Hollow capsule for dry powder inhalation based on interface synergy and method for its preparation

The preparation method using interfacial synergy solves the problems of drug adsorption, puncture debris, and mold release oil seepage in dry powder inhalers using hollow capsules, achieving efficient drug delivery and improved safety, and is suitable for industrial production.

CN123148264APending Publication Date: 2026-11-24JIANGSU LEFAN CAPSULE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611650897.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing empty capsules in dry powder inhalers have problems such as strong drug adsorption, excessive puncture debris, and severe internal leakage of release oil, which affect drug delivery efficiency and safety.

Method used

A preparation method based on interface synergy was adopted. By adjusting the isoelectric point of gelatin and using a TEC/GMS composition to form a hydrophobic interface modifier with amino acids, combined with a specific release oil and gradient drying technology, hollow capsules with low charge adsorption and good toughness were prepared.

Benefits of technology

It increases the drug clearance rate to over 95%, reduces puncture debris and release oil residue, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148264A_ABST
    Figure CN123148264A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of pharmaceutical preparations and excipients technology, specifically relating to a dry powder inhalation empty capsule based on interfacial synergistic effects and its preparation method. The empty capsule comprises the following components by weight: 100 parts by weight of film-forming matrix material, 1.1-7 parts by weight of hydrophobic interface modifier, and 0.5-6 parts by weight of toughening enhancer. The hydrophobic interface modifier comprises 1-3 parts by weight of TEC / GMS composition and 0.1-4 parts by weight of amino acid, wherein the amino acid is L-leucine or L-valine. This invention, through innovative formulation components and preparation method, utilizes thermodynamic incompatibility to induce self-modification of the inner wall, resulting in a high-performance inhalation empty capsule with low charge adsorption. The capsule obtained by this invention has an emptying rate of over 95%, a low puncture fragmentation rate, and less than 0.05% residual release oil, making it suitable for dry powder inhalation formulations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of pharmaceutical preparations and excipients technology, specifically relating to a dry powder inhalation empty capsule based on interfacial synergistic effects and its preparation method. Background Technology

[0002] Dry powder inhalers (DPIs) rely on the turbulence generated by the patient's inhalation to depolymerize the drug powder from the capsule and deliver it to the lungs. However, existing empty capsules face three major bottlenecks:

[0003] The inner wall of gelatin or HPMC capsules has high surface energy and is charged, making it easy for micronized APIs with opposite charges (such as budesonide and tiotropium bromide) to undergo electrostatic adsorption, resulting in an emptying rate of less than 95%. Although CN1439360A discloses the addition of leucine to powder to improve flowability, no reports have been found on the in-situ enrichment technology of leucine on the inner wall of capsules.

[0004] Traditional capsules have brittle walls, and puncture produces fibrous debris that enters the deep airways with the airflow, triggering a cough reflex. While conventional plasticizers (such as glycerin and sorbitol) can toughen the capsules, excessive use can lead to softening and slow disintegration.

[0005] Current capsule manufacturing processes commonly use light mineral oil as a release agent. Its small molecules can easily penetrate into the capsule wall, with residual levels reaching 0.05%-0.5%. CN112606277A attempted to use a compound of soybean phospholipids, but phospholipids are easily oxidized and difficult to control their migration to the inner wall, causing changes in API wettability or stability.

[0006] Therefore, there is an urgent need to develop a dry powder inhalation empty capsule and its corresponding preparation method to solve the above problems. Summary of the Invention

[0007] To address the technical problems of existing inhalation capsules, such as strong drug adsorption, excessive puncture debris, and severe internal leakage of release oil, this invention provides a dry powder inhalation empty capsule based on interfacial synergistic effects and its preparation method. By innovating the formulation components and combining them with the preparation method, thermodynamic incompatibility is used to induce self-modification of the inner wall, resulting in a high-performance inhalation empty capsule with low charge adsorption.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] A dry powder inhalation empty capsule based on interfacial synergy, the empty capsule comprising the following parts by weight: 100 parts by weight of film-forming matrix material, 1.1-7 parts by weight of hydrophobic interface modifier and 0.5-6 parts by weight of toughening enhancer, wherein the hydrophobic interface modifier comprises 1-3 parts by weight of TEC / GMS composition and 0.1-4 parts by weight of amino acid, wherein the amino acid is L-leucine or L-valine.

[0010] Furthermore, the isoelectric point of the film-forming substrate material is 4.6 to 5.3.

[0011] Furthermore, the toughness enhancer is 0.5-3 parts polyvinyl alcohol, 1-3 parts polyvinyl ketone, 2-5 parts trehalose, 2-4 parts sorbitol, or 0.5-6 parts polyethylene glycol.

[0012] Furthermore, the mass ratio of TEC to GMS in the TEC / GMS composition is 2.5:1 to 3.5:1.

[0013] A method for preparing a dry powder inhalation empty capsule based on interfacial synergy includes the following steps: Step 1: After swelling the film-forming matrix material with water, a toughening enhancer and a TEC / GMS composition are added, the pH is adjusted to the isoelectric point using a regulator, and then amino acids are added for dispersion to obtain a gel solution; Step 2: After preheating the mold, a release oil is applied and then the glue is applied, followed by gradient drying. After drying, the empty capsule is demolded and cut to obtain the empty capsule.

[0014] Invention Concept: The pH of the gelatin solution is adjusted to 4.6–5.3 (near the isoelectric point of gelatin). At this pH, the gelatin carries a weak positive charge, and the hydrophobic L-leucine / L-valine undergoes phase separation from the low-polarity microphase formed by TEC-GMS. Due to thermodynamic repulsion, in the initial drying stage, moisture on the inner membrane side migrates to the mold-membrane gap and undergoes micro-evaporation, resulting in the enrichment of hydrophobic isobutyl side chains on the subsurface of the inner membrane. After demolding, the inner membrane surface exhibits weak hydrophobicity. The hydrophilic gelatin backbone tends to accumulate outwards, while the hydrophobic amino acid-TEC-GMS microphase is repelled inwards. Combined with a specific drying curve, a near-neutral modified layer rich in hydrophobic amino acids is ultimately formed on the inner wall of the capsule.

[0015] Furthermore, in step one, the mass ratio of the film-forming substrate material to water is 1:1.5 to 3, and the regulator is glacial acetic acid or sodium hydroxide.

[0016] Furthermore, in step two, the mold preheating temperature is 28–36°C, and the release oil comprises the following components by mass fraction: 70%–90% medium-chain triglycerides, 5%–15% triethyl citrate, 0.5%–2% Span-80, and 5–10% soybean lecithin, wherein the viscosity of the medium-chain triglycerides is 26–32 mPa·s. Further, in step two, the release oil is prepared by the following method: after heating the medium-chain triglycerides to 40-50°C, Span-80 is poured into the medium-chain triglycerides and stirred at 80-120 rpm for 5-10 min; then soybean lecithin is slowly added and stirred at 300-500 rpm for 10-20 min until it becomes transparent and clear; then triethyl citrate preheated to 30-40°C is added and stirred at 40-100 rpm for 5-20 min to obtain an oil phase mixture; the oil phase mixture is placed in a vacuum environment of -0.05 MPa to -0.1 MPa and degassed at room temperature for 5-10 min; after degassed, it is filtered to remove impurities to obtain the release oil.

[0017] Further, in step two, the gradient drying includes the following steps: drying the mold in an environment of 15-28°C and 55-65% relative humidity for 15-20 minutes, and then drying the mold in an environment of 35-40°C and 25-35% relative humidity for 30-60 minutes.

[0018] The present invention has the following beneficial effects:

[0019] The hollow capsules prepared by this invention can increase the emptying rate to over 95% and possess low adsorption properties on the inner wall. Simultaneously, the hydrogen bond network formed by PVA / PVP / trehalose / sorbitol / polyethylene glycol in this invention gives the capsule wall excellent extensibility, resulting in extremely low fragment generation during puncture testing. Puncture tests show that the number of fragments >50μm is ≤1 per capsule. The residual release oil in the finished capsules is lower than the industry requirement for inhalation capsules (not exceeding 0.05%). This invention achieves the transformation from a thermodynamically unstable system to a stable dual-interface structure through precise control of pH and drying curves, exhibiting good repeatability and suitability for industrial production. Attached Figure Description

[0020] Figure 1 These are capsule powder adhesion test images of the hollow capsules prepared in the embodiments and comparative examples of this invention;

[0021] Figure 2 This is a test diagram of the puncture position status of the hollow capsules prepared in the embodiments and comparative examples of the present invention. Detailed Implementation

[0022] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the specific embodiments according to the present invention will be described in detail below with reference to the embodiments and accompanying drawings.

[0023] Example 1

[0024] A dry powder inhalation hollow capsule based on interface synergy, the hollow capsule comprising the following parts by weight: 100 parts by weight of film-forming matrix material, 4.3 parts by weight of hydrophobic interface modifier and 3 parts by weight of toughness enhancer.

[0025] Specifically, the film-forming matrix material is 100g of gelatin, preferably acid-peeled gelatin with an isoelectric point of 4.6–5.3. The hydrophobic interface modifier includes 2.5g of triethyl citrate (TEC) and 1.0g of glyceryl monostearate (GMS), with L-leucine at 0.8g. The toughness enhancer is 3g of polyvinyl alcohol (PVA).

[0026] This embodiment provides a method for preparing a dry powder inhalation empty capsule based on interfacial synergy, comprising the following steps:

[0027] Step 1: After the film-forming matrix material is swollen with water, a toughening enhancer and a TEC / GMS composition are added. The pH is adjusted to the isoelectric point using a regulator, and then amino acids are added for dispersion to obtain the adhesive solution.

[0028] Specifically, 100g of acid-treated peeled gelatin is dissolved in 200g of hot pure water. 2.5g of triethyl citrate, 1.0g of glyceryl monostearate, and 3g of polyvinyl alcohol are added and stirred until dissolved. After dissolution, the solution is cooled to 50℃, and the pH is adjusted to 4.8 using glacial acetic acid. Then, 0.8g of L-leucine is added, and the mixture is dispersed by low-speed shearing to obtain the gel. Step two: After preheating the mold, a release oil is applied, followed by dipping in the gel. Gradient drying is then performed. After drying, the gel is demolded and cut to obtain hollow capsules.

[0029] Specifically, the mold is preheated to 30°C, and a release oil is applied to the mold. In this embodiment, the release oil comprises the following components by weight fraction: 82% medium-chain triglycerides, 10% triethyl citrate, 1% Span-80, and 7% soybean lecithin. It is prepared by the following method:

[0030] After heating the medium-chain triglycerides to 45°C, Span-80 was poured into the medium-chain triglycerides and stirred at 100 rpm for 5 minutes. Then, soybean lecithin was slowly added and stirred at 300 rpm for 20 minutes until it became transparent and clear. Then, triethyl citrate preheated to 35°C was added and stirred at 80 rpm for 10 minutes to obtain an oil phase mixture. The oil phase mixture was placed in a vacuum environment of -0.05 MPa and degassed at room temperature for 5 minutes. After degassed, the mixture was filtered to remove impurities to obtain the release oil.

[0031] The mold is dipped into the adhesive solution and then subjected to gradient drying. The first stage is the anchoring stage, where the mold is dried for 18 minutes at 20°C and 60% relative humidity. During this stage, the internal temperature of the mold is higher than the external drying environment temperature, causing the inner gelatin shell to lose water at a faster rate than the outside. This rapid dehydration and setting of the internal gelatin simultaneously anchors the hydrophobic microphase firmly to the inner wall. The next stage is the vitrification stage, where the mold is dried for 75 minutes at 36°C and 30% relative humidity. The high temperature and low humidity environment in this stage promotes the overall vitrification transition of the capsule, physically locking in the dual-interface structure.

[0032] After drying, the product is demolded and cut to obtain the finished product.

[0033] Example 2

[0034] This embodiment provides a method for preparing a dry powder inhalation empty capsule based on interfacial synergy, comprising the following steps:

[0035] Step 1: After the film-forming matrix material is swollen with water, a toughening enhancer and a TEC / GMS composition are added. The pH is adjusted to the isoelectric point using a regulator, and then amino acids are added for dispersion to obtain the adhesive solution.

[0036] Specifically, 100g of alkaline gelatin (isoelectric point 5.0) is dissolved in 250g of hot pure water. 1.75g ​​of triethyl citrate, 0.5g of glyceryl monostearate, and 2g of polyethylene glycol (PEG 3350) are added and stirred until dissolved. After dissolution, the solution is cooled to 50℃, and the pH is adjusted to 4.8 using glacial acetic acid. Then, 0.8g of L-valine is added, and the solution is dispersed by low-speed shearing to obtain the gel. Step two: After preheating #3 stainless steel, a release oil is applied, followed by dipping in the gel. Gradient drying is then performed. After drying, the gel is demolded and cut to obtain hollow capsules.

[0037] Specifically, the mold is preheated to 30°C, and a release oil is applied to the mold. In this embodiment, the release oil comprises the following components by weight fraction: 82% medium-chain triglycerides, 10% triethyl citrate, 1% Span-80, and 7% soybean lecithin. It is prepared by the following method:

[0038] After heating the medium-chain triglycerides to 45°C, Span-80 was poured into the medium-chain triglycerides and stirred at 100 rpm for 5 minutes. Then, soybean lecithin was slowly added and stirred at 300 rpm for 20 minutes until it became transparent and clear. Then, triethyl citrate preheated to 35°C was added and stirred at 80 rpm for 10 minutes to obtain an oil phase mixture. The oil phase mixture was placed in a vacuum environment of -0.05 MPa and degassed at room temperature for 5 minutes. After degassed, the mixture was filtered to remove impurities to obtain the release oil.

[0039] The mold is dipped into the adhesive solution and then subjected to gradient drying. The first stage is the anchoring stage, where the mold is dried for 18 minutes at 20°C and 60% relative humidity. During this stage, the internal temperature of the mold is higher than the external drying environment temperature, causing the inner gelatin shell to lose water at a faster rate than the outer shell. This rapid dehydration and setting of the internal gelatin simultaneously anchors the hydrophobic microphase firmly to the inner wall. The next stage is the vitrification stage, where the mold is dried for 45 minutes at 36°C and 30% relative humidity. The high temperature and low humidity environment in this stage promotes the overall vitrification transition of the capsule, physically locking in the dual-interface structure.

[0040] After drying, the product is demolded and cut to obtain the finished product.

[0041] Example 3

[0042] This embodiment provides a method for preparing a dry powder inhalation empty capsule based on interfacial synergy, comprising the following steps:

[0043] Step 1: After the film-forming matrix material is swollen with water, a toughening enhancer and a TEC / GMS composition are added. The pH is adjusted to the isoelectric point using a regulator, and then amino acids are added for dispersion to obtain the adhesive solution.

[0044] Specifically, 100g of alkaline gelatin (isoelectric point 5.0) is dissolved in 150g of hot pure water. 2.5g of triethyl citrate (TEC), 1.0g of glyceryl monostearate (GMS), and 2g of trehalose are added and stirred until dissolved. After dissolution, the solution is cooled to 50℃, and the pH is adjusted to 4.8 using glacial acetic acid. Then, 1.0g of L-leucine is added, and the mixture is dispersed by low-speed shearing to obtain the gel. Step two: After preheating a #3 stainless steel mold, a release oil is applied, followed by dipping the mold in the gel. Gradient drying is then performed. After drying, the mold is demolded and cut to obtain hollow capsules.

[0045] Specifically, the mold is preheated to 32°C, and a release oil is applied to the mold. In this embodiment, the release oil comprises the following components by weight fraction: 88.5% medium-chain triglycerides, 5% triethyl citrate, 1.5% Span-80, and 5% soybean lecithin. It is prepared by the following method:

[0046] After heating the medium-chain triglycerides to 45°C, Span-80 was poured into the medium-chain triglycerides and stirred at 100 rpm for 5 minutes. Then, soybean lecithin was slowly added and stirred at 300 rpm for 20 minutes until it became transparent and clear. Then, triethyl citrate preheated to 35°C was added and stirred at 80 rpm for 10 minutes to obtain an oil phase mixture. The oil phase mixture was placed in a vacuum environment of -0.05 MPa and degassed at room temperature for 5 minutes. After degassed, the mixture was filtered to remove impurities to obtain the release oil.

[0047] The mold is dipped into the adhesive solution and then subjected to gradient drying. The first stage is the anchoring stage, where the mold is dried for 18 minutes at 20°C and 60% relative humidity. During this stage, the internal temperature of the mold is higher than the external drying environment temperature, causing the inner gelatin shell to lose water at a faster rate than the outer shell. This rapid dehydration and setting of the internal gelatin simultaneously anchors the hydrophobic microphase firmly to the inner wall. The next stage is the vitrification stage, where the mold is dried for 45 minutes at 36°C and 30% relative humidity. The high temperature and low humidity environment in this stage promotes the overall vitrification transition of the capsule, physically locking in the dual-interface structure.

[0048] After drying, the product is demolded and cut to obtain the finished product.

[0049] Comparative Example 1

[0050] Compared to Example 1, the release oil used in this comparative example comprises the following components by weight fraction: 92% medium-chain triglycerides, 1% Span-80 and 7% soybean lecithin, without the addition of triethyl citrate, and otherwise consistent with Example 1.

[0051] Comparative Example 2

[0052] Compared with Example 1, in step one of the preparation method of this comparative example, the pH of the adhesive solution was adjusted to 7.0, and other parameters and steps were the same as in Example 1.

[0053] Comparative Example 3

[0054] Compared with Example 1, the hollow capsule prepared in this comparative example does not contain a hydrophobic interface modifier and includes the following weight parts: 100 parts by weight of film-forming matrix material and 3 parts by weight of toughness enhancer. In step two of the preparation method, the release oil is a conventional release agent purchased from Yushe County Pengcheng Fine Additives Factory. Other parameters and steps are the same as in Example 1.

[0055] Comparative Example 4

[0056] Compared to Example 1, this comparative example uses hollow capsules prepared by conventional methods. Specifically, the hollow capsules consist of 100 parts by weight of film-forming matrix material and 200 parts by weight of hot pure water, using a compound release agent purchased from Yushe County Pengcheng Fine Additives Factory. The molding process was controlled as follows: the mold temperature was controlled at 20-25℃, no gradient drying was performed, and drying was carried out in a drying oven at 26-32℃ and 30%-65% relative humidity for 60-90 minutes.

[0057] The empty capsules prepared in the above embodiments and comparative examples were subjected to performance testing. The method for testing the emptying rate was as follows: The total mass of 10 empty capsules was weighed and recorded as M1 (g); the capsule cap and body were separated, and 0.03g of 200-mesh lactose was added to each capsule segment. After fitting the capsules together, they were rotated horizontally to ensure that the lactose fully contacted the inner surface of the capsules. The lactose was then poured out, and the total mass of the capsules after pouring out the lactose was weighed again and recorded as M2 (g). The formula for calculating the emptying rate is: .

[0058] The puncture debris test method is as follows: Take 50 empty capsules to be tested and place them in a closed environment at 25℃ and 25%±5%RH relative humidity for 24 hours to equilibrate. After equilibration, immediately remove them, lock them in place, and insert them one by one into the inhalation device for puncture. After the operation, remove the capsules, separate the caps, and observe and record whether free debris is generated in each capsule.

[0059] The test method for residual release oil is as follows: According to the first method Soxhlet extraction method specified in GB 5009.6-2025 "National Food Safety Standard Determination of Fat in Food", the lubricating oil content in the prepared capsules is determined. A blank correction is performed using capsule substrate without release oil, and the percentage of residual oil in the total mass of the capsules is calculated.

[0060] The test results are shown in Table 1 below. Figure 1-2 As shown:

[0061] Table 1. Performance test results of the empty capsules prepared in the examples and comparative examples.

[0062] Testing items Emptying rate puncture debris Mold release oil residue on the inner wall Example 1 97.9% 1 pill 0.010% Example 2 97.2% 0 grains 0.010% Example 3 98.1% 1 pill 0.009% Comparative Example 1 95.2% 1 pill 0.015% Comparative Example 2 93.0% 1 pill 0.01% Comparative Example 3 84.9% 1 pill 0.039% Comparative Example 4 83.1% 5 pills 0.052%

[0063] Analysis of experimental results:

[0064] From the emptying rate and capsule powder adhesion diagram ( Figure 1 It can be seen that the capsules prepared using the release agent and capsule shell formulation of the present invention (Examples 1-3, Comparative Example 2) have a 10-15% higher emptying rate compared with capsules prepared using commercially available compound release agents (Comparative Example 3, Comparative Example 4). This indicates that the release agent and capsules provided by the present invention can effectively reduce the adhesion of inhaled preparation APIs inside the capsule, ensuring an effective dosage. The difference between Comparative Example 1 and Example 1 is that TEC (triethyl citrate) was not added, resulting in uneven distribution of adhesive powder in the prepared capsules, indirectly indicating that the release agent failed to form a uniform oil film on the mold surface. The difference between Comparative Example 2 and Example 1 lies in the different isoelectric points of the encapsulating gel. Comparative Example 2 did not control the isoelectric point of gelatin within the range of 4.6-5.3, resulting in more severe adhesive powder in the prepared capsules.

[0065] Based on the results of the release oil residue test, it can be indirectly verified that the lubricating oil content of the capsules prepared using the technology of this invention is 0.027-0.043% lower than that of capsules prepared using commercially available compound release agents. This means that using the release agent for capsule molds of this invention to produce similar empty capsules can reduce the amount of release agent used, thereby improving product quality while reducing costs. Puncture test results show that in Comparative Example 4, which did not use the plasticizer described in this invention, the proportion of puncture fragments detached from the capsule shell significantly increased after equilibration in a low-humidity environment, indicating that the capsules of this invention can effectively reduce the puncture fragmentation rate.

[0066] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A dry powder inhalation empty capsule based on interfacial synergy, the empty capsule comprising the following parts by weight: 100 parts by weight of film-forming matrix material, 1.1-7 parts by weight of hydrophobic interface modifier and 0.5-6 parts by weight of toughening enhancer, wherein the hydrophobic interface modifier comprises 1-3 parts by weight of TEC / GMS composition and 0.1-4 parts by weight of amino acid, wherein the amino acid is L-leucine or L-valine.

2. The dry powder inhalation empty capsule based on interface synergy according to claim 1, characterized in that, The isoelectric point of the film-forming substrate material is 4.6 to 5.

3.

3. The dry powder inhalation empty capsule based on interface synergy according to claim 1, characterized in that, The toughness enhancer is 0.5-3 parts polyvinyl alcohol, 1-3 parts polyvinyl ketone, 2-5 parts trehalose, 2-4 parts sorbitol, or 0.5-6 parts polyethylene glycol.

4. The dry powder inhalation empty capsule based on interface synergy according to claim 1, characterized in that, The mass ratio of TEC to GMS in the TEC / GMS composition is 2.5:1 to 3.5:

1.

5. The method for preparing the dry powder inhalation empty capsule based on interfacial synergy as described in any one of claims 1-4, characterized in that, Includes the following steps: Step 1: After the film-forming matrix material is swollen with water, a toughening enhancer and a TEC / GMS composition are added. The pH is adjusted to the isoelectric point using a regulator, and then amino acids are added for dispersion to obtain a glue solution. Step 2: After preheating the mold, a release oil is applied and then the glue is applied. Gradient drying is then carried out. After drying, the mold is demolded and cut to obtain hollow capsules.

6. The method for preparing a dry powder inhalation empty capsule based on interfacial synergy according to claim 5, characterized in that, In step one, the mass ratio of the film-forming substrate material to water is 1:1.2 to 3, and the regulator is glacial acetic acid or sodium hydroxide.

7. The method for preparing a dry powder inhalation empty capsule based on interfacial synergy according to claim 5, characterized in that, In step two, the mold preheating temperature is 28-36℃, and the mold oil includes the following components by mass fraction: 70%-90% medium-chain triglycerides, 5%-15% triethyl citrate, 0.5%-2% Span-80 and 5-10% soybean lecithin, and the viscosity of the medium-chain triglycerides is 26-32 mPa·s.

8. The method for preparing a dry powder inhalation empty capsule based on interfacial synergy according to claim 5, characterized in that, The release oil is prepared by the following method: medium-chain triglycerides are heated to 40-50°C, and Span-80 is poured into the medium-chain triglycerides and stirred at 80-120 rpm for 5-10 min; then soybean lecithin is slowly added and stirred at 300-500 rpm for 10-20 min until it becomes transparent and clear. Then, triethyl citrate preheated to 30-40°C is added and stirred at 40-100 rpm for 5-20 min to obtain an oil phase mixture. The oil phase mixture is placed in a vacuum environment of -0.05 MPa to -0.1 MPa and degassed at room temperature for 5-10 min. After degassed, the mixture is filtered to remove impurities to obtain the release oil.

9. The method for preparing a dry powder inhalation empty capsule based on interfacial synergy according to claim 5, characterized in that, In step two, the gradient drying includes the following steps: drying the mold in an environment of 15-28°C and 55-65% relative humidity for 15-20 minutes, and then drying the mold in an environment of 35-40°C and 25-35% relative humidity for 30-60 minutes.

Citation Information

Patent Citations

  • Process for preparing triethyl citrate demoulding oil for empty capsules

    CN112606277A

  • Dry powder composition for improvement of effective position medical deposit

    CN1439360A