High-load artemisia vulgaris essential oil intelligent slow-release film

Artemisia argyi essential oil was loaded onto a polylactic acid/spiral carbon fiber porous nanofiber membrane prepared by electrospinning technology. Combined with a voice interaction system and a flexible heating unit, this solved the problems of smoke pollution, uncontrollable temperature, and inconvenient operation in moxibustion therapy, and achieved a smart sustained-release membrane with high load capacity, stable release, and convenient use.

CN123148146APending Publication Date: 2026-11-24NANJING TECH UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611639832.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing moxibustion therapies suffer from problems such as smoke pollution, uncontrollable temperature, low utilization rate of effective ingredients, and inconvenience of use. Existing non-open flame moxibustion patches cannot simultaneously ensure safety, temperature controllability, effective ingredient release efficiency, and user comfort. The load stability and release behavior of mugwort essential oil are difficult to regulate, and existing intelligent temperature control products are inconvenient to operate.

Method used

Polylactic acid/spiral carbon fiber porous nanofiber membranes were prepared using electrospinning technology. Artemisia argyi essential oil was loaded onto the membranes using an impregnation method. Combined with a voice interaction system and a flexible heating unit, a high-load Artemisia argyi essential oil intelligent slow-release membrane was constructed to achieve efficient adsorption and controllable release of the essential oil.

Benefits of technology

It achieves high load capacity, stable preservation, intelligent slow release, synergistic heating and warming of mugwort essential oil, and convenient operation, improving safety and practicality, and is suitable for daily family health care and acupoint moxibustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148146A_ABST
    Figure CN123148146A_ABST
Patent Text Reader

Abstract

This invention discloses a high-load intelligent sustained-release membrane for Artemisia argyi essential oil. The sustained-release membrane has a layered structure, consisting of, from the outside in: a control unit, a flexible heating unit, and a porous nanofiber drug-loaded layer. The control unit includes a main control module and a voice interaction module, a visual information display module, and a temperature control module, all electrically connected to the main control module, for voice control and broadcasting, real-time parameter display, and intelligent temperature control. The flexible heating unit includes a heating network formed by interconnected conductive fibers. The temperature control module is connected to a temperature sensor and the heating network for real-time adjustment of the heating power. The porous nanofiber drug-loaded layer uses polylactic acid as the matrix and helical carbon fiber as the aggregate, formed by electrospinning and impregnated with Artemisia argyi essential oil. It has a large specific surface area and numerous adsorption sites, enabling high drug loading, long-lasting sustained release, and uniform heat-drug synergy, helping to solve problems such as smoke pollution, easy burns, difficulty in temperature control, and low utilization rate associated with traditional moxibustion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of intelligent healthcare technology and relates to a high-load Artemisia argyi essential oil intelligent sustained-release membrane. Background Technology

[0002] Moxibustion is a traditional Chinese medicine therapy that utilizes the volatile active ingredients released from burning mugwort leaves and the resulting heat stimulation to exert analgesic, anti-inflammatory, and anti-tumor effects, while also promoting local blood circulation and metabolism and enhancing the body's immune function. However, this therapy still has significant limitations in clinical application. First, the smoke and ash produced during combustion may cause environmental pollution and health risks. Second, the temperature of moxibustion is difficult to control precisely, easily leading to burns or insufficient heat stimulation, affecting the therapeutic effect; the utilization rate of active ingredients in mugwort leaves is low, and a large amount of effective components are lost with the smoke during combustion, resulting in resource waste. These problems severely limit the modernization and home application of moxibustion therapy.

[0003] There are many types of non-flame moxibustion patches on the market, often using a combination of a moxa sachet and a heating pack. While this avoids the problems of open flame combustion and smoke to some extent, it still has many shortcomings. The effective utilization rate of the active ingredients in ordinary moxa sachets is low, and they are prone to insects and mold, resulting in poor storage stability and safety. The iron powder in the heating pack releases heat through an oxidation reaction, making the temperature uncontrollable and increasing the risk of burns from accidental direct application to the skin. Furthermore, the heat released by the heating pack, passing through the thick moxa sachet, makes it difficult for the active ingredients in the moxa to be fully released, leading to lower therapeutic effects. Therefore, existing non-flame moxibustion patches struggle to simultaneously achieve safety, controllable temperature, efficient release of active ingredients, and user comfort.

[0004] Artemisia argyi essential oil, the main active ingredient in Artemisia argyi leaves, possesses pharmacological activities such as anti-inflammatory, antibacterial, and antioxidant properties. Loading Artemisia argyi essential oil onto a suitable carrier to create a medicinal sachet allows for the continuous release of active ingredients without open flame or smoke, thus achieving the therapeutic effects of smokeless moxibustion and overcoming the drawbacks of traditional moxibustion, such as smoke, ash, and difficulty in temperature control. However, Artemisia argyi essential oil is highly volatile, and even after loading, it still suffers from insufficient storage stability, difficulty in controlling release behavior, and short duration of efficacy. Therefore, selecting appropriate loading strategies and carrier materials to improve the loading capacity, storage stability, and controllable release of Artemisia argyi essential oil is of significant research importance for enhancing the effect of smokeless moxibustion sustained-release films.

[0005] Nanofibers are a common carrier for loading Artemisia argyi essential oil. Methods for loading essential oils onto nanofibers include impregnation, blended electrospinning, coaxial electrospinning, and particle coating-blending. Among these, impregnation is simple to operate, operates under mild conditions, and causes minimal damage to active ingredients. It allows essential oils to be loaded onto the fiber interior and surface through physical adsorption after fiber formation, avoiding damage to the essential oil activity caused by organic solvents or high-voltage electric fields during spinning. However, impregnation relies heavily on physical adsorption, resulting in limited interaction between the essential oil and the fiber. Typical electrospun fiber membranes are constructed from solid nanofibers; while they can adsorb essential oils, the loading capacity is small, the interaction between the fiber and the essential oil is weak, and the essential oil easily evaporates quickly, making it difficult to meet the requirements for high loading and long-lasting sustained release. Porous nanofibers, on the other hand, have high porosity, good air permeability and transparency, and their surface and internal channels provide numerous adsorption sites. Furthermore, the pore confinement, surface tension, and capillary action enhance the stability of essential oil adsorption. However, porous nanofibers are difficult to prepare, and the pore structure is difficult to control and is prone to collapse and deformation; most polymers have poor thermal conductivity and are difficult to work synergistically with thermal stimulation; the high porosity also leads to insufficient fiber strength and toughness, and the mechanical properties and structural stability of the sustained-release membrane further decline after high loading.

[0006] Furthermore, existing essential oil slow-release or intelligent temperature-controlled moxibustion products still have shortcomings in terms of system integration and ease of use. Some products are wired and limited in their location, making it difficult to meet the needs of wearing them on the go or using them conveniently at home; at the same time, they lack intelligent operation methods such as voice interaction, which is not user-friendly for the elderly or those with mobility impairments, making operation relatively inconvenient. In summary, existing technologies cannot simultaneously meet the requirements of high load capacity, stable preservation, intelligent slow release, synergistic heating, and convenient operation of mugwort essential oil. Summary of the Invention

[0007] To address the shortcomings of existing sustained-release membranes, this invention provides a high-load intelligent sustained-release membrane for artemisia essential oil and its preparation method. This invention utilizes electrospinning technology to prepare a polylactic acid / spiral carbon fiber porous nanofiber membrane. Essential oil is then loaded via an impregnation method to construct an essential oil sustained-release membrane based on the polylactic acid porous nanofiber membrane. Furthermore, a voice interaction system and a flexible heating unit are coupled to develop an intelligent essential oil sustained-release membrane. The sustained-release membrane prepared by this method features uniform fiber diameter, high specific surface area, and a porous structure on and inside the nanofibers, which is beneficial for the efficient adsorption and loading of artemisia essential oil. Simultaneously, the integration of an intelligent interaction system and a flexible heating unit improves the practicality and portability of the sustained-release membrane, and simultaneously achieves intelligent sustained-release of essential oil while incorporating thermotherapy and pharmacotherapy functions.

[0008] The technical solution of the present invention is: a high-load Artemisia argyi essential oil intelligent sustained-release membrane, wherein the sustained-release membrane has a layered structure, and from the outside to the inside are: a control unit, a flexible heating unit and a porous nanofiber drug-carrying layer; The control unit includes a main control module and a voice interaction module, a visual information display module, and a temperature control module, which are electrically connected to the main control module, respectively, for realizing voice control and broadcasting, real-time parameter display, and intelligent temperature control; The flexible heating unit includes a heating network formed by interconnected conductive fibers, and a temperature control module connected to a temperature sensor and the heating network for real-time adjustment of heating power. The slow-release membrane is a wireless portable structure, powered by a rechargeable battery output line connected to the main control module, enabling heating, digital display, and voice functions. The rechargeable battery input line is retractable and hidden, used to connect to an external charging power source.

[0009] The porous nanofiber drug-carrying layer is a porous nanofiber membrane with a high load of Artemisia argyi essential oil. The drug-carrying layer is loaded with Artemisia argyi essential oil by impregnation method. The volume ratio of essential oil to ethanol is 10:0-1:9, the impregnation time is 6-24 h, and the drying temperature is 25-50°C.

[0010] The porous nanofiber membrane was prepared by electrospinning with the following parameters: injection rate 0.6-1.5 mL / h, positive voltage 7-10 kV, negative voltage 1 kV, receiving distance 17-24 cm, temperature 20-30 °C, humidity 20%-70%, and spinning time 2-4 h. The spinning solution comprises: polylactic acid, polyvinylpyrrolidone, spiral carbon fibers, and a mixed solvent of dichloromethane and N,N-dimethylformamide. The spiral carbon fibers have a wire diameter of 50-350 nm, a helix diameter of 0.2-1.8 μm, a helix pitch of 0.2-2.5 μm, and are added at 1%-10% of the mass of polylactic acid. The spinning solution is first ultrasonically dispersed for 30-60 min and then magnetically stirred for 12-24 h to ensure uniform dispersion of the spiral carbon fibers in the polylactic acid matrix. The mass-to-volume ratio of polylactic acid to the mixed solvent is 0.08-0.16 g / mL; the mass ratio of polyvinylpyrrolidone to polylactic acid is 1%-2%; and the volume ratio of dichloromethane to N,N-dimethylformamide is 9:1 to 1:1.

[0011] The voice interaction module includes a voice recognition chip, a microphone array, and a speaker. The voice commands that can be recognized include power on, power off, heating up, cooling down, constant temperature setting, mode switching, and timer. The main control module can recognize and convert voice commands and temperature sensor signals, and dynamically adjust the output power of the temperature control module, the imaging behavior of the information display module, and the voice broadcast content in real time.

[0012] The main control module has a built-in overheat protection mechanism to keep the heating temperature within 25-50 °C. After power-on, it continuously monitors anti-scalding keywords and immediately stops power supply when it recognizes key voice messages such as "scalding" or "too hot" to ensure safety.

[0013] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention utilizes electrospinning technology to prepare a high-load Artemisia argyi essential oil intelligent sustained-release membrane. This method offers advantages such as high efficiency and convenience, simple process, low production cost, and environmental friendliness. By adjusting parameters such as polylactic acid concentration, helical carbon fiber doping amount, operating voltage, and ambient humidity, the fiber morphology, pore structure, and mechanical properties of the fiber membrane can be effectively modified, thereby adapting to the needs of different application scenarios.

[0014] 2. The spiral carbon fiber reinforced polylactic acid porous nanofibers prepared by this invention have uniform fiber diameter and high specific surface area. Both their surface and interior exhibit porous structures, which is beneficial for the efficient loading and release of essential oils.

[0015] The selected polylactic acid (PLA) not only possesses excellent biocompatibility and biodegradability, but its superior spinnability also provides an ideal platform for constructing stable drug delivery systems, making it an excellent carrier material for essential oils. Compared to hydrophilic biopolymers such as polyvinyl alcohol and gelatin, PLA, although less hydrophilic, avoids the problems of excessive swelling or rapid degradation of water-soluble fibers in bodily fluid environments.

[0016] Spiral carbon fibers, embedded within the fiber structure as aggregate, possess a spring-like, helical configuration that provides the fiber membrane with elastic buffering capabilities. Even after essential oil adsorption and swelling, the membrane maintains unobstructed pores and prevents structural collapse, ensuring a high essential oil loading capacity. Simultaneously, the three-dimensional thermally conductive network formed by the interconnected spiral carbon fibers ensures uniform heat conduction within the drug-loaded layer, enhancing the thermo-drug synergistic efficiency. The introduction of spiral carbon fibers also strengthens the interaction between essential oils and fibers, improving the membrane material's sustained-release effect and extending its duration of action. Compared to existing technologies using hollow carbon nanospheres or straight carbon nanotubes as fillers, spiral carbon fibers avoid the performance degradation caused by structural collapse when using isolated hollow carbon nanospheres as fillers. The three-dimensional skeletal network and three-dimensional thermally conductive network formed by spiral carbon fibers achieve uniform thermo-drug synergy, a feature not found in isolated, dispersed hollow carbon nanospheres.

[0017] 3. The high-load Artemisia argyi essential oil intelligent sustained-release membrane prepared by this invention possesses excellent air permeability, moisture permeability, mechanical properties, and biocompatibility. Simultaneously, the addition of essential oil endows it with good antibacterial, anti-inflammatory, and antioxidant properties. Therefore, this sustained-release membrane is particularly suitable for intelligent physiotherapy sustained-release and transdermal drug delivery applications.

[0018] 4. The high-load Artemisia argyi essential oil intelligent sustained-release membrane integrated voice interaction temperature control system prepared by this invention can quickly realize on / off, temperature adjustment, timer and mode switching through voice commands. With precise temperature control logic, voice broadcast and real-time display, it greatly improves the convenience and freedom of use. The system has built-in overheat protection and constant temperature maintenance mechanism, which can stably output a safe therapeutic temperature and effectively avoid the risk of burns. It has a higher level of practicality and intelligence in scenarios such as daily family health care, acupoint moxibustion, and personalized transdermal drug delivery. Attached Figure Description

[0019] Figure 1 The images show cross-sectional scanning electron microscope (SEM) images of the polylactic acid / spiral carbon fiber membrane prepared in Example 1 before and after adsorption of Artemisia argyi essential oil.

[0020] Figure 2 (a) Nitrogen isothermal adsorption curve and (b) infrared spectrum of porous nanofiber membranes with high loading of Artemisia argyi essential oil with different helical carbon fiber contents prepared for Example 2.

[0021] Figure 3 (a) Fracture tensile deformation diagram and (b) oil loading diagram of porous nanofiber membranes with different helical carbon fiber contents and high load of Artemisia argyi essential oil prepared in Example 2.

[0022] Figure 4 These are scanning electron microscope (SEM) images of the high-load Artemisia argyi essential oil intelligent sustained-release membrane prepared in Example 3, where (a)-(c) are without added helical carbon fibers, (d)-(i) are with 1% carbon fiber addition, and (f)-(i) are SEM images taken 20 seconds after electron beam irradiation.

[0023] Figure 5 These are electron micrographs of porous nanofibers with different helical parameters prepared in Example 4. (a)-(f) correspond to helical carbon fibers with pitches of 500 nm, 800 nm, 1.2 μm, 1.6 μm, 2.0 μm, and 2.5 μm.

[0024] Figure 6 The comparison of (a) temperature control and (b) essential oil release rate of the intelligent sustained-release membrane and the ordinary sustained-release membrane in Example 5 is shown.

[0025] Figure 7 This is a schematic diagram of the structure of a high-load mugwort essential oil intelligent sustained-release membrane.

[0026] Figure 8 This is a schematic diagram of the structure of the intelligent slow-release membrane control unit for high-load artemisia essential oil.

[0027] In the diagram: 1. Control unit; 2. Flexible heating unit; 3. Porous nanofiber drug-carrying layer; 4. Speaker; 5. Display screen; 6. Heating wire; 7. Temperature sensor; 8. Voice interaction circuit board; 9. Main control module circuit board; 10. Rechargeable battery; 11. Battery charging port; 12. Battery output port.

[0028] Figure 9 This is a circuit diagram of a high-load intelligent slow-release membrane for artemisia essential oil. Detailed Implementation

[0029] To make the technical solution of the present invention clearer, the following are specific embodiments of the present invention, but they are by no means limited thereto. Example 1

[0030] 1.4 g of polylactic acid and 0.028 g of polyvinylpyrrolidone were dissolved in 10 mL of a 9:1 (v / v) mixture of dichloromethane and N,N-dimethylformamide, and magnetically stirred at 300 rpm for 12 h to obtain a homogeneous solution. 0.056 g of helical carbon fiber was added to the homogeneous solution, sonicated for 60 min, and then magnetically stirred at 300 rpm for 24 h to obtain a homogeneous dispersion. The helical carbon fiber used had a wire diameter of 50-150 nm, a helix diameter of 200-250 nm, a pitch of 200-250 nm, and was added at 4% of the mass of polylactic acid. The homogeneous dispersion was placed in a 5 mL syringe driven by an electrospinning machine pump, and the injection rate of the syringe pump was set to 1.5 mL / h. A positive pressure of 10 kV and a negative pressure of 1 kV were applied to the syringe, and the distance between the needle and the receiving end was adjusted to 24 cm. A polylactic acid / spiral carbon fiber porous nanofiber membrane was prepared by spinning for 2 hours at a constant temperature of 30 °C and humidity of 70%. The resulting membrane was dried in a 55 °C oven for 24 hours to remove residual solvent. The membrane was then immersed in 10 mL of a 1:4 volume ratio Artemisia argyi oil / ethanol solution for 12 hours, and excess solution was dried at 40 °C to obtain a polylactic acid / spiral carbon fiber porous nanofiber membrane with a high Artemisia argyi oil loading. The porous nanofiber membrane with the high Artemisia argyi oil loading, a control unit, and a flexible heating unit were sequentially assembled to obtain a smart sustained-release membrane with a high Artemisia argyi oil loading.

[0031] Figure 1The images show cross-sectional scanning electron microscopy (SEM) images of the polylactic acid (PLA) / spiral carbon fiber porous nanofiber membrane prepared in Example 1 before and after adsorption of Artemisia argyi essential oil. Before adsorption, the porous nanofibers exhibit a uniform structure with an average fiber diameter of 1.61 μm and a uniform pore structure on the fiber surface. After adsorption, the porous fiber diameter significantly increases to 2.05 μm. This change is mainly attributed to the swelling effect of organic components such as terpenes and esters in Artemisia argyi essential oil on the PLA fibers. The high specific surface area and porous structure of the PLA / spiral carbon fiber porous nanofibers provide an effective diffusion path for Artemisia argyi essential oil molecules, making it easier for them to penetrate into the fiber interior. Small molecules in Artemisia argyi essential oil can permeate between PLA molecular chains, increasing the interchain spacing and thus causing an increase in fiber diameter. Example 2

[0032] The preparation method and parameters were the same as in Example 1, except that the amount of spiral carbon fiber added was 0, 0.014 g, 0.028 g, 0.056 g, 0.112 g, and 0.14 g (i.e., the amount of spiral carbon fiber added was 0%, 1%, 2%, 4%, 8%, and 10% of polylactic acid, respectively), and the other parameters were the same as in Example 1. A high-load Artemisia argyi essential oil intelligent sustained-release membrane with different spiral carbon fiber contents was prepared and characterized accordingly.

[0033] Figure 2 (a) shows the nitrogen adsorption isotherms of polylactic acid / spiral carbon fiber porous nanofiber membranes with different carbon fiber contents. It can be seen that the adsorption capacity of the original polylactic acid-spun porous nanofibers is relatively small. With the increase of carbon fiber addition (0%, 1%, 2%, 4%, 8%, 10%), the adsorption capacity first increases and then decreases. This is due to the large specific surface area (182.86 m²). 2 At low addition levels, the spiral carbon fibers ( / g) not only act as the framework of porous carbon nanomaterials but also contribute to the specific surface area, resulting in a final specific surface area of ​​11.63 m² for the porous nanofibers. 2 / g, 14.20 m 2 / g, 19.38 m 2 / g、24.09 m 2 / g, 23.56 m 2 / g、21.33 m 2 / g. However, when the amount of spiral carbon fiber added increased from 4% to 8% and 10%, the aggregation of carbon fibers in the spinning solution began to appear, resulting in low fiber utilization. Furthermore, the aggregated carbon fibers increased the viscosity of the spinning solution, which hindered jet stretching and made it easier to form beaded nanofibers, thus reducing their specific surface area.

[0034] Figure 2(b) Fourier transform infrared spectra of polylactic acid / spiral carbon fiber porous nanofiber membranes with different carbon fiber contents. The characteristic peak of the polylactic acid substrate includes: 2943.7 cm⁻¹. -1 With 2993.6 cm -1 The stretching vibrations of CH and OH are respectively, 1751.8 cm. -1 The point represents the stretching vibration of an ester bond (C=O); 1452.2 cm⁻¹ -1 and 1359.8 cm -1 Corresponding to C=O stretching vibration and CH3 bending vibration respectively, 1182.0 cm -1 and 1085.7 cm -1 The values ​​represent asymmetric and symmetric stretching vibrations of the COC ether bond. With the addition of helical carbon fibers, the spectral shapes of all fiber membranes are basically the same, with only slight changes in peak intensity. This indicates that the helical carbon fibers are embedded in the porous fiber membrane, and mainly act as a framework with the polylactic acid matrix through van der Waals forces. The characteristic peak signals are covered or masked by the strong peaks of polylactic acid.

[0035] Figure 3 (a) shows the tensile strength of polylactic acid / spiral carbon fiber porous nanofiber membranes with different carbon fiber contents. It can be seen that as the carbon fiber content increases, the tensile strength of the material increases, but the tensile deformation does not change significantly. This is because the spiral carbon fiber acts as a skeleton. When stretching causes deformation, the porous structure formed by polylactic acid gradually deforms from the outside of the carbon fiber, eventually partially splitting and embedding itself between the pitches of the spiral carbon fiber like a spider web. Since the spiral carbon fiber itself has high strength, the tensile strength range (MPa) of the tensile tester is much smaller than the tensile strength (GPa) of the carbon fiber. This explains why, as the carbon fiber content increases from 0% to 1%, 2%, and 4%, the tensile breaking point increases from 0.135 MPa to 0.164 MPa, 0.295 MPa, and 0.321 MPa, respectively. It should be noted that, similar to the change in specific surface area, when the carbon fiber content increases to 8% and 10%, the quality defects of the porous nanofiber membrane increase, leading to a decrease in tensile breaking strength. The changes in specific surface area and tensile breaking strength are also related to the Artemisia argyi essential oil loading of the porous nanofibers, such as... Figure 3 As shown in (b), when the carbon fiber addition amount is 0%-4%, the essential oil loading gradually increases and the error bar is also small. When the carbon fiber addition amount becomes 8% and 10%, agglomerated spiral carbon fibers appear in the spun fibers, which affects the quality of the porous nanofiber membrane. This leads to a decrease in the essential oil loading amount and an increase in the error bar. Example 3

[0036] 1.4 g of polylactic acid and 0.014 g of polyvinylpyrrolidone were dissolved in 17.5 mL of a 1:1 mixture of dichloromethane and N,N-dimethylformamide and magnetically stirred at 300 rpm for 12 h to obtain a homogeneous solution. 0.014 g of helical carbon fiber was added to the homogeneous solution, sonicated for 30 min, and then magnetically stirred at 300 rpm for 12 h to obtain a homogeneous dispersion. The helical carbon fiber used had a wire diameter of 150-350 nm, a helix diameter of 0.4-0.9 μm, a helix pitch of 1-2.5 μm, and was added at 1% of the mass of polylactic acid. The homogeneous dispersion was placed in a 5 mL syringe driven by an electrospinning machine pump, and the injection rate of the syringe pump was set to 0.6 mL / h. A positive pressure of 7 kV and a negative pressure of 1 kV were applied to the syringe, and the distance between the needle and the receiving end was adjusted to 17 cm. A polylactic acid / spiral carbon fiber porous nanofiber membrane was prepared by spinning for 4 hours at a constant temperature of 20 °C and humidity of 20%. The resulting membrane was dried in a 55 °C oven for 24 hours to remove residual solvent. The membrane was then immersed in 10 mL of a 1:4 volume ratio Artemisia argyi oil / ethanol solution for 12 hours, and excess solution was dried at 40 °C to obtain a polylactic acid / spiral carbon fiber porous nanofiber membrane with a high Artemisia argyi oil loading. The porous nanofiber membrane with the high Artemisia argyi oil loading, a control unit, and a flexible heating unit were sequentially assembled to obtain a smart sustained-release membrane with a high Artemisia argyi oil loading.

[0037] Figure 4 (a) shows the microstructure of the spinning solution without helical carbon fibers under a scanning electron microscope. Due to the low boiling point of dichloromethane, it is more easily volatilized and detached from the spinning solution under the influence of ambient temperature and electron beam irradiation, leading to the formation of a porous structure. This is the main reason why the spinning solution eventually becomes a porous nanofiber membrane after being subjected to an electrostatic field. It can be seen that this spinning solution without helical carbon fibers can also form a porous nanofiber membrane, such as... Figure 4 As shown in (b). Due to the high energy of the electron beam in scanning electron microscopy, the porous nanofibers without added carbon fibers continuously shrink. The areas of the fiber receiving concentrated electron beam irradiation shrink uniformly (e.g., ...). Figure 4 (c) This is because the internal and external composition of the porous fiber is consistent. When helical carbon fibers are added to the spinning solution, due to the small amount added, the carbon fibers are more easily encapsulated by polylactic acid, but the presence of carbon fibers can still be seen, such as... Figure 4 As shown in (d). Although the microstructure of the spiral carbon fiber polylactic acid porous nanofiber with an addition of 1% is ( Figure 4 (e) Similar to polylactic acid porous nanofibers without carbon fibers, but it can be observed that, under continuous electron beam irradiation under a scanning electron microscope, the final shrinkage structure of the fiber is affected by the helical carbon fiber skeleton and is no longer uniform, such as... Figure 4(f)-(i) show that the presence of helical carbon fibers does indeed enhance the physical microstructure of the porous fiber membrane.

[0038] Test results: The essential oil loading rate of the drug-loaded layer of the sustained-release membrane was approximately 180% of the porous nanofiber membrane mass. The cumulative release rates of essential oils in the sustained-release tests at room temperature and 40 °C were 30% and 85%, respectively, which were better than those of the fiber membrane without spiral carbon fibers (42% and 78% of the cumulative release rates of essential oils in the sustained-release tests at room temperature and 40 °C, respectively). This indicates that the presence of spiral carbon fibers effectively increased the adsorption of essential oils by the porous fiber membrane at room temperature. However, the excellent thermal conductivity of carbon fibers allowed the essential oils to be released well when heated, effectively increasing the room temperature storage period and efficacy of the sustained-release membrane. Example 4

[0039] The preparation method is the same as in Example 3, except that the diameter of the spiral carbon fiber used is 100-350 nm, the spiral diameter is 0.7-1.5 μm, the spiral pitch is 0.5-2.5 μm, and the other parameters are the same as in Example 3, thus obtaining a high-load Artemisia argyi essential oil intelligent sustained-release membrane with a spiral carbon fiber addition of 1%.

[0040] The microstructure of materials, such as Figure 5 As shown, spiral carbon fibers of different specifications can all effectively serve as the supporting framework for porous nanofibers. However, relatively speaking, porous nanofibers with smaller wire diameters, spiral diameters, and regular pitch carbon fibers have more uniform diameters. Example 5

[0041] 1.6 g of polylactic acid (PLA) and 0.032 g of polyvinylpyrrolidone (PVP) were dissolved in 10 mL of a 1:1 mixture of dichloromethane and N,N-dimethylformamide (dichloromethane / N,N-dimethylformamide), i.e., the mass-to-volume ratio of PLA to the mixed solvent was 0.16 g / mL, and the mass ratio of PPV to PLA was 2%. The mixture was magnetically stirred at 500 rpm for 12 h to obtain a homogeneous solution. 0.064 g of helical carbon fiber was added to the homogeneous solution, sonicated for 60 min, and then magnetically stirred at 500 rpm for 12 h to obtain a homogeneous dispersion. The helical carbon fiber used had a wire diameter of 50-150 nm, a helix diameter of 0.8-1.8 μm, a pitch of 0.9-1.5 μm, and was added at 4% of the mass of PLA. The mixture was spun, dried, and impregnated for loading. The membrane material was then uniformly divided into two parts: one part was assembled with the control unit and flexible heating unit, and the other part was only connected to the control unit and flexible heating unit with heating output. All other parameters were the same as in Example 1, resulting in a high-load Artemisia argyi essential oil intelligent sustained-release membrane and a high-load Artemisia argyi essential oil ordinary sustained-release membrane. A practicality test was then conducted at 2V.

[0042] like Figure 6 As shown in (a), the control unit in the intelligent slow-release membrane can effectively control the flexible heating unit to output heat stably. During the 20 minutes of use, the temperature is always maintained at the optimal body temperature of 45 °C. In contrast, ordinary slow-release membranes do not have multi-level overheat protection and other programs, resulting in large temperature fluctuations and potential safety hazards.

[0043] On the other hand, we also tested the essential oil release effect of the intelligent sustained-release membrane, from Figure 6 (b) It can be seen that the essential oil release rate of the intelligent sustained-release membrane is only about 50% within 24 hours, while that of the ordinary sustained-release membrane is 61%, which also shows that the intelligent sustained-release membrane has a significant sustained-release function. Comparative Example 1

[0044] The difference between this comparative example and Example 1 is that the spiral carbon fibers are replaced with hollow carbon nanospheres of equal mass (particle size 100-200 nm), while the other conditions are the same as in Example 1.

[0045] Test results: The essential oil loading rate of the fiber membrane prepared in Comparative Example 1 was approximately 72% of that in Example 1, and the cumulative release of essential oil in the 12-hour sustained-release test was approximately 85% of that in Example 1, indicating that helical carbon fibers are more effective at storing essential oils for a longer period compared to carbon nanospheres. This is attributed to the balance between the surface forces of the helical structure and the gravity and capillary forces of the essential oil. Comparative Example 2

[0046] The difference between this comparative example and Example 1 is that the spiral carbon fibers are replaced with straight carbon nanotubes of equal mass (50-100 nm in diameter and 5-10 μm in length), while the other conditions are the same as in Example 1.

[0047] Test results: The essential oil loading rate of the fiber membrane prepared in Comparative Example 2 was approximately 68% of that in Example 1, and its ability to adsorb essential oil was significantly lower than that of the spiral carbon fibers. This indicates that straight carbon nanotubes cannot form an effective three-dimensional porous network, making the spinning solution more prone to clogging the spinning needles. This suggests that spiral carbon fibers with graphite lattice defects are more likely to connect with each other and form a three-dimensional porous nanofiber membrane structure.

Claims

1. A high-load mugwort essential oil intelligent sustained-release membrane, characterized in that, The sustained-release membrane has a layered structure, consisting of, from the outside to the inside: a control unit, a flexible heating unit, and a porous nanofiber drug-carrying layer; The control unit includes a main control module and a voice interaction module, a visual information display module, and a temperature control module, which are electrically connected to the main control module, respectively, for realizing voice control and broadcasting, real-time parameter display, and intelligent temperature control; The flexible heating unit includes a heating network formed by interconnected conductive fibers, and a temperature control module connected to a temperature sensor and the heating network for real-time adjustment of heating power. The slow-release membrane is a wireless portable structure, powered by a rechargeable battery output line connected to the main control module, enabling heating, digital display, and voice functions. The rechargeable battery input line is retractable and hidden, used to connect to an external charging power source. The porous nanofiber drug-carrying layer is a porous nanofiber membrane with a high load of Artemisia argyi essential oil. The drug-carrying layer is loaded with Artemisia argyi essential oil by impregnation method. The volume ratio of essential oil to ethanol is 10:0-1:9, the impregnation time is 6-24 h, and the drying temperature is 25-50°C. The porous nanofiber membrane was prepared by electrospinning. The spinning parameters were: injection rate 0.6-1.5 mL / h, positive voltage 7-10 kV, negative voltage 1 kV, receiving distance 17-24 cm, temperature 20-30 °C, humidity 20%-70%, and spinning time 2-4 h. The spinning solution included polylactic acid (PLA), polyvinylpyrrolidone (PVP), helical carbon fibers, and a mixed solvent of dichloromethane and N,N-dimethylformamide. The helical carbon fibers had a wire diameter of 50-350 nm, a helix diameter of 0.2-1.8 μm, a helix pitch of 0.2-2.5 μm, and were added at 1%-10% of the PLA mass. The spinning solution was first ultrasonically dispersed for 30-60 min and then magnetically stirred for 12-24 h to ensure uniform dispersion of the helical carbon fibers in the PLA matrix. The mass-to-volume ratio of PLA to the mixed solvent was 0.08-0.

16. g / mL; the mass ratio of polyvinylpyrrolidone to polylactic acid is 1%-2%; the volume ratio of dichloromethane to N,N-dimethylformamide is 9:1 to 1:

1.

2. The high-load Artemisia argyi essential oil intelligent sustained-release membrane according to claim 1, characterized in that, The voice interaction module includes a voice recognition chip, a microphone array, and a speaker. The voice commands that can be recognized include power on, power off, heating up, cooling down, constant temperature setting, mode switching, and timer. The main control module can recognize and convert voice commands and temperature sensor signals, and dynamically adjust the output power of the temperature control module, the imaging behavior of the information display module, and the voice broadcast content in real time.

3. The high-load Artemisia argyi essential oil intelligent sustained-release membrane according to claim 1, characterized in that, The main control module has a built-in overheat protection mechanism to control the heating temperature within 25-50 °C. After power-on, it continuously monitors anti-scalding keywords and immediately stops power supply when it recognizes key voice messages such as "scalding" or "too hot" to ensure safety.