactive group selected from (meth)acryloyl, vinyl, epoxy, styrene, amino, isocyanurate, urea, cyanate, isocyanate, mercapto, hydroxy, and carboxyl groups. A cured product containing a crosslinked polymer can be formed through the reaction of these reactive groups. From the viewpoint of improving heat resistance, the crosslinking component is preferably a compound having at least one reactive group selected from epoxy, amino, hydroxy, and carboxyl groups. Crosslinking components can be used alone or in combination of two or more.
[0101] For example, by combining rubbers with maleic anhydride or carboxyl groups with compounds with epoxy groups, particularly superior effects can be achieved in terms of elasticity, heat resistance, low moisture permeability, tightness of the flexible substrate with the wiring conductor, and low adhesion of the flexible substrate. If the flexible substrate has low adhesion, workability is good.
[0102] Compounds containing epoxy groups are not particularly limited as long as they have epoxy groups within the molecule; for example, they can be general epoxy resins. Examples of epoxy resins include monofunctional epoxy resins, difunctional epoxy resins, and polyfunctional epoxy resins. There are no particular limitations, but from the viewpoint of obtaining sufficient curability, it is preferable to select at least one from difunctional epoxy resins and polyfunctional epoxy resins.
[0103] Examples of epoxy resins include bisphenol A type, bisphenol F type, phenolic varnish type, naphthalene type, dicyclopentadiene type, cresol varnish type, and resins incorporating aliphatic chain backbones into these epoxy resins. By using epoxy resins incorporating aliphatic chain backbones, flexibility can be imparted to flexible substrates. Examples of commercially available epoxy resins incorporating aliphatic chain backbones include EXA-4816 (DIC Corporation). From the viewpoints of curability, low viscosity, and heat resistance, phenolic varnish type, cresol varnish type, naphthalene type, and dicyclopentadiene type epoxy resins are preferred. These epoxy resins can be used alone or in combination of two or more.
[0104] [1-2] (Wiring formation process)
[0105] If an adhesive sheet is attached to the lower surface of substrate 32, peel it off, such as Figure 3 As shown in (b), wiring 30, patterned into a predetermined shape, is formed on the lower surface of the substrate 32 opposite to the surface where the semiconductor element 34 and electronic element 36 are disposed, in a manner electrically connected to the conductor post 26. Adhesive sheets can be attached to the lower surface of the substrate 32 and the wiring 30 at this stage, and the process can proceed to step [1-5].
[0106] There are no particular limitations on the method for forming the wiring 30, and examples include: I: a method of forming the wiring 30 using plating methods such as electroplating or electroless plating; II: a method of forming the wiring 30 by supplying a liquid material containing a conductive material to the substrate 32, drying and curing it. Method I is particularly preferred for forming the wiring 30 using electroplating. According to the electroplating method, wiring 30 with excellent adhesion can be easily and reliably formed on the conductor post 26.
[0107] [1-3] (Covering formation process)
[0108] like Figure 3 As shown in (c), the covered portion 40 is formed in such a way as a covered substrate 32 and wiring 30.
[0109] Such a coating 40 is typically composed primarily of a thermosetting resin. Examples of thermosetting resins include epoxy resin, phenolic resin, urea resin, melamine resin, unsaturated polyester resin, polyimide resin, silicone resin, and polyurethane resin. Two or more thermosetting resins can be used alone or in combination. Epoxy resin is preferred due to its ease of acquisition and excellent heat resistance.
[0110] Examples of epoxy resins include substances obtained by reacting compounds having two phenolic hydroxyl groups, such as bisphenol A, bisphenol F, bisphenol AD, hydroquinone, methylhydroquinone, dimethylhydroquinone, dibutylhydroquinone, resorcinol, methylresorcinol, biphenol, tetramethylbiphenol, dihydroxynaphthalene, and dihydroxydiphenyl ether, with epichlorohydrin and / or methylepimercinol; substances obtained by reacting compounds that have undergone glycidyl etherification of one or more of the above-mentioned compounds having two phenolic hydroxyl groups, condensates of one or more of the above-mentioned compounds having two phenolic hydroxyl groups, with epichlorohydrin and / or methylepimercinol; phenolic varnish resins, cresol varnish resins, bisphenol A varnish resins, dicyclopentadiene phenol resins, terpene phenol resins, phenol aralkyl resins, and naphthol varnish resins.
[0111] The covered portion 40 can be formed, for example, using the same method as that used to form the sealing portion 42 described later.
[0112] [1-4]
[0113] like Figure 3 As shown in (d), an opening 41 is formed in the covered portion 40 such that a portion of the wiring 30 is exposed. Adhesive sheets can be applied to the wiring 30, the covered portion 40, and the opening 41 at this stage, and the process can proceed to step [1-5]. Alternatively, the process can proceed to step [1-7] before step [1-5].
[0114] The opening 41 is formed in the subsequent process [1-7] in a manner corresponding to the position where the bump 28 is formed. As for the method of forming the opening 41 on the cover portion 40, there is no particular limitation. For example, a method of etching the cover portion 40 using a resist layer formed on the cover portion 40 in a manner that exposes the area where the opening 41 is to be formed as a mask.
[0115] [1-5]
[0116] If an adhesive sheet is attached to the upper surface of substrate 32, peel it off, such as Figure 3 As shown in (e), a semiconductor element 34 and an electronic element 36 are disposed on the upper surface of a substrate 32, which has wiring 30 and a cover portion 40 having an opening 41.
[0117] When semiconductor element 34 and electronic element 36 are disposed on substrate 32, semiconductor element 34 and electronic element 36 are disposed in such a way that the positions of the electrode pads of semiconductor element 34 and electronic element 36 correspond to the positions of the conductor pillars 26 of substrate 32.
[0118] Semiconductor element 34 and electronic element 36 may or may not be fixed to substrate 32, but are preferably fixed by adhesives such as epoxy adhesives (also known as underfill materials). Thus, during the sealing of semiconductor element 34 and electronic element 36 in processes [1-6], positional displacement of semiconductor element 34 and electronic element 36 can be effectively prevented.
[0119] [1-6]
[0120] like Figure 3 As shown in (f), a sealing portion 42 is formed on the upper side of the substrate 32, that is, the side on which the semiconductor element 34 and the electronic element 36 are disposed, in such a way as to cover the substrate 32, the semiconductor element 34 and the electronic element 36.
[0121] Thus, an electronic component sealing connector 500 can be obtained in which the substrate 32, semiconductor element 34 and electronic component 36 are sealed on the upper surface of the substrate 32 by the sealing part 42, with wiring 30 and covering part 40 provided on its lower surface side.
[0122] The method for forming the sealing portion 42 is not particularly limited. For example, a method in which a thermosetting resin composition, such as a granular epoxy resin composition, is supplied to the upper surface of the substrate 32 in a molten state to cover the substrate 32, the semiconductor element 34, and the electronic component 36, and then the molten thermosetting resin composition is compressed and molded. According to such a method, the semiconductor element 34 and the electronic component 36 can be easily and densely sealed on the substrate 32.
[0123] [1-7] (Bump connection process)
[0124] If an adhesive sheet is attached to the lower surface of substrate 32, peel it off, such as Figure 3 As shown in (g), the bump 28 is formed in such a way that it is electrically connected to the wiring 30 exposed at the opening 41 of the covered portion 40. If steps [1-5] and [1-6] are performed after step [1-7], the process can proceed to step [1-5] after the adhesive sheet is attached to the covered portion 40 and the bump 28.
[0125] By configuring the connection between the conductor post 26 and the bump 28 via the wiring 30, the bump 28 can be positioned at a different location from the conductor post 26 in the surface direction of the substrate 32. In other words, the bump 28 and the conductor post 26 can be arranged such that their centers do not overlap. Therefore, the bump 28 can be formed at a desired location on the lower surface of the resulting electronic device 400.
[0126] There are no particular limitations on the method of joining the bump 28 to the wiring 30. For example, a method in which a viscous flux is applied between the bump 28 and the wiring 30 can be used.
[0127] Examples of materials that can be used to form the bump 28 include solder, silver brazing filler metal, copper brazing filler metal, phosphor bronze brazing filler metal, and other brazing materials.
[0128] The electronic component sealing connector 500, which is equipped with wiring 30, covering part 40 and bump 28, is prepared by the above-described processes [1-1] to [1-7].
[0129] As described above, since the wiring 30, the covering portion 40, the opening portion 41, and the bump 28 are formed together with the electronic component sealing connector 500, rather than the electronic component sealing body 600 described later, the process of forming the wiring 30, the covering portion 40, and the bump 28 is simplified, saving time and effort. As a result, the productivity of the electronic device 400 is improved.
[0130] It should be noted that, in Figure 3 In this paper, the case in which wiring 30 and a cover portion 40 with an opening 41 are formed on the lower surface side of substrate 32 before the formation of electronic component sealing connector 500 is described, is described. However, the method of manufacturing electronic device 400 is not limited to this method. For example, wiring 30 and a cover portion 40 with an opening 41 can be formed on the lower surface side of substrate 32 after the formation of electronic component sealing connector 500.
[0131] The formation of the opening 41 of the protrusion 28 on the covered portion 40 can be performed not after the formation of the electronic component sealing connector 500, but before the formation of the semiconductor element 34 and electronic element 36, and the formation of the sealing portion 42. In this case, the semiconductor element 34 and electronic element 36 can be arranged and the sealing portion 42 can be formed after the adhesive sheet is attached to the covered portion 40 and the protrusion 28, and the cutting process of the electronic component sealing connector 500 can proceed with the adhesive sheet being attached.
[0132] (Cutting process)
[0133] like Figure 4 (a) In the case where the adhesive sheet is not attached to the covered portion 40 and the protrusion 28, such as Figure 4 (b) Attach the adhesive sheet 15 to the covered portion 40 and the protrusion 28 as described above. Next, as follows... Figure 4As shown in (c), the electronic component sealing connector 500 is fixed using, for example, a wafer ring. Then, using a cutting blade, the electronic component sealing connector 500 is cut along the thickness direction at a position corresponding to each electronic component seal 600 to be formed, that is, corresponding to each area sealed by the sealing portion 42 for the one semiconductor element 34 and two electronic elements 36 to be included in the electronic device 400, so that the side of the electronic component seal 600 is exposed.
[0134] Thus, the electronic component sealing connector 500 is monolithically formed in a grid-like manner in view of top view in correspondence with each combination of one semiconductor element 34 and two electronic elements 36, and the electronic component sealing body 600 is attached to the adhesive sheet 15 via wiring 30, covering portion 40 and bump 28.
[0135] At this time, the adhesive sheet 15 has a buffering effect, which can suppress or prevent cracks or missing parts of the electronic component sealing connector 500, further wiring 30, covering part 40 and bump 28 when the electronic component sealing connector 500 is cut.
[0136] Cutting of the electronic component sealing connector 500 using a cutting blade, such as Figure 4 As shown in (c), it is preferable to extend along the thickness direction of the cover portion 40 to a position corresponding to the thickness of the wiring 30, up to the middle of the cover portion 40. This ensures that the electronic component sealing connector 500 can be reliably made a single piece. Furthermore, while the electronic component seal 600 is attached to the adhesive sheet 15 via the wiring 30, the cover portion 40, and the bump 28, the sides of the electronic component seal 600—that is, the sides of the sealing portion 42 and the substrate 32, and a portion of the sides of the cover portion 40—can be reliably exposed in the recess 43.
[0137] (Noise suppression layer formation process)
[0138] Next, as Figure 4 As shown in (d), a noise suppression layer 38 is formed on the upper surface and side surface of the covered electronic component seal 600, and on a portion of the side surface of the covered portion 40.
[0139] The noise suppression layer 38 is formed, for example, by performing the following processes [2-1] and [2-2]. In addition to the following processes, the noise suppression layer 38 can also be formed by PVD.
[0140] [2-1]
[0141] An electromagnetic wave shielding film having a release layer as an insulating layer and a noise suppression layer 38 laminated on the release layer is prepared. On the side of the electronic component sealing body 600 where the sealing part 42 is formed, the electromagnetic wave shielding film is laminated on the electronic component sealing body 600 with the noise suppression layer 38 facing the electronic component sealing body 600.
[0142] There are no particular limitations on the method for attaching the electromagnetic wave shielding film to the electronic component sealing body 600, and examples include vacuum pressure forming and compression molding. Vacuum pressure forming, for example, is a method of covering the upper surface and sides of the electronic component sealing body 600 with the electromagnetic wave shielding film using a vacuum pressure laminator. Vacuum pressure forming is performed by placing the electronic component sealing body 600 and the electromagnetic wave shielding film in an overlapping state within a closed space that can be made into a vacuum atmosphere, with the surface of the electronic component sealing body 600 where the sealing part 42 is formed facing the surface of the electromagnetic wave shielding film on the noise suppression layer 38 side, and then heating them to uniformly bring the electromagnetic wave shielding film and the electronic component sealing body 600 close to each other to create a vacuum atmosphere in the closed space, and then applying pressure.
[0143] In this way, by uniformly applying pressure from the electromagnetic wave shielding membrane side while simultaneously creating a vacuum atmosphere in the enclosed space, the release layer is pressed into the noise suppression layer 38 in a shape corresponding to the recess 43. With this pressing, the noise suppression layer 38 deforms in a shape corresponding to the recess 43. Thus, with the noise suppression layer 38 pressed into the recess 43 in a shape corresponding to the recess 43, the upper surface and side surfaces of the electronic component seal 600, as well as a portion of the side surface of the covered portion 40, are covered by the noise suppression layer 38.
[0144] Thus, by covering the upper surface and sides of the electronic component sealing body 600 with the noise suppression layer 38, electromagnetic wave shielding can be imparted to the resulting electronic device 400. On the side of the covered portion 40, since a portion of the wiring 30 is exposed, covering a portion of the side of the covered portion 40 with the noise suppression layer 38 allows the wiring 30 to be electrically connected to the noise suppression layer 38. As a result, the noise suppression layer 38 is electrically grounded via the wiring 30.
[0145] It should be noted that if the electrical grounding of the noise suppression layer 38 is not required, the formation of the noise suppression layer 38 on the side of the covered portion 40 can be omitted. In this case, the formation of the recess 43, that is, the cutting of the electronic component sealing connector 500, does not need to be carried out in a manner that reaches the middle of the covered portion 40, but only needs to be carried out until the substrate 32 is penetrated.
[0146] In the bonding process of the electromagnetic wave shielding film formed by vacuum pressure molding, there is no particular limitation on the bonding temperature, but it is preferably 15°C or higher and 220°C or lower, and more preferably 20°C or higher and 210°C or lower.
[0147] There is no particular limitation on the pressure for applying the adhesive, but it is preferably 0.1 MPa or more and 20.0 MPa or less, and more preferably 0.5 MPa or more and 15.0 MPa or less.
[0148] There is no particular limitation on the pasting time, but it is preferred to be more than 5 seconds and less than 90 minutes, and more preferably more than 30 seconds and less than 10 minutes.
[0149] By setting the conditions in the process of applying the electromagnetic wave shielding film within the above range, the upper surface and side surface of the electronic component sealing body 600, as well as a portion of the side surface of the covered portion 40, can be reliably covered by the noise suppression layer 38 when the recess 43 between adjacent electronic component sealing bodies 600 is pressed into each other.
[0150] In this process, an electromagnetic wave shielding film is used to cover the electronic component seal 600 and the covered portion 40 with the noise suppression layer 38, which is pressed into the recess 43 between adjacent electronic component seals 600.
[0151] The compression molding method is implemented, for example, by placing an electromagnetic wave shielding film on the surface of the electronic component seal 600, which is attached to the adhesive sheet 15, where the sealing portion 42 is formed. Furthermore, the electromagnetic wave shielding film is clamped from its upper and lower surface sides with two flat plates while a buffer material is placed on it. Then, the two flat plates are brought close together and pressure is applied.
[0152] In this way, by bringing the electromagnetic wave shielding film close to the electronic component sealing body 600 while a buffer material is disposed on it, the release layer can be pressed into the noise suppression layer 38 in accordance with the shape of the recess 43. Accompanying this pressing, the noise suppression layer 38 is deformed in accordance with the shape of the recess 43. Therefore, with the noise suppression layer 38 pressed into the recess 43 in accordance with its shape, the upper surface and side surfaces of the electronic component sealing body 600, as well as a portion of the side surface of the covered portion 40, can be covered by the noise suppression layer 38.
[0153] In the electromagnetic wave shielding film, the release layer acts as a buffer material to prevent the noise suppression layer 38 from breaking when it is pressed into the upper surface and side surfaces of the electronic component seal 600 and part of the side surface of the covered portion 40 by following the shape of the recess 43. It should be noted that the release layer of the electromagnetic wave shielding film is peeled off from the noise suppression layer 38 in process [2-2].
[0154] The materials used to form the release layer are not particularly limited, and examples include syndiotactic polystyrene, polymethylpentene, polybutylene terephthalate, polyethylene terephthalate, axially stretched polypropylene and biaxially stretched polypropylene, cyclic olefin polymers, silicone, styrene elastomer resins, styrene-butadiene rubber, acrylic rubbers, epoxy resins, polyphenols, polyurethanes, and other resin materials. Among these, axially stretched polypropylene is preferred from the viewpoint of the release layer's ability to penetrate the noise suppression layer and its heat resistance.
[0155] The energy storage modulus of the stripping layer at 100°C is preferably 1.0E+04 Pa or more and 1.0E+11 Pa or less, more preferably 1.0E+05 Pa or more and 1.0E+10 Pa or less, and even more preferably 1.0E+06 Pa or more and 5.0E+09 Pa or less.
[0156] The thickness of the release layer is not particularly limited, but it is preferably 20 μm or more and 1000 μm or less, more preferably 70 μm or more and 500 μm or less.
[0157] The noise suppression layer 38 has the function of blocking electromagnetic waves generated from at least one of the semiconductor elements 34 and electronic elements 36 included in the electronic component seal 600 and other electronic components located outside the electronic component seal 600.
[0158] The noise suppression layer 38 is not particularly limited and can block electromagnetic waves in any form. Examples of noise suppression layers 38 include a reflective layer that blocks electromagnetic waves by reflecting them and an absorptive layer that blocks them by absorbing them.
[0159] [2-2]
[0160] In this process, the release layer is peeled off from the electromagnetic wave shielding film that is adhered to the electronic component seal 600.
[0161] Regarding the peeling of the release layer, the interface between the release layer and the noise suppression layer 38 in the electromagnetic wave shielding film peels off, resulting in the release layer being peeled off from the noise suppression layer 38.
[0162] Therefore, while being attached to the adhesive sheet 15 via the cover portion 40, wiring 30 and bump 28, a plurality of electronic component seals 600 with noise suppression layers 38 provided on the upper surface and side surfaces are formed together.
[0163] There is no particular limitation on the method for peeling off the release layer, but peeling by hand is preferred, for example. For peeling by hand, for example, first, one end of the release layer is held, and the release layer is peeled off from the noise suppression layer 38 from the held end. Then, the release layer is peeled off from that end towards the center and then towards the other end in sequence, thereby peeling the release layer off from the noise suppression layer 38.
[0164] The temperature for peeling is preferably below 180°C, more preferably below 165°C, and even more preferably below 150°C.
[0165] By going through the above-described processes [2-1] and [2-2], thus achieving... Figure 4 As shown in (d), the upper surface and side surfaces of the electronic component seal 600, as well as a portion of the side surface of the covered portion 40, can be covered by the noise suppression layer 38 while the release layer has been peeled off from the noise suppression layer 38.
[0166] Examples of PVD methods include sputtering. Sputtering methods include, for example, magnetron sputtering, bipolar sputtering, DC (direct current) sputtering, RF (high frequency) sputtering, reactive sputtering, and ion beam sputtering. There are no particular restrictions on sputtering conditions. For example, metals such as Cr, Cu, Ti, Ag, Pt, and Au, alloys such as Ni-Cr, SUS, and Cu-Zn, or metal oxides such as ITO, SiO2, TiO2, Nb2O5, and ZnO can be used as targets, and inert gases such as Ar can be used for film formation.
[0167] (Single-piece manufacturing process)
[0168] like Figure 5 (a) In this way, the adhesive sheet 15 that is pasted on the covered part 40 and the protrusion 28 will be peeled off, as follows: Figure 5 (b) As shown, other adhesive sheets 15 are attached to the noise suppression layer 38 on the upper surface of the multiple electronic component seal 600.
[0169] Next, the electronic component seal 600, to which the adhesive sheet 15 is attached via the noise suppression layer 38, is secured using, for example, a chip ring. Then, as... Figure 5 (c) In this manner, the recess 43 is cut along the thickness direction using a cutting blade, allowing the covered portion 40 to pass through. By cutting the covered portion 40, a monolithic electronic device 400 can be obtained in a state where it is adhered to the adhesive sheet 15. Furthermore, as... Figure 5(d) Thus, the electronic device 400 can be obtained by peeling off the adhesive sheet 15. Alternatively, an adhesive sheet with other adhesive layers can be used instead of the adhesive sheet 15.
[0170] (Paste process)
[0171] The bonding of the adhesive sheet 15 to the surface of the substrate 32 having insulating and conductive regions in the above method can be achieved, for example, by placing the adhesive sheet 15 on the cutting machine worktable, placing the adhesive surface of the substrate 32 on the adhesive sheet 15, and gently pressing it. If the adhesive surface has protrusions 28, this can be achieved by embedding the protrusions 28 into the adhesive sheet 15. It should be noted that the adhesive sheets 15 can also be pre-attached to the adhesive surface before being placed on the cutting machine worktable.
[0172] The adhesive sheet 15 protects the adhesion surface of the substrate 32 during bonding and also serves as a temporary fixing material during various processing of the surface of the substrate 32. It should be noted that in some processes, an adhesive sheet with other adhesive layers can be used instead of the adhesive sheet 15.
[0173] (UV irradiation process and peeling process)
[0174] Since the adhesive sheet 15 is not needed during the processing of the adhesive surface or the placement on other substrates, the adhesive sheet 15 is peeled off from the adhesive surface. The peeling of the adhesive sheet 15 is performed after the adhesive force of the adhesive sheet 15 is reduced by UV irradiation.
[0175] It should be noted that the method for manufacturing the electronic device 400 together has been described here, but the electronic device 400 can also be manufactured separately. Furthermore, the method for manufacturing the electronic device 400 having a noise suppression layer 38 has been described here, but the formation of the noise suppression layer 38 may not be performed. In this case, the electronic device 400 can be obtained by performing monolithic fabrication in the above-described cutting process.
[0176] <Transfer Sheet>
[0177] One embodiment of the transfer sheet includes: an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer; and a wiring conductor partially disposed on the ultraviolet-curable adhesive layer. The transfer sheet can be used, for example, to manufacture a wiring substrate.
[0178] (Wire conductor)
[0179] The wiring conductor is a substance obtained by forming a wiring pattern on a conductor layer disposed on a UV-curable adhesive layer. There are no particular limitations on the wiring material, as long as it is a commonly used material capable of electrical conductivity. In particular, from the viewpoint of wiring formability, copper or copper-containing alloys are suitable. Examples of conductor layers include conductor foils such as metal foils and conductor coatings. Metal foils are preferred. Examples of metal foils suitable for forming wiring patterns include copper foil, titanium foil, stainless steel foil, nickel foil, permalloy foil, 42 alloy foil, kovar foil, nickel-chromium alloy foil, beryllium copper foil, phosphor bronze foil, brass foil, cerium foil, aluminum foil, tin foil, lead foil, zinc foil, solder foil, iron foil, tantalum foil, niobium foil, molybdenum foil, zirconium foil, gold foil, silver foil, palladium foil, Monel alloy foil, Inconel nickel alloy foil, Hastelloy foil, etc. From the viewpoint of suitable elastic modulus, the metal foil is preferably selected from copper foil, gold foil, nickel foil, and iron foil, and copper foil is more preferred. Copper foil can be easily formed into wiring patterns using photolithography.
[0180] There are no particular restrictions on the type of copper foil used; electrolytic copper foil and rolled copper foil, such as those used in copper-clad laminates and flexible wiring boards, can be used. Examples of commercially available electrolytic copper foil include 3EC-M3-VLP-18 (Mitsui Metals & Minerals Co., Ltd.), F0-WS-18 (Furukawa Electric Co., Ltd., trade name), NC-WS-20 (Furukawa Electric Co., Ltd., trade name), YGP-12 (Nippon Electrolytic Co., Ltd., trade name), GTS-18 (Furukawa Electric Co., Ltd., trade name), and F2-WS-12 (Furukawa Electric Co., Ltd., trade name). Examples of commercially available rolled copper foil include TPC foil (JX Metals Co., Ltd., trade name), HA foil (JX Metals Co., Ltd., trade name), HA-V2 foil (JX Metals Co., Ltd., trade name), and C1100R (Mitsui Sumitomo Metal Mining Shindoh Co., Ltd., trade name). From the viewpoint of ensuring a tight seal with the insulating sheet used to transfer the wiring conductor, copper foil that has undergone a roughening treatment can be used. From the viewpoint of bending resistance, rolled copper foil can be used.
[0181] The metal foil can have a roughened surface formed through a roughening process. In this case, the metal foil is typically placed on the UV-curable adhesive layer with the roughened surface facing opposite directions to the UV-curable adhesive layer. From the viewpoint of ensuring good adhesion between the insulating sheet and the metal foil for transferring the wiring conductor, the surface roughness Ra of the roughened surface can be 0.1–3 μm or 0.2–2.0 μm. To facilitate the formation of fine wiring, the surface roughness Ra of the roughened surface can be 0.3–1.5 μm.
[0182] Surface roughness Ra was measured using a Wyko NT9100 surface shape measuring device (Veeco) under the following conditions.
[0183] Internal lens: 1x
[0184] External lens: 50x
[0185] Measurement range: 0.120 × 0.095 mm
[0186] Measurement depth: 10 μm
[0187] Measurement method: Vertical scanning interferometry (VSI method)
[0188] Wiring conductors can be disposed on the aforementioned UV-curable adhesive layer, for example, by forming a conductor layer on a UV-curable adhesive layer and etching it into a predetermined pattern using photolithography.
[0189] The thickness of the wiring conductor or conductor layer is preferably 0.5 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the wiring conductor or conductor layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. The thickness of the wiring conductor or conductor layer is preferably 0.5 to 100 μm, more preferably 5 to 50 μm, and even more preferably 10 to 30 μm. If the thickness of the wiring conductor or conductor layer is 0.5 μm or more, poor transfer of the wiring conductor is suppressed. If the thickness of the wiring conductor or conductor layer is 100 μm or less, the resistivity is sufficiently low, making it easy to form a high-precision microstructure, which can smooth the surface of the substrate after transfer and prevent defects when stacking insulating sheets with transferred wiring conductors.
[0190] The thickness of the wiring conductor or conductor layer is preferably 0.01 times or more, more preferably 0.1 times or more, and even more preferably 0.6 times or more, relative to the thickness of the UV-curable adhesive layer. The thickness of the wiring conductor or conductor layer is preferably 1.20 times or less, more preferably 1.15 times or less, and even more preferably 1.00 times or less, relative to the thickness of the UV-curable adhesive layer. The thickness of the wiring conductor or conductor layer is preferably 0.01 to 1.20 times, more preferably 0.1 to 1.15 times, relative to the thickness of the UV-curable adhesive layer.
[0191] <Method for manufacturing transfer film>
[0192] The transfer sheet can be manufactured, for example, from a sheet with a conductor layer, which includes: an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer; and a conductor layer disposed on the ultraviolet-curable adhesive layer. A method for manufacturing the transfer sheet according to one embodiment includes the following steps: a pattern forming step of providing a resist layer on the exposed surface of the conductor layer of the sheet with the conductor layer, exposing the resist layer via a photomask, and developing it with a developer; an etching step of removing the exposed area of the conductor layer formed in the pattern forming step to form a wiring conductor by etching; and a removal step of removing the resist layer on the wiring conductor formed by the etching step.
[0193] The material used for the resist layer in the pattern forming process can be any known material, as long as it has pattern forming capabilities. The form of the resist is also not particularly limited; it can be applied as a dry film to the exposed surface of the conductor layer, or it can be coated as a liquid onto the exposed surface of the conductor layer and then heated and dried to form a film. The resist layer can be either negative or positive.
[0194] The resist layer is patterned by exposure through a photomask and development with a developer. Thus, the portion of the resist layer washed away by the developer becomes the exposed area of the conductor layer, while the remaining portion of the resist layer becomes the masked area of the conductor layer.
[0195] Examples of developing solutions include, for example, sodium carbonate solution.
[0196] In the etching process, the areas of the conductor layer not covered by the resist layer, i.e., the exposed areas of the conductor layer, are removed by etching methods such as plasma etching and chemical etching. Examples of etching solutions include, for example, a mixture of concentrated sulfuric acid and hydrogen peroxide water, and a ferric chloride solution.
[0197] In the removal process, the removal of the resist layer on the wiring conductor can be performed, for example, by using a stripping solution. Cleaning is preferably performed after removal. Examples of stripping solutions include, for instance, sodium hydroxide solution.
[0198] Transfer sheets can be manufactured, for example, by a process of obtaining an adhesive sheet by laminating a UV-curable adhesive layer on a substrate layer, a process of obtaining a sheet with a conductor layer for transfer sheets by laminating a conductor layer on the UV-curable adhesive layer of the adhesive sheet, and a process of forming a wiring conductor by etching the conductor layer of the sheet with a conductor layer for transfer sheets into a specified pattern using photolithography.
[0199] <Method for manufacturing a transfer film with a conductive layer>
[0200] One embodiment of a transfer sheet with a conductor layer comprises: an adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and a conductor layer disposed on the UV-curable adhesive layer. A method for manufacturing a transfer sheet with a conductor layer according to one embodiment includes the steps of: providing an adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and providing a conductor layer on the exposed surface of the UV-curable adhesive layer. As described above, examples of conductor layers include, for instance, conductor foil and conductor coating.
[0201] There are no particular limitations on the method of setting the conductor foil. Examples include, for instance, directly coating the conductor foil with an adhesive composition, coating an adhesive composition for forming a UV-curable adhesive layer onto a substrate to form a UV-curable adhesive layer, and then laminating the formed UV-curable adhesive layer onto the conductor foil.
[0202] Conductor coatings can be formed, for example, using conventional plating methods such as addition or semi-addition methods. For instance, after treating a UV-curable adhesive layer on a substrate with a plating catalyst that allows palladium adhesion, the UV-curable adhesive layer is immersed in an electroless plating solution to deposit an electroless plating layer of 0.3–1.5 μm thickness across the entire surface of the primer, thus forming a conductor coating. Electrolytic plating can be further performed as needed to adjust the thickness. Any electroless plating solution can be used without particular limitation. Conventional methods can also be employed for electrolytic plating without particular limitation. From the viewpoint of cost and resistivity, copper plating can be used as a conductor coating.
[0203] Transfer sheets with a conductor layer can be manufactured, for example, by the method shown below.
[0204] In the first embodiment, a conductor layer is provided on the UV-curable adhesive layer of the adhesive sheet, and pressure treatment using an autoclave is performed. The pressure treatment using an autoclave typically requires a temperature of 10–50°C and a pressure of 20–80 N / cm. 2 Apply pressure for about 5 to 60 minutes, but the optimal conditions can be determined appropriately based on the composition of the adhesive composition used.
[0205] In the second embodiment, a conductor layer is applied to the UV-curable adhesive layer midway through the curing process of the adhesive sheet, followed by curing. In this case, during the curing process, while adjusting the gel fraction of the adhesive layer, the conductor layer is laminated at a stage before the final gel fraction is reached.
[0206] In the third embodiment, the adhesive composition is directly coated onto the conductor layer to form an ultraviolet-curable adhesive layer for curing.
[0207] These methods ensure a seamless, gapless interface between the UV-curable adhesive layer and the conductor layer, suppressing the intrusion of the etching solution used in subsequent etching processes and resulting in a well-formed wiring conductor. By appropriately adjusting the stacking conditions, the balance between the adhesive strength of the UV-curable adhesive layer and its peelability after UV irradiation can be adjusted.
[0208] <Manufacturing Method of Wiring Board>
[0209] One embodiment of the wiring board manufacturing method includes the following steps: a transfer step of contacting the surface of a transfer sheet where the wiring conductor is disposed with an insulating sheet, thereby transferring the wiring conductor to the insulating sheet. Examples of insulating sheets include, for example, a heat-resistant fiber substrate impregnated with a thermosetting resin composition, a core substrate, a multilayer substrate, and a flexible substrate. The same type as described above can be used as the core substrate, multilayer substrate, and flexible substrate.
[0210] The form of the heat-resistant fiber substrate is not particularly limited, and examples include, for example, woven fabrics and nonwoven fabrics. Examples of heat-resistant fibers include, for example, glass fibers, aramid fibers, and fully aromatic polyester fibers. Examples of thermosetting resin compositions include, for example, resin compositions containing thermosetting resins such as epoxy resins, bismaleimide triazine resins, polyimide resins, fluoropolymers, phenolic resins, and allyl-modified polyphenylene ether resins. It is preferable to use thermosetting resins that are liquid at room temperature. From the viewpoint of adhesion of the transfer sheet and peelability in the peeling process, the thermosetting resin composition preferably contains epoxy resin.
[0211] The transfer of the wiring conductor to the insulating sheet can be performed, for example, by the following method: The side of the transfer sheet containing the wiring conductor is overlapped with at least one main side of the insulating sheet, and they are pressed together. Next, UV irradiation is performed to peel the substrate layer and the photocured adhesive layer of the transfer sheet from the insulating sheet, thereby transferring the wiring conductor to the aforementioned main side of the insulating sheet. The light source and UV irradiation amount used during UV irradiation are the same as described above.
[0212] Taking a wiring board as an example, in which an insulating layer and a wiring conductor are alternately laminated as a cured product of a heat-resistant fiber substrate impregnated with a thermosetting resin composition, and the wiring conductors sandwiching the insulating layer are electrically connected to each other through conductor posts provided in through holes formed in the insulating layer, the manufacturing method of the wiring board will be described in more detail below. Such a wiring board can be manufactured, for example, as described below.
[0213] (a) A protective resin film is peelably adhered to both main surfaces of an insulating sheet in which an uncured thermosetting resin composition is impregnated with a heat-resistant fiber substrate.
[0214] (b) Next, multiple through holes are formed by laser processing of the insulating sheet with the protective resin film attached to it, thereby forming multiple through holes that penetrate the resin film and the insulating sheet.
[0215] (c) Next, conductive paste containing conductive powder such as metal is screen-printed into the resin film on one side of the aforementioned through-hole. It should be noted that in this case, the resin film forming the through-hole functions as a mask for printing.
[0216] (d) Next, the resin film is peeled off from the two main surfaces of the insulating sheet that has been filled with conductive paste in the through holes.
[0217] (e) Next, the transfer sheet and at least one main surface of the insulating sheet are overlapped in such a way that the ends of the wiring conductor and the conductive paste are grounded, and they are pressed together so that the wiring conductor is embedded in the main surface of the insulating sheet.
[0218] (f) Next, by UV irradiation, the substrate layer and the photocured adhesive layer of the transfer sheet are peeled off from the main surface of the insulating sheet in which the wiring conductor is embedded, thereby transferring the wiring conductor to the main surface of the insulating sheet.
[0219] (g) Finally, multiple insulating sheets with the wire conductors transferred are stacked and heated and pressed using a press to cure the insulating sheets and conductive paste to obtain a wiring substrate.
[0220] The following will describe (a) to (g) in further detail. In (a), firstly, an insulating sheet and a resin film with an adhesive layer are prepared to serve as the insulating layer of the wiring board. The thickness of the insulating sheet is, for example, 30 to 200 μm.
[0221] The thickness of the resin film is, for example, 5 to 25 μm. Examples of materials for the resin film include heat-resistant resins such as polyethylene terephthalate. An adhesive layer is adhered to one main surface of the resin film. The adhesive layer is preferably an acrylic resin-based adhesive. The thickness of the adhesive layer is, for example, 3 to 7 μm.
[0222] Next, a protective film is adhered to the upper and lower main surfaces of the insulating sheet via an adhesive layer. Then, in (b), a plurality of through holes are formed in the insulating sheet on which the resin film is adhered via the adhesive layer on both the upper and lower surfaces. The through holes are formed, for example, by irradiating the insulating sheet on which the resin film is adhered via the adhesive layer on both the upper and lower surfaces with a laser from the upper surface side.
[0223] Next, in (c), conductive paste is filled into the through-hole. One method for filling the through-hole with conductive paste is, for example, supplying the conductive paste onto a resin film on the upper surface side and then sliding it onto the film while scraping the paste with a hard rubber scraper. In this case, the resin film on the upper surface side acts as a mask for filling the through-hole with conductive paste.
[0224] An exemplary conductive paste contains metal powder composed of an alloy of tin, silver, bismuth, and copper, and triazine thermosetting resins such as triallyl cyanurate, triallyl isocyanurate, triglycidyl isocyanurate, and tris(2-hydroxyethyl) isocyanurate. The conductive paste exhibits conductivity through the contact between the aforementioned metal powders. The content of the aforementioned metal powder relative to the total amount of the conductive paste is preferably 80-95% by mass. If the content of metal powder is 80% by mass or more, the metal powders can easily contact each other, which can reduce resistivity. If it is 95% by mass or less, the viscosity of the conductive paste containing the metal powder and the triazine thermosetting resin is moderate, thus providing good filling properties.
[0225] Next, in (d), the resin film, along with the adhesive layer, is peeled off from both main surfaces of the insulating sheet.
[0226] Next, in (e), a transfer sheet is prepared, the transfer sheet comprising: an adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and a wiring conductor partially disposed on the UV-curable adhesive layer. The wiring conductor is peelably held on the UV-curable adhesive layer.
[0227] The transfer sheet is overlapped with at least one main surface of the insulating sheet in such a way that the ends of the wiring conductor and the conductive paste are grounded, and they are pressed together, for example, at a temperature of 100 to 150°C and a pressure of 0.2 to 1.0 MPa, so that the wiring conductor is embedded in the main surface of the insulating sheet.
[0228] Next, in (f), the transfer sheet is UV-cured by UV irradiation from the substrate layer side of the transfer sheet. After the UV-cured adhesive layer is cured, the substrate layer of the transfer sheet and the cured adhesive layer are removed from the insulating sheet and the wiring conductor, thereby transferring the wiring conductor in a manner that leaves it on the insulating sheet. Through these operations, multiple insulating sheets with the wiring conductor transferred are manufactured.
[0229] Next, in (g), the above-mentioned multiple insulating sheets are pressed and heated in a prescribed configuration with the upper and lower parts overlapping, so that the thermosetting resin of the insulating sheets and the thermosetting resin of the conductive paste are thermally cured, thereby obtaining an insulating layer and wiring conductors that are alternately laminated as a cured product of a heat-resistant fiber substrate impregnated with a thermosetting resin composition, and the wiring conductors located on the upper and lower parts sandwiching the insulating layer are electrically connected to each other through conductor posts provided in through holes formed in the insulating layer.
[0230] A method for manufacturing a wiring board according to one embodiment includes: providing a sealing layer on a surface of a transfer sheet where wiring conductors are disposed. The method for manufacturing a wiring board according to another embodiment further includes: providing a conductive path through the sealing layer such that a portion of the wiring conductor is connected to a conductive path.
[0231] As a method for setting a sealing layer, one example is to supply a thermosetting resin composition, such as a particulate epoxy resin composition, to the upper surface of a transfer sheet in a molten state in order to cover a wiring conductor, and then compress and mold the molten thermosetting resin composition.
[0232] As a method for setting a through-hole to penetrate the sealing layer, for example, a resist layer is provided in the sealing layer, the area where the through-hole is set is exposed by photolithography, the exposed area is removed by etching to form a through-hole, and a conductor post is formed in the through-hole.
[0233] <Adhesive Sheet>
[0234] The adhesive sheet has a substrate layer and a UV-curable adhesive layer disposed on the substrate layer.
[0235] (Substrate layer)
[0236] As the substrate layer, known inorganic substrates, as well as polymer sheets and polymer films, can be used without particular limitation. Examples of inorganic substrates include glass and glass cloth. Specific examples of polymer sheets and polymer films include polymer sheets and polymer films containing at least one of the following materials: crystalline polypropylene, amorphous polypropylene, high-density polyethylene, medium-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, low-density linear polyethylene, polybutene, polymethylpentene and other polyolefins, ethylene-vinyl acetate copolymers, ionically crosslinked polymer resins, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylic acid (random or alternating) copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, polyurethanes, polyethylene terephthalate, polyethylene naphthalate and other polyesters, polycarbonate, polyimide, polyetheretherketone, polyetherimide, polyamide, fully aromatic polyamide, polyphenylene sulfide, aromatic polyamide, fluoropolymers, polyvinyl chloride, polyvinylidene 1,1-dichloroethylene, cellulose resins, silicone resins and mixtures thereof containing plasticizers, and cured products obtained by crosslinking them by electron beam irradiation.
[0237] The substrate layer preferably has transparency, and its total light transmittance is preferably 70% or more, more preferably 80% or more. From the viewpoint of heat resistance, the substrate layer preferably contains at least one selected from polyethylene terephthalate, polyethylene naphthalate, polyamide, polyimide, and polyetheretherketone. In applications requiring flexibility, it is preferable to contain at least one selected from polyolefins and polyvinyl chloride.
[0238] The thickness of the substrate layer is preferably 5 to 500 μm, more preferably 5 to 100 μm, and even more preferably 5 to 50 μm. If the thickness of the substrate layer is 5 μm or more, wrinkles and twisting of the adhesive sheet are suppressed. Therefore, when the adhesive sheet is used as a transfer sheet, wire breakage is prevented, and workability is good. If the thickness of the substrate layer is 500 μm or less, peelability is good. Furthermore, when the adhesive sheet is used as a transfer sheet, lamination and positioning accuracy during the transfer process are also good.
[0239] (UV-curable adhesive layer)
[0240] The UV-curable adhesive layer is a thermosetting product of the adhesive composition described below. Because the adhesive layer is UV-curable, the adhesive sheet protects the surface of electronic components or provides good adhesion during temporary fixing, and can be easily peeled off from the substrate without leaving adhesive residue after the adhesive sheet is no longer needed. Because the adhesive layer is UV-curable, the adhesive sheet maintains good adhesion during the formation of wiring conductors until they are transferred to the substrate, resulting in excellent dimensional accuracy of the wiring conductors and positioning accuracy during transfer. After the wiring conductors are transferred, UV irradiation reduces the adhesive strength of the adhesive layer, allowing for easy peeling off from the substrate without leaving adhesive residue.
[0241] There are no particular limitations on the heat-curing conditions. Generally, after applying the adhesive composition, it is heat-cured by drying and / or curing. The drying conditions are typically 25–180°C, preferably 60–150°C, for 1–20 minutes, preferably 1–10 minutes. By drying within the above range, solvents can be removed if the adhesive composition contains solvents. There are no particular limitations on the conditions for curing the dried sheet in an oven for a certain period, typically 25–100°C, preferably 30–80°C, for 1–30 days, preferably 1–14 days. By curing under these conditions, the gel content of the adhesive layer can be adjusted to the desired range.
[0242] The thickness of the UV-curable adhesive layer is preferably 1 μm or more, more preferably 5 μm or more. The thickness of the UV-curable adhesive layer is preferably 300 μm or less, more preferably 100 μm or less, and even more preferably 30 μm or less. The thickness of the UV-curable adhesive layer is preferably 1 to 300 μm, more preferably 5 to 100 μm, and even more preferably 5 to 30 μm. If the thickness of the UV-curable adhesive layer is 1 μm or more, the UV-curable adhesive layer has sufficient adhesive force, wrinkles and twisting of the adhesive sheet are suppressed, and workability is good. Therefore, when the adhesive sheet is used as a transfer sheet, wire breakage of the wiring conductor is prevented. If the thickness of the UV-curable adhesive layer is 1 μm or more, when the adhesive sheet is used as a transfer sheet, poor transfer is suppressed. If the thickness of the UV-curable adhesive layer is 300 μm or less, transfer of the adhesive layer to the substrate can be suppressed. If the thickness of the UV-curable adhesive layer is 300 μm or less, when the adhesive sheet is used as a transfer sheet, lamination and positioning accuracy in the transfer process are good.
[0243] <Adhesive Composition>
[0244] The adhesive composition comprises a (meth)acrylic resin (A), which contains structural units of formulas (1) to (3) and optionally contains structural units of formula (4).
[0245]
[0246] (In equation (1), R) 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
[0247] The adhesive composition preferably contains, in addition to (meth)acrylic resin (A), a photopolymerization initiator (B) and a crosslinking agent (C). By containing the photopolymerization initiator (B) and the crosslinking agent (C), thermosetting and photocuring properties can be imparted.
[0248] ((Meth)acrylic resin (A))
[0249] [Structural unit of equation (1)]
[0250] (Meth)acrylic resin (A) contains structural units of the following formula (1). The structural units of formula (1) contribute to the imparting of adhesive strength.
[0251]
[0252] In equation (1), R 1 R represents a hydrogen atom or a methyl group. 2 R indicates an alkyl group having 1 to 20 carbon atoms. 2Preferably, it is a straight-chain or branched alkyl group, more preferably a straight-chain or branched alkyl group with 1 to 10 carbon atoms, and even more preferably a straight-chain or branched alkyl group with 4 to 8 carbon atoms. The structural unit of formula (1) may not be a single type. The R of each structural unit... 1 They can be different for each structural unit, and the R value can vary. 2 They can also be different.
[0253] Specific examples of monomers forming the structural unit of formula (1) include methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, decyl methacrylate, and other alkyl methacrylates. Among these, from the viewpoint of ease of synthesis of the methacrylate resin (A), adhesive properties, and peelability after UV irradiation, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate are preferred, and from the viewpoint of peelability after UV irradiation, 2-ethylhexyl methacrylate is more preferred.
[0254] The individual units of the structural unit of formula (1) can be used alone or in combination with two or more types.
[0255] The proportion of the structural units of Formula (1) relative to all structural units of the (meth)acrylic resin (A) is preferably 50 to 99 mol%, more preferably 60 to 98 mol%, and even more preferably 70 to 95 mol%. If the proportion of structural units of Formula (1) is 50 mol% or more, sufficient adhesion to the adherend can be obtained before UV irradiation. If the proportion of structural units of Formula (1) is 99 mol% or less, sufficient proportions of structural units of Formulas (2) and (3) described later can be ensured, thus sufficient photocurability as an adhesive composition can be obtained, and consequently, the desired peelability after UV irradiation.
[0256] [Structural unit of equation (2)]
[0257] The (meth)acrylic resin (A) contains structural units of the following formula (2). Thus, the hydroxyl groups can be crosslinked with the crosslinking agent (C) to form a UV-curable adhesive layer by thermosetting. Furthermore, the adhesive composition can be given photocurability by the olefinic unsaturated groups introduced into the side chains, which reduce adhesive strength and improve peelability from the adhered objects after UV irradiation.
[0258]
[0259] In equation (2), R 3 R represents a hydrogen atom or a methyl group. 4This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the adjacent carbon atom. From the viewpoint of heat resistance, the carbon atom having the hydroxyl group preferably has one hydrogen atom, and the carbon atom having the residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid preferably has one or two hydrogen atoms. The structural unit of formula (2) may not be a single type. The R of each structural unit 3 They can be different for each structural unit, and the R value can vary. 4 They can also be different.
[0260] As a component of R 4 Specific examples of residues obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid include residues obtained by removing a hydrogen atom from the carboxyl group of unsaturated monocarboxylic acids such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, crotonic acid, propynic acid, cinnamic acid, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, monomethyl fumarate, and monoethyl itaconic acid. From the viewpoint of ease of synthesis of (meth)acrylic acid resin (A), residues obtained by removing a hydrogen atom from the carboxyl group of (meth)acrylic acid, i.e., (meth)acryloyloxy, are preferred.
[0261] As specific examples of structural units of equation (2), structural units of equation (2-1-1) and equation (2-1-2) can be given below.
[0262]
[0263] (In equation (2-1-1), R) 9 R represents a hydrogen atom or a methyl group. 10 R represents a binary linker base. 11 R 12 R 14 and R 15 Each independently represents an alkyl group having 1 to 6 hydrogen atoms or carbon atoms, R 13 R represents a single bond or a divalent linker. 16 This indicates a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group.
[0264] (In equation (2-1-2), R) 17 R represents a hydrogen atom or a methyl group. 18 R represents a binary linker base. 19 R 20 R 22 and R 23 Each independently represents an alkyl group having 1 to 6 hydrogen atoms or carbon atoms, R21 R represents a single bond or a divalent linker. 24 This indicates a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group.
[0265] In equation (2-1-1), R is... 10 Examples of divalent linkers include alkylene groups with 1 to 20 carbon atoms, and -R 55 -OR 56 -(where R is in the formula) 55 and R 56 Each independently represents an alkylene group having 1 to 10 carbon atoms. (e.g., as R) 10 Examples of alkylene groups with 1 to 20 carbon atoms include methylene, ethylene, and butylene. From the viewpoint of ensuring good adhesion to the adhered material, alkylene groups with 1 to 10 carbon atoms are preferred, and methylene and ethylene are more preferred. As R 55 and R 56 Examples of alkylene groups with 1 to 10 carbon atoms include methylene, ethylene, and butylene. From the viewpoint of photocurability, alkylene groups with 1 to 6 carbon atoms are preferred. As R 10 Preferably, it is an alkylene group having 1 to 10 carbon atoms and -R 55 -OR 56 -, more preferably methylene, ethylene, and -(CH2) n -O-(CH2) y -(n is an integer from 1 to 6, y is an integer from 1 to 2.). n is preferably an integer from 2 to 6, and y is preferably an integer from 1 to 2.
[0266] In equation (2-1-1), R 11 R 12 R 14 and R 15 Each can independently represent an alkyl group having 1 to 6 hydrogen atoms or carbon atoms. As R 11 R 12 R 14 and R 15 Alkyl groups having 1 to 6 carbon atoms can be exemplified by, for example, methyl. From a heat resistance perspective, R... 11 and R 12 Ideally, all atoms should be hydrogen atoms. From a heat resistance perspective, R... 14 Preferably, it contains hydrogen atoms or methyl groups. From the viewpoint of photocurability, R... 15 Hydrogen atoms are preferred.
[0267] In equation (2-1-1), R 13 This indicates a single bond or a divalent linker. Examples of divalent linkers include alkylene groups with 1 to 20 carbon atoms, and -R...57 -OR 58 -(where R is in the formula) 57 and R 58 Each can independently represent an alkylene group having 1 to 10 carbon atoms. (-R) 59 -CO-OR 60 -CO-、-R 61 -CO-OR 62 -(where R is in the formula) 59 ~R 62 Each independently represents an alkylene group having 1 to 10 carbon atoms. (e.g., as R) 13 Alkylenes, representing 1 to 20 carbon atoms, include methylene, ethylene, and butylene. As R... 13 From the viewpoint of photocurability, it is preferred to have a single bond and an alkylene group having 1 to 6 carbon atoms, and more preferably a single bond.
[0268] In equation (2-1-1), R 16 Represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group. As R... 16 Alkyl groups having 1 to 6 carbon atoms can be exemplified by, for example, methyl and ethyl. From the viewpoint of photocurability, R... 16 Hydrogen atoms are preferred.
[0269] In equation (2-1-2), R 18 ~R 24 Specific examples and suitable examples are related to R in equation (2-1-1). 10 ~R 16 The same applies to each other.
[0270] As a method for forming a structural unit of formula (2-1-1) or formula (2-1-2), specifically, an example is a method in which a structural unit of formula (4-1) is introduced, followed by reacting the carboxyl group of an unsaturated monocarboxylic acid with an epoxy group of formula (4-1) to introduce a residue obtained by removing a hydrogen atom from the carboxyl group of the unsaturated monocarboxylic acid. The monomers forming the structural unit of formula (4-1) can be used alone or in combination with two or more monomers, and the unsaturated monocarboxylic acids undergoing the reaction can also be used alone or in combination with two or more monomers.
[0271] As a specific example of the structural unit of equation (2), the structural unit of equation (2-2) can also be given below.
[0272]
[0273] (In equation (2-2), R) 37 R represents a hydrogen atom or a methyl group. 38 R represents a single bond or a divalent linker. 39 R41 and R 42 Each independently represents an alkyl group having 1 to 6 hydrogen atoms or carbon atoms, R 40 R represents a single bond or a divalent linker. 43 The symbol represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group, and X1 represents a saturated hydrocarbon ring.
[0274] As R 38 Examples of divalent linkers include, for example, alkylene groups having 1 to 20 carbon atoms, and -R 63 -OR 64 -(where R is in the formula) 63 and R 64 Each can independently represent an alkylene group having 1 to 10 carbon atoms. (-R) 65 -O-(where R is the formula) 65 Represents alkylene groups with 1 to 10 carbon atoms. (e.g., -COO- and combinations thereof.) As constituents of R... 38 Alkylenes having 1 to 20 carbon atoms, examples of which include methylene, ethylene, butylene, and cyclohexylene. From the viewpoint of adhesion to the adhered material, alkylenes having 1 to 10 carbon atoms are preferred, and methylene and ethylene are more preferred. As R 63 and R 64 Examples of alkylene groups with 1 to 10 carbon atoms include methylene, ethylene, and butylene. From the viewpoint of photocurability, alkylene groups with 1 to 6 carbon atoms are preferred. As R 65 Examples of alkylene groups with 1 to 10 carbon atoms include methylene, ethylene, and butylene. From the viewpoint of photocurability, alkylene groups with 1 to 6 carbon atoms are preferred. As R 38 Preferably, it consists of a single bond, an alkylene group having 1 to 10 carbon atoms, and -R. 65 -O-, more preferably a single bond, methylene, ethylene, and -(CH2). m -O- (m is an integer from 1 to 3.)
[0275] In equation (2-2), R 39 R 41 and R 42 Each can independently represent an alkyl group having 1 to 6 hydrogen atoms or carbon atoms. As R 39 R 41 and R 42 Alkyl groups having 1 to 6 carbon atoms can be exemplified by, for example, methyl. From a heat resistance perspective, R... 39 Preferably, it contains hydrogen atoms. From a heat resistance perspective, R... 41 Preferably, it contains hydrogen atoms or methyl groups. From the viewpoint of photocurability, R... 42Hydrogen atoms are preferred.
[0276] In equation (2-2), R 40 and R 43 Specific examples and suitable examples are related to R in equation (2-1-1). 13 and R 16 The same applies to each other.
[0277] In formula (2-2), X1 represents a saturated hydrocarbon ring. The saturated hydrocarbon ring preferably has 4 to 20 carbon atoms, more preferably 5 to 10, and even more preferably 5 to 8. The saturated hydrocarbon ring can be a monocyclic or fused ring. Cyclohexyl, cyclopentyl, and tricyclodecyl are preferred as saturated hydrocarbon rings.
[0278] From the perspective of heat resistance, the structural unit of formula (2) preferably includes the structural unit of formula (2-2).
[0279] Specifically, as a method for forming the structural unit of formula (2-2), an example is to introduce the structural unit of formula (4-2) described later, and then react the carboxyl group of the unsaturated monocarboxylic acid with the epoxy group of formula (4-2) to introduce a residue obtained by removing a hydrogen atom from the carboxyl group of the unsaturated monocarboxylic acid. The monomers forming the structural unit of formula (4-2) can be used alone or in combination with two or more types, and the unsaturated monocarboxylic acids undergoing the reaction can also be used alone or in combination with two or more types.
[0280] The proportion of the structural unit of formula (2) relative to all structural units of (meth)acrylic resin (A) is preferably 0.1 to 40 mol%, more preferably 0.5 to 18 mol%, and even more preferably 1 to 15 mol%. If the structural unit of formula (2) is 0.1 mol% or more, the thermosetting properties of the adhesive composition are sufficient. As a result, sufficient adhesion to the adhered objects and cohesive force of the adhesive composition are obtained. If the structural unit of formula (2) is 40 mol% or less, a sufficient proportion of the structural unit of formula (1) can be ensured, and good adhesion is obtained.
[0281] [Structural unit of equation (3)]
[0282] (Meth)acrylic resin (A) contains structural units of the following formula (3). The adhesive composition is given photocurability by introducing two olefinic unsaturated groups into the side chain, thereby reducing the adhesive strength of the adhesive layer after UV irradiation and improving the peelability from the adhered object.
[0283]
[0284] In equation (3), R 5 R represents a hydrogen atom or a methyl group. 6This refers to a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. From the viewpoint of heat resistance, each carbon atom having a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid preferably has one or two hydrogen atoms. The structural unit of formula (3) may not be a single type. The R of each structural unit 5 They can be different for each structural unit, and the R value can vary. 6 They can also be different.
[0285] As a component of R 6 Specific examples of residues obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid include residues obtained by removing a hydrogen atom from the carboxyl group of unsaturated monocarboxylic acids such as (meth)acrylic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, crotonic acid, propynic acid, cinnamic acid, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, monomethyl fumarate, and monoethyl itaconic acid. From the viewpoint of ease of synthesis of (meth)acrylic acid resin (A), residues obtained by removing a hydrogen atom from the carboxyl group of (meth)acrylic acid, i.e., (meth)acryloyloxy, are preferred.
[0286] As a specific example of the structural unit of equation (3), the structural unit of equation (3-1) can be given below.
[0287]
[0288] (In equation (3-1), R) 25 R represents a hydrogen atom or a methyl group. 26 R represents a binary linker base. 27 R 28 R 30 R 31 R 34 and R 35 Each independently represents an alkyl group having 1 to 6 hydrogen atoms or carbon atoms, R 29 and R 33 Each independently represents a single bond or a divalent linker, R 32 and R 36 Each of these can independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group.
[0289] In equation (3-1), R 26 ~R 32 Specific examples and suitable examples are related to R in equation (2-1-1). 10 ~R 16 Similarly, in equation (3-1), R 33 ~R36 Specific examples and suitable examples are related to R in equation (2-1-1). 13 ~R 16 The same applies to each other.
[0290] Specifically, as a method for forming the structural unit of formula (3-1), an example is to react an unsaturated monocarboxylic anhydride with the hydroxyl group of the structural unit of formula (2-1-1) or formula (2-1-2) to introduce a residue obtained by removing a hydrogen atom from the carboxyl group of the unsaturated monocarboxylic acid. The unsaturated monocarboxylic anhydride used in the reaction can be used alone or in combination with two or more. (Meth)acrylic anhydride is an example of an unsaturated monocarboxylic anhydride.
[0291] As a specific example of the structural unit of equation (3), the structural unit of equation (3-2) can also be given below.
[0292]
[0293] (In equation (3-2), R) 44 R represents a hydrogen atom or a methyl group. 45 R represents a single bond or a divalent linker. 46 R 48 R 49 R 52 and R 53 Each independently represents an alkyl group having 1 to 6 hydrogen atoms or carbon atoms, R 47 and R 51 Each independently represents a single bond or a divalent linker, R 50 and R 54 Each of these elements independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, -COOR (where R represents an alkyl group having 1 to 6 carbon atoms), or a phenyl group, and X2 represents a saturated hydrocarbon ring.
[0294] In equation (3-2), R 45 ~R 50 Specific examples and suitable examples are related to R in equation (2-2). 38 ~R 43 Similarly, in equation (3-2), R 51 ~R 54 Specific examples and suitable examples are related to R in equation (2-2). 40 ~R 43 Similarly, in equation (3-2), the specific examples and suitable examples of X2 are the same as those of X1 in equation (2-2).
[0295] Specifically, as a method for forming the structural unit of formula (3-2), an example is to react an unsaturated monocarboxylic anhydride with the hydroxyl group of the structural unit of formula (2-2) above, thereby introducing a residue obtained by removing a hydrogen atom from the carboxyl group of the unsaturated monocarboxylic acid. The unsaturated monocarboxylic anhydride used in the reaction can be used alone or in combination with two or more. (Meth)acrylic anhydride is an example of an unsaturated monocarboxylic anhydride.
[0296] The proportion of the structural unit of formula (3) relative to all structural units of (meth)acrylic resin (A) is preferably 0.1 to 30 mol%, more preferably 0.2 to 28 mol%, and even more preferably 0.5 to 26 mol%. If the structural unit of formula (3) is 0.1 mol% or more, a sufficient improvement in photocurability is achieved. As a result, the adhesive strength of the adhesive layer can be sufficiently reduced under UV irradiation, improving the peelability of the adhered object. If the structural unit of formula (3) is 30 mol% or less, good adhesion is achieved.
[0297] [Structural unit of equation (4)]
[0298] (Meth)acrylic resin (A) may contain structural units of formula (4) below. From the viewpoint of reducing residual monomers during the synthesis of (meth)acrylic resin (A), namely, residual unsaturated monocarboxylic acids and unsaturated monocarboxylic anhydrides used to introduce the structural units of formulas (2) and (3) above, it is preferable to contain a certain amount of structural units of formula (4) below. On the other hand, from the viewpoint of reducing the degradation of the adhesive composition over time, it is preferable to minimize the content of structural units of formula (4).
[0299]
[0300] In equation (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group. The structural unit in formula (4) may not be a single type. The R of each structural unit... 7 They can be different for each structural unit, and the R value can vary. 8 They can also be different.
[0301] As specific examples of structural units of equation (4), structural units of equation (4-1) and equation (4-2) can be given below.
[0302]
[0303] (In equation (4-1), R) 66 R represents a hydrogen atom or a methyl group. 67 R represents a binary linker base. 68 and R 69Each of the following independently represents an alkyl group having 1 to 6 carbon atoms, in formula (4-2), R 70 R represents a hydrogen atom or a methyl group. 71 R represents a single bond or a divalent linker. 72 This indicates an alicyclic epoxy group.
[0304] In equation (4-1), R 67 R 68 and R 69 Specific examples and suitable examples are related to R in equation (2-1-1). 10 R 11 and R 12 The same applies to each other.
[0305] Specific examples of monomers forming structural units of formula (4-1) include glycidyl (meth)acrylate and hydroxybutyl (meth)acrylate glycidyl ether. From the viewpoint of the ease of reaction with unsaturated monocarboxylic acids when forming structural units of formulas (2-1-1), (2-1-2), and (3-1), glycidyl (meth)acrylate and hydroxybutyl (meth)acrylate glycidyl ether are preferred.
[0306] The structural unit of formula (4-1) can be used alone or in combination with two or more types.
[0307] In equation (4-2), R 71 Specific examples and suitable examples are related to R in equation (2-2). 38 same.
[0308] In equation (4-2), R 72 The term "alicyclic epoxy group" can be represented by specific examples such as 3,4-epoxycyclohexyl, epoxycyclopentyl, and 3,4-epoxytricyclic [5.2.1.0]. 2,6 [Kephalogen, etc.]
[0309] Specific examples of monomers that form the structural unit of formula (4-2) include methyl 3,4-epoxycyclohexyl methacrylate (e.g., Daicel Co., Ltd., Cyclomer A200, and M100), and 3,4-epoxytricyclic acrylate [5.2.1.0]. 2,6[4-2] Decanoyloxyethyl ester, (meth)acrylates having a 3,4-epoxycyclohexyl lactone adduct, mono(meth)acrylates of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, epoxides of dicyclopentenyl(meth)acrylate, and epoxides of dicyclopentenyloxyethyl(meth)acrylate, etc. Among these, from the viewpoint of the ease of reaction with unsaturated monocarboxylic acids when forming structural units of formulas (2-2) and (3-2), 3,4-epoxycyclohexylmethyl(meth)acrylate is preferred. Monomers forming structural units of formula (4-2) can be used alone or in combination of two or more.
[0310] The proportion of the structural unit of formula (4) relative to all structural units of (meth)acrylic resin (A) is preferably 0 to 10 mol%, more preferably 0 to 5 mol%, and even more preferably 0 to 1 mol%. If the structural unit of formula (4) is less than 10 mol%, sufficient heat resistance and storage stability are obtained, the adhesive force is sufficiently reduced after UV irradiation, and it can be peeled off without contamination of the adhered material.
[0311] Using all structural units of (meth)acrylic resin (A) as a reference, the total proportion of structural units of formulas (2) to (4) is preferably 1 mol% or more, more preferably 2 mol% or more, and even more preferably 5 mol% or more. Using all structural units of (meth)acrylic resin (A) as a reference, the total proportion of structural units of formulas (2) to (4) is preferably 50 mol% or less, more preferably 40 mol% or less, and even more preferably 30 mol% or less. Using all structural units of (meth)acrylic resin (A) as a reference, the total proportion of structural units of formulas (2) to (4) is preferably 1 to 50 mol%, more preferably 2 to 40 mol%, and even more preferably 5 to 30 mol%. If the total proportion of structural units of formulas (2) to (4) is 1 mol% or more, sufficient photocurability and the desired peelability after UV irradiation can be obtained. If the total proportion of structural units of formulas (2) to (4) is 50 mol% or less, the adhesive force as an adhesive sheet is good.
[0312] The total proportion of the structural units of formulas (2) and (3) relative to the total proportion of the structural units of formulas (2) to (4) is preferably 50 mol% or more, more preferably 55 mol% or more, and even more preferably 60 mol% or more. The total proportion of the structural units of formulas (2) and (3) relative to the total proportion of the structural units of formulas (2) to (4) is preferably 100 mol% or less, more preferably 95 mol% or less, and even more preferably 90 mol% or less. The total proportion of the structural units of formulas (2) and (3) relative to the total proportion of the structural units of formulas (2) to (4) is preferably 50 to 100 mol%, more preferably 55 to 95 mol%, and even more preferably 60 to 90 mol%. If the total proportion of the structural units of formulas (2) and (3) is 50 mol% or more, sufficient photocurability and the desired peelability after UV irradiation can be obtained.
[0313] [Physical properties of (meth)acrylic resin (A)]
[0314] The olefin unsaturated group equivalent of the (meth)acrylic resin (A) is preferably 350 g / mol or more, more preferably 400 g / mol or more, and even more preferably 450 g / mol or more. The olefin unsaturated group equivalent of the (meth)acrylic resin (A) is preferably 4000 g / mol or less, more preferably 3000 g / mol or less, and even more preferably 2000 g / mol or less. The olefin unsaturated group equivalent of the (meth)acrylic resin (A) is preferably 350 to 4000 g / mol, more preferably 400 to 3000 g / mol, and even more preferably 450 to 2000 g / mol. If the olefin unsaturated group equivalent is 350 g / mol or more, the adhesive strength as an adhesive sheet is good. If the olefin unsaturated group equivalent is 4000 g / mol or less, the adhesion before UV irradiation is good, and sufficient photocurability and the desired peelability after UV irradiation can be obtained.
[0315] In this specification, the term "ene unsaturated group equivalent" of a (meth)acrylic resin refers to the mass (g / mol) of (meth)acrylic resin per mole of ene unsaturated bonds. The ene unsaturated group equivalent of a (meth)acrylic resin is calculated from the amount of halogen bound to the (meth)acrylic resin. The amount of halogen bound to the (meth)acrylic resin is evaluated according to JIS K 0070:1992.
[0316] The glass transition temperature (Tg) of the (meth)acrylic resin (A) is preferably -80°C or higher, more preferably -70°C or higher, and even more preferably -65°C or higher. The glass transition temperature (Tg) of the (meth)acrylic resin (A) is preferably 0°C or lower, more preferably -10°C or lower, and even more preferably -20°C or lower. The glass transition temperature (Tg) of the (meth)acrylic resin (A) is preferably -80°C to 0°C, more preferably -70°C to -10°C, and even more preferably -65°C to -20°C. If the glass transition temperature is -80°C or higher, the adhesive strength as an adhesive sheet is good. If the glass transition temperature is 0°C or lower, the adhesion before UV irradiation is good.
[0317] In this specification, "glass transition temperature (Tg)" refers to the endothermic onset temperature caused by the glass transition, measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min, changing the temperature of the sample from -100°C to 200°C. If more than two endothermic onset temperatures are observed, Tg is the simple average of these two or more endothermic onset temperatures.
[0318] The weight-average molecular weight of the (meth)acrylic resin (A) is preferably 100,000 or more, more preferably 200,000 or more, and even more preferably 300,000 or more. The weight-average molecular weight of the (meth)acrylic resin (A) is preferably 1,000,000 or less, more preferably 900,000 or less, and even more preferably 800,000 or less. The weight-average molecular weight of the (meth)acrylic resin (A) is preferably 100,000 to 1,000,000, more preferably 200,000 to 900,000, and even more preferably 300,000 to 800,000. If the weight-average molecular weight is 100,000 or more, the agglomeration before UV irradiation is good. If the weight-average molecular weight is 1,000,000 or less, the workability during coating is good.
[0319] In this specification, "weight-average molecular weight" is a value determined using gel permeation chromatography (GPC) at room temperature (23°C) under the following conditions, using a standard polystyrene standard curve.
[0320] Device: Shodex (trademark) GPC-101 (Raykin Co., Ltd.)
[0321] Column: Shodex (trademark) LF-804 (Raykin Co., Ltd.)
[0322] Column temperature: 40℃
[0323] Sample: 0.2% by mass tetrahydrofuran solution of the sample
[0324] Flow rate: 1 mL / min
[0325] Eluent: Tetrahydrofuran
[0326] Detector: Shodex RI-71S (trademark)
[0327] The hydroxyl value of the (meth)acrylic resin (A) is preferably 1 mg KOH / g or more, more preferably 2 mg KOH / g or more, and even more preferably 3 mg KOH / g or more. The hydroxyl value of the (meth)acrylic resin (A) is preferably 60 mg KOH / g or less, more preferably 50 mg KOH / g or less, and even more preferably 40 mg KOH / g or less. The hydroxyl value of the (meth)acrylic resin (A) is preferably 1 to 60 mg KOH / g, more preferably 2 to 50 mg KOH / g, and even more preferably 3 to 40 mg KOH / g. If the hydroxyl value is 1 mg KOH / g or more, the desired cohesive strength is obtained when reacting with the crosslinking agent (C). If the hydroxyl value is 60 mg KOH / g or less, the peelability after UV irradiation is good.
[0328] In this specification, the hydroxyl value is defined as the mass (mg) of potassium hydroxide required to neutralize acetic acid bound to the hydroxyl group when 1g of resin is acetylated, according to JIS K 0070:1992.
[0329] [Method for manufacturing (meth)acrylic resin (A)]
[0330] (Meth)acrylic resin (A) is obtained, for example, through the following process: Step (i) is the polymerization of monomers with epoxy groups with other monomers to obtain copolymers. In the step (ii) of adding unsaturated monocarboxylic acids to the epoxy groups of the copolymer; and In step (iii), an unsaturated monocarboxylic acid anhydride is generated by the addition reaction of the epoxy group through the addition reaction described in step (ii), and an unsaturated monocarboxylic acid derived from the free unsaturated monocarboxylic acid anhydride is added to the remaining epoxy group.
[0331] [Step (i) of polymerizing monomers to obtain copolymers]
[0332] As polymerization methods, solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and alternating copolymerization can be used. Among these polymerization methods, solution polymerization is preferred in terms of the ease of reaction, considering the addition reactions in steps (ii) and (iii).
[0333] As monomers, alkyl (meth)acrylates, epoxy-containing (meth)acrylates, and alternatively other monomers may be used.
[0334] (alkyl methacrylate)
[0335] As for alkyl methacrylates, there are no particular limitations on the monomers that form the structural unit of formula (1). Specific examples include methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, and decyl methacrylate. Among these, from the viewpoint of ease of synthesis of the methacrylic resin (A), adhesive properties, and peelability after UV irradiation, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate are preferred, and from the viewpoint of peelability after UV irradiation, 2-ethylhexyl methacrylate is more preferred. Alkyl methacrylates can be used alone or in combination of two or more.
[0336] (Meth)acrylates containing epoxy groups)
[0337] As for (meth)acrylates containing epoxy groups, there are no particular limitations on the monomers that form the structural unit of formula (4). Specific examples include glycidyl (meth)acrylate, hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexyl methyl (meth)acrylate (e.g., Cyclomer A200 and M100, Daicel Co., Ltd.), and 3,4-epoxytricyclic acrylate [5.2.1.0]. 2,6 Decanoyl acrylate, (meth)acrylates having a 3,4-epoxycyclohexyl lactone adduct, mono(meth)acrylates of 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate, epoxides of dicyclopentenyl (meth)acrylate, and epoxides of dicyclopentenyl oxyethyl (meth)acrylate, etc. Among these, glycidyl (meth)acrylate, 3,4-epoxycyclohexyl methyl (meth)acrylate, and hydroxybutyl (meth)acrylate glycidyl ether are preferred from the viewpoint of ease of reaction with unsaturated monocarboxylic acids. (Meth)acrylates containing epoxy groups can be used alone or in combination of two or more.
[0338] (Other monomers)
[0339] As for other monomers, there are no particular limitations as long as they do not have a carboxyl group, form structural units other than those in formulas (1) to (4), and can copolymerize with the above-mentioned alkyl methacrylates and epoxy-containing methacrylates. Specifically, examples include methacrylates containing alicyclic rings, methacrylates containing aromatic rings, methacrylates containing hydroxyl groups, and methacrylates containing amide groups.
[0340] Examples of (meth)acrylates containing alicyclic rings include cyclohexyl (meth)acrylate, methylcyclohexyl (meth)acrylate, norbornyl (meth)acrylate, 5-ethyl norbornyl (meth)acrylate, isobornyl (meth)acrylate, and adamantyl (meth)acrylate.
[0341] Examples of (meth)acrylates containing aromatic rings include benzyl (meth)acrylate, triphenylmethyl (meth)acrylate, phenyl (meth)acrylate, cumyl (meth)acrylate, 4-phenoxyphenyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol mono(meth)acrylate, biphenoxyethyl (meth)acrylate, naphthyl (meth)acrylate, and anthracene (meth)acrylate.
[0342] Examples of hydroxyl-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.
[0343] Examples of (meth)acrylates containing amide groups include (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, and anthracene (meth)acrylamide.
[0344] The content of alkyl (meth)acrylate in all monomers is preferably 50-99 mol, more preferably 60-98 mol, and even more preferably 70-95 mol.
[0345] The content of epoxy-containing (meth)acrylate in all monomers is preferably 1 to 50 mol, more preferably 2 to 40 mol, and even more preferably 5 to 30 mol.
[0346] (Free radical polymerization initiator)
[0347] The polymerization is preferably carried out in the presence of a free radical polymerization initiator. Examples of free radical polymerization initiators include, for instance, conventional organic free radical polymerization initiators; specifically, examples include, 2,2'-azobis(isobutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylpentanitrile), 2,2'-azobis(2,4-dimethylpentanitrile), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-formonitrile), 2,2'-azobis(2, Azo polymerization initiators such as 4,4-trimethylpentane and dimethyl-2,2'-azobis(2-methylpropionate); and oil-soluble polymerization initiators such as benzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxide benzoate, dicumyl peroxide, 1,1-bis(tert-butylperoxide)-3,3,5-trimethylcyclohexane, and 1,1-bis(tert-butylperoxide)cyclododecane.
[0348] Free radical polymerization initiators can be used alone or in combination of two or more.
[0349] The amount of free radical polymerization initiator used relative to 100 parts by mass of the total monomer is preferably 0.001 to 5 parts by mass, more preferably 0.005 to 3 parts by mass, and even more preferably 0.01 to 1 part by mass.
[0350] (solvent)
[0351] Common solvents can be used as solvents for solution polymerization. Examples of solvents include esters such as ethyl acetate, propyl acetate, and butyl acetate; aromatic hydrocarbons such as toluene, xylene, and benzene; aliphatic hydrocarbons such as hexane and heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone; glycols such as ethylene glycol, propylene glycol, and dipropylene glycol; glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether; and glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate. Solvents can be used alone or in combination of two or more.
[0352] (Reaction conditions)
[0353] Although the polymerization reaction temperature depends on the type of free radical polymerization initiator used, it is typically 30°C to 130°C, preferably 40°C to 120°C, and more preferably 50°C to 110°C. Sufficient reaction rates can be obtained if the polymerization temperature is above 30°C.
[0354] Although the reaction time of polymerization depends on the type of monomer and free radical polymerization initiator used, it is typically 3 to 30 hours, preferably 4 to 20 hours, and more preferably 5 to 15 hours. If the reaction time is more than 3 hours, copolymers can be produced from monomers with an appropriate degree of polymerization, and if the reaction time is less than 30 hours, production can be carried out efficiently.
[0355] [In the process of adding unsaturated monocarboxylic acids to the epoxy groups of the copolymer (ii) and in the process of adding unsaturated monocarboxylic anhydrides (iii)]
[0356] Processes (ii) and (iii) can be performed sequentially or simultaneously. From the viewpoint of ease of operation, it is preferable to perform processes (ii) and (iii) simultaneously.
[0357] (Unsaturated monocarboxylic acids)
[0358] There is no particular limitation on the type of unsaturated monocarboxylic acid as long as it has an olefinic unsaturated group. Specific examples include (meth)acrylic acid, 2-(meth)acryloyloxyethyl succinic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, crotonic acid, propargyl acid, cinnamic acid, monomethyl maleate, monoethyl maleate, monoisopropyl maleate, monomethyl fumarate, and monoethyl itaconic acid. Among these, (meth)acrylic acid is preferred from the viewpoint of ease of synthesis of (meth)acrylic acid resin (A). Unsaturated monocarboxylic acids can be used alone or in combination of two or more.
[0359] (Unsaturated monocarboxylic anhydrides)
[0360] There are no particular limitations on unsaturated monocarboxylic anhydrides, as long as they contain an olefinic unsaturated group. A specific example is (meth)acrylic anhydride. Unsaturated monocarboxylic anhydrides can be used alone or in combination of two or more.
[0361] The addition rate of the unsaturated monocarboxylic acid to the epoxy groups derived from the epoxy-containing (meth)acrylate present in the copolymer is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. If the addition rate is 50% or more, good peelability is obtained after UV irradiation. From the viewpoint of heat resistance, a higher addition rate is preferred. In one embodiment, the addition rate of the unsaturated monocarboxylic acid to the epoxy groups derived from the epoxy-containing (meth)acrylate present in the copolymer is 100%. The upper limit of the addition rate can be, for example, 99% or 98%. The addition rate of the unsaturated monocarboxylic acid to the epoxy groups derived from the epoxy-containing (meth)acrylate present in the copolymer is calculated from the amount added.
[0362] Regarding the ratio of unsaturated monocarboxylic acid to unsaturated monocarboxylic acid anhydride, the unsaturated monocarboxylic acid is preferably 5–130 mol relative to 100 mol of unsaturated monocarboxylic acid anhydride, more preferably 10–120 mol, and even more preferably 15–110 mol. If the unsaturated monocarboxylic acid is less than 130 mol relative to 100 mol of unsaturated monocarboxylic acid anhydride, the adhesion to the adhered material is improved. If the unsaturated monocarboxylic acid is more than 5 mol relative to 100 mol of unsaturated monocarboxylic acid anhydride, the peelability after UV irradiation is improved.
[0363] (catalyst)
[0364] For the addition reactions in steps (ii) and (iii), known catalysts may be used as needed. Known substances may be used as catalysts without particular limitation; examples include triphenylphosphine, tris(p-tolyl)phosphine, and tris(2,6-dimethoxyphenyl)phosphine. Catalysts may be used alone or in combination of two or more.
[0365] When using a catalyst, the amount of catalyst used is preferably 2.5 to 10 mol relative to 100 mol of the epoxy-containing (meth)acrylate used in the production of the copolymer, more preferably 3.0 to 9.0 mol, and even more preferably 3.5 to 8.0 mol. If the amount of catalyst used is 2.5 mol or more, the addition reaction can be promoted. On the other hand, if the amount of catalyst used is 10 mol or less, gelation during the addition reaction can be suppressed.
[0366] (polymerization inhibitor)
[0367] For the addition reactions in steps (ii) and (iii), known polymerization inhibitors may be used as needed. Known substances may be used as polymerization inhibitors without particular limitation; examples include 4-methoxyphenol, hydroquinone, hydroquinone monomethyl ether, 2,6-di-tert-butylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), and phenothiazine. Polymerization inhibitors may be used alone or in combination of two or more.
[0368] When using a polymerization inhibitor, the amount of inhibitor used is preferably 0.005 to 5 parts by mass relative to 100 parts by mass of the copolymer, more preferably 0.03 to 3 parts by mass, and even more preferably 0.05 to 1.5 parts by mass. If the amount of the polymerization inhibitor used is 0.005 parts by mass or more, gelation during the addition reaction can be prevented. On the other hand, if the amount of the polymerization inhibitor used is 5 parts by mass or less, sufficient exposure sensitivity of the (meth)acrylic resin (A) under UV irradiation is obtained.
[0369] (solvent)
[0370] As a solvent, a general solvent can be used. For example, the same substance used in the solution polymerization of step (i) can be used. Alcohols such as toluene or 1-methoxy-2-propanol, which readily undergo chain transfer reactions, can also be used. Solvents can be used alone or in combination of two or more.
[0371] (Reaction conditions)
[0372] The addition reaction temperature is preferably 25°C to 130°C, particularly preferably 40°C to 120°C. A sufficient reaction rate can be obtained if the addition reaction temperature is above 25°C. If the addition reaction temperature is below 130°C, cross-linking of the double bonds due to heat-induced free radical polymerization can be prevented, thus avoiding the formation of gels. The addition reaction time is preferably 2 to 24 hours, more preferably 2 to 12 hours.
[0373] During addition reactions, a gas with polymerization inhibitory effects can be introduced into the reaction system. By introducing a gas with polymerization inhibitory effects into the reaction system, gelation during the addition reaction can be prevented.
[0374] Gases that have an inhibitory effect on polymerization include gases containing oxygen in amounts that do not fall into the explosive range of substances within the system, such as air.
[0375] If a gas with a polymerization inhibitor is used in combination with a polymerization inhibitor, the amount of polymerization inhibitor used can be reduced or the polymerization inhibitory effect can be improved, which is therefore a better approach.
[0376] (Photopolymerization initiator (B))
[0377] Examples of photopolymerization initiators (B) include, for example, benzophenone, benzoin, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminoacetophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, michalcone, benzoin methyl ether, and benzoin. Carbonyl-based photopolymerization initiators such as isobutyl ether, benzoin-n-butyl ether, benzoylmethyl ketal, 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, methyl benzoyl carboxylate, 4'-dimethylaminoacetophenone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one.
[0378] Examples of photopolymerization initiators (B) include sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethylthiuram disulfide, and tetramethylammonium monosulfide; acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfonyl chloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.
[0379] Among these photopolymerization initiators (B), carbonyl photopolymerization initiators and acylphosphine oxides are preferred in terms of solubility in the adhesive composition, and more preferably at least one selected from 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl diphenylphosphine oxide.
[0380] Photopolymerization initiator (B) can be used alone or in combination of two or more.
[0381] The photopolymerization initiator (B) is preferably 0.1 to 5.0 parts by weight, more preferably 0.5 to 2.0 parts by weight, relative to 100 parts by weight of the (meth)acrylic resin (A). If the content of the photopolymerization initiator (B) relative to 100 parts by weight of the (meth)acrylic resin (A) is 0.1 parts by weight or more, the UV-curable adhesive layer can be cured at a sufficiently fast curing speed under UV irradiation, thus resulting in sufficiently low adhesive strength of the adhesive layer after UV irradiation. If the content of the photopolymerization initiator (B) relative to 100 parts by weight of the (meth)acrylic resin (A) is 5.0 parts by weight or less, when an adhesive sheet having a UV-curable adhesive layer, which is a thermosetting component of the adhesive composition, is adhered to an adherend and then peeled off, adhesive residue is less likely to remain on the adherend. Even if the content of photopolymerization initiator (B) exceeds 5.0 parts by mass relative to 100 parts by mass of (meth)acrylic resin (A), no effect commensurate with the content of photopolymerization initiator (B) is observed. Therefore, by keeping the content at 5.0 parts by mass or less, the adhesive composition can be manufactured economically.
[0382] <Crosslinking agent (C)>
[0383] The crosslinking agent (C) is a compound without olefinic unsaturated bonds and has two or more functional groups that react with the hydroxyl groups contained in the (meth)acrylic resin (A). Through the crosslinking agent (C), a good balance is achieved between the adhesive strength before and after UV irradiation.
[0384] Examples of functional groups that are reactive to hydroxyl groups include isocyanate groups, epoxy groups, carboxyl groups, acid anhydride groups, and aziridinyl groups. However, from the viewpoint of reactivity, isocyanate groups and epoxy groups are preferred, and isocyanate groups are particularly preferred.
[0385] Examples of crosslinking agents (C) include, for example, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, hydrogenated toluene diisocyanate, 1,3-phenylenedimethylene diisocyanate, 1,4-phenylenedimethylene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, isocyanurate forms of 1,6-hexanediisocyanate, tetramethylphenylenedimethylene diisocyanate, 1,5-naphthalene diisocyanate, and toluene diisocyanate of trimethylolpropane. Additives, trimethylolpropane phenyl diisocyanate adduct, triphenylmethane triisocyanate, methylene bis(4-phenylmethane) triisocyanate and other polyisocyanates; 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, bisphenol A-epimerol type epoxy resin, N,N'-[1,3-phenylenebis(methylene)]bis[bis(ethylene oxide-2-ylmethyl)amine], ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, 1 Polyepoxides such as 6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether; N,N'-diphenylmethane-4,4'-bis(1-aziridinyl carboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinyl carboxamide), ethylene glycol-bis-[3-(2-aziridinyl)propionate], trimethylolpropane-tris[3-(2-aziridinyl)propionate], tri... Aziridine compounds such as hydroxymethylpropane-tris[3-(1-aziridinyl)propionate], trimethylolpropane-tris[3-(2-methyl-1-aziridinyl)propionate], tetramethylolmethane-tris[3-(2-aziridinyl)propionate], pentaerythritol-tris[3-(1-aziridinyl)propionate]; and melamine compounds such as hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexabutoxymethylmelamine, hexapentyloxymethylmelamine, and hexahexyloxymethylmelamine.
[0386] Among these crosslinking agents (C), considering their good reactivity with (meth)acrylic resins (A), at least one selected from polyisocyanates and polyepoxides is preferred, with polyisocyanates being more preferred.
[0387] Crosslinking agent (C) can be used alone or in combination of two or more.
[0388] The crosslinking agent (C) is preferably 0.1 to 30 parts by weight relative to 100 parts by weight of the (meth)acrylic resin (A), more preferably 0.1 to 20 parts by weight, further preferably 0.1 to 10 parts by weight, and even more preferably 0.1 to 5 parts by weight. If the content of the crosslinking agent (C) relative to 100 parts by weight of the (meth)acrylic resin (A) is 0.1 parts by weight or more, a crosslinking structure with the (meth)acrylic resin (A) is fully formed upon heating, resulting in good strength of the UV-curable adhesive layer before UV irradiation. If the content of the crosslinking agent (C) relative to 100 parts by weight of the (meth)acrylic resin (A) is 30 parts by weight or less, the adhesive force of the UV-curable adhesive layer before UV irradiation is good.
[0389] (Other ingredients)
[0390] The adhesive composition may contain other components besides (meth)acrylic resin (A), photopolymerization initiator (B), and crosslinking agent (C), as needed. Other components include, for example, tackifiers, solvents, and various additives.
[0391] (Thickening agent)
[0392] As a tackifier, conventionally known substances can be used without particular limitation. Examples of tackifiers include terpene-based tackifying resins, phenolic tackifying resins, rosin-based tackifying resins, aliphatic petroleum resins, aromatic petroleum resins, copolymer petroleum resins, alicyclic petroleum resins, xylene resins, epoxy tackifying resins, polyamide tackifying resins, ketone tackifying resins, and elastic tackifying resins. These tackifiers can be used alone or in combination of two or more.
[0393] When using a tackifier, its content is preferably 30 parts by weight or less, more preferably 5 to 20 parts by weight, relative to 100 parts by weight of (meth)acrylic resin (A).
[0394] (solvent)
[0395] Solvents can be used to dilute adhesive compositions for the purpose of adjusting their viscosity. For example, in the case of coating adhesive compositions, solvents can be used to adjust the viscosity of the adhesive composition to an appropriate viscosity.
[0396] Examples of solvents include methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, propyl acetate, tetrahydrofuran, and dimethyl ethyl ketone. Organic solvents such as alkanes, cyclohexanone, hexane, toluene, xylene, n-propanol, and isopropanol. Solvents can be used alone or in combination of two or more.
[0397] (additive)
[0398] Examples of additives include, for example, plasticizers, surface lubricants, leveling agents, softeners, antioxidants, anti-aging agents, light stabilizers such as benzotriazoles, ultraviolet absorbers, polymerization inhibitors, phosphate esters and other flame retardants, surfactants, and antistatic agents.
[0399] [Method for manufacturing adhesive sheet]
[0400] Adhesive sheets can be manufactured, for example, by the methods shown below.
[0401] First, an adhesive solution is prepared to dissolve or disperse the adhesive composition in a solvent. The adhesive composition can then be used directly as an adhesive solution.
[0402] Next, an adhesive solution is applied to the substrate layer, and the solvent is removed by heating and drying while still containing the solvent, forming a pre-thermo-curable UV-curable adhesive layer. Then, a release liner is attached to the pre-thermo-curable UV-curable adhesive layer as needed. Further, the resulting liner is cured in an oven for a certain period of time as needed to allow a cross-linked structure to form, thereby obtaining an adhesive sheet.
[0403] The adhesive sheet can also be manufactured by the following method. An adhesive solution is applied to a release sheet, and the solvent is removed by heating and drying while still containing the solvent, forming a pre-thermo-curable UV-curable adhesive layer. Then, the release sheet with the pre-thermo-curable UV-curable adhesive layer is placed on a substrate layer with the side of the pre-thermo-curable UV-curable adhesive layer facing the substrate layer, and the pre-thermo-curable UV-curable adhesive layer is transferred onto the substrate layer. Further, the resulting sheet is cured in an oven for a certain period of time as needed to allow a cross-linked structure to form, thereby obtaining the adhesive sheet.
[0404] As a method for applying an adhesive solution to a substrate layer or release sheet, known methods can be used. Specifically, methods can be exemplified by using conventional coating machines such as gravure roller coating machines, reverse roller coating machines, kiss roller coating machines, dip roller coating machines, bar coating machines, doctor blade coating machines, jet coating machines, comma coating machines, and direct coating machines.
[0405] There are no particular restrictions on the conditions for heating and drying the coated adhesive solution. Typically, heating and drying are performed at 25–180°C, preferably 60–150°C, for 1–20 minutes, more preferably 1–10 minutes. Heating and drying within this range removes the solvent contained in the adhesive solution. There are no particular restrictions on the conditions for curing the heated and dried sheet in an oven for a certain period. Curing is typically performed at 25–100°C, preferably 30–80°C, for 1–30 days, more preferably 1–14 days. Curing under these conditions allows the (meth)acrylic resin (A) to crosslink via the crosslinking agent (C), adjusting the gel fraction of the UV-curable adhesive layer to the desired range.
[0406] Example
[0407] The present invention will be further described in detail below through examples and comparative examples, but the present invention is not limited to the following examples.
[0408] The following shows the raw materials used in the synthesis of (meth)acrylic resins (A) and (cA).
[0409] Methyl acrylate, Nippon Shokubai Co., Ltd. n-Butyl acrylate, Osaka Organic Chemical Industry Co., Ltd. 2-Ethylhexyl acrylate, Osaka Organic Chemical Industry Co., Ltd. Glycidyl methacrylate, Nippon Oil Co., Ltd. 4-Hydroxybutylacrylate glycidyl ether, Mitsubishi Microgreen Co., Ltd. 3,4-Epoxycyclohexylmethyl methacrylate, Daiser Co., Ltd. 3,4-Epoxy Tricyclic Acrylic Acid [5.2.1.0] 2,6 Decanoyl oxyethyl ester, Acrylic, Nippon Shokubai Co., Ltd. 2-hydroxyethyl acrylate, Nippon Shokubai Co., Ltd. Methacrylic acid, Nippon Shokubai Co., Ltd. Methacrylic anhydride, Edotron Co., Ltd. Karens (trademark) MOI, 2-isocyanate-ethyl methacrylate, Rezonack Co., Ltd. Free radical polymerization initiators: 2,2'-Azobis(isobutyronitrile), Fujifilm Wako Junyu Co., Ltd. catalyst: Triphenylphosphine, Hokuko Chemical Industry Co., Ltd. Dioctyltin dilaurate, Nitto Chemical Co., Ltd. [Synthesis example 1] 32 parts by mass of propylene glycol monomethyl ether were added to a reaction apparatus equipped with a stirrer, temperature controller, reflux cooler, dropping funnel, and thermometer, and reflux heating was initiated. 90 parts by mass of 2-ethylhexyl acrylate and 10 parts by mass of glycidyl methacrylate were mixed to prepare a monomer mixture. The monomer mixture containing 0.10 parts by mass of 2,2'-azobis(isobutyronitrile) as a polymerization initiator was added dropwise to the reaction apparatus. After the addition was complete, the mixture was maintained at 85°C for 4 hours. Next, the reaction temperature was raised to 120°C, and 3.00 parts by mass of methacrylic acid and 5.00 parts by mass of methacrylic anhydride were added along with 1.00 parts by mass of triphenylphosphine as a catalyst. The mixture was maintained at 120°C for 4 hours, and the disappearance of methacrylic acid was confirmed by acid value determination. Propylene glycol monomethyl ether was added to the reaction solution obtained through the above steps at a concentration of 40% by mass (excluding solvent), resulting in a liquid (40% by mass solids) containing (meth)acrylic resin (A1).
[0410] [Synthesis Examples 2 to 4]
[0411] Using the composition shown in Table 1, except that the procedure was the same as in Synthesis Example 1, a liquid (solid content 40% by mass) containing (meth)acrylic resins (A2) to (A4) was obtained.
[0412] [Comparative Synthesis Example 1]
[0413] 32 parts by mass of propylene glycol monomethyl ether were added to a reaction apparatus equipped with a stirrer, temperature controller, reflux cooler, dropping funnel, and thermometer, and reflux heating was initiated. 20 parts by mass of n-butyl acrylate, 70 parts by mass of 2-ethylhexyl acrylate, and 10 parts by mass of acrylic acid were mixed to prepare a monomer mixture. A monomer mixture containing 0.10 parts by mass of 2,2'-azobis(isobutyronitrile) as a polymerization initiator was added dropwise to the reaction apparatus. After the addition was complete, the mixture was maintained at 85°C for 4 hours. Next, the reaction temperature was increased to 120°C, and 20.00 parts by mass of 3,4-epoxycyclohexyl methacrylate and 1.00 parts by mass of triphenylphosphine as a catalyst were added, maintaining the temperature at 120°C for 4 hours. Propylene glycol monomethyl ether was added to the reaction mixture obtained through the above steps at a concentration of 40% by mass (excluding solvent), resulting in a liquid (40% by mass) containing (meth)acrylic resin (cAl).
[0414] [Comparative Synthesis Example 2]
[0415] In a reaction apparatus equipped with a stirrer, temperature controller, reflux cooler, dropping funnel, and thermometer, 32 parts by mass of ethyl acetate were added, and reflux was initiated. A monomer mixture was prepared by mixing 20 parts by mass of methyl acrylate, 12 parts by mass of n-butyl acrylate, 50 parts by mass of 2-ethylhexyl acrylate, and 18 parts by mass of 2-hydroxyethyl acrylate. The monomer mixture containing 0.10 parts by mass of 2,2'-azobis(isobutyronitrile) as a polymerization initiator was added dropwise to the reaction apparatus. After the addition was complete, the mixture was maintained under reflux for 4 hours. Next, the reaction temperature was raised to 60°C, and a mixture of 20.00 parts by mass of 2-isocyanate-ethyl methacrylate and 0.10 parts by mass of dioctyltin dilaurate as a carbamate catalyst was added dropwise. After the addition was complete, the reaction system was maintained at 60°C for 4 hours to allow the isocyanate groups to disappear. Ethyl acetate was added to the reaction solution obtained through the above steps in such a way that the components other than the solvent were 40% by mass, and a liquid (solid content 40% by mass) containing (meth)acrylic resin (cA2) was obtained.
[0416] [Table 1]
[0417] The following shows the raw materials used in the preparation of the adhesive composition.
[0418] Photopolymerization initiator (B): TPO: 2,4,6-Trimethylbenzoyl diphenylphosphine oxide (BASF, trade name: Omnirad-TPO) Crosslinking agent (C) L-45E: Toluene diisocyanate adduct of trimethylolpropane (Toso Co., Ltd., trade name: Coronato L-45E) [Preparation of adhesive composition] Ethyl acetate was added as a diluent to the liquids containing (meth)acrylic resins (A1) to (A4) and (cA1) to (cA2) obtained in Synthetic Examples 1 to 4 and Comparative Synthetic Examples 1 to 2, respectively, to adjust the content of (meth)acrylic resins (A1) to (A4) and (cA1) to (cA2) to 30% by mass, respectively. Using these liquids, an adhesive composition was obtained by the method shown below.
[0419] In a room where active radiation was blocked, the (meth)acrylic resin (A), photopolymerization initiator (B), and crosslinking agent (C) shown in Table 2 were added to plastic containers in the amounts (parts by mass) shown in Table 2 and stirred to obtain adhesive compositions (B1) to (B4) and (cB1) to (cB2). The values for (meth)acrylic resin (A) in Table 2 represent the amount (parts by mass) of (meth)acrylic resin used.
[0420] [Manufacturing Example 1] Fabrication of Adhesive Sheets
[0421] A silicone-based light-release PET film (Toyobo Co., Ltd., product name: E7006, thickness 25μm) was prepared as a release sheet. An adhesive composition (B1) was applied to the surface after release treatment using a coater to achieve a heat-cured thickness of 20μm. The film was then heated and dried at 100°C for 2 minutes to form a pre-heat-curing UV-curable adhesive layer. Next, a 50μm thick polyethylene naphthalate resin film was prepared as a sheet-like substrate layer. The polyethylene naphthalate resin film was adhered to the pre-heat-curing UV-curable adhesive layer using a rubber roller, with the corona-treated surface of the polyethylene naphthalate resin film bonded to the exposed surface of the pre-heat-curing UV-curable adhesive layer. The pre-heat-curing UV-curable adhesive layer was cross-linked and cured in an oven at 40°C for 3 days to obtain the adhesive sheet of Manufacturing Example 1.
[0422] [Manufacturing Examples 2-4 and Comparative Manufacturing Examples 1-2] Fabrication of Adhesive Sheets
[0423] Instead of adhesive composition (B1), the adhesive composition described in Table 2 was used. Otherwise, the same procedure as in Manufacturing Example 1 was followed to obtain adhesive sheets of Manufacturing Examples 2-4 and Comparative Manufacturing Examples 1-2.
[0424] [Refer to Examples 1-4 and compare with Examples 1-2]
[0425] <Making of Insulating Sheets with Adhesive Sheets>
[0426] An insulating sheet with a width of 100 mm and a length of 200 mm was prepared by impregnating a thermosetting resin composition consisting of 100 parts by weight of epoxy resin (YX-4000, Mitsubishi Kemica Co., Ltd.), 30 parts by weight of phenolic varnish resin (Shounor BRG-557, Iika Kogyo Co., Ltd.), 0.5 parts by weight of 2-ethyl-4-methylimidazol (Cuarazore 2E4MZ, Shikoku Kasei Kogyo Co., Ltd.), and 20 parts by weight of styrene-ethylene-butene-styrene (SEBS) (MD1653MO, Creton Co., Ltd.) into glass cloth (NE-2116, Nitto Spinning Co., Ltd.). The material from which the lightly peelable PET film was removed from the adhesive sheet of Manufacturing Examples 1-4 and Comparative Manufacturing Examples 1-2 was laminated with the main surface of the insulating sheet by means of an ultraviolet-curable adhesive layer, and then pressed at a temperature of 120°C and a pressure of 0.5 MPa to obtain an insulating sheet with an adhesive sheet.
[0427] <Evaluation of the adhesive strength of the adhesive sheet to the insulating sheet>
[0428] (1) Determination of adhesive strength (180° peel strength) before UV irradiation
[0429] As described below, the adhesion between the adhesive sheet and the insulating sheet was evaluated by measuring the 180° peel strength. Samples with a width of 25 mm and a length of 100 mm were cut from the insulating sheet with the adhesive sheet. The insulating sheet side of each sample was adhered to a polycarbonate sheet using double-sided tape. The peel strength between the adhesive sheet and the insulating sheet was measured using a tensile testing machine (VPA-H200, Kyowa Interface Science Co., Ltd.), and determined to be the adhesion strength before UV irradiation. The test conditions were set at a peel angle of 180° and a tensile speed of 300 mm / min. It should be noted that the samples were stored and the peel strength was measured at 23°C and 40% relative humidity. The results are shown in Table 2.
[0430] (2) Determination of adhesive strength (180° peel strength) after UV irradiation
[0431] The insulating sheet with the adhesive sheet is viewed from the substrate layer side of the adhesive sheet under an irradiation of 300 mJ / cm. 2 Under UV irradiation conditions, specimens with a width of 25 mm and a length of 100 mm were cut. A conveyor-type UV irradiation device (Igravex Co., Ltd., 2KW lamp, 80W / cm) was used for UV irradiation. The peel strength of the adhesive sheet to the insulating sheet was measured using the same method as the determination of the adhesive strength (180° peel strength) before UV irradiation, and this was determined as the adhesive strength after UV irradiation. The results are shown in Table 2.
[0432] [Refer to Examples 5-8 and compare with Examples 3-4]
[0433] <Evaluation of the adhesive strength of the adhesive sheet on the copper plate>
[0434] (1) Determination of adhesive strength (180° peel strength) before UV irradiation
[0435] The adhesion of the adhesive sheet to the copper plate was evaluated by measuring the 180° peel strength. A 10 μm thick electrolytic copper foil (3EC-M3-VLP-18, Mitsui Metals & Mining Co., Ltd.) was adhered to a polycarbonate plate using double-sided tape. Samples with a width of 25 mm and a length of 100 mm were cut from the adhesive sheets of Manufacturing Examples 1-4 and Comparative Manufacturing Examples 1-2. The light-peel PET film of the adhesive sheet was peeled off, and the UV-curable adhesive layer was pressed onto the electrolytic copper foil on the polycarbonate plate at a temperature of 120°C and a pressure of 0.5 MPa to obtain samples for evaluating the adhesion of the adhesive sheet to the copper plate. The peel strength of the adhesive sheet to the copper plate was measured using a tensile testing machine (VPA-H200, Kyowa Interface Science Co., Ltd.) to determine the adhesion strength before UV irradiation. The test conditions were set as a peel angle of 180° and a tensile speed of 300 mm / min. It should be noted that the samples were stored and the peel strength was measured at an environment of 23°C and 40% relative humidity. The results are shown in Table 2.
[0436] (2) Determination of adhesive strength (180° peel strength) after UV irradiation
[0437] The adhesion strength of the adhesive sheet to the copper plate was evaluated from the substrate layer side of the adhesive sheet using samples exposed to an irradiation dose of 300 mJ / cm². 2 The substrate was irradiated with ultraviolet (UV) light under specific conditions. A conveyor-type UV irradiation device (Aigravics Co., Ltd., 2KW lamp, 80W / cm) was used for UV irradiation. The peel strength of the adhesive sheet to the copper plate was then measured using the same method as the determination of the adhesive strength (180° peel strength) before UV irradiation, and this was determined as the adhesive strength after UV irradiation. The results are shown in Table 2.
[0438] [Examples 1-4 and Comparative Examples 1-2]
[0439] <Preparation of Samples for Evaluation of Transfer Sheets>
[0440] An insulating sheet with a width of 300 mm, a length of 500 mm, and a thickness of 100 μm was prepared by impregnating a thermosetting resin composition consisting of 100 parts by weight of epoxy resin (YX-4000, Mitsubishi Kemica Co., Ltd.), 30 parts by weight of phenolic varnish resin (Shounor BRG-557, Iika Kogyo Co., Ltd.), 0.5 parts by weight of 2-ethyl-4-methylimidazol (Cuarazore 2E4MZ, Shikoku Kasei Kogyo Co., Ltd.), and 20 parts by weight of styrene-ethylene-butene-styrene (SEBS) (MD1653MO, Creton Co., Ltd.) with glass cloth (NE-2116, Nitto Spinning Co., Ltd.). Next, a light-peel PET film was peeled off from the adhesive sheets of Manufacturing Examples 1-4 and Comparative Manufacturing Examples 1-2. An electrolytic copper foil (3EC-M3-VLP-18, Mitsui Metals & Mining Co., Ltd.) with a thickness of 10 μm was then laminated onto the UV-curable adhesive layer. After being rolled into a roll, it was subjected to a curing temperature of 20°C at 40 N / cm. 2 The pressure was applied for 30 minutes using an autoclave to produce a sheet with a conductor layer. A photosensitive resist was coated on the surface of a copper foil, exposed through a photomask, and developed to form a circuit pattern. Then, the foil was immersed in a ferric chloride solution to etch away the exposed copper foil, forming a circuit patterned wiring conductor. Further, the remaining resist layer on the wiring conductor was removed using a sodium hydroxide aqueous solution, creating a transfer sheet. The circuit pattern consisted of numerous 12μm wide strips of wiring conductor arranged at 30μm intervals. Next, the transfer sheets were overlapped with the wiring conductors of the transfer sheet touching the main surface of the insulating sheet, and pressed together at 120°C and 0.5MPa to obtain a sample for evaluation of the transfer sheet.
[0441] <Evaluation of Samples Used for Transfer Film Evaluation>
[0442] (1) Evaluation of the adhesion of the transfer sheet to the insulating sheet
[0443] The same procedure was followed as for evaluating the adhesion between the adhesive sheet and the insulating sheet, and the adhesion strength (180° peel strength) before and after UV irradiation was measured.
[0444] (2) Appearance evaluation
[0445] The substrate layer side of the transfer sheet used for evaluation was subjected to an irradiation dose of 300 mJ / cm. 2Under ultraviolet light, the UV-curable adhesive layer was peeled off from the wiring conductor, transferring the conductor onto the insulating sheet. The main surface of the insulating sheet with the transferred conductor was observed using a scanning electron microscope at 1000x magnification to check for surface damage, adhesive residue, and discoloration of the wiring conductor. Discoloration of the wiring conductor indicated the penetration of the chemical solution. A good result was defined as no observed surface damage, adhesive residue, or discoloration of the wiring conductor, while an observed result was defined as poor. The results are recorded in Table 2.
[0446] In Examples 1-4, the adhesive sheet can be peeled off from the surface of the adhered object without leaving any adhesive residue, even though the adhesive contains insulating regions and conductor regions. Therefore, it suggests that the adhesive sheets of Examples 1-4 can be peeled off from electronic components without leaving any adhesive residue by UV irradiation after being adhered to electronic components having insulating and conductor regions.
[0447] [Examples 5-8 and Comparative Examples 3-4]
[0448] <Preparation of Samples for Wiring Board Evaluation>
[0449] The substrate layer side of the transfer sheet used for evaluation was subjected to an irradiation dose of 300 mJ / cm. 2 Under ultraviolet light, the UV-curable adhesive layer is peeled off from the wiring conductor, transferring the wiring conductor onto the insulating sheet. Three insulating sheets with the transferred wiring conductor are then laminated and hot-pressed at 200°C and 1.0 MPa for 3 hours using a hot press, resulting in an evaluation wiring substrate in which the three insulating sheets with wiring conductors are cured and integrated.
[0450] Evaluation of samples used for evaluating wiring board
[0451] After the wiring board evaluation samples were placed in a high-temperature and high-humidity environment of 85% humidity, 85℃, and 5V for 1000 hours, the insulation resistance between adjacent wiring conductors in each wiring board evaluation sample was measured. The results are shown in Table 2. It should be noted that the above insulation resistance values are 1×10⁻⁶. 6 Cases above Ω are considered good, while those less than 1×10 are considered good. 6 The case of Ω is considered defective. A defective result indicates the presence of foreign matter on the surface of the insulation sheet on which the wiring conductor has been transferred, or surface damage.
[0452] [Table 2]
[0453] Explanation of symbols
[0454] 12 Substrate Layer
[0455] 14 UV-curable adhesive layer
[0456] 15 Adhesive Sheets
[0457] 16 Insulation Area
[0458] 18 Conductor Region
[0459] 20 Semiconductor chips
[0460] 22 Sealing resin
[0461] 24 Rewiring Layer
[0462] 26 Conductor Posts
[0463] 28 bumps
[0464] 30 wiring
[0465] 32 substrate
[0466] 34 Semiconductor Components
[0467] 36 Electronic Components
[0468] 38 Noise Suppression Layer
[0469] 40 covered part
[0470] 41 Opening
[0471] 42 Sealing part
[0472] 43 recess
[0473] 100, 110 Electronic components with adhesive tabs
[0474] 200 Semiconductor Component Connectors
[0475] 300 Semiconductor Components
[0476] 400 electronic devices
[0477] 500 Electronic Component Sealing Connection
[0478] 600 Electronic component seal.
Claims
1. An electronic component with an adhesive sheet, comprising: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and Electronic components disposed on the UV-curable adhesive layer of the adhesive sheet. The surface of the electronic component that contacts the UV-curable adhesive layer has an insulating region and a conductive region. The UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition comprises a (meth)acrylic resin (A) containing structural units of formulas (1) to (3) and optionally structural units of formula (4). In equation (1), R 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
2. A transfer film, comprising: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and Wiring conductors are locally disposed on the UV-curable adhesive layer. The UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition comprises a (meth)acrylic resin (A) containing structural units of formulas (1) to (3) and optionally structural units of formula (4). In equation (1), R 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
3. A transfer sheet with a conductive layer, comprising: An adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and The conductor layer disposed on the UV-curable adhesive layer, The UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition comprises a (meth)acrylic resin (A) containing structural units of formulas (1) to (3) and optionally structural units of formula (4). In equation (1), R 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
4. The electronic component with an adhesive sheet according to claim 1, the transfer sheet according to claim 2, or the transfer sheet according to claim 3, using a sheet with a conductive layer. The thickness of the substrate layer is 5–500 μm. The thickness of the UV-curable adhesive layer is 1–300 μm.
5. The transfer sheet according to claim 2 or the transfer sheet according to claim 3, wherein the thickness of the wiring conductor or the conductor layer is 0.5 to 100 μm and is in the range of 0.01 to 1.20 times the thickness of the UV-curable adhesive layer.
6. The electronic component with an adhesive sheet according to claim 1, the transfer sheet according to claim 2, or the transfer sheet according to claim 3, using a sheet with a conductive layer. The adhesive composition contains The (meth)acrylic resin (A), Photopolymerization initiator (B), and Crosslinking agent (C).
7. The method for manufacturing a transfer sheet with a conductor layer according to claim 3, comprising the following steps: A process for providing an adhesive sheet having a substrate layer and a UV-curable adhesive layer disposed on the substrate layer; and The process of setting a conductor layer on the exposed surface of the ultraviolet-curable adhesive layer.
8. A method for manufacturing a transfer film, comprising the following steps: A process for forming a pattern of a resist layer in a transfer sheet having a conductor layer as described in claim 3, wherein a resist layer is provided on the exposed surface of the conductor layer, exposed via a photomask, and developed with a developer. An etching process that removes the exposed areas of the conductor layer formed by the pattern forming process to form a wiring conductor. as well as The removal process is a process of removing the resist layer on the wiring conductor formed by the etching process.
9. A method for manufacturing a wiring board, comprising the following steps: The transfer process involves placing the surface of the transfer sheet described in claim 2, whereby the surface of the wiring conductor is in contact with the insulating sheet, thereby transferring the wiring conductor to the insulating sheet.
10. A method for manufacturing a wiring substrate, comprising: providing a sealing layer on the surface of the transfer sheet of claim 2 on which the wiring conductor is disposed.
11. The method of manufacturing a wiring substrate according to claim 10, comprising: providing a conductive path through the sealing layer such that a portion of the wiring conductor is connected to a conductive path.
12. A method for manufacturing an electronic device, comprising the following steps: Preparation process for a substrate having insulating and conductive areas on its surface; A bonding process in which an adhesive sheet having a substrate layer and an ultraviolet-curable adhesive layer disposed on the substrate layer is bonded to the surface of the substrate; A processing step of processing the substrate to which the adhesive sheet is attached; The process of subjecting the adhesive sheet to ultraviolet irradiation to light-cur the ultraviolet-curable adhesive layer; and The peeling process of detaching the adhesive sheet from the substrate. The UV-curable adhesive layer is a thermosetting product of the adhesive composition. The adhesive composition comprises a (meth)acrylic resin (A) containing structural units of formulas (1) to (3) and optionally structural units of formula (4). In equation (1), R 1 R represents a hydrogen atom or a methyl group. 2 R represents an alkyl group having 1 to 20 carbon atoms, in formula (2). 3 R represents a hydrogen atom or a methyl group. 4 This refers to a group having a hydroxyl group on a carbon atom and a residue obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid on the carbon atom adjacent to that carbon atom, in formula (3), R 5 R represents a hydrogen atom or a methyl group. 6 R represents a group having a residue on a carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid, and having a residue on an adjacent carbon atom obtained by removing a hydrogen atom from the carboxyl group of an unsaturated monocarboxylic acid. In formula (4), R 7 R represents a hydrogen atom or a methyl group. 8 This indicates a group containing an epoxy group.
Citation Information
Patent Citations
Method of manufacturing wiring board
JP2010129910A