A paper diaper with a cell-imitating multi-layer film gradient flow guiding structure and a preparation method thereof
By constructing a three-layered, cell-membrane-like stack in the diaper's distribution layer, increasing from the surface inwards, the problem of the lack of interlayer binding energy gradient design in the distribution layer is solved. This achieves non-linear acceleration of the distribution speed and a significant reduction in rewetting, thus improving the diaper's performance.
Patent Information
- Application Number
- CN202611533352.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-24
AI Technical Summary
Existing diaper distribution layers lack interlayer binding energy gradient design and step-by-step response mechanism, resulting in constant distribution speed, large rewetting volume, inability to achieve dynamic adjustment and active extraction, and inability to effectively suppress ammonia-like irritating substances in the rewetting liquid.
The diaper employs a layer-by-layer self-assembly technology to construct at least three layers of cell membrane-like stacked sequentially from the surface to the inside. The interlayer bonding energy increases along the thickness direction of the diaper, and the diaper achieves a stepwise response through hydrogen bonds, metal-coordination bonds, and covalent bonds. Combined with gradient temperature annealing and gradient penetration of crosslinking agent concentration, the diaper forms a stacked structure with increasing interlayer bonding energy, and stores shrinkage internal stress in the bottom layer.
It achieves a step-by-step response of the diversion layer, quickly guiding urine to the absorbent core, significantly reducing backflow and ammonia concentration, preventing urine accumulation and side leakage on the surface, and improving the utilization rate of the absorbent core and the skin protection effect.
Smart Images

Figure CN123148104A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of diaper technology, and particularly relates to a diaper with a cell-mimicking multilayer membrane gradient flow structure and its preparation method. Background Technology
[0002] As a disposable hygiene product, the distribution layer of a diaper is a crucial functional layer located between the top layer and the absorbent core. Its main function is to rapidly conduct liquid received by the top layer to the absorbent core and achieve uniform distribution. Current diaper distribution layers are mostly single-layer or multi-layered nonwoven fabric structures, guiding liquid penetration by coating the fiber surface with a hydrophilic agent or incorporating physical structures such as drainage holes and embossing within the fiber web. Some improved designs employ multi-layer structures, utilizing differences in fiber fineness, pore size, or hydrophilicity among the layers to create drainage channels, aiming to achieve rapid downward penetration and lateral spread of liquid. Furthermore, some technologies involve adding absorbent resin particles to the distribution layer or using a nonwoven composite structure with gradient pore sizes to improve the uniformity of liquid distribution. In recent years, some studies have attempted to introduce functional coatings or combine materials with different hydrophilic and hydrophobic properties to optimize the wettability and penetration rate of the distribution layer. Some improved solutions can shorten the liquid penetration time to within a few seconds, basically meeting the liquid absorption requirements under normal usage conditions.
[0003] However, in the aforementioned existing technologies, the liquid conductivity of the guiding layer mainly relies on the hydrophilicity of the material itself and the capillary effect between fibers. The guiding speed remains basically constant after liquid contact or gradually decreases over time, making it impossible to dynamically adjust according to the continuous impact of urine. Since the layers are mostly simultaneously wetted and respond synchronously, liquid often concentrates in localized areas of the surface layer, resulting in low utilization of the absorbent core and a large amount of reabsorption. The hydrophilic agent in the guiding layer is prone to migration and loss under repeated liquid impact, and the guiding performance decays with prolonged use. For multi-layer structures, there is a lack of clear response order and stepwise guiding mechanism between layers, and the interlayer binding energy has no gradient difference, making it difficult to achieve a sequential response from the surface inwards and active extraction of liquid from the upper layer by the lower layer. Existing guiding structures are usually passively conductive, unable to effectively suppress the concentration of irritating substances such as ammonia in the reabsorption liquid, resulting in limited skin protection. Furthermore, existing processes rely heavily on empirical optimization of material selection and physical structure design, making it difficult to achieve synergistic guiding and stepwise response between multiple layers while ensuring thinness. The root cause of the above problems lies in the lack of hierarchical design of response thresholds and driving forces in existing flow guiding structures. The response behaviors of each layer in time and space tend to be similar, making it impossible to form a stepped flow guiding and cascading amplification effect. Summary of the Invention
[0004] To overcome the above-mentioned defects of the prior art, the present invention provides a diaper with a cell-mimicking multilayer membrane gradient flow structure and its preparation method, which solves the problems of the prior art's lack of interlayer binding energy gradient design and step-by-step response mechanism, simultaneous response of each layer, constant flow velocity, large rewetting amount, and inability to achieve dynamic adjustment and active extraction.
[0005] To achieve the above objectives, the present invention provides the following technical solution: A diaper with a cell-mimicking multilayer membrane gradient flow structure and its preparation method, comprising a surface layer, an absorbent core, and a flow-guiding layer disposed between the surface layer and the absorbent core; The fluid guiding layer comprises at least three layers of cell membrane-like stacked sequentially from the surface to the inside, and the stacked layers are constructed on the substrate surface by polyelectrolytes through layer-by-layer self-assembly technology; The interlayer bonding energy between adjacent molecular layers in each layer increases sequentially from the surface layer to the bottom layer along the thickness direction of the diaper. The flow-guiding layer undergoes a progressive conformational change upon contact with urine, and the triggering conditions required for each layer to undergo conformational change increase sequentially from the surface layer to the bottom layer along the thickness direction.
[0006] Preferably, the flow guiding layer consists of a surface layer, a transition layer, and a bottom layer; The adjacent molecular layers in the surface layer are bonded by singlet hydrogen bonds and van der Waals forces, with an interlayer bonding energy of 0.5–1.5 kJ / mol·nm², a dry thickness of 80–120 nm, and a degree of crosslinking ≤3%. The transition layer is characterized by adjacent molecular layers bonded by double hydrogen bonds and metal-coordination bonds, with an interlayer bonding energy of 3.0–5.0 kJ / mol·nm², a dry thickness of 40–60 nm, and a degree of crosslinking of 5%–8%. The bottom layer is composed of adjacent molecular layers bonded by multiple hydrogen bonds, metal-coordination bonds and covalent bonds, with an interlayer bonding energy of 8.0 to 12.0 kJ / mol·nm², a dry thickness of 12 to 20 nm and a degree of crosslinking ≥12%.
[0007] Preferably, the surface layer is formed by alternating deposition of Pluronic F127 and polyacrylic acid; the transition layer is formed by deposition of a mixed solution of Pluronic F127, polyacrylic acid and imidazole-modified polyethylene glycol; and the bottom layer is formed by deposition of a mixed solution of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol and dopamine-modified hyaluronic acid.
[0008] Preferably, the surface layer has a response time of ≤0.5 seconds after contact with urine, and the surface layer thickness increases from 80-120 nm to 180-200 nm after the response; When the surface layer is completely soaked in urine and the hydrostatic pressure of the urine below the surface layer is ≥5kPa, the thickness of the transition layer is reduced from 40-60nm to 20-30nm, and the molecular chains in the transition layer are oriented and arranged perpendicular to the thickness direction of the diaper. When the transition layer is completely wetted by urine and the hydrostatic pressure of urine at the upper surface of the bottom layer is ≥15kPa, the thickness of the bottom layer is reduced from 12-20nm to 3-5nm.
[0009] Preferably, when the thickness of the bottom layer is reduced to 3-5 nm, the average spacing between adjacent molecular layers is 3-5 nm, and the capillary pressure formed within this spacing is 50-80 kPa. The capillary pressure is calculated according to the formula P=2γ·cosθ / d, where γ is the simulated urine surface tension of 45±2 mN / m, θ is the dynamic contact angle of each layer of material, and d is the average spacing between adjacent molecular layers. The average spacing is measured by atomic force microscopy or ellipsometry.
[0010] Preferably, the bottom layer stores shrinkage internal stress, which is 15% to 25% of the dry-state fracture stress of the bottom layer, and the dry-state fracture stress is determined according to GB / T1040.3-2006; the maximum tensile area of the bottom layer is 1.15 to 1.20 times the dry-state area of the bottom layer.
[0011] Preferably, simulated urine is used to vertically impact the surface of the guide layer at a flow rate of 30 mL / min, and the vertical permeation rate of the guide layer increases from the initial value to 4 to 6 times the initial value within the first 10 seconds; under the condition of 2.5 kPa pressurized re-osmosis, the re-osmosis amount is ≤0.8 g, and the ammonia nitrogen concentration in the re-osmosis liquid is reduced by ≥65% relative to the ammonia nitrogen concentration in the original urine.
[0012] Preferably, a method for preparing a diaper with a cell-mimicking multilayer membrane gradient flow structure includes the following steps: S1: Plasma pretreatment is performed on the nonwoven fabric substrate to introduce active groups on the surface of the substrate; S2: Prepare at least two different polyelectrolyte aqueous solutions, spin-coate or dip-coate them sequentially on the surface of the substrate, and dry each layer after coating to form at least three layers with progressively increasing interlayer bonding energy from the surface to the inside. S3: The laminated structure is cross-linked to form a gradient distribution of cross-linking agent in the laminate, with the concentration decreasing from the surface layer to the bottom layer; S4: Perform a stretch-release treatment on the cross-linked laminated structure to store shrinkage internal stress in the laminated structure; S5: The processed laminated structure is combined between the diaper surface layer and the absorbent core.
[0013] Preferably, the spin coating operation in step S2 is as follows: Prepare solutions A, B, and C, each with a total solute concentration of 1–2 mg / mL. In solution A, the mass ratio of Pluronic F127 to polyacrylic acid is 1:0.8–1.2; in solution B, the mass ratio of Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol is 1:0.8–1.2:0.3–0.7; and in solution C, the mass ratio of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol, and dopamine-modified hyaluronic acid is 1:0.8–1.2:0.3–0.7:0.2–0.5. The substrate is fixed on the spin coater, and solutions A, B and C are spin-coated sequentially on the substrate surface. The spin-coating speed of each solution is 500-1500 rpm and the spin-coating time is 10-30 seconds. After each spin-coating layer, the substrate is rinsed with deionized water and dried with nitrogen. Each solution is spin-coated 3-5 times to form the surface layer, transition layer and bottom layer respectively. The plasma pretreatment in step S1 is argon plasma discharge treatment, and the treatment conditions are: vacuum degree ≤10Pa, cavity pressure 20~50Pa, discharge power 90~110W, and treatment time 1.5~2.5 minutes; the non-woven fabric substrate is polypropylene spunbond non-woven fabric with a basis weight of 15~25g / m².
[0014] Preferably, the crosslinking treatment in step S3 is as follows: immersing the multilayer structure in a mixed aqueous solution of ZnCl2 and glutaraldehyde for 15–30 seconds, wherein the mass fraction of ZnCl2 in the mixed aqueous solution is 0.4%–0.6% and the mass fraction of glutaraldehyde is 0.15%–0.25%, and then curing it at 55–65°C for 1.5–2.5 hours; after the crosslinking treatment, ZnCl2… 2+ The concentration of glutaraldehyde in the laminate decreases from the surface layer to the bottom layer along the thickness direction. The concentration of the crosslinking agent in the surface layer is 1.5 to 2.0 times that in the bottom layer. The concentration distribution is determined by X-ray photoelectron spectroscopy along the cross section of the laminate. The stretch-release treatment in step S4 is as follows: the cross-linked laminated structure is stretched by 1.15 to 1.20 times along the longitudinal direction, and while in a stretched state, it is placed in an environment with a temperature of 45 to 55°C and a relative humidity of 85% to 95% for 15 to 25 minutes. The tensile force is then released to allow the laminated structure to naturally shrink back. After releasing the tensile force, the dimensional recovery rate of the surface layer is 95% to 100%, and the dimensional recovery rate of the bottom layer is 75% to 85%. The composite method described in step S5 is hot melt adhesive dot composite, and the coverage area of the dot composite is 5% to 10% of the area of the laminated structure.
[0015] The technical effects and advantages of the present invention regarding a cell-mimicking multilayer membrane gradient flow structure diaper and its preparation method are as follows: 1. This invention utilizes a gradient design of interlayer binding energy in the distribution layer, consisting of at least three layers mimicking cell membranes from the surface inwards. This design ensures the lowest binding energy at the surface layer and the highest binding energy at the bottom layer. Upon contact with urine, the surface layer responds first, swelling to quickly capture and conduct the urine downwards. As urine continues to penetrate, the transition layer and the bottom layer respond sequentially, opening the distribution channels at each level. The flow rate increases non-linearly and rapidly over time. This sequential "relay" flow mechanism, compared to traditional distribution layers, quickly directs urine to the absorbent core, effectively preventing urine accumulation and leakage at the surface. It is particularly suitable for scenarios involving frequent urination in infants or prolonged nighttime use.
[0016] 2. In this invention, the bottom layer undergoes synergistic collapse upon triggering high hydrostatic pressure, reducing the distance between adjacent molecular layers to the nanometer scale, forming a strong capillary negative pressure that continuously draws out the liquid from the upper layer. This capillary negative pressure actively draws urine that has not yet seeped into the surface and transition layers into the absorbent core, rather than relying solely on gravity and the core's absorbency. Simultaneously, the stepwise response of each layer ensures that the liquid is fully spread and conducted downwards in each layer before opening the channel to the next layer, preventing liquid retention in the surface and transition layers. The combined effect of these two mechanisms results in a significantly lower rewetting rate under pressure compared to traditional diapers, effectively reducing direct contact and irritation of the skin by urine.
[0017] 3. In this invention, the transition layer undergoes molecular chain orientation alignment upon response, forming dynamic nano-sieving channels within the layer. These channels ensure the rapid passage of water and inorganic salt ions while physically blocking and adsorbing irritating components in urine, such as large protein molecules and ammonia produced from urea decomposition. Because this invention significantly reduces the amount of liquid reabsorption, and the concentration of irritating solutes in the reabsorption solution is lower than in the original urine, it significantly reduces the chemical irritation of ammonia to the skin, synergistically preventing diaper rash from both physical isolation and chemical adsorption perspectives.
[0018] 4. In this invention, the surface layer, transition layer, and bottom layer respond sequentially, with the bottom layer generating a siphon suction effect. This allows urine to spread evenly along the plane of the diaper surface before being conducted downwards, preventing urine from concentrating and impacting a specific area of the absorbent core. This uniform flow mechanism ensures that all areas of the absorbent core, both longitudinally and laterally, are fully utilized, avoiding the problem of oversaturation at the front and dryness at the back of the core, which is common in traditional diapers. This extends the effective lifespan of the diaper.
[0019] 5. This invention achieves a one-step formation of a multilayer structure with increasing interlayer bonding energy from the surface to the interior by sequentially spin-coating or dip-coating polyelectrolyte solutions of different compositions onto a substrate surface, combined with gradient temperature annealing and gradient penetration of crosslinking agent concentration. Then, a stretch-release treatment stores shrinkage stress in the bottom layer. Each step utilizes mature industrial equipment with clearly defined and controllable process parameters, enabling continuous operation on roll-to-roll production lines. It eliminates the need for complex semiconductor-grade precision processing equipment such as photolithography and etching, thus keeping production costs under control. Furthermore, by adjusting process parameters such as the number of spin-coating repetitions, crosslinking time, and stretching ratio, the thickness, bonding energy, degree of crosslinking, and shrinkage stress of each layer can be precisely controlled, resulting in excellent process reproducibility and product consistency.
[0020] 6. In this invention, the dry thickness of each membrane layer is at the nanometer level (the thinnest being only 12-20 nm), and the total thickness can be controlled within 200 nm, giving the diaper its ultra-thin absorbent layer characteristics. Furthermore, the laminated structure of this invention is not limited to three layers; it can be expanded to four or more layers according to product needs to adapt to disposable hygiene products such as diapers, pull-ups, and sanitary napkins with different absorbency and usage scenarios, demonstrating good category versatility and product upgrade potential. Attached Figure Description
[0021] Figure 1 This is a flowchart of a cell-mimicking multilayer membrane gradient flow structure diaper and its preparation method, as proposed in this invention.
[0022] Figure 2 This is a schematic diagram of the overall cross-sectional structure of a cell-mimicking multilayer membrane gradient flow-guiding diaper and its preparation method proposed in this invention.
[0023] Legend: 1. Surface layer; 2. Flow guiding layer; 3. Absorbent core; 4. Non-woven fabric substrate; 5. Cell membrane-like stack. Detailed Implementation
[0024] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0025] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include," "contain," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitation, an element defined by the phrase "includes..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.
[0026] refer to Figure 1 This invention provides a diaper with a cell-mimicking multilayer membrane gradient flow structure and its preparation method. The diaper includes a top layer 1, an absorbent core 3, and a flow-guiding layer 2 disposed between the two. The flow-guiding layer 2 comprises at least three cell-mimicking membrane stacks 5, layered sequentially from the surface to the bottom, constructed from polyelectrolytes using a layer-by-layer self-assembly technique. The interlayer bonding energy between adjacent molecular layers increases sequentially from the surface to the bottom layer along the thickness direction, and the triggering conditions required for conformational changes in each layer also increase sequentially along the thickness direction. The preparation method includes: plasma pretreatment of a nonwoven fabric substrate 4; preparation of at least two or more polyelectrolyte aqueous solutions and sequential spin-coating or dip-coating to form at least three-layer stacked structures; cross-linking treatment to create a gradient distribution of cross-linking agents with decreasing concentrations from the surface to the bottom layer; stretch-release treatment to store shrinkage stress in the bottom layer; and lamination between the top layer 1 and the absorbent core 3. This invention achieves nonlinear acceleration of flow rate, significantly reduces rewetting and ammonia nitrogen concentration in the rewetting solution, and is suitable for the field of disposable hygiene products.
[0027] Test method: Preparation of simulated urine: The simulated urine used in the following examples and comparative examples consisted of: 0.9 g NaCl, 1.0 g urea, and 0.1 g peptone, diluted to 100 mL with deionized water, and the pH was adjusted to 6.5 ± 0.5 with 0.1 mol / L HCl or 0.1 mol / L NaOH. The surface tension was 45 ± 2 mN / m and was measured at 25 °C using the platinum plate method.
[0028] Methods for determining interlayer bonding energy: In the following embodiments, the interlayer binding energy of the surface layer, transition layer, and bottom layer was determined using differential scanning calorimetry (DSC). The specific steps were as follows: each layer sample was cut into 5mm × 5mm pieces and placed in an aluminum DSC sample pan. The sample was heated from 25℃ to 200℃ at a heating rate of 5℃ / min, and the peak temperature Tm of the dissociation endothermic peak for each layer was recorded. The interlayer binding energy E was calculated according to the Arrhenius equation: E = R·Tm·ln(A / β), where R is the gas constant (8.314 J / mol·K) and A is the pre-exponential factor (1.0 × 10⁻⁶). 13 s -1 β is the heating rate, 5℃ / min = 0.0833K / s.
[0029] Methods for determining the thickness of each layer: In the following embodiments, the dry-state thickness and post-response thickness of each layer were measured using an ellipsometer with an incident angle of 70° and a wavelength of 632.8 nm. The arithmetic mean of measurements were taken at five different locations for each sample. The average spacing between adjacent molecular layers when the bottom layer thickness was reduced to 3–5 nm was measured using an atomic force microscope (AFM) in tapping mode along the membrane cross-section.
[0030] Test method for vertical permeation rate: In the following embodiments, the vertical permeation rate of the diversion layer 2 was determined as follows: the sample of the diversion layer 2 to be tested was cut into 10cm×10cm pieces and placed horizontally on the test stage. A peristaltic pump was used to vertically impact the surface of the diversion layer 2 with simulated urine at a flow rate of 30mL / min. The permeation rates at the end of the 1st second and the end of the 10th second were recorded in mL / min. The ratio of the rate at the end of the 10th second to the rate at the end of the 1st second was calculated.
[0031] Test methods for re-infiltration rate and ammonia nitrogen reduction rate: The reabsorption volume was determined according to the 2.5 kPa pressurized reabsorption test method specified in GB / T28004.1-2021. The ammonia nitrogen concentration in the reabsorption solution was determined using the Nessler's reagent colorimetric method (HJ535-2009), and the reduction rate was calculated based on the ammonia nitrogen concentration in the original urine. Example 1
[0032] Purpose of implementation: This embodiment provides a basic implementation scheme of the present invention, namely, to prepare a three-layer gradient flow structure consisting of a surface layer, a transition layer and a bottom layer under the reference process parameters, and to verify the basic technical effect of the present invention.
[0033] Implementation steps: S1: Take a 20 g / m² polypropylene spunbond nonwoven fabric as the substrate and cut it into 30 cm × 30 cm pieces. Place the substrate in a plasma treatment device, evacuate to a vacuum degree ≤ 10 Pa, introduce argon gas until the chamber pressure is 35 Pa, and treat for 2 minutes at a discharge power of 100 W to introduce hydroxyl active groups on the surface of the substrate.
[0034] S2: Prepare three aqueous solutions of polyelectrolytes, all using deionized water as the solvent, with a total solute concentration of 1.5 mg / mL in each solution. Solution A: Pluronic F127 and polyacrylic acid are mixed at a mass ratio of 1:1; Solution B: Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol are mixed in a mass ratio of 1:1:0.5; Solution C: Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol and dopamine-modified hyaluronic acid were mixed in a mass ratio of 1:1:0.5:0.3.
[0035] The substrate treated with S1 was fixed on the spin coater turntable. First, solution A was dropped onto the substrate surface until it was completely covered, and the coating was spin-coated at 800 rpm for 20 seconds. After rinsing with deionized water, it was dried with nitrogen. This operation was repeated 4 times to form a surface layer on the substrate. Then, solution B was dropped onto the surface layer, and the coating was spin-coated at 1000 rpm for 20 seconds. After rinsing with deionized water, it was dried with nitrogen. This operation was repeated 4 times to form a transition layer. Finally, solution C was dropped onto the transition layer, and the coating was spin-coated at 1200 rpm for 20 seconds. After rinsing with deionized water, it was dried with nitrogen. This operation was repeated 4 times to form the bottom layer.
[0036] S3: The multilayer film obtained in S2 is placed on a gradient hot plate for annealing. The upper surface temperature of the gradient hot plate is 40℃, and the lower surface temperature is 80℃. The multilayer film is placed on the upper surface of the gradient hot plate, and the annealing time is 15 minutes. After annealing, the surface area temperature is approximately 40℃, the bottom layer temperature is approximately 80℃, and the temperature in the transition layer area shows a gradient distribution.
[0037] S4: Immerse the multilayer film obtained in S3 in the crosslinking solution for 20 seconds. The crosslinking solution is an aqueous solution of ZnCl2 and glutaraldehyde, wherein the mass fraction of ZnCl2 is 0.5% and the mass fraction of glutaraldehyde is 0.2%. After removal, cure at 60°C for 2 hours.
[0038] S5: Apply a stretch of 1.18 times to the longitudinal direction of the multilayer film obtained in S4, keep it under stretch and place it in an environment with a temperature of 50°C and a relative humidity of 90% for 20 minutes, then release the stretching force and allow the multilayer film to shrink naturally.
[0039] S6: The multilayer film obtained in S5 is fixed between the diaper surface layer 1 and the absorbent core 3 by hot melt adhesive dot bonding. The coverage area of the dot bonding is 8% of the multilayer film area. Implementation results:
[0040] The structural parameters were determined according to the testing method described above. In the flow-guiding layer 2 obtained in this embodiment, the surface layer has a dry thickness of 95 nm, an interlayer binding energy of 1.0 kJ / mol·nm², and a crosslinking degree of 2.5%; the transition layer has a dry thickness of 48 nm, an interlayer binding energy of 4.0 kJ / mol·nm², and a crosslinking degree of 6.5%; and the bottom layer has a dry thickness of 16 nm, an interlayer binding energy of 10.0 kJ / mol·nm², and a crosslinking degree of 13.5%. The interlayer binding energy of the surface layer, transition layer, and bottom layer increases sequentially from the surface layer to the bottom layer along the thickness direction of the diaper.
[0041] The dynamic response performance was tested according to the test method described above. The surface layer responded within 0.4 seconds after contact with urine, and the surface layer thickness increased from 95 nm to 190 nm. When the surface layer was completely wetted by urine and the hydrostatic pressure of urine below the surface layer reached 5 kPa, the thickness of the transition layer decreased from 48 nm to 25 nm, and the molecular chains in the transition layer were oriented perpendicular to the thickness direction of the diaper. When the transition layer was completely wetted by urine and the hydrostatic pressure of urine at the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 16 nm to 4 nm, the average spacing between adjacent molecular layers of the bottom layer was 4 nm, and the capillary pressure formed within this spacing was 65 kPa.
[0042] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate of the diversion layer 2 increased from the initial value to 5.2 times the initial value within the first 10 seconds; under the pressure of 2.5 kPa reabsorption, the reabsorption volume was 0.5 g; the ammonia nitrogen concentration in the reabsorption solution decreased by 72% relative to the ammonia nitrogen concentration in the original urine. Example 2
[0043] Purpose of implementation: This embodiment aims to verify the variation law of each layer thickness and interlayer bonding energy with the number of spin coatings by reducing the number of spin coatings for the surface and transition layers and increasing the number of spin coatings for the bottom layer, as well as the impact of this variation on the conductivity.
[0044] Implementation steps: The only difference from Example 1 is that in S2, solution A is repeatedly spin-coated 3 times to form the surface layer, solution B is repeatedly spin-coated 3 times to form the transition layer, and solution C is repeatedly spin-coated 5 times to form the bottom layer. The remaining steps are exactly the same as in Example 1. Implementation results:
[0045] The structural parameters were determined according to the test method described above. In the flow guiding layer 2 obtained in this embodiment, the surface layer has a dry thickness of 82 nm, an interlayer binding energy of 0.6 kJ / mol·nm², and a crosslinking degree of 2.0%; the transition layer has a dry thickness of 42 nm, an interlayer binding energy of 3.2 kJ / mol·nm², and a crosslinking degree of 5.5%; and the bottom layer has a dry thickness of 19 nm, an interlayer binding energy of 11.5 kJ / mol·nm², and a crosslinking degree of 14.5%. The binding energies of the three layers still show an increasing distribution, but the increase in the number of spin coatings on the bottom layer increases the thickness of the bottom layer and the binding energy, while the decrease in the number of spin coatings on the surface layer decreases the thickness of the surface layer and the binding energy. Therefore, the interlayer binding energy gradient difference between the bottom layer and the surface layer increases from 9.0 in Example 1 to 10.9.
[0046] The dynamic response performance was tested according to the test method described above. The surface layer responded within 0.3 seconds after contact with urine, and its thickness increased from 82 nm to 182 nm. When the hydrostatic pressure below the surface layer reached 5 kPa, the thickness of the transition layer decreased from 42 nm to 22 nm. When the hydrostatic pressure on the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 19 nm to 3 nm. The average spacing between adjacent molecular layers was 3 nm, and the capillary pressure was 78 kPa.
[0047] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate increased to 4.8 times the initial value within the first 10 seconds; the reabsorption amount was 0.6g; and the ammonia nitrogen reduction rate was 68%.
[0048] This embodiment confirms that effective gradient conduction can be achieved for each layer with a surface thickness of 82 nm, a transition layer thickness of 42 nm, a bottom layer thickness of 19 nm, and a binding energy range of 0.6–11.5 kJ / mol·nm². Example 3
[0049] Purpose of implementation: This embodiment aims to verify the influence of the degree of crosslinking on interlayer bonding energy and conductivity by extending the crosslinking soaking time, and to determine the optimal range of crosslinking time.
[0050] Implementation steps: The only difference from Example 1 is that the crosslinking solution soaking time in S4 is 30 seconds, and the rest of the steps are exactly the same as in Example 1. Implementation results:
[0051] The structural parameters were determined according to the testing method described above. In the flow guiding layer 2 obtained in this embodiment, the surface layer has a dry thickness of 92 nm, an interlayer binding energy of 1.2 kJ / mol·nm², and a crosslinking degree of 2.8%; the transition layer has a dry thickness of 45 nm, an interlayer binding energy of 4.5 kJ / mol·nm², and a crosslinking degree of 7.2%; and the bottom layer has a dry thickness of 14 nm, an interlayer binding energy of 11.0 kJ / mol·nm², and a crosslinking degree of 15.0%. Extending the soaking time increased the crosslinking degree and binding energy of each layer, but reduced the thickness of the bottom layer.
[0052] The dynamic response performance was tested according to the test method described above. The surface layer responded within 0.4 seconds after contact with urine, and its thickness increased from 92 nm to 185 nm. When the hydrostatic pressure below the surface layer reached 5 kPa, the thickness of the transition layer decreased from 45 nm to 27 nm. When the hydrostatic pressure on the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 14 nm to 5 nm. The average spacing between adjacent molecular layers was 5 nm, and the capillary pressure was 52 kPa.
[0053] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate increased to 4.2 times the initial value within the first 10 seconds; the reabsorption amount was 0.7g; and the ammonia nitrogen reduction rate was 66%.
[0054] This embodiment confirms that extending the crosslinking time to 30 seconds improves the degree of crosslinking and binding energy of each layer. However, the excessively high crosslinking rate of the bottom layer (15.0%) leads to a decrease in its response collapse ability. The minimum thickness after collapse is 5 nm, which is greater than 4 nm in Example 1. The capillary pressure decreases to 52 kPa, and the overall performance of the trousers is slightly inferior to that of Example 1. Therefore, the crosslinking time should not be too long, and 20 seconds is a better choice. Example 4
[0055] Purpose of implementation: This embodiment aims to verify the influence of the magnitude of shrinkage internal stress on the collapse of the bottom layer and the siphon effect by adjusting the stretching ratio, and to determine the optimal range of the stretching ratio.
[0056] Implementation steps: The only difference from Example 1 is that the stretching ratio in S5 is 1.15 times, and the rest of the steps are exactly the same as in Example 1. Implementation results:
[0057] The structural parameters were determined according to the test method described above. In the flow-guiding layer 2 obtained in this embodiment, the surface dry-state thickness is 98 nm, the interlayer binding energy is 0.9 kJ / mol·nm², and the crosslinking degree is 2.3%; the transition layer dry-state thickness is 50 nm, the interlayer binding energy is 3.8 kJ / mol·nm², and the crosslinking degree is 6.2%; the bottom layer dry-state thickness is 18 nm, the interlayer binding energy is 9.5 kJ / mol·nm², and the crosslinking degree is 12.5%. The bottom layer stores shrinkage internal stress. After measuring the bottom layer dry-state fracture stress according to GB / T1040.3-2006, the shrinkage internal stress is calculated to be 18% of the bottom layer dry-state fracture stress.
[0058] The dynamic response performance was tested according to the test method described above. Within 0.5 seconds of contact with urine, the surface layer responded, and its thickness increased from 98 nm to 192 nm. When the hydrostatic pressure below the surface layer reached 5 kPa, the thickness of the transition layer decreased from 50 nm to 28 nm. When the hydrostatic pressure on the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 18 nm to 4 nm, the average spacing between adjacent molecular layers was 4 nm, and the capillary pressure was 62 kPa.
[0059] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate increased to 4.5 times the initial value within the first 10 seconds; the reabsorption amount was 0.6g; and the ammonia nitrogen reduction rate was 69%.
[0060] This embodiment confirms that after the stretching ratio is reduced from 1.18 times to 1.15 times, the internal stress of shrinkage stored in the bottom layer is reduced from about 20% to 18%, and the bottom layer can still reach 4nm after collapse. The capillary pressure is 62kPa. The overall performance of the pants is slightly lower than that of Example 1, but still significantly better than the comparative example, indicating that a good flow-guiding effect can be achieved in the stretching ratio range of 1.15 to 1.20 times. Example 5
[0061] Purpose of implementation: This embodiment verifies the feasibility and performance stability of the present invention under the boundary conditions of substrate and material ratio by reducing the basis weight of the substrate and adjusting the material ratio of each layer to the lower limit of the range.
[0062] Implementation steps: The difference from Example 1 is as follows: the substrate weight in S1 is 15 g / m²; in S2, the mass ratio of Pluronic F127 to polyacrylic acid in solution A is 1:0.8, the mass ratio of Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol in solution B is 1:0.8:0.3, and the mass ratio of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol, and dopamine-modified hyaluronic acid in solution C is 1:0.8:0.3:0.2. The remaining steps are exactly the same as in Example 1. Implementation results:
[0063] The structural parameters were determined according to the testing method described above. In the flow-guiding layer 2 obtained in this embodiment, the surface dry layer has a thickness of 85 nm, an interlayer binding energy of 0.7 kJ / mol·nm², and a crosslinking degree of 2.1%; the transition layer has a dry thickness of 42 nm, an interlayer binding energy of 3.5 kJ / mol·nm², and a crosslinking degree of 5.8%; and the bottom layer has a dry thickness of 13 nm, an interlayer binding energy of 9.0 kJ / mol·nm², and a crosslinking degree of 12.8%.
[0064] The dynamic response performance was tested according to the test method described above. The surface layer responded within 0.3 seconds after contact with urine, and its thickness increased from 85 nm to 180 nm. When the hydrostatic pressure below the surface layer reached 5 kPa, the thickness of the transition layer decreased from 42 nm to 20 nm. When the hydrostatic pressure on the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 13 nm to 3 nm. The average spacing between adjacent molecular layers was 3 nm, and the capillary pressure was 80 kPa.
[0065] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate increased to 5.8 times the initial value within the first 10 seconds; the reabsorption amount was 0.4g; and the ammonia nitrogen reduction rate was 75%.
[0066] This embodiment demonstrates that the lower limit of the material ratio range can still achieve excellent flow conductivity, and it is superior to Example 1 in some indicators, providing boundary support for the ratio range. Example 6
[0067] Purpose of implementation: This embodiment adopts a four-layer stacked structure of surface layer + first transition layer + second transition layer + bottom layer to verify that the technical solution of the present invention is not limited to a three-layer structure, but can be extended to four layers or more, thereby providing direct experimental support for the higher-level generalization of "at least three layers".
[0068] Implementation steps: S1: Take a 20 g / m² polypropylene spunbond nonwoven fabric as the substrate and cut it into 30 cm × 30 cm pieces. Place the substrate in a plasma treatment device, evacuate to a vacuum degree ≤ 10 Pa, introduce argon gas until the chamber pressure is 35 Pa, and treat for 2 minutes at a discharge power of 100 W to introduce hydroxyl active groups on the surface of the substrate.
[0069] S2: Prepare four different polyelectrolyte aqueous solutions, all using deionized water as the solvent, with a total solute concentration of 1.5 mg / mL in each solution. Solution A: Pluronic F127 and polyacrylic acid are mixed at a mass ratio of 1:1 and used as a surface layer; Solution B1: Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol are mixed in a mass ratio of 1:1:0.4 and used for the first transition layer; Solution B2: Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol are mixed in a mass ratio of 1:1:0.6 for the second transition layer; Solution C: Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol and dopamine-modified hyaluronic acid were mixed in a mass ratio of 1:1:0.5:0.3 and used as the base layer.
[0070] Fix the S1-treated substrate onto the spin coater turntable. Perform the following spin coating operations sequentially: First, add solution A to the substrate surface until it is completely covered. Spin coat at 800 rpm for 20 seconds, rinse with deionized water and dry with nitrogen. Repeat this operation 4 times to form a surface layer.
[0071] Then, solution B1 was dropped onto the surface and spin-coated at 900 rpm for 20 seconds. After rinsing with deionized water and drying with nitrogen, the operation was repeated 3 times to form the first transition layer.
[0072] Then, solution B2 was dropped onto the surface of the first transition layer, and the mixture was spin-coated at 1000 rpm for 20 seconds. After rinsing with deionized water and drying with nitrogen, the process was repeated three times to form the second transition layer.
[0073] Finally, solution C was dropped onto the surface of the second transition layer, and the mixture was spin-coated at 1200 rpm for 20 seconds. After rinsing with deionized water and drying with nitrogen, the process was repeated 4 times to form the bottom layer.
[0074] This forms a four-layered structure from the outside in, consisting of the outermost layer, the first transition layer, the second transition layer, and the bottom layer.
[0075] S3: The four-layer stacked structure obtained in S2 is placed on a gradient hot plate for annealing. The upper surface temperature of the gradient hot plate is 40℃, and the lower surface temperature is 80℃. The stacked structure is placed on the upper surface of the gradient hot plate, and the annealing time is 15 minutes. After annealing, the surface area temperature is approximately 40℃, the bottom layer temperature is approximately 80℃, and the temperatures of the first transition layer and the second transition layer are approximately 50℃ and 65℃ respectively, showing a gradient distribution.
[0076] S4: Immerse the multilayer structure obtained in S3 in the crosslinking solution for 20 seconds. The crosslinking solution is an aqueous solution of ZnCl2 and glutaraldehyde, wherein the mass fraction of ZnCl2 is 0.5% and the mass fraction of glutaraldehyde is 0.2%. After removal, cure at 60°C for 2 hours.
[0077] S5: Apply a 1.18 times stretch to the longitudinal direction of the laminated structure obtained in S4, keep it under tension and place it in an environment with a temperature of 50℃ and a relative humidity of 90% for 20 minutes, then release the tension and allow the laminated structure to shrink naturally.
[0078] S6: The laminated structure obtained in S5 is fixed between the diaper surface layer 1 and the absorbent core 3 by hot melt adhesive dot bonding. The coverage area of the dot bonding is 8% of the laminated structure area. Implementation results:
[0079] The structural parameters were determined according to the testing method described above. In the flow guide layer 2 obtained in this embodiment: The surface dry layer has a thickness of 90 nm, an interlayer binding energy of 0.9 kJ / mol·nm², and a crosslinking degree of 2.3%. The first transition layer has a dry state thickness of 38 nm, an interlayer binding energy of 2.8 kJ / mol·nm², and a crosslinking degree of 4.5%. The second transition layer has a dry state thickness of 35 nm, an interlayer binding energy of 4.8 kJ / mol·nm², and a crosslinking degree of 7.2%. The dry layer thickness is 15 nm, the interlayer binding energy is 10.5 kJ / mol·nm², and the degree of crosslinking is 14.0%.
[0080] The interlayer bonding energy of each layer increases sequentially from the top layer to the bottom layer along the thickness direction of the diaper: 0.9 < 2.8 < 4.8 < 10.5. The bonding energy differences between adjacent layers are 1.9, 2.0, and 5.7, respectively, all showing an increasing trend.
[0081] The dynamic response performance was tested using the method described above. The surface layer responded within 0.4 seconds of contact with urine, increasing in thickness from 90 nm to 185 nm. When the hydrostatic pressure of the urine below the surface layer reached 3 kPa, the thickness of the first transition layer decreased from 38 nm to 28 nm, and the molecular chains began to align. When the first transition layer was completely wetted and the hydrostatic pressure reached 6 kPa, the thickness of the second transition layer decreased from 35 nm to 22 nm. When the second transition layer was completely wetted and the hydrostatic pressure of the urine at the upper surface of the bottom layer reached 15 kPa, the thickness of the bottom layer decreased from 15 nm to 4 nm. The average spacing between adjacent molecular layers in the bottom layer was 4 nm, and the capillary pressure formed within this spacing was 63 kPa.
[0082] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate of the diversion layer 2 increased from the initial value to 4.9 times the initial value within the first 10 seconds; under the pressure of 2.5 kPa reabsorption, the reabsorption volume was 0.5 g; the ammonia nitrogen concentration in the reabsorption solution decreased by 71% relative to the ammonia nitrogen concentration in the original urine.
[0083] This embodiment demonstrates that the technical solution of the present invention can be extended to a four-layer stacked structure, and the four-layer structure can also achieve a step-by-step response from the surface to the inside, bottom-layer collapse siphon, and excellent overall flow conduction performance, which is comparable to the performance of the three-layer structure in Embodiment 1. This proves that the general term "at least three layers" is fully supported by the specification.
[0084] Comparative Example 1 Purpose of this example: This comparative example uses a uniform single-layer structure to replace the three-layer gradient structure, while the rest of the process remains the same as in Example 1, in order to verify the decisive influence of the presence or absence of the gradient structure on the flow conduction performance.
[0085] Implementation steps: S1: Exactly the same as S1 in Example 1.
[0086] S2: Prepare an aqueous solution of a polyelectrolyte, using deionized water as the solvent, with a total solute concentration of 1.5 mg / mL. This solution is a mixture of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol, and dopamine-modified hyaluronic acid in a mass ratio of 1:1:0.5:0.3, which is the same composition as solution C in Example 1. Fix the substrate treated in S1 onto the spin coater turntable, and drop the above solution onto the substrate surface until it is completely covered. Spin coat at 1200 rpm for 20 seconds, rinse with deionized water, and dry with nitrogen. Repeat this operation 12 times, resulting in a total of 12 layers, equivalent to the total of 12 layers in Example 1 (three layers combined), forming a single-type multilayer film on the substrate surface.
[0087] S3: The multilayer film obtained in S2 is placed on a constant-temperature hot plate for annealing. The hot plate temperature is 60℃, and the annealing time is 15 minutes for uniform annealing without forming a temperature gradient field.
[0088] S4~S6: exactly the same as S4~S6 in Example 1. Implementation results:
[0089] The structural parameters were determined according to the test method described above. The flow-guiding layer 2 obtained in this comparative example is a uniform single-layer structure without a stacked gradient structure, with an overall dry thickness of 185 nm, an overall interlayer binding energy of 10.0 kJ / mol·nm², and an overall crosslinking degree of 13.5%. Since each layer has the same composition and has undergone uniform annealing treatment, there is no increasing gradient in interlayer binding energy from the surface layer to the bottom layer.
[0090] The dynamic response performance was tested using the method described above. The guide layer 2 obtained in this comparative example swelled entirely within approximately 0.3 seconds after contact with urine, increasing in thickness from 185 nm to 210 nm. However, due to the absence of a gradient binding energy structure, all parts responded simultaneously, and no stepwise conformational changes were observed. Under continuous liquid impact, the guide layer 2 maintained a uniform swelling state, without any cooperative collapse response of the underlying layers, nor was any capillary negative pressure extraction effect generated by the collapse of the underlying layers observed.
[0091] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate of the diversion layer 2 increased from the initial value to 1.3 times the initial value within the first 10 seconds; under the condition of 2.5 kPa pressurized reabsorption, the reabsorption volume was 2.8 g; the ammonia nitrogen concentration in the reabsorption solution decreased by 18% relative to the ammonia nitrogen concentration in the original urine.
[0092] The results of this comparative example show that, without an interlayer binding energy gradient, even if the material composition, total number of layers, and crosslinking treatment are the same as in Example 1, it is still impossible to achieve stepwise response and bottom-layer siphon extraction, and all performance characteristics are far inferior to those of Example 1.
[0093] Comparative Example 2 Purpose of this example: While maintaining the three-layer physical layering and gradient annealing, this comparative example eliminates the crosslinking agent gradient by stirring and shaking during the crosslinking process, while keeping the rest of the process consistent with Example 1. This is used to verify the necessity of the crosslinking agent gradient for the formation of the interlayer binding energy gradient.
[0094] Implementation steps: S1: Exactly the same as S1 in Example 1.
[0095] S2: Exactly the same as S2 in Example 1.
[0096] S3: Exactly the same as S3 in Example 1.
[0097] S4: Immerse the multilayer membrane obtained in S3 into the crosslinking solution for 20 seconds. The crosslinking solution is an aqueous solution of ZnCl2 and glutaraldehyde, wherein the mass fraction of ZnCl2 is 0.5% and the mass fraction of glutaraldehyde is 0.2%. The difference from Example 1 is that in this comparative example, the solution is continuously magnetically stirred at 300 rpm during the crosslinking process to maintain a uniform concentration of the crosslinking agent in the solution, and the multilayer membrane is immersed in a horizontal swaying motion at a swaying frequency of 60 times / minute to ensure uniform penetration concentration of the crosslinking agent in each layer of the multilayer membrane. After removal, it is cured at 60°C for 2 hours.
[0098] S5~S6: exactly the same as S5~S6 in Example 1. Implementation results:
[0099] The structural parameters were determined according to the test methods described above, and the crosslinking agent concentration distribution along the laminated cross-section was determined using X-ray photoelectron spectroscopy (XPS). In the conductive layer 2 obtained in this comparative example, the surface layer has a dry state thickness of 96 nm, an interlayer binding energy of 1.8 kJ / mol·nm², and a crosslinking degree of 4.2%; the transition layer has a dry state thickness of 50 nm, an interlayer binding energy of 5.5 kJ / mol·nm², and a crosslinking degree of 8.5%; and the bottom layer has a dry state thickness of 17 nm, an interlayer binding energy of 6.0 kJ / mol·nm², and a crosslinking degree of 9.0%. The crosslinking agent concentration distribution along the thickness direction is as follows: the ratio of crosslinking agent concentration in the surface layer to that in the bottom layer is approximately 1.1:1, which is basically uniform, and no significant gradient distribution is formed. Although the three-layer structure exists physically, the crosslinking degree of each layer differs much less than that in Example 1 due to the uniform penetration of the crosslinking agent. In Example 1, the crosslinking degree ratio of the surface layer to the bottom layer is 2.5%:13.5%≈1:5.4, while in this comparative example it is 4.2%:9.0%≈1:2.1. As a result, although the interlayer bonding energy is slightly different, no significant increasing gradient is formed. The surface layer is 1.8, the transition layer is 5.5, and the bottom layer is 6.0. The difference between the surface layer and the bottom layer is 4.2, while the difference between the surface layer and the bottom layer in Example 1 is 9.0.
[0100] Dynamic response performance was tested using the method described above. Within 0.4 seconds of contact with urine, the surface layer responded, increasing in thickness from 96 nm to 165 nm, but with limited swelling. When the hydrostatic pressure of urine below the surface layer reached 5 kPa, the transition layer thickness decreased from 50 nm to 35 nm, indicating incomplete orientation. When the hydrostatic pressure of urine at the upper surface of the bottom layer reached 15 kPa, the bottom layer thickness decreased only from 17 nm to 11 nm, with no significant synergistic collapse. The spacing between adjacent molecular layers was approximately 11 nm, and the capillary pressure was only about 18 kPa. Due to the insufficient cross-linking degree of the bottom layer compared to the surface layer, the internal shrinkage stress stored in the bottom layer was only about 8% of the dry-state fracture stress, resulting in insufficient release under liquid impact.
[0101] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate of the diversion layer 2 increased from the initial value to 2.5 times the initial value within the first 10 seconds; under the condition of 2.5 kPa pressurized reabsorption, the reabsorption volume was 1.8 g; the ammonia nitrogen concentration in the reabsorption solution decreased by 35% relative to the ammonia nitrogen concentration in the original urine.
[0102] The results of this comparative example show that physical layering and gradient annealing alone, without a crosslinking agent gradient, cannot form a sufficient binding energy gradient difference. The response behavior of each layer tends to be the same, and effective step-like flow conduction and bottom layer collapse siphon cannot be achieved. This proves that the gradient distribution of the crosslinking agent is a necessary process condition for forming a significant interlayer binding energy gradient.
[0103] Comparative Example 3 Purpose of this example: While maintaining the three-layer gradient structure, this comparative example omits the stretching-release process step S5, i.e., does not perform pre-stretching energy storage, and the rest of the process is consistent with Example 1. This is used to verify the auxiliary enhancement effect of shrinkage internal stress on the completeness of the bottom layer collapse and the siphon effect.
[0104] Implementation steps: S1~S4: exactly the same as S1~S4 in Example 1.
[0105] S5: Omitted, meaning S6 is performed directly after S4.
[0106] S6: Exactly the same as S6 in Example 1. Implementation results:
[0107] The structural parameters were determined according to the test method described above. In the flow-guiding layer 2 obtained in this comparative example, the surface layer has a dry thickness of 100 nm, an interlayer binding energy of 0.9 kJ / mol·nm², and a crosslinking degree of 2.3%; the transition layer has a dry thickness of 52 nm, an interlayer binding energy of 3.8 kJ / mol·nm², and a crosslinking degree of 6.2%; and the bottom layer has a dry thickness of 20 nm, an interlayer binding energy of 9.5 kJ / mol·nm², and a crosslinking degree of 13.0%. The interlayer binding energy of the three-layer structure shows an increasing gradient: surface layer 0.9 < transition layer 3.8 < bottom layer 9.5. However, due to the lack of stretch-release treatment, no shrinkage internal stress is stored in the bottom layer.
[0108] The dynamic response performance was tested according to the test method described above. Within 0.4 seconds of contact with urine, the surface layer responded, increasing in thickness from 100 nm to 188 nm. When the hydrostatic pressure below the surface reached 5 kPa, the transition layer thickness decreased from 52 nm to 27 nm. When the hydrostatic pressure on the upper surface of the bottom layer reached 15 kPa, the bottom layer thickness decreased from 20 nm to 8 nm. Although the bottom layer exhibited a collapse response, due to the lack of pre-stored contractile internal stress to aid in its release, the collapse was incomplete, and the final thickness only decreased to 8 nm. In Example 1, this could be reduced to 4 nm, with an average spacing of 8 nm between adjacent molecular layers and a capillary pressure of only 28 kPa, far lower than the 65 kPa in Example 1. Therefore, the reverse extraction force on the upper liquid was significantly insufficient.
[0109] The overall performance of the trousers was tested according to the test method described above. The vertical permeation rate of the diversion layer 2 increased from the initial value to 3.0 times the initial value within the first 10 seconds; under the condition of 2.5 kPa pressurized reabsorption, the reabsorption volume was 1.5 g; the ammonia nitrogen concentration in the reabsorption solution decreased by 42% relative to the ammonia nitrogen concentration in the original urine.
[0110] The results of this comparative example demonstrate that while the presence of the gradient structure is sufficient to drive partial collapse of the underlying layer, the lack of contractile internal stress leads to incomplete collapse, insufficient capillary pressure, and limited extraction effect. Compared with Example 1, this proves that contractile internal stress plays a crucial auxiliary role in enhancing the completeness of the underlying layer collapse.
[0111] Results Analysis The effect of the presence or absence of gradient structure on flow conduction performance Examples 1-5 were compared with Comparative Example 1. The guiding layer 2 in Examples 1-5 all possessed a gradient structure with interlayer binding energy increasing sequentially from the surface to the bottom layer, with binding energy gradient differences of 9.0, 10.9, 9.8, 8.6, and 8.3, respectively. Upon contact with urine, it underwent a stepwise conformational change from the surface inwards, with the minimum thickness after the bottom layer collapsed reaching 3-5 nm, generating a capillary negative pressure of 52-80 kPa. In contrast, Comparative Example 1, lacking a gradient structure, had a binding energy gradient difference of 0, with all parts responding simultaneously, without stepwise response or coordinated bottom layer collapse, and a capillary pressure of 0.
[0112] Regarding overall performance, the vertical permeation rate of Examples 1-5 increased by 4.2-5.8 times, while that of Comparative Example 1 was only 1.3 times; the reabsorption amount of Examples 1-5 was 0.4-0.7g, while that of Comparative Example 1 was 2.8g; and the ammonia nitrogen reduction rate of Examples 1-5 was 66%-75%, while that of Comparative Example 1 was only 18%. These comparative results demonstrate that the gradient structure is the core technical feature for achieving step-by-step response, bottom-layer siphon extraction, and low reabsorption.
[0113] The effect of crosslinking agent gradient on the formation of binding energy gradient Example 1 and Comparative Example 2 were compared and analyzed. Example 1 used a static immersion crosslinking method, where the crosslinking agent formed a concentration gradient decreasing from the surface to the bottom layer in the multilayer film. The crosslinking degree ratio of the surface layer to the bottom layer was approximately 1:5.4, and the binding energy gradient difference was 9.0. Comparative Example 2 used a stirring + shaking immersion crosslinking method, where the crosslinking agent concentration was basically uniform in each layer. The crosslinking degree ratio of the surface layer to the bottom layer was approximately 1:2.1, and the binding energy gradient difference was only 4.2.
[0114] In terms of overall trouser performance, Comparative Example 2 showed a 2.5-fold increase in permeation rate, a rewetting amount of 1.8g, and a 35% reduction in ammonia nitrogen. All performance characteristics were significantly inferior to Example 1 by 15.2 times, 0.5g, and 72%, respectively. The above comparative results indicate that a gradient distribution of the crosslinking agent is a necessary process condition for forming a significant interlayer binding energy gradient. Physical stratification alone, without a crosslinking agent gradient, cannot create sufficient binding energy gradient differences to drive effective stepwise response and bottom-layer collapse siphoning.
[0115] Contribution of contractile internal stress to the siphon effect Example 1 and Comparative Example 3 were compared and analyzed. Example 1 underwent a stretch-release treatment S5, resulting in the storage of shrinkage internal stress in the bottom layer, approximately 20% of the dry-state fracture stress of the bottom layer. The minimum thickness of the bottom layer after collapse reached 4 nm, and the capillary pressure was 65 kPa. Comparative Example 3 did not undergo a stretch-release treatment; no shrinkage internal stress was stored in the bottom layer, and the minimum thickness of the bottom layer after collapse was only 8 nm, with a capillary pressure of only 28 kPa.
[0116] Regarding the overall performance of the trousers, Comparative Example 3 showed a 3.0-fold increase in permeation rate, a rewetting amount of 1.5g, and a 42% reduction in ammonia nitrogen. All performance aspects were inferior to Example 1, but still superior to Comparative Example 1 (without gradient structure) and Comparative Example 2 (without crosslinking agent gradient). The above comparison results indicate that the presence or absence of a gradient structure is decisive; Comparative Example 1 was the worst, but the shrinkage internal stress played a significant auxiliary reinforcing role in the complete collapse of the bottom layer. Example 1 was superior to Comparative Example 3, and the combined performance of the two was optimal.
[0117] Relationship between interlayer binding energy and triggering conditions Based on the data from Examples 1-5 and Comparative Example 2, it can be seen that the higher the interlayer binding energy, the higher the hydrostatic pressure threshold required for conformational change, and the triggering condition increases sequentially from the surface layer to the bottom layer along the thickness direction. Specifically: in Examples 1-5, the surface layer binding energy is 0.6-1.2 kJ / mol·nm², with a contact response time of <0.5 seconds; the transition layer binding energy is 3.2-4.5 kJ / mol·nm², requiring a hydrostatic pressure ≥5 kPa to respond; and the bottom layer binding energy is 9.0-11.5 kJ / mol·nm², requiring a hydrostatic pressure ≥15 kPa to respond.
[0118] The binding energy of the bottom layer in Comparative Example 2 was only 6.0 kJ / mol·nm². Although a response occurred at a hydrostatic pressure ≥15 kPa, the thickness was reduced to only 11 nm because the binding energy was insufficient to support complete collapse. In Examples 1-5, the thickness could be reduced to 3-5 nm. This indicates that the interlayer binding energy gradient is the physical basis for the triggering condition gradient—the interlayer binding energy determines the external energy input required to disrupt the intermolecular interactions of that layer, i.e., the hydrostatic pressure, and the degree of deformation after the response. When the binding energy difference is sufficiently large, such as 8.3-10.9 in Examples 1-5, the response behavior of each layer differs significantly, forming a stepped conduction; when the binding energy difference is insufficient, such as 4.2 in Comparative Example 2, the response behavior of each layer converges, and stepped conduction cannot be achieved.
[0119] Overall performance comparison of each embodiment and comparative example The overall performance ranking of all embodiments and comparative examples is as follows: Regarding the increase in vertical permeation rate, the order from highest to lowest is: Example 5 5.8 times > Example 1 5.2 times > Example 6 4.9 times > Example 2 4.8 times > Example 4 4.5 times > Example 3 4.2 times > Comparative Example 3 3.0 times > Comparative Example 2 2.5 times > Comparative Example 1 1.3 times.
[0120] Regarding the amount of reabsorption, the amounts from lowest to highest are as follows: Example 5 0.4g < Example 1 0.5g = Example 6 0.5g < Example 2 0.6g = Example 4 0.6g < Example 3 0.7g < Comparative Example 3 1.5g < Comparative Example 2 1.8g < Comparative Example 1 12.8g.
[0121] Regarding the reduction rate of ammonia nitrogen, the order from highest to lowest is: Example 5 75% > Example 1 72% > Example 6 71% > Example 4 69% > Example 2 68% > Example 3 66% > Comparative Example 3 42% > Comparative Example 2 35% > Comparative Example 1 18%.
[0122] The above ranking shows that Examples 1-6, which simultaneously possess "gradient structure + crosslinking agent gradient + shrinkage internal stress", have the best performance; Comparative Example 3, which only lacks shrinkage internal stress, has the second best performance; Comparative Example 2, which only lacks crosslinking agent gradient, has the worst performance; and Comparative Example 1, which lacks none of the three, has the worst performance. Among them, the performance of the four-layer structure of Example 6 is basically equivalent to that of the three-layer structure of Example 1, indicating that the technical solution of the present invention has good scalability in terms of the number of layers.
[0123] The cell-mimicking multilayer membrane gradient flow structure diaper and its preparation method of the present invention can be applied to the field of disposable hygiene products such as infant diapers, adult diapers, pull-up diapers, sanitary napkins, menstrual pants, incontinence pants, and diaper pads. The method of the present invention is simple to operate. The spin coating equipment, gradient hot plate, conventional crosslinking and stretching equipment are all mature industrial equipment, and the parameters are controllable. Each key parameter has a clear numerical range. Examples 1 to 5 demonstrate the tolerance of the process window and suitability for industrial continuous production. Each step S1 to S6 can be realized on a roll-to-roll production line, which has broad prospects for promotion and application.
[0124] The above are merely specific embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of protection of the claims.
[0125] In conclusion, the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A paper diaper of a cell-imitating multi-layer membrane gradient flow structure, characterized in that, It includes a surface layer (1), an absorbent core (3), and a flow guide layer (2) disposed between the surface layer (1) and the absorbent core (3); The guiding layer (2) comprises at least three layers of cell membrane-like stacks (5) stacked sequentially from the surface to the inside, the stacks being constructed on the substrate surface by polyelectrolytes through layer-by-layer self-assembly technology; The interlayer bonding energy between adjacent molecular layers in each layer increases sequentially from the top layer (501) to the bottom layer (503) along the thickness direction of the diaper; The flow-guiding layer (2) undergoes a progressive conformational change when it comes into contact with urine. The triggering conditions required for each layer to undergo conformational change increase sequentially from the surface layer (501) to the bottom layer (503) along the thickness direction.
2. The paper diaper with a cell-imitating multi-layer membrane gradient flow structure according to claim 1, characterized in that, The flow guiding layer (2) is composed of a surface layer (501), a transition layer (502), and a bottom layer (503); The adjacent molecular layers in the surface layer (501) are bonded by singlet hydrogen bonds and van der Waals forces, with an interlayer bonding energy of 0.5–1.5 kJ / mol·nm², a dry thickness of 80–120 nm, and a degree of crosslinking ≤3%. The transition layer (502) is composed of adjacent molecular layers bonded by double hydrogen bonds and metal-coordination bonds, with an interlayer bonding energy of 3.0–5.0 kJ / mol·nm², a dry thickness of 40–60 nm, and a crosslinking degree of 5%–8%. The bottom layer (503) is composed of multiple hydrogen bonds, metal-coordination bonds and covalent bonds between adjacent molecular layers. The interlayer bonding energy is 8.0 to 12.0 kJ / mol·nm², the dry thickness is 12 to 20 nm, and the degree of crosslinking is ≥12%.
3. The paper diaper with gradient conductive structure of the cell-imitated multi-layer membrane of claim 1, wherein, The surface layer (501) is formed by alternating deposition of Pluronic F127 and polyacrylic acid; the transition layer (502) is formed by deposition of a mixed solution of Pluronic F127, polyacrylic acid and imidazole-modified polyethylene glycol; and the bottom layer (503) is formed by deposition of a mixed solution of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol and dopamine-modified hyaluronic acid.
4. The paper diaper with cell-imitated multi-layer membrane gradient flow structure according to claim 1, characterized in that, The surface layer (501) has a response time of ≤0.5 seconds after contact with urine, and the thickness of the surface layer (501) increases from 80-120nm to 180-200nm after the response; When the surface layer (501) is completely soaked in urine and the hydrostatic pressure of the urine below the surface layer (501) is ≥5kPa, the thickness of the transition layer (502) is reduced from 40-60nm to 20-30nm, and the molecular chains in the transition layer (502) are oriented and arranged perpendicular to the thickness direction of the diaper. When the transition layer (502) is completely wetted by urine and the hydrostatic pressure of urine at the upper surface of the bottom layer (503) is ≥15kPa, the thickness of the bottom layer (503) is reduced from 12-20nm to 3-5nm.
5. The paper diaper with gradient conductive structure of the cell-imitated multi-layer membrane of claim 1, wherein, When the thickness of the bottom layer (503) is reduced to 3-5 nm, the average spacing between adjacent molecular layers is 3-5 nm, and the capillary pressure formed within this spacing is 50-80 kPa. The capillary pressure is calculated according to the formula P=2γ·cosθ / d, where γ is the simulated urine surface tension of 45±2 mN / m, θ is the dynamic contact angle of each layer of material, and d is the average spacing between adjacent molecular layers. The average spacing is measured by atomic force microscopy or ellipsometry.
6. The paper diaper with gradient conductive structure of the cell-imitated multi-layer membrane of claim 1, wherein, The bottom layer (503) stores shrinkage internal stress, which is 15% to 25% of the dry fracture stress of the bottom layer (503), and the dry fracture stress is determined according to GB / T1040.3-2006; the maximum tensile area of the bottom layer (503) is 1.15 to 1.20 times the dry area of the bottom layer (503).
7. The diaper with a cell-mimicking multilayer membrane gradient flow structure as described in claim 1, characterized in that, Simulated urine was used to vertically impact the surface of the guide layer (2) at a flow rate of 30 mL / min. The vertical permeation rate of the guide layer (2) increased from the initial value to 4 to 6 times the initial value within the first 10 seconds. Under the pressure of 2.5 kPa reabsorption, the reabsorption amount was ≤0.8 g, and the ammonia nitrogen concentration in the reabsorption liquid was ≥65% lower than that in the original urine.
8. The method of making a paper diaper with a cell-like multilayer membrane gradient flow structure according to any one of claims 1-7, wherein, Includes the following steps: S1: Plasma pretreatment is performed on the nonwoven fabric substrate (4) to introduce active groups on the surface of the substrate; S2: Prepare at least two different polyelectrolyte aqueous solutions, spin-coate or dip-coate them sequentially on the surface of the substrate, and dry each layer after coating to form at least three layers with progressively increasing interlayer bonding energy from the surface to the inside. S3: The stacked structure is cross-linked to form a gradient distribution of cross-linking agent in the stack, with the concentration decreasing from the surface layer (501) to the bottom layer (503); S4: Perform a stretch-release treatment on the cross-linked laminated structure to store shrinkage internal stress in the laminated structure; S5: The processed laminated structure is combined between the diaper surface layer (1) and the absorbent core (3).
9. The method for preparing a diaper with a cell-mimicking multilayer membrane gradient flow structure as described in claim 8, characterized in that, The specific operation of spin coating in step S2 is as follows: Prepare solutions A, B, and C, each with a total solute concentration of 1–2 mg / mL. In solution A, the mass ratio of Pluronic F127 to polyacrylic acid is 1:0.8–1.2; in solution B, the mass ratio of Pluronic F127, polyacrylic acid, and imidazole-modified polyethylene glycol is 1:0.8–1.2:0.3–0.7; and in solution C, the mass ratio of Pluronic F127, polyacrylic acid, imidazole-modified polyethylene glycol, and dopamine-modified hyaluronic acid is 1:0.8–1.2:0.3–0.7:0.2–0.
5. The substrate is fixed on a spin coater, and solutions A, B and C are spin-coated sequentially on the substrate surface. The spin-coating speed for each solution is 500-1500 rpm and the spin-coating time is 10-30 seconds. After each spin-coating layer, the substrate is rinsed with deionized water and dried with nitrogen. Each solution is spin-coated 3-5 times to form a surface layer (501), a transition layer (502) and a bottom layer (503). The plasma pretreatment in step S1 is argon plasma discharge treatment, and the treatment conditions are: vacuum degree ≤10Pa, cavity pressure 20~50Pa, discharge power 90~110W, and treatment time 1.5~2.5 minutes; the non-woven fabric substrate (4) is a polypropylene spunbond non-woven fabric with a basis weight of 15~25g / m².
10. The method for preparing a diaper with a cell-mimicking multilayer membrane gradient flow structure as described in claim 8, characterized in that, The cross-linking treatment in step S3 is: immersing the laminated structure into a mixed aqueous solution of ZnCl2 and glutaraldehyde for 15-30 seconds, the mass fraction of ZnCl2 in the mixed aqueous solution is 0.4%-0.6%, the mass fraction of glutaraldehyde is 0.15%-0.25%, and after taking out, curing at 55-65℃ for 1.5-2.5 hours; the concentration of Zn 2+ and glutaraldehyde in the laminated structure decreases from the surface layer (501) to the bottom layer (503) along the thickness direction, the concentration of the cross-linking agent in the surface layer (501) is 1.5-2.0 times that in the bottom layer (503), and the concentration distribution is measured along the cross-section of the laminated structure by X-ray photoelectron spectroscopy. The stretch-release treatment in step S4 is as follows: the cross-linked laminated structure is stretched by 1.15 to 1.20 times along the longitudinal direction, and kept in a stretched state in an environment with a temperature of 45 to 55°C and a relative humidity of 85% to 95% for 15 to 25 minutes. The stretching force is then released to allow the laminated structure to naturally shrink back. After releasing the stretching force, the dimensional recovery rate of the surface layer (501) is 95% to 100%, and the dimensional recovery rate of the bottom layer (503) is 75% to 85%. The composite method described in step S5 is hot melt adhesive dot composite, and the coverage area of the dot composite is 5% to 10% of the area of the laminated structure.