Silver-coated copper strip
By using silver-coated copper strip, the problems of poor conductivity and easy oxidation of existing bonding wires under high temperature and high current environments are solved, achieving high-strength and long-life bonding, which is suitable for interconnection of power electronic devices.
Patent Information
- Application Number
- CN202580028143.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-13
- Filing Date
- 2025-04-07
- Publication Date
- 2026-11-20
AI Technical Summary
Existing bonding wires and strips suffer from poor conductivity, easy oxidation, insufficient bonding strength, and short lifespan in high-temperature applications. In particular, they face accelerated migration and interface instability when bonding with new semiconductor materials such as SiC and GaN, making it difficult to meet the requirements of high temperature and high current.
The copper strip is coated with silver, and the copper core is coated with a silver layer. The resulting strip has a height-to-width ratio of less than 0.8, which is suitable for wedge bonding. It combines the conductivity of copper with the oxidation resistance of silver to enhance the bonding strength and reliability.
It improves the conductivity and oxidation resistance of the strip, enhances the bonding strength, extends the lifespan, is suitable for high temperature and high current environments, reduces the risk of substrate damage from bonding forces, and is suitable for interconnection of power electronic devices.
Smart Images

Figure CN123147308A_ABST
Abstract
Description
[0001] This invention relates to a strip, preferably a strip for bonding in power electronic devices, comprising a coating and a copper core having a surface, the coating being deposited on the surface of the copper core, wherein the coating contains silver. The strip has a height and a width perpendicular to the height in a cross-sectional region perpendicular to its longitudinal axis, wherein the ratio of the height to the width is less than 0.8, and the height is in the range of 50 μm to 500 μm. The invention further relates to a method for manufacturing the strip, a strip obtainable by said method, an electronic assembly comprising at least two electronic components and at least the aforementioned strip, an apparatus comprising said electronic assembly, and a method for connecting two components via a wedge-wedge bonding using the aforementioned strip.
[0002] Bonding wires and strips are electrical connection elements in the field of electronic module assembly and connection technology. Bonding wires are used, for example, in the manufacture of semiconductor devices to electrically interconnect integrated circuits and printed circuit boards during semiconductor device manufacturing. Furthermore, bonding wires and strips are used in power electronics applications to electrically connect transistors, diodes, etc., to pads or pins on a housing. In the field of power electronics, thicker bonding wires and strips are used for electrical connections in power modules. The high current requirements in this field necessitate larger cross-sections for bonding wires and strips compared to the thinner cross-sections present in the finer bonding wires used in microelectronics.
[0003] Although bonding wires were originally made of gold, cheaper materials such as copper or aluminum are now used. Wires made of aluminum can be easily wedge-jointed by applying only low force, but they are less conductive than copper wires.
[0004] Wedge bonding is a method in which one end of a bonding wire or strip is pressed against the area to be bonded using a wedge bonding tool. This area is typically a bonding pad that provides the contact surface of an electronic module. An electrical connection is formed between the bonding wire and the module carrying the bonding pad using short ultrasonic pulses. Subsequently, the bonding tool can be moved along with the bonding wire from a first bonding point to a second bonding point on the contact surface. Here, the bonding process is repeated, thereby further cutting the bonding wire.
[0005] Copper wires and strips offer excellent electrical and thermal conductivity, but wedge bonding of such items presents challenges compared to bonding items made of aluminum. Furthermore, copper wires and strips are susceptible to oxidation. To overcome this issue, development has focused on bonding wires and strips with a core and a protective shell, such as a coating. Copper or gold can be chosen as the core material due to their high conductivity. Aluminum has also been used for the coating. These core-shell bonding wires and strips combine the high conductivity of copper with the advantageous bonding capabilities of aluminum. Aluminum-coated copper wires are particularly suitable for wedge-to-wedge bonding applications. However, with the rise of new semiconductor materials, especially wide-bandgap (WBG) semiconductors such as SiC and GaN, which require operating temperatures exceeding 200°C compared to previous generations of semiconductors, this material combination faces several challenges, particularly accelerated migration between different materials, leading to shortened component lifespan. Therefore, there is a continuous need for further improvements in bonding wire and / or strip technologies, both in terms of the bonding wires and / or strips themselves and the bonding processes.
[0006] Regarding wire geometries, the most common are joined wires with circular cross-sections and joined strips with more or less rectangular or elliptical cross-sections. Both types of wire geometries have their advantages, making them suitable for specific applications. Therefore, both types of geometries have their respective market shares. The larger, but also flatter, geometry of strip wires has practical advantages, namely faster processing, because contact can be achieved by joining only a small number of strip wires rather than many thinner joined wires. Therefore, for a given cross-sectional area, joined strips have a larger contact area. Furthermore, the flat geometry of strip wires allows for the generation of lower arc heights. Additionally, with comparable arc height geometries, root damage (i.e., damage in the sensitive arc region of the joined material) is less noticeable than with wires of comparable thickness. This allows for bridging exceptionally high steps with short joins, and thus enabling densely packed geometries in housing joins.
[0007] For bonding wires and strips used in high-current power devices (such as motors), a minimum diameter of 100 μm is required to withstand high temperatures and / or high current densities during operation. Such wires and strips are typically bonded to the corresponding substrate via wedge bonding. This technique presents different challenges and requirements for bonding wires compared to ball bonding, which is typically used for fine wires with diameters much smaller than 100 μm. During wedge bonding, the bonding wire is heated and pressed against the contact pads of the electronic component to be bonded (e.g., a semiconductor substrate or housing) with a certain force. If the required force is too high, it can damage the surface of the substrate, especially the semiconductor. Therefore, it is desirable to reduce the force during the wedge bonding process while still ensuring a strong bond to minimize the risk of damage to the semiconductor or substrate surface.
[0008] Therefore, one object of the present invention is to provide an improved strip.
[0009] A further object of the present invention is to provide a strip exhibiting excellent bonding properties. Therefore, one object of the present invention is to provide a strip particularly suitable for wedge-shaped joints with low bonding forces. In the context of the present invention, good wedge-shaped bonding properties should be understood as the property of the bonding strip to achieve good performance in the bonding process under low bonding forces and simultaneously obtain the high bonding strength of the resulting wedge-shaped joint.
[0010] Another object of the present invention is to provide a strip suitable for operating temperatures exceeding 200°C or even exceeding 225°C.
[0011] Another object of the present invention is to provide a strip with good processability and no special requirements for interconnection, thereby saving costs.
[0012] Another object of the present invention is to provide a strip with excellent electrical and thermal conductivity.
[0013] A further object of the present invention is to provide a strip that exhibits improved reliability.
[0014] Another object of the present invention is to provide a strip with improved corrosion resistance and / or oxidation resistance.
[0015] Another objective is to provide a new type of strip that can be used with standard bonding techniques and is particularly suitable for contacting WBG semiconductors, especially in wedge bonding applications, which ensures a longer lifespan than conventional wires.
[0016] A further object of the present invention is to provide means for realizing smaller sizes of electronic components in electrical assemblies.
[0017] A further objective is to provide improved electronic components, particularly for power electronic devices, which have an extended lifespan compared to conventional components in which electrical elements are interconnected by copper wires and / or strips or aluminum-coated copper wires and / or strips.
[0018] Another objective is to provide improved electronic components, particularly for power electronic devices, which operate at higher currents compared to conventional components in which bonding is provided by copper wire and / or strip or aluminum-coated copper wire and / or strip.
[0019] Another object of the present invention is to provide such improved electronic components having the same dimensions and similar semiconductor design as the conventional components mentioned above. Another object is to provide means for manufacturing such improved electrical components on production lines originally designed for manufacturing conventional electronic components. This will minimize the cost of implementing the improved technology.
[0020] Surprisingly, the tapes of the present invention have been found to solve at least one of the aforementioned objectives. Furthermore, a method for manufacturing these tapes has been discovered that overcomes at least one of the challenges in manufacturing tapes. Further, electronic assemblies incorporating the tapes of the present invention have stronger bonded connections and can withstand more temperature cycles and higher temperature differences, thereby exhibiting higher reliability at the interface between the tapes of the present invention and other electronic components.
[0021] The contribution to the solution of at least one of the above objectives is provided by the subject matter of the claims forming the class, wherein the dependent claims of the independent claims forming the class represent preferred aspects of the invention, the subject matter of which also contributes to solving at least one of the objectives mentioned above.
[0022] A first aspect of the present invention is a strip comprising:
[0023] (i) a copper core having a surface; and
[0024] (ii) A coating, which is superimposed on the surface of the copper core.
[0025] The coating contains silver.
[0026] The strip has a height and a width perpendicular to the height in a cross-sectional region perpendicular to the longitudinal axis of the strip, wherein the ratio of the height to the width is less than 0.8, and wherein the height is in the range of 50 μm to 500 μm.
[0027] Surprisingly, silver-coated copper strips have been found to be particularly suitable for high-temperature applications. Specifically, these strips have demonstrated improved reliability compared to previously used aluminum-coated copper strips. They maintain high conductivity under temperature loads, and no intermetallic phase formation between the copper core and the silver coating has been observed.
[0028] The strip is preferably a bonding strip for bonding in power electronic devices. Preferably, the strip is a single-piece object. The aforementioned cross-sectional dimensions, width, and height standards should be met within at least 80%, preferably 90%, of the strip's longitudinal extension. It should be understood that, unless otherwise stated, these geometric parameters are defined for strips not bonded to electronic components (such as semiconductors or substrates).
[0029] The height of the strip is in the range of 50 μm to 500 μm, preferably in the range of 100 μm to 450 μm or 150 μm to 400 μm.
[0030] The height and width of the strip can be defined as follows: A cross-sectional region perpendicular to the longitudinal axis of the strip has a profile, a geometric center, and a height axis H, which extends through the geometric center and intersects the profile at two points (P1, P2) on the shortest path. The height is the distance between the two intersection points (P1, P2). The cross-sectional region also includes a width axis W, which extends through the geometric center and intersects the profile at two points (P3, P4) on the longest path, wherein the width axis W is perpendicular to the height axis H. The width is the distance between the two intersection points (P3, P4).
[0031] Preferably, the width of the strip is in the range of 100 μm to 5,000 μm, more preferably in the range of 500 μm to 4,500 μm or 800 μm to 4,000 μm.
[0032] The aspect ratio of height to width is less than 0.8, preferably less than 0.6, and more preferably less than 0.5. For example, the ratio is in the range of 0.03 to less than 0.8, preferably in the range of 0.05 to 0.6, and more preferably in the range of 0.1 to 0.5. For example, a strip having a rectangular cross-section with dimensions of 1,000 μm × 600 μm has an aspect ratio of 0.6.
[0033] Preferred combinations of strip width and height are 500μm×50μm, 1000μm×100μm, 2000μm×200μm, 2000μm×300μm and 2000μm×400μm.
[0034] In a preferred embodiment, the cross-sectional area of the strip is 25,000 μm. 2 Up to 2mm 2 Within the range, preferably within 35,000 μm 2 Up to 1.5mm 2 Within the range, more preferably within 40,000 μm 2 Up to 1mm 2 Within the range.
[0035] In the context of this invention, the term "cross-sectional view" refers to a cut view through the strip, wherein the cutting plane is perpendicular to the longitudinal extension of the strip. The cross-sectional view can be taken at any point along the longitudinal extension of the strip.
[0036] Preferably, the strip of the present invention has a substantially rectangular or elliptical cross-sectional shape, and more preferably, the cross-section has a rectangular shape.
[0037] The strip may have rounded edges. Rounded edges should be understood as edges where a circular arc can be fitted; in other words, these edges do not contain sharp angles. Rounded edges have proven advantageous for bonding processes because they are less likely to cause problems during strip unwinding and damage to the substrate to be bonded.
[0038] The perimeter of the strip can be described by the lines of the cross-sectional view of the strip. Preferably, the perimeter C of the cross-sectional view of the strip is less than the sum of twice the length of the strip width W and twice the length of the strip height H (C < 2). W+2 H). In this case, the edges of the strip are not sharp. In other words, the perimeter of the strip is preferably smaller than the perimeter of the rectangle constructed from the length and height of the strip.
[0039] Based on the total weight of the copper core, the copper core according to the present invention preferably contains at least 95% by weight, preferably at least 98% by weight, even more preferably at least 99% by weight, and most preferably less than 99.99% by weight of elemental copper (Cu).
[0040] Preferably, the copper core contains less than 100 ppm, more preferably less than 50 ppm of additional components. In other words, the copper core preferably consists of copper and unavoidable impurities. The low content of these additional components ensures good electrical properties of the strip. In the context of this invention, additional components (generally also referred to as "unavoidable impurities") are impurities originating from the raw materials used or small amounts of chemical elements and / or compounds originating from the manufacturing process of producing the strip. Examples of such additional components are: Ni, Mn, Pt, Cr, Ca, La, Al, B, Zr, Ti, S, Fe. Additional components present in the copper core are generally not added separately.
[0041] The "surface" of the copper core of an uncoated copper wire or strip is the wire / air interface.
[0042] The “surface” of the copper core of the coated, possibly annealed strip is defined as a virtual boundary around the center of the copper core, where the Cu concentration deviates from the Cu concentration at the core center by more than 3% by weight, and the center is defined by the intersection of the width and height as defined above.
[0043] The core of a strip is a homogeneous region of bulk material. Since any bulk material always has surface areas that can exhibit different properties to some extent, the properties of the strip's core are understood as the properties of the homogeneous region of the bulk material. The surface of the bulk material region can differ in morphology, composition (e.g., sulfur, chlorine, and / or oxygen content), and other characteristics. This surface is the interface region between the copper core and the coating superimposed on it. Typically, the coating is completely superimposed on the surface of the copper core. In the region of the strip between the core and the coating superimposed thereon, a combination of materials from both the core and the coating may exist. This layer can also be referred to as an "intermediate layer."
[0044] The copper core has a width and a height, which can be defined as follows: A cross-sectional region perpendicular to the longitudinal axis of the copper core has a profile, a geometric center, and a height axis H. This height axis extends through the geometric center and intersects the profile at two points (P5, P6) on the shortest path. The height is the distance between the two intersection points (P5, P6). The cross-sectional region also includes a width axis W, which extends through the geometric center and intersects the profile at two points (P7, P8) on the longest path, where the width axis W is perpendicular to the height axis H. The width is the distance between the two intersection points (P7, P8).
[0045] Preferably, the width of the copper core is in the range of 90 μm to 4,990 μm, more preferably in the range of 200 μm to 4,000 μm, or in the range of 300 μm to 3,500 μm, each determined in a cross-sectional view of the copper core perpendicular to its longitudinal axis. Preferably, the height of the copper core is in the range of 40 μm to 450 μm, more preferably in the range of 90 μm to 400 μm, or in the range of 140 μm to 350 μm.
[0046] The strip includes a coating comprising silver, which is superimposed on the surface of a copper core. In the context of this invention, the term "superimposed" is used to describe the relative position of a first article (e.g., the copper core) with respect to a second article (e.g., the coating). Possibly, additional articles (such as an intermediate layer) may be disposed between the first and second articles. Preferably, the coating is at least partially superimposed on the surface of the copper core, for example, at least 30%, 50%, 70%, or at least 90% of the total surface area of the copper core.
[0047] Preferably, the coating completely covers the surface of the copper core. It has been found that complete coating of the copper core enhances the strip's corrosion resistance. If the copper core is only partially surrounded by a silver layer and the core is oxidized in the exposed areas, this can cause problems during the bonding process, in addition to optical distortion, especially if the oxidized portion loosens or even detaches.
[0048] The coating containing silver is preferably composed of free silver, silver alloys, or a combination of both.
[0049] Preferably, based on the total weight of the coating, the coating contains at least 85% by weight, preferably at least 90% by weight, more preferably at least 95% by weight, and even more preferably at least 98% by weight of elemental silver (Ag).
[0050] Preferably, the coating contains less than 1000 ppm, more preferably less than 500 ppm of additional components. The low content of these additional components ensures good electrical properties of the strip. In the context of this invention, additional components (often also referred to as "unavoidable impurities") are impurities originating from the raw materials used or small amounts of chemical elements and / or compounds originating from the manufacturing process of producing the strip, particularly the raw materials used during the coating process. In other words, the coating preferably consists of silver and unavoidable impurities. Examples of such additional components are: Ni, Mn, Pt, Cr, Ca, La, Al, B, Zr, Ti, S, Fe. Additional components present in the coating are generally not added separately.
[0051] According to another aspect of the invention, the coating thickness is in the range of 5 μm to 60 μm, preferably 10 μm to 50 μm, preferably 15 μm to 40 μm, or 20 μm to 35 μm, each determined in a cross-sectional view of the strip. The aforementioned criteria for coating thickness should be met within at least 80%, preferably 90%, of the longitudinal extension of the strip.
[0052] In the context of this invention, the term "thickness" is used to define the size of a layer in a direction perpendicular to the longitudinal axis of the strip, which is at least partially superimposed on the surface of the copper core.
[0053] All the length dimensions mentioned above (e.g., width, height, thickness, diameter, longest path, shortest path) are determined in the cross-sectional view as defined above.
[0054] Preferably, within a given cross-sectional area, the coating thickness does not deviate around the copper core. In other words, within a given cross-sectional area, the layer thickness has a substantially constant thickness. For example, within a given cross-sectional area, the coating thickness deviation does not exceed 5%, preferably not exceeding 3%.
[0055] The coating has two "surfaces". The first "surface" of the coating is the strip / air interface. The second "surface" of the coating is defined as a virtual boundary of the coating, which is defined by a deviation of Ag concentration from Ag concentration in the bulk region of the coating exceeding 3% by weight. The bulk region is defined as the area located at an equidistant point between the first and second "surfaces" of the coating.
[0056] According to another aspect of the invention, an intermediate layer is arranged between the copper core and the coating. In the context of this invention, the term "intermediate layer" refers to a region in the strip located between the copper core and the coating. In this region, a combination of materials, such as those in the core and those in the coating, is present, for example, in the form of at least one intermetallic phase. In this context, "intermetallic" is understood accordingly as a diffusion region.
[0057] Due to diffusion, the clear boundary between the copper core and the coating may disappear during strip production (e.g., introduced via heat treatment steps) and / or storage. Specifically, material from the copper core can diffuse into the coating material, and material from the coating can diffuse into the copper core material. This can, for example, lead to the formation of an alloying or intermetallic phase between the copper core and the coating. These alloying or intermetallic phases typically consist of elements present in both the copper core and coating materials, and often include a gradient, whereby the elemental content of the copper core material decreases from the center of the strip toward the surface, and the elemental content of the coating material decreases from the surface or near the surface of the strip toward the interior. This diffusion phenomenon can result in the presence of an intermediate layer.
[0058] Preferably, the intermediate layer comprises only the material of the copper core and the material of the coating. According to a preferred aspect of the invention, an intermediate layer is disposed between the core and the coating, wherein the intermediate layer is adjacent to both the copper core and the coating. Such an intermediate layer enhances the adhesion between the copper core and the coating and ensures the functionality of the strip.
[0059] Preferably, the intermediate layer contains less than 800 ppm, more preferably less than 500 ppm of additional components. In other words, the intermediate layer is preferably composed of copper, silver, and unavoidable impurities.
[0060] In a preferred embodiment, the intermediate layer of the strip is defined as the region in the strip located between the copper core and the coating, wherein the concentration of Cu differs from the concentration of Cu in the copper core by more than 3% by weight based on the total weight of the copper core, and wherein the concentration of Ag differs from the concentration of Ag in the coating by more than 3% by weight based on the total weight of the coating.
[0061] In other words, based on the total weight of the coating, the concentration of copper in the intermediate layer is preferably at least 3% by weight lower than the concentration of Cu in the copper core, and the concentration of silver in the intermediate layer is preferably at least 3% by weight lower than the concentration of Ag in the coating.
[0062] Preferably, the intermediate layer does not contain any materials and / or elements that are not present in the copper core or coating.
[0063] The intermediate layer may contain at least one intermetallic phase, which includes the material of the copper core and the material of the coating.
[0064] Preferably, the intermediate layer comprises a copper concentration gradient from the copper core toward the coating and a silver concentration gradient from the coating toward the copper core in a direction perpendicular to the longitudinal axis of the strip. The concentration gradient should be understood as a decrease in the concentration of the respective element. Such a concentration gradient can further enhance the adhesion of the coating on the copper core surface, making production easier and improving strip productivity.
[0065] According to another aspect of the invention, the thickness of the interlayer is in the range of 0.05 μm to 5 μm, preferably 0.1 μm to 3 μm. The aforementioned standard for the interlayer thickness should be met within at least 80%, preferably 90%, of the longitudinal extension of the strip. Sometimes, the thickness of the interlayer may deviate due to defects (e.g., porosity) in the interlayer.
[0066] Preferably, within a given cross-sectional region, the thickness of the interlayer does not deviate around the copper core. In other words, within a given cross-sectional region, the thickness of the interlayer has a substantially constant thickness. For example, within a given cross-sectional region, the thickness deviation of the interlayer does not exceed 5%, preferably not exceeding 3%.
[0067] According to an alternative aspect of the invention, the thickness of the interlayer is less than 0.05 μm, for example, in the range of 0 μm to 0.05 μm. The aforementioned criteria for interlayer thickness should be met within at least 80%, preferably 90%, of the longitudinal extension of the bonded wire. Preferably, the thickness of the interlayer deviates from each other by no more than 10%, preferably no more than 5%, in the bonded section and in one or more free sections.
[0068] The dimensions mentioned above (i.e., the thickness of the coating, the thickness of the interlayer, and the width and height of the strip and copper core) can be determined, for example, using an optical microscope or a scanning electron microscope in a cross-sectional view of the strip. Under an optical microscope, the copper core appears copper-red, the coating appears silvery-white, and the interlayer appears gray. The concentrations of copper and silver described above can be determined using a combination of SEM / EDX (scanning electron microscopy / energy-dispersive X-ray spectroscopy).
[0069] The strip according to the invention can be manufactured by the following operations: providing a strip precursor having a greater height and width than the strip according to the invention, the strip precursor comprising a copper core precursor and a silver-coated precursor; and shaping the strip precursor into the final strip shape and / or size.
[0070] The strip can also be manufactured by: providing a copper core precursor; reshaping the copper core precursor into the final shape and / or dimensions of the copper core of the strip; and coating the shaped copper core with a silver coating.
[0071] Preferably, the strip formed and coated according to the two alternative schemes is annealed in another step.
[0072] Another aspect of the present invention is a method for manufacturing a strip according to the invention, the method comprising at least the following steps:
[0073] I.) Provides a strip precursor comprising a copper core precursor having a surface and a coating precursor, the coating precursor being superimposed on the surface of the copper core precursor, wherein the coating precursor comprises silver.
[0074] II.) Shape the strip precursor so that
[0075] The strip has a height and width in a cross-sectional region perpendicular to its longitudinal axis, wherein the width is perpendicular to the height.
[0076] Where the ratio of height to width is less than 0.8, and
[0077] The height ranges from 50 μm to 500 μm.
[0078] The aspects of the present invention relating to the strip described above are also preferred aspects of the strip obtained by the methods for manufacturing the strip mentioned above.
[0079] Precursor items are preliminary items that have not yet reached the expected final size of the final strip.
[0080] Based on the total weight of the copper core precursor, the copper core precursor according to the invention preferably contains at least 95% by weight, preferably at least 98% by weight, even more preferably at least 99% by weight, and most preferably less than 99.99% by weight of elemental copper (Cu).
[0081] Preferably, the copper core precursor contains less than 100 ppm, more preferably less than 50 ppm of additional components. In other words, the copper core precursor preferably consists of copper and unavoidable impurities. In the context of this invention, additional components (generally referred to as "unavoidable impurities") are impurities originating from the raw materials used or from trace amounts of chemical elements and / or compounds arising from the manufacturing process of producing the strip. Examples of such additional components are: Ni, Mn, Pt, Cr, Ca, La, Al, B, Zr, Ti, S, Fe. Additional components present in the copper core precursor are typically not added separately.
[0082] The coating precursor superimposed on the surface of the copper core precursor of the strip precursor contains silver. The silver-containing coating precursor is preferably selected from the group consisting of free silver, silver alloys, or a combination of both.
[0083] Preferably, each coating precursor contains at least 85% by weight, preferably at least 90% by weight, more preferably at least 95% by weight, or even more preferably at least 98% by weight of elemental silver (Ag) based on the total weight of the coating precursor.
[0084] The cross-sectional area of the strip precursor may already have a height-to-width ratio of less than 0.8, or it may have a ratio greater than 0.8. The shape of the cross-section is not further restricted; it may be, for example, substantially circular, elliptical, or rectangular.
[0085] Preferably, the width of the strip precursor is in the range of 0.3 mm to 5 mm, more preferably 0.5 mm to 3 mm, or 0.75 mm to 2 mm.
[0086] The strip precursor as in step I.) can be obtained by forming a silver-coated precursor on at least a portion of the surface of the copper core precursor. Preferably, the silver-coated precursor is formed on 100%, or 80% to 100%, or 60% to 80% of the surface of the copper core precursor, each relative to the total surface area of the copper core precursor. Various techniques for forming a silver layer on a copper surface are known. Preferred techniques include silver deposition from vapor deposition (such as electroplating and electroless plating), such as sputtering, ion plating, vacuum evaporation, and chemical vapor deposition, as well as silver deposition from melt.
[0087] The strip precursor can also be obtained by a process in which the copper core precursor is enclosed in a silver sheath, and optionally the assembly is drawn to the desired diameter, width, height and / or shape, and / or annealed.
[0088] Preferably, the silver coating precursor is applied by electroplating. Silver plating is performed using a silver plating bath (i.e., a plating bath that allows silver to be electroplated onto the surface of a copper cathode). In other words, a silver plating bath is a composition that allows the direct application of elemental, metallic silver onto the copper surface on which the wiring serves as the cathode.
[0089] The electroplating of the silver-coated precursor is performed by guiding the copper core precursor, which serves as the cathode, through a silver plating bath. The silver-coated copper core precursor thus obtained from the silver plating bath can be rinsed and dried. Using water as the rinsing medium is advantageous, with alcohols and alcohol / water mixtures being further examples. Silver plating of the copper core precursor through the silver plating bath can be performed at a DC voltage, for example, in the range of 0.2V to 20V, and at a current, for example, in the range of 0.001A to 5A, particularly 0.001A to 1A or 0.001A to 0.2A. The contact time is typically in the range of, for example, 0.1 seconds to 120 seconds, preferably 5 seconds to 60 seconds. The current density used in this context can be, for example, 0.01A / dm³. 2 Up to 150A / dm 2 Within a certain range. The silver plating bath may have a temperature in the range of, for example, 25°C to 50°C, preferably 30°C to 40°C.
[0090] The thickness of the silver coating precursor can be adjusted as needed, primarily by the following parameters: the chemical composition of the silver plating bath, the contact time between the copper core precursor and the silver plating bath, and the current density. In this context, the thickness of the silver coating precursor can typically be increased by increasing the concentration of silver in the silver plating bath, by increasing the contact time between the copper core precursor (used as the cathode) and the silver plating bath, and by increasing the current density.
[0091] Pretreatment of the copper core precursor can be used to adjust surface roughness and / or add patterns to the surface of the copper core precursor. Several techniques are known for adjusting the surface of the copper core precursor. Preferred techniques are cold rolling, grinding, and electrochemical polishing.
[0092] Forming is preferably understood as a process in which the shape of the workpiece changes without a significant change in its quality. For example, cutting is not a forming process because it is associated with a reduction in the quality of the cut parts and the overall quality of the workpiece. Various techniques are known to form the strip precursor in step II.). Preferred techniques are flat rolling, die drawing, etc. In the latter case, the precursor article is drawn in several process steps until the desired cross-sectional shape and / or dimensions are achieved. Such wire drawing processes are well known to those skilled in the art. Conventional tungsten carbide and diamond dies can be used, and conventional drawing lubricants can be used to support the drawing process.
[0093] According to one embodiment of the invention, forming is performed by means of flat rolling. In this context, the rolling conditions are appropriately adjusted so that the final strip has an aspect ratio of less than 0.8 after rolling.
[0094] According to another embodiment of the invention, forming is performed by drawing and / or extruding a strip precursor through a drawing die. For this purpose, a drawing die is first provided. These drawing dies have openings whose shape and cross-section substantially correspond to the shape and cross-section of the strip to be joined. Therefore, the drawing die preferably includes at least partially openings with an aspect ratio not exceeding 0.8. However, the exact geometry of the openings in the drawing die is a function of the material used for joining the strip. Since the joining strip may experience some increase in cross-section after drawing due to the elasticity of the material used for joining the strip, the openings in the drawing die may need to have a cross-section smaller than the desired cross-section of the joining wire or strip. Finally, the strip is drawn through the openings of the provided drawing die, and thus the strip takes on the shape of the drawing die openings.
[0095] Another aspect of the present invention is an alternative method for manufacturing the strip according to the invention, the alternative method comprising at least the following steps:
[0096] I.) Provide a copper core precursor with a surface;
[0097] II.) Shape the copper core precursor so that
[0098] The copper core precursor has a height and width in a cross-sectional region perpendicular to the longitudinal axis of the strip, wherein the width is perpendicular to the height.
[0099] Where the ratio of height to width is less than 0.8, and
[0100] The height ranges from 40 μm to 450 μm.
[0101] III.) Coat the surface of the shaped copper core with a coating containing silver.
[0102] The aspects of the present invention relating to the strip described above are also preferred aspects of the strip obtained by the methods for manufacturing the strip mentioned above.
[0103] Each copper core precursor preferably comprises at least 95% by weight, preferably at least 98% by weight, elemental copper (Cu) with a purity of at least 99.9% Cu, based on the total weight of the copper core. Preferably, the purity of the copper core is at least 99.99%, or 99.999%, or 99.9999%.
[0104] Preferably, the copper core precursor contains an additional component of 0 ppm to 100 ppm, more preferably less than 30 ppm. Examples of such additional components are: Ni, Mn, Pt, Cr, Ca, La, Al, B, Zr, Ti, S, and Fe. The additional components present in the copper core are typically not added separately.
[0105] Preferably, the width of the copper core precursor is in the range of 0.3 mm to 5 mm, more preferably 0.5 mm to 3 mm, or 0.75 mm to 2 mm.
[0106] The cross-sectional area of the copper core precursor may already have a height-to-width ratio of less than 0.8, or it may have a ratio greater than 0.8. The shape of the cross-section is not further restricted; it may be, for example, substantially circular, elliptical, or rectangular.
[0107] Preferably, the width of the strip precursor is in the range of 0.3 mm to 5 mm, more preferably 0.5 mm to 3 mm, or 0.75 mm to 2 mm.
[0108] The copper core precursor can be formed as described above for alternative methods used to manufacture the strip of the present invention.
[0109] The coating of the shaped copper core precursor can be performed as described herein for alternative methods used in manufacturing the strip of the present invention.
[0110] Preferably, both of the foregoing aspects of the method according to the invention may include a subsequent step of annealing the strip.
[0111] Various procedures are known in the art for annealing wires, wire precursors, strips, or strip precursors. Annealing can be performed as a continuous or discontinuous process, such as by heat treatment in an oven or plasma annealing. In specific applications, even continuous and discontinuous processes can be combined.
[0112] According to a preferred embodiment of the invention, annealing is performed by heating the strip to a temperature in the range of 140°C to 400°C, preferably 160°C to 350°C, or 200°C to 300°C, or 220°C to 280°C, and holding this temperature for 30 minutes to 5 hours, preferably 30 minutes to 3 hours. The annealed strip is then cooled to room temperature. Cooling can be performed in various ways. A suitable method is to expose the wire or strip to ambient air at ambient temperature as it leaves the heating zone. Cooling the strip to room temperature (T=20°C) can typically be achieved within 24 hours according to the aforementioned procedure. Quenching of the strip should be avoided, for example, by immersion in cold water. Therefore, another aspect is a process in which cooling of the strip is performed without quenching upon leaving the heating zone.
[0113] Preferably, annealing is performed dynamically as the strip or strip precursor moves through the annealing furnace and is wound onto a spool after leaving the furnace. According to another aspect of the invention, annealing is performed as a continuous process, more preferably in a tube furnace.
[0114] During annealing in a tube furnace, the speed of the wire or strip depends on the length of the furnace tube. The longer the tube, the higher the feasible speed, in order to achieve a certain energy exposure to the wire or strip segment. Preferred tube lengths for tube furnaces are in the range of 0.8m to 2.5m, or 1m to 2m, or 1.5m to 2.5m.
[0115] The temperature in the furnace tube can be adjusted or evaluated independently depending on the drawing process. Preferred temperatures in the tube are in the range of 150°C to 600°C, 200°C to 600°C, or 250°C to 550°C. Generally, the temperature is selected below the liquefaction temperature of at least one component or a mixture of at least two components present in the strip. For example, if annealing a partially soluble or insoluble two-component or multi-component alloy, the temperature in the oven should not exceed the eutectic temperature of the alloy.
[0116] According to another aspect of the invention, the temperature in the furnace is selected to be at least 30°C, 50°C, or 80°C lower than the liquefaction temperature of at least one component or a mixture of at least two components of the strip.
[0117] According to another aspect of the invention, the annealing rate is selected from the range of 1 m / min to 100 m / min, or 5 m / min to 30 m / min, or 10 m / min to 20 m / min.
[0118] According to another aspect of the invention, annealing in a tube furnace can be performed in an inert atmosphere or a reducing atmosphere. This is applicable to both continuous and discontinuous annealing processes. Many inert atmospheres and reducing atmospheres are known in the art. Among the known inert atmospheres, nitrogen is preferred. Among the known reducing atmospheres, hydrogen is preferred. Furthermore, a nitrogen and hydrogen mixture is preferred. Preferably, the nitrogen and hydrogen mixture, each based on the total volume of the mixture, is in the range of 90% to 98% by volume of nitrogen and 10% to 2% by volume of hydrogen. Each based on the total volume of the mixture, the preferred nitrogen / hydrogen mixture is equal to 90 / 10% / volume%, 93 / 7% / volume%, 95 / 5% / volume%, and 97 / 3% / volume%. If some portions of the strip surface are sensitive to oxidation by oxygen in the air, for example, if the copper of the strip is exposed on its surface, then the application of a reducing atmosphere in annealing is particularly preferred.
[0119] According to another aspect of the invention, an intermediate layer is formed during annealing.
[0120] Another aspect of the present invention is a strip that can be obtained by the method defined above.
[0121] Another aspect of the present invention is an electronic component comprising at least a strip according to the present invention or a strip manufactured according to the present invention.
[0122] Electronic components are to be understood herein as electronic or power electronic sub-components comprising at least one substrate (as a circuit carrier), at least one semiconductor component (semiconductor), or (if applicable) at least one passive electronic component. Preferably, the electronic component is a power module.
[0123] Examples of substrates include IMS (insulating metal substrate), cermet substrates such as DCB substrates (direct copper bonding substrates) or AMB substrates (active metal soldering substrates), PCBs (printed circuit boards), and lead frames.
[0124] Examples of semiconductor components include diodes, LEDs (light-emitting diodes), dies (semiconductor chips), IGBTs (insulated-gate bipolar transistors), ICs (integrated circuits), and MOSFETs (metal-oxide-semiconductor field-effect transistors).
[0125] Preferably, the electronic component includes at least two electronic elements, and the strip electrically connects the two electronic elements.
[0126] According to another aspect of the invention, at least one strip in the electronic assembly is connected to the electronic element of the electronic assembly by wedge-wedge bonding, preferably by ultrasonic or laser-assisted wedge-wedge bonding.
[0127] Wedge bonding technology is known in the art and is extensively described in publications such as Shankara K. Prasad, "Advanced Wirebond Interconnection Technology," Kluwer Academic Publishers, 2004, ISBN 1-4020-7762-9, particularly Chapter I (Introduction) and Chapter IV (Process Technology). During bonding, a certain force (typically measured in grams) is applied, which is supported by the application of ultrasonic energy (typically measured in mA). The tape of the present invention is particularly suitable for bonding processes in which relatively low bonding forces are applied.
[0128] Another aspect of the present invention is a method for manufacturing electronic components, the method comprising the following steps:
[0129] I.) Provide at least two electronic components;
[0130] II.) Provide a strip according to an embodiment of the present invention or an embodiment thereof, or a strip obtained by a method according to an embodiment of the present invention or an embodiment thereof;
[0131] III.) The two electronic components are connected by a strip, wherein at least one of the connections is performed by a wedge engagement.
[0132] Preferably, all connections are performed via wedge engagement.
[0133] In another preferred aspect of the invention, the electronic component includes a first bonding pad and a second bonding pad, and the strip is connected to the bonding pad by a wedge-wedge joint.
[0134] Another aspect of the present invention is a method for connecting electronic components, the method comprising the following steps:
[0135] I.) Provide a strip according to an embodiment of the present invention or an embodiment thereof, or a strip obtained by a method according to an embodiment of the present invention or an embodiment thereof;
[0136] II.) Provide an electronic component including a first bonding pad and a second bonding pad;
[0137] III.) Joining the strip provided in step I.) to the first bonding pad of the electronic component using a wedge joint; and
[0138] IV.) The strip that was bonded to the first bonding pad in step I.) is bonded to the second bonding pad of the electronic component by wedge bonding.
[0139] Preferably, steps III.) and / or IV.) are performed without the use of an inert gas or a forming gas. A forming gas is referred to in the art as a mixture of an inert gas (such as nitrogen) and hydrogen, wherein the hydrogen content provides for the reduction reaction of the oxidized strip material. In the context of this invention, omitting the forming gas means not using reactive compounds (such as hydrogen).
[0140] Another aspect of the invention is the use of the tape according to the invention or the tape manufactured according to the method of the invention in wedge-wedge bonding interconnects in electronic components.
[0141] Another aspect of the invention is an apparatus comprising at least one electronic component as described above, preferably an electronic vehicle, a solar cell, or a wind turbine.
[0142] The following schematic diagrams illustrate aspects of the invention to aid in understanding the invention in conjunction with some exemplary illustrations. However, it should be understood that the invention is not limited to the precise arrangements and tools shown. Elements in the drawings are not necessarily to scale relative to each other. Similar reference numerals denote corresponding similar parts. In this document…
[0143] Figure 1 The strip and its cross-section are shown.
[0144] Figure 2 A cross-sectional view of the strip is shown;
[0145] Figure 3 A cross-sectional view of the strip including the intermediate layer is shown;
[0146] Figure 4 The process according to the present invention is shown;
[0147] Figure 5 An alternative process for manufacturing strip is shown;
[0148] Figure 6 An electronic assembly comprising two electronic components and a strip is shown;
[0149] Figure 7 An electronic assembly comprising five electronic components and four strips is shown.
[0150] exist Figure 1 In section A, strip 1 is depicted. Figure 1B shows a cross-sectional view of strip 1 perpendicular to its longitudinal axis; the internal structure is not shown. The cross-section can be defined by height H. R Characterized by the height, this is the distance between two intersection points P1 and P2 on the profile or wire. The two intersection points P1 and P2 are located on the height axis H, which extends through the geometric center 5 of the strip, and the two intersection points P1 and P2 lie on the shortest path through the cross-section. The width W of the strip... R It is the distance between two intersection points P3 and P4 on the outer surface of the strip. Points P3 and P4 are located on the width axis W, which extends through the geometric center 5 and intersects the profile at the two intersection points (P3, P4) on the longest path. The width axis W is perpendicular to the height axis H.
[0151] Figure 2 A cross-sectional view of strip 1 is shown. The copper core 2 is coated with a material of thickness T. AG The coating 3 surrounds the core. The core surface 4 lies on the boundary of the copper core 2. Furthermore, the width W of the strip is depicted. R and height H R and the width W of the copper core C and height H C .
[0152] exist Figure 3 The image depicts a strip 1 having a copper core 2, an intermediate layer 6, and a coating 3. (The image is not directly related to the previous sentence.) Figure 2 In addition to the described items, the thickness T of the intermediate layer 6 is also shown. I .
[0153] Figure 4 A process for manufacturing strip according to the present invention is shown.
[0154] Figure 5 An alternative process for manufacturing strip according to the present invention is shown.
[0155] Figure 6 An electronic module 10 is depicted, comprising two electronic components 11 and a strip 1. The strip 1 electrically connects the two electronic components 11 via a wedge-shaped connector 12. One of the electronic components 11 may be a semiconductor, which is connected to a substrate via the bonding strip 1.
[0156] Figure 7 Another electronic module 10 is depicted. Five electronic components 11 are electrically connected via four strips 1. For clarity, only one of the eight wedge joints 12 is assigned a reference numeral.
[0157] Test methods
[0158] Unless otherwise stated, all tests and measurements were performed at T=20°C and 50% relative humidity.
[0159] Layer thickness
[0160] To determine the coating thickness, interlayer thickness, and core diameter, the strip is cut perpendicular to its maximum elongation. The cut is carefully ground and polished to avoid smearing of soft materials (e.g., Ag). Photographs are recorded using an optical microscope or scanning electron microscope (SEM), where a magnification is selected to show the entire cross-section of the strip.
[0161] The procedure is repeated at least 15 times. All values are provided as the arithmetic mean of at least 15 measurements.
[0162] thermal aging
[0163] The thermal aging behavior of the silver-coated copper strip of the present invention was compared with that of the aluminum-coated copper strip. Strip samples were stored in an air atmosphere at 200°C for up to 2000 hours. After temperature exposure, the intermetallic phase between the copper core and the coating, as well as the resistivity of the aged strip, were examined and compared with the original condition.
[0164] The cross-section of the wire was observed using an optical microscope (DM8000 M, Leica, magnification ×1000) to examine the intermetallic phase between the copper core and the Ag or Al layer. For sample preparation, the strip was cut perpendicular to its maximum elongation, potted with epoxy resin (Epo-Fix, Sterling Ltd.), and polished using an automated polishing device (Tegrapol, Sterling Ltd.). Chemical mechanical polishing was performed using a polishing suspension (OP-S, Sterling Ltd., with added hydrogen peroxide and ammonia).
[0165] The resistivity of fresh and aged strip samples was measured according to the following procedure: Both ends of a 0.5 m long test strip were connected to a power source providing a constant current / voltage. The resistance was recorded using a voltage supply device. The measuring apparatus was a RESISTOMAT 2316 model, and the test was repeated with at least 10 test strips. The arithmetic mean of the measurements was used for the calculations given below.
[0166] The resistance R is calculated using the formula R=U / I, where U is the voltage and I is the current.
[0167] The resistivity ρ is calculated using ρ = (R × A) / L, where A is the average cross-sectional area of the strip and L is the strip length between two measuring points of the device used to measure the voltage.
[0168] The specific conductivity σ is calculated based on σ=1 / ρ.
[0169] The present invention is further illustrated by representative examples. These examples are provided to illustrate the invention and are not intended to limit the scope of the invention or the claims in any way.
[0170] A round copper wire with a diameter of 943 µm was rolled to obtain a strip with a width of 2,000 µm and a height of 300 µm. The copper strip was then electroplated to obtain a coating with a thickness of 50 µm. Subsequently, the obtained strip was placed on a metal spool and annealed in an oven at 350 °C for 1 hour. After annealing, the strip was cooled to ambient temperature over 5 hours.
[0171] The bonding parameters and characteristics of the present invention's strip (Ag-coated Cu strip) according to the embodiments were compared with those of commonly used bonded strips (Al strip, Cu strip, and Al-coated Cu strip with a 50 μm Al coating) with a width of 2,000 μm and a height of 300 μm. The strips were wedge-bonded on different substrates, and the quality of the resulting bonds was evaluated. Temperature stability was tested by exposing the bonded strips to appropriate temperatures and evaluating the bond failure time. Corrosion resistance was evaluated for thermal stress tolerance during use.
[0172] Table 1 summarizes the qualitative comparisons of the results. Therefore...
[0173] ++ indicates that the performance is highly suitable or there are no failures / failures occur very late;
[0174] + indicates that the overall performance is good or the failure occurred relatively late;
[0175] 0 indicates average performance;
[0176] - Indicates low performance or early failure;
[0177] --Indicates that the performance is unsuitable or fails very early.
[0178] Table 1 .
[0179]
[0180] The performance parameters of Ag-coated Cu strips are usually comparable to those of pure Ag strips, but the cost is significantly reduced.
[0181] Table 2 summarizes the qualitative results of the thermal aging assessment of Ag-coated Cu wire and Al-coated wire.
[0182] Table 2 .
[0183]
[0184] No IMP growth was detected in the Ag-coated tape, indicating that the tape configuration of the present invention has high stability. As is known to those skilled in the art, IMP reduces the conductivity of the tape. Furthermore, they are highly brittle and may therefore lead to tape failure due to fracture. Moreover, no increase in resistivity was observed even after temperature exposure for up to 750 hours.
[0185] Especially for high-temperature applications and in terms of reliability, the Ag-coated Cu strip of the present invention exhibits excellent performance in terms of thermal aging behavior.
[0186] Figure Labels
[0187] (1) Strip
[0188] (2) Copper core
[0189] (3) Coating
[0190] (4) Surface of copper core
[0191] (5) Geometric center of the copper core
[0192] (6) Intermediate layer
[0193] (10) Electronic components
[0194] (11) Electronic components
[0195] (12) Wedge-shaped joint
[0196] W R strip width
[0197] H R strip height
[0198] W C Width of copper core
[0199] H C The height of the copper core
[0200] T AG Thickness of silver coating
[0201] T I thickness of intermediate layer
[0202] H-height axis
[0203] W-width axis
[0204] Intersection of P1, P2, P3, and P4
Claims
1. A strip material, the strip material comprising: (i) A copper core having a surface; and (ii) A coating, said coating being superimposed on said surface of the copper core. The coating contains silver. The strip has a height and a width perpendicular to the height in a cross-sectional region perpendicular to the longitudinal axis of the strip. Wherein the ratio of height to width is less than 0.8, and The height is in the range of 50 μm to 500 μm.
2. The strip according to claim 1, wherein the cross-sectional area is 25,000 μm. 2 Up to 2mm 2 Within the range.
3. The strip according to claim 1 or 2, wherein the strip has a substantially rectangular or elliptical cross-sectional shape.
4. The strip according to any one of the preceding claims, wherein the copper core comprises at least 95% by weight of elemental copper (Cu) based on the total weight of the copper core.
5. The strip according to any one of the preceding claims, wherein the copper core contains less than 100 ppm of an additional component.
6. The strip according to any one of the preceding claims, wherein the height of the copper core is in the range of 40µm to 450µm.
7. The strip according to any one of the preceding claims, wherein the coating contains at least 85% by weight of elemental silver (Ag) based on the total weight of the coating.
8. The strip according to any one of the preceding claims, wherein the thickness of the coating is in the range of 5µm to 60µm.
9. The strip according to any one of the preceding claims, wherein an intermediate layer is disposed between the copper core and the coating.
10. The strip according to claim 9, wherein the intermediate layer comprises only the material of the copper core and the material of the coating.
11. A method for manufacturing a strip according to claims 1 to 10, the method comprising at least the following steps: I.) Provide a strip precursor comprising a copper core having a surface and a coating, wherein the coating is superimposed on the surface of the copper core, and wherein the coating comprises silver; II.) Form the strip precursor such that... The strip has a height and width in a cross-sectional region perpendicular to its longitudinal axis, wherein the width is perpendicular to the height. Wherein the ratio of height to width is less than 0.8, and The height is in the range of 50 μm to 500 μm.
12. A method for manufacturing a strip according to claims 1 to 10, the method comprising at least the following steps: I.) Provide a copper core precursor with a surface; II.) Shape the copper core precursor so that The copper core precursor has a height and width in a cross-sectional region perpendicular to the longitudinal axis of the copper core precursor, wherein the width is perpendicular to the height. Wherein the ratio of height to width is less than 0.8, and The height is in the range of 40 μm to 450 μm. III.) Coat the surface of the shaped copper core with a silver-containing coating.
13. An electronic component comprising at least the strip according to any one of claims 1 to 10 or the strip manufactured according to claim 11 or 12.
14. The electronic assembly of claim 13, wherein the strip is joined by a wedge-wedge joint.
15. A method for manufacturing an electronic component, the method comprising the following steps: I.) Provide at least two electronic components; II.) Provide a strip according to any one of claims 1 to 10 or a strip obtained by the method according to claim 11 or 12; III.) The two electronic components are connected by the strip, wherein at least one of the connections is performed by a wedge engagement.