Modified oil-control silicon powder loaded with active substances, and preparation method and application thereof

By modifying the oil-controlling silicone powder with loaded active ingredients, a hydrophobic and breathable shell-pore active core structure is constructed, which solves the problems of poor oil control and short makeup time in liquid foundation, achieving long-lasting oil control and stable dispersion, and improving the user experience of cosmetics.

CN123148176APending Publication Date: 2026-11-24GUANGZHOU HUACHUJIAN BIOTECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611650020.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing oil-control powders used in liquid foundations have problems such as poor oil control, short makeup duration, and easy to cause dullness and dryness of the makeup. In addition, the active ingredients are unevenly dispersed in complex and multi-component systems and have poor compatibility stability.

Method used

Modified oil-controlling silica powder loaded with active ingredients is used. A hydrophobic and breathable shell-pore active core structure is constructed by using porous silica powder as the core layer and polydimethylsiloxane coating film as the shell layer to achieve stable loading and sustained release of active ingredients. Combined with the supergravity powder surface coating reactor process, the stable dispersion of powder in cosmetic systems is ensured.

Benefits of technology

It achieves a sebum inhibition rate of over 65% within 1 to 6 hours, while also providing an immediate matte and soft-focus effect, extending makeup wear time, ensuring a smooth and non-drying finish, and ensuring that active ingredients are evenly dispersed in the cosmetic formula, thus avoiding the shortcomings of traditional powders.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148176A_ABST
    Figure CN123148176A_ABST
Patent Text Reader

Abstract

This invention relates to the field of cosmetic technology, specifically to a modified oil-controlling silicone powder loaded with active ingredients, its preparation method, and its application. The modified oil-controlling silicone powder comprises: porous silicone powder as the core layer loaded with active ingredients and a polydimethylsiloxane coating film as the shell layer; the mass ratio of the porous silicone powder, active ingredients, and polydimethylsiloxane is 80-100:1-8:3-10. It retains the advantages of physical powders in terms of immediate oil absorption and soft-focus effect, while also stably loading and slowly releasing oil-controlling active ingredients. Furthermore, it can be stably dispersed in complex systems such as liquid foundation, better meeting practical application needs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cosmetic technology, specifically to a modified oil-controlling silicone powder loaded with active ingredients, its preparation method, and its application. Background Technology

[0002] Foundation is one of the core formulations of base makeup products. With the upgrading of consumer demand, consumers are increasingly demanding that base makeup products simultaneously possess the dual requirements of oil control, long-lasting wear, and lightweight, adherent finish. Currently, most commercially available oil-controlling base makeup products contain physically adsorbing powders such as porous silica and silicone elastomer microspheres. These powders rely on their high specific surface area to instantly adsorb excess sebum from the skin's surface, achieving an immediate matte effect.

[0003] However, this type of physically adsorbed powder is a passive and indiscriminate adsorption. While adsorbing excessive sebum, it also removes the essential sebum film from the skin's surface, easily leading to dry makeup and caking. More importantly, the oil absorption capacity of the powder is limited, and it usually becomes saturated within 2 to 4 hours. After the gaps between the particles are filled with sebum, the refractive index changes from a light scattering state to a translucent state, directly causing problems such as patchy and dull makeup, resulting in insufficient makeup staying power.

[0004] To compensate for the shortcomings of physical oil control, the industry has tried adding bioactive ingredients such as azelaic acid and its derivatives, and niacinamide to inhibit sebum secretion at its source. However, in the complex multi-phase system of liquid foundation (coexisting oil phase, water phase, powder, and emulsifier), these active ingredients often face compatibility challenges: water-soluble active ingredients are not evenly dispersed on the powder surface and are prone to precipitation or inactivation during emulsification; at the same time, simple physical mixing of powder and active ingredients cannot achieve the slow release and long-lasting effect of active ingredients.

[0005] With the development of powder processing technology, hypergravity technology has begun to be applied to the preparation of oil-controlling powders for cosmetics. A Chinese patent (authorization announcement number CN115363971B) discloses an oil-controlling powder prepared by a hypergravity acceleration method. This method uses synthetic fluorophlogopite, hydroxyapatite, and nano-zinc oxide as raw materials. After premixing, water is added to form a mixture, which is then passed through a rotating packed bed (RPB) for hypergravity acceleration treatment. Following washing, filtration, and drying, the finished product is obtained, which can improve the powder's spreadability and smooth skin feel to a certain extent. However, this composite powder, mainly composed of hydrophilic minerals, still faces challenges in achieving uniform dispersion and compatibility stability in complex multi-phase systems where oil, water, and powder coexist, such as in foundation liquids. Summary of the Invention

[0006] To address the aforementioned issues, this invention provides a modified oil-controlling silicone powder loaded with active ingredients. This powder retains the advantages of physical powders, such as immediate oil absorption and soft-focus properties, while also stably loading and slowly releasing oil-controlling active ingredients. Furthermore, it can be stably dispersed in complex systems such as foundation liquids, thus better meeting practical application needs.

[0007] This invention provides a modified oil-controlling silicone powder loaded with active ingredients, the modified oil-controlling silicone powder comprising: Porous silica powder as the core layer supporting active material and polydimethylsiloxane coating membrane as the shell layer; The mass ratio of the porous silica powder, active material, and polydimethylsiloxane is 80-100:1-8:3-10.

[0008] Existing hydrophobic coatings easily clog the pores of silica powder, leading to a significant decrease in physical oil absorption capacity. Conversely, insufficient film density results in excessively rapid release of active ingredients, failing to achieve long-lasting oil control; a balance between these two aspects is difficult to achieve. This invention constructs a core-shell structure—a hydrophobic and breathable outer shell and an active inner core within pores—using porous silica powder loaded with active ingredients as the core layer and a polydimethylsiloxane coating as the shell layer. This ensures that the sebum inhibition rate remains stable above 65% for 1-6 hours after application, while retaining an immediate matte, soft-focus effect. It fundamentally solves the problem of traditional physical oil-control powders becoming saturated with oil and causing makeup to darken after 2-4 hours, achieving a balance between oil control strength and makeup longevity.

[0009] The reasons for this invention may be as follows: On the one hand, the hydrophobic polydimethylsiloxane membrane has a breathable structure that does not clog the pores of the silica powder, allowing sebum to enter the pores normally and be absorbed by the silica powder, ensuring immediate physical oil absorption and a soft-focus effect; the active ingredients deep in the pores are slowly released, continuously exerting a biological oil-controlling effect; it can achieve an immediate matte makeup effect quickly through physical oil absorption, and inhibit sebum secretion from the source through biological oil control, which in turn reduces the oil absorption load of the silica powder, slows down the rate at which the silica powder is saturated by sebum, and thus slows down the change in refractive index and the dulling of the makeup; on the other hand, by regulating the release rate of active ingredients through the film density and pore load state, sudden release and release that is too slow are avoided, achieving stable release and continuous oil control for more than 6 hours.

[0010] Furthermore, since liquid foundation is a complex multi-phase system containing water, oil, powder, and emulsifier, exposed water-soluble active ingredients are prone to precipitation during emulsification, or to inactivation due to interaction with other ingredients in the formula, or even to damage the emulsion system, leading to product demulsification and layering. The modified silicone powder provided by this invention can directly replace all or part of the conventional oil-controlling silicone powder in foundation formulas without significant adjustments to the original formula system. It has good compatibility and stability, and provides a smooth, non-drying finish, balancing oil control and gentleness. On the one hand, after being coated with polydimethylsiloxane, the powder surface becomes hydrophobic and oleophilic, significantly improving its compatibility with cosmetic oil phase systems and powder matrices, resulting in uniform dispersion in the formulation and preventing agglomeration and sedimentation. On the other hand, the hydrophobic film encapsulates the active ingredients within the silica powder channels, preventing direct contact with other components in the formulation. This prevents premature deactivation of the active ingredients and avoids interference with the stability of the emulsion system. Furthermore, the active ingredients are slowly released through the channels, avoiding localized high-concentration irritation. At the same time, the bio-oil control reduces the indiscriminate adsorption requirements of physical powders, minimizing excessive damage to the sebum film and alleviating dryness and powder caking issues.

[0011] In one embodiment, the mass ratio of the porous silica powder, active material, and polydimethylsiloxane is 80-100:1-5:3-6.

[0012] In one embodiment, the porous silica powder is cosmetic-grade porous silica powder that has not undergone hydrophobic modification, has a specific surface area of ​​200-300 m² / g, an average particle size of 7-11 μm, and an oil absorption capacity of 230-280 mL / 100g.

[0013] In one embodiment, the polydimethylsiloxane has a nominal kinematic viscosity of 1-5 mm² / s at 25°C (tolerance ±0.2 mm² / s).

[0014] In one embodiment, the active ingredient includes potassium azeloyl diglycinate and nicotinamide.

[0015] In one embodiment, the mass ratio of potassium azeloyl diglycinate and niacinamide is 1-3:1. The two active ingredients work synergistically: potassium azeloyl diglycinate inhibits excessive sebum secretion, while niacinamide regulates sebum metabolism and repairs the skin barrier.

[0016] Another aspect of the present invention provides a method for preparing modified oil-controlling silicone powder loaded with active ingredients, comprising the following steps: Dissolve the active ingredient in deionized water to prepare an aqueous solution of the active ingredient; Porous silica powder is added to the aqueous solution of the active material and stirred for 30-60 minutes to obtain loaded wet powder. The loaded wet powder is vacuum dried at 40-50°C to obtain pre-dried loaded powder; A coating solution is prepared by mixing polydimethylsiloxane with a volatile organic solvent. The pre-dried loaded powder is then immersed in the coating solution and stirred to obtain a flowing slurry. The flowing slurry was added to the ultragravity powder surface coating reactor, and the coating and penetration treatment was carried out under the conditions of 40-50°C in the reactor cavity and 1600-3200 rpm to obtain the coated slurry. The coated slurry was dried and cured, and then sieved to obtain modified oil-controlling silicone powder loaded with active ingredients.

[0017] In one embodiment, the mass fraction of the active ingredient in the aqueous solution is 28% to 32%.

[0018] In one embodiment, the moisture content of the pre-dried loaded powder is 1-3 wt%.

[0019] In one embodiment, the moisture content of the pre-dried loaded powder is 2.0 ± 0.5 wt%.

[0020] Existing conventional impregnation methods only allow active ingredients to adhere to the particle surface and shallow pore areas, leaving a large amount of active ingredients remaining in the solution and unable to enter the pores, resulting in low loading efficiency and significant raw material waste. Furthermore, during ordinary drying, the evaporation of moisture to the particle surface causes water-soluble active ingredients to migrate simultaneously, ultimately resulting in active ingredients accumulating on the particle surface and pore openings in a loosely attached state, easily washed away by sebum, completely losing their sustained-release ability. This invention utilizes a specific surface area of ​​200–300 m² / g. 2 Cosmetic-grade porous silica powder, which has not undergone hydrophobic modification, is stirred for 30-60 minutes to fully impregnate the powder. After being vacuum dried at 40-50℃, a pre-dried loaded powder with a water content of 2.0±0.5wt% is obtained, which achieves a target active ingredient loading rate of over 100%. After 4 hours of artificial sebum agitation washing, the active ingredient residue rate is as high as 98.5%.

[0021] The reason for this may be that the aforementioned porous silica powder balances sufficient loading pore volume with a balanced capillary permeation rate, allowing the active material to be uniformly deposited within the pores while avoiding the drying and agglomeration problems caused by excessive micropores. Under vacuum drying conditions, moisture content control removes only free water from the particle surface, retaining bound water in the pores to fix the active material. This not only inhibits the migration of active material during the drying process at its source but also eliminates the problem of oil-water incompatibility and stratification during subsequent oil phase coating. If the specific surface area of ​​the silica powder is too low, the pore volume is insufficient, and the active material loading capacity cannot meet the requirements for long-term effectiveness. If the specific surface area is too high, the proportion of micropores is too large, and the drying difficulty increases dramatically after water absorption, making the powder prone to hard agglomeration, and subsequent coating processes cannot proceed normally.

[0022] In one embodiment, the volatile organic solvent includes isododecane.

[0023] In one embodiment, the mass fraction of polydimethylsiloxane in the coating liquid is 5% to 20%.

[0024] In one embodiment, the coating and permeation treatment is repeated 5-6 times, with each coating and permeation treatment lasting 4-7 minutes, and the cumulative coating and permeation treatment time lasting 22-36 minutes.

[0025] In one embodiment, the coating and permeation treatment is repeated 5-6 times, with each coating and permeation treatment lasting 4.5-6 minutes, and the cumulative coating and permeation treatment time lasting 22-30 minutes.

[0026] Furthermore, during product development, since the pores are loaded with water-soluble active ingredients while the coating layer is oil-phase polydimethylsiloxane, if free water remains on the particle surface, the polydimethylsiloxane cannot spread and wet, resulting in coating delamination and film detachment, completely failing to achieve the sealing effect. This invention, by employing a supergravity powder surface coating reactor process, combined with parameter optimization and polydimethylsiloxane dosage control, forms a continuous, dense, breathable, and hydrophobic sealing film on the silicon powder surface. This film firmly locks in the active ingredients within the pores, ensuring sustained-release performance, without clogging the oil absorption channels of the silicon powder. The powder exhibits excellent dispersibility and flowability, with no clumping or adhesion, and its spreadability meets the requirements for cosmetic applications.

[0027] Specifically, at temperatures below 40℃, the coating solution has high viscosity and slow molecular diffusion, leading to uneven coating, insufficient loading, and an increase in free active substances on the surface. At temperatures above 50℃, volatile solvents such as isododecane evaporate too quickly, causing polydimethylsiloxane to dry rapidly with the solvent before it can spread sufficiently, resulting in dot-like agglomerates. Simultaneously, the 1.5cst low-viscosity polydimethylsiloxane is lost due to rapid solvent evaporation, resulting in film defects, increased active substance precipitation, and potential damage to the chemical structure of the active substances, yellowing of the product, and reduced oil-controlling activity over prolonged periods at high temperatures. Therefore, when the reactor chamber temperature is kept constant at 40-50℃, volatile solvents such as isododecane can evaporate uniformly and gently. Combined with high shear, polydimethylsiloxane has sufficient time to spread evenly on the silicon powder surface, ultimately forming a continuous and dense hydrophobic film.

[0028] When the rotation speed is less than 1600 rpm, the shear force is insufficient, the slurry film is too thick, and the particles are prone to agglomeration during solvent evaporation, resulting in uneven coating thickness and poor hydrophobic consistency. When the rotation speed is greater than 3200 rpm, the shear force is too strong, which will break the mesoporous structure of silicon powder and destroy the active substances adsorbed in the pores. At the same time, the high-speed collision of particles intensifies, which will lead to secondary agglomeration. Therefore, when the rotation speed of the ultragravity powder surface coating reactor is 1600-3200 rpm, the thickness of the slurry film can be controlled to 3-6 μm to achieve independent coating of single particles. At the same time, continuous shearing can prevent particle adhesion during solvent evaporation.

[0029] When the processing time is less than 22 minutes: the solvent removal is incomplete, the polydimethylsiloxane film layer is not fully formed, the powder is prone to agglomeration after discharge, and the storage stability is poor; when the processing time is greater than 36 minutes: the particles collide and rub for a long time, some of the polydimethylsiloxane film layer is worn away, the sealing effect decreases, and the production efficiency is reduced. Therefore, the processing time of 22 to 36 minutes can balance the solvent removal efficiency and film integrity, making the film uniform and dense, and also making the powder dispersibility and flowability optimal.

[0030] In one embodiment, the drying and curing temperature is 60-80°C, and the time is 2-4 hours.

[0031] The process provided by this invention is stable and controllable, with small performance differences between batches, and can be scaled up for industrial production; at the same time, the product has excellent and stable performance indicators, meeting the quality requirements of cosmetic raw materials.

[0032] The third aspect of this invention provides the application of modified oil-controlling silicone powder loaded with active ingredients in the preparation of cosmetics.

[0033] In one embodiment, the cosmetic product includes a base makeup product, which includes liquid foundation, loose powder, or pressed powder.

[0034] Beneficial effects 1. This invention provides a modified oil-controlling silicone powder loaded with active ingredients, which retains the advantages of physical powder in immediate oil absorption and soft focus, while also being able to stably load and slowly release oil-controlling active ingredients. At the same time, it can be stably dispersed in complex systems such as foundation liquid, better meeting the needs of practical applications.

[0035] 2. This invention constructs a core-shell structure with a hydrophobic and breathable outer shell and an active inner core, using porous silica powder loaded with active ingredients as the core layer and a polydimethylsiloxane coating membrane as the shell layer. This ensures that the sebum inhibition rate remains stable at over 65% for 1 to 6 hours after product application, while retaining an immediate matte soft-focus effect. This fundamentally solves the problem of traditional physical oil-control powders becoming saturated with oil and dulling of makeup after 2 to 4 hours, achieving a balance between oil control strength and makeup staying power.

[0036] 3. The modified silicone powder provided by this invention can directly replace all or part of the conventional oil-controlling silicone powder in the base makeup formula without significantly adjusting the original formula system. It has good compatibility and stability, and the makeup effect is smooth and non-drying, taking into account both oil control effect and gentleness of use.

[0037] 4. This invention utilizes a specific surface area of ​​200-300 m². 2 Cosmetic-grade porous silica powder, which has not undergone hydrophobic modification, is stirred for 30-60 minutes to fully impregnate the powder. After being vacuum dried at 40-50℃, a pre-dried loaded powder with a water content of 2.0±0.5wt% is obtained, which achieves a target active ingredient loading rate of over 100%. After 4 hours of artificial sebum agitation washing, the active ingredient residue rate is as high as 98.5%.

[0038] 5. This invention employs a supergravity powder surface coating reactor process, combined with parameter optimization and polydimethylsiloxane dosage control, to form a continuous and dense breathable and hydrophobic sealing membrane on the surface of silicon powder. This membrane not only firmly locks in the active ingredients within the pores and ensures sustained-release performance, but also does not clog the oil absorption channels of the silicon powder. The powder exhibits excellent dispersibility and flowability, with no clumping or adhesion, and its spreadability meets the requirements for cosmetic applications. Attached Figure Description

[0039] Figure 1 This is a photograph of a modified oil-controlling silicone powder loaded with active ingredients. Detailed Implementation

[0040] The raw material information for each comparative example is shown in Table 1.

[0041] Table 1

[0042] Example 1 Embodiment 1 of the present invention provides a modified oil-controlling silicone powder loaded with active ingredients, the modified oil-controlling silicone powder comprising: Porous silica powder as the core layer supporting active material and polydimethylsiloxane coating membrane as the shell layer; The porous silica powder, active ingredient (potassium azeloyl diglycinate and nicotinamide in a mass ratio of 2:1), and polydimethylsiloxane are in a mass ratio of 100:5:6.

[0043] Example 1 of the present invention provides a method for preparing modified oil-controlling silicone powder loaded with active ingredients, comprising the following steps: Dissolve the active ingredient in deionized water to prepare an aqueous solution of the active ingredient; Porous silica powder was added to the aqueous solution of the active material and stirred for 60 min to obtain loaded wet powder; The loaded wet powder was vacuum dried at 45°C to obtain pre-dried loaded powder; A coating solution is prepared by mixing polydimethylsiloxane with a volatile organic solvent. The pre-dried loaded powder is then immersed in the coating solution and stirred to obtain a flowing slurry. The flowing slurry was added to the ultragravity powder surface coating reactor, and the coating and penetration treatment was carried out under the conditions of 45°C in the reactor cavity and 2300 rpm of rotor speed to obtain the coated slurry. The coated slurry was dried and cured, and then passed through a 200-mesh sieve to obtain modified oil-controlling silicone powder loaded with active ingredients.

[0044] The active ingredient in the aqueous solution has a mass fraction of 30%.

[0045] The moisture content of the pre-dried loaded powder is 2.0 ± 0.5 wt%.

[0046] The coating solution contains 10% polydimethylsiloxane by mass.

[0047] The coating and permeation treatment was repeated 5 times, with each coating and permeation treatment lasting 6 minutes, and the total coating and permeation treatment time lasting 30 minutes.

[0048] The drying and curing temperature is 65℃ and the time is 3 hours.

[0049] Example 2 Example 2 of the present invention provides a modified oil-controlling silica powder loaded with active material and its preparation method. The specific implementation method is the same as that of Example 1, except that the mass ratio of the porous silica powder, active material and polydimethylsiloxane is 80:1:3.

[0050] The preparation steps are the same as in Example 1.

[0051] Example 3 Example 3 of the present invention provides a modified oil-controlling silicone powder loaded with active material and its preparation method. The specific implementation method is the same as that in Example 1, except that the preparation steps are as follows: the parameters of the hypergravity reactor are adjusted to a temperature of 40°C and a rotor speed of 1600 rpm, and the coating is circulated 5 times, with each cycle lasting 4.5 min and the cumulative treatment time being 22.5 min; the remaining steps are the same as those in Example 1.

[0052] Comparative Example 1 Comparative Example 1 of the present invention provides a modified oil-controlling silicone powder with supported active ingredients and a method for preparing the same. The method for preparing the modified oil-controlling silicone powder with supported active ingredients includes the following steps: Dissolve the active ingredient in deionized water to prepare an aqueous solution with a mass fraction of 30%; Porous silica powder was added to the aqueous solution of the active ingredient, and the mixture was continuously stirred and soaked at 50°C for 6 hours. Then, it was vacuum dried at 55°C until the moisture content was <2%, and the modified oil-controlling silica powder loaded with the active ingredient was obtained by passing it through a 200-mesh sieve.

[0053] The mass ratio of porous silicon powder to active material is the same as in Example 1.

[0054] Comparative Example 2 Comparative Example 2 of the present invention provides a modified oil-controlling silicone powder loaded with active ingredients and its preparation method. The specific implementation method is the same as that of Example 1, except that the temperature inside the reactor chamber is 25°C.

[0055] Comparative Example 3 Comparative Example 3 of the present invention provides a modified oil-controlling silica powder loaded with active ingredients and its preparation method. The specific implementation method is the same as that of Example 1, except that the rotor speed in the reactor chamber is 800 rpm.

[0056] Comparative Example 4 Comparative Example 4 of the present invention provides a modified oil-controlling silicone powder loaded with active material and its preparation method. The specific implementation method is the same as that of Example 1, except that the coating and penetration treatment is cycled twice, the time of a single coating and penetration treatment is 6 minutes, and the cumulative time of the coating and penetration treatment is 12 minutes.

[0057] Comparative Example 5 Comparative Example 5 of the present invention provides a modified oil-controlling silica powder loaded with active ingredients and its preparation method. The specific implementation method is the same as that of Example 1, except that the rotor speed in the reactor chamber is 4000 rpm.

[0058] Comparative Example 6 Comparative Example 6 of the present invention provides a modified oil-controlling silicone powder loaded with active ingredients and its preparation method. The specific implementation method is the same as that of Example 1, except that the temperature inside the reactor chamber is 70°C.

[0059] Performance testing The products obtained in the examples and comparative examples were subjected to the following tests.

[0060] 1. Determination of actual loading of active ingredient Test method: Thermogravimetric analyzer (TGA) was used. Under nitrogen protection, the temperature was increased to 800℃ at a rate of 10℃ / min. The percentage of thermal weight loss of active material in the sample was measured, and the actual loading was calculated.

[0061] Loading rate calculation formula: Loading rate (%) = (Mass of active material / Mass of silicon powder) × 100% The target value for the active ingredient loading in this test is 20%.

[0062] The test results are shown in Table 2.

[0063] Table 2

[0064] Analysis of the data in Table 2 shows that: The actual loading rates of the examples were closest to the target values. Comparative Example 1 used a conventional impregnation method, resulting in a large amount of active ingredient remaining in the solution, with an actual loading rate of only 76.5%, causing significant waste. Comparative Examples 2-4 all failed to meet the target loading rates due to insufficient loading drive force or time caused by parameter deviations. Although Comparative Examples 5-6 had similar loading rates, subsequent tests showed a significant deterioration in uniformity and skin feel.

[0065] 2. Determination of the coating strength (wash resistance) of active ingredients Test method: Accurately weigh 1.0 g of the powder to be tested, add 50 mL of artificial sebum, and place in a 37℃ constant temperature shaker. Wash at 150 rpm for 4 hours. After washing, centrifuge at 10000 rpm, discard the supernatant, gently rinse the powder surface with acetone to remove residual sebum, and vacuum dry at room temperature (25℃). The active ingredient content of the powder before and after washing is determined by TGA method, and the residual active ingredient rate is calculated.

[0066] Residual rate calculation formula: Active ingredient residual rate (%) = (Active ingredient content after washing / Active ingredient content before washing) × 100% The test results are shown in Table 3.

[0067] Table 3

[0068] Analysis of the data in Table 3 shows that after 4 hours of vigorous shaking and washing, the residual rate of active material in the example was ≥96%, proving that the super-gravity coating firmly anchored the active material deep within the pores, rather than loosely adhering it. Comparative Example 1 (conventional impregnation method) had a residual rate of only 72.1%, indicating that a large amount of active material only accumulated on the surface or pore openings, making it very easy to wash off. Other comparative examples, due to insufficient coating driving force, had active materials mostly remaining in the shallow layer, and their adhesion was significantly less than that of Example 1. The residual rate of Comparative Example 6 (70℃) increased slightly, but combined with the appearance evaluation, the high temperature caused the product to yellow, suggesting possible chemical changes in the active material.

[0069] 3. Oil control durability test Test Method: Thirty healthy volunteers with oily skin were randomly divided into 6 groups of 5 each. A 3cm × 3cm test area was marked on the forehead, and the same base emulsion containing 5wt% of the test powder was applied to each group. The amount of sebum secreted by the skin was measured before application (T0), 1 hour after application (T1h), 3 hours after application (T3h), and 6 hours after application (T6h) using a skin oil analyzer, and the sebum inhibition rate was calculated.

[0070] Formula for calculating sebum inhibition rate: Sebum inhibition rate (%) = (Sebum amount at T0 - Sebum amount at Tn) / Sebum amount at T0 × 100% The test results are shown in Table 4.

[0071] Table 4

[0072] Analysis of the data in Table 4 shows that Example 1 maintained a high sebum inhibition rate of over 65% for 1-6 hours after application, demonstrating excellent long-lasting oil control. This is because the active ingredient exerts a sustained chemical oil-controlling effect through slow release. The sebum inhibition rate of Comparative Example 1 decreased rapidly over time, reaching only 28.3% after 6 hours. This is because the surfactant was rapidly consumed, and there was insufficient reserve within the pores. Other comparative examples also exhibited relatively poor oil control durability due to insufficient loading or poor uniformity.

Claims

1. A modified oil-controlling silicone powder loaded with active ingredients, characterized in that, The modified oil-controlling silicone powder includes: Porous silica powder as the core layer supporting active material and polydimethylsiloxane coating membrane as the shell layer; The mass ratio of the porous silica powder, active material, and polydimethylsiloxane is 80-100:1-8:3-10.

2. The modified oil-controlling silicone powder with supported active ingredients according to claim 1, characterized in that, The porous silica powder is cosmetic-grade porous silica powder that has not undergone hydrophobic modification, and has a specific surface area of ​​200–300 m². 2 / g, with an average particle size of 7-11μm and an oil absorption of 230-280mL / 100g.

3. The modified oil-controlling silicone powder with supported active ingredients according to claim 1, characterized in that, The active ingredients include potassium azeloyl diglycinate and nicotinamide.

4. A method for preparing modified oil-controlling silicone powder according to any one of claims 1-3, characterized in that, Includes the following steps: Dissolve the active ingredient in deionized water to prepare an aqueous solution of the active ingredient; Porous silica powder is added to the aqueous solution of the active material and stirred for 30-60 minutes to obtain loaded wet powder. The loaded wet powder is vacuum dried at 40-50°C to obtain pre-dried loaded powder; A coating solution is prepared by mixing polydimethylsiloxane with a volatile organic solvent. The pre-dried loaded powder is then immersed in the coating solution and stirred to obtain a flowing slurry. The flowing slurry was added to the ultragravity powder surface coating reactor, and the coating and penetration treatment was carried out under the conditions of 40-50°C in the reactor cavity and 1600-3200 rpm to obtain the coated slurry. The coated slurry was dried and cured, and then sieved to obtain modified oil-controlling silicone powder loaded with active ingredients.

5. The preparation method according to claim 4, characterized in that, The moisture content of the pre-dried loaded powder is 1-3 wt%.

6. The preparation method according to claim 4, characterized in that, The coating and permeation treatment is repeated 5-6 times, with each coating and permeation treatment lasting 4-7 minutes, and the total coating and permeation treatment time lasting 22-36 minutes.

7. The preparation method according to claim 4, characterized in that, The volatile organic solvent includes isododecane.

8. The preparation method according to claim 4, characterized in that, The drying and curing temperature is 60-80℃, and the time is 2-4 hours.

9. The application of a modified oil-controlling silicone powder loaded with active ingredients according to any one of claims 1-3 or a modified oil-controlling silicone powder loaded with active ingredients prepared by the preparation method according to any one of claims 4-8 in the preparation of cosmetics.

10. The application according to claim 9, characterized in that, The cosmetics include base makeup products, which include liquid foundation, loose powder, or pressed powder.

Citation Information

Patent Citations

  • Oil-controlling powder prepared by a supergravity acceleration method and its application

    CN115363971B