A moisture permeable microporous medical polyurethane dressing film and a method for preparing the same
By introducing silica matting powder into medical polyurethane dressing films, a non-penetrating surface microporous structure and micro-uneven structure are formed, which solves the problems of insufficient liquid water barrier and moisture permeability, improves the matte feel and waterproof performance, and reduces the risk of isocyanate migration.
Patent Information
- Application Number
- CN202611614767.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-24
AI Technical Summary
Existing medical polyurethane dressing films struggle to balance liquid water barrier properties, moisture permeability, and a matte finish. The lack of matching control between the particle size and distribution of matte powder and the film thickness leads to insufficient or discontinuous surface microstructure.
A continuous polyurethane matrix is combined with silica matting powder to form a non-penetrating surface microporous structure and micro-uneven structure, while the back side maintains a continuous and dense polyurethane surface. By controlling the ratio of silica matting powder particle size to film thickness, the stability and continuity of the microporous structure are ensured.
It achieves a balance between liquid water barrier and water vapor permeability, improves the matte feel, enhances the waterproof performance and adhesion of the film, and reduces the risk of isocyanate migration.
Smart Images

Figure CN123148441A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of medical polymer dressing materials, and relates to a breathable microporous medical polyurethane dressing film and its preparation method. Background Technology
[0002] Medical dressings are used for wound covering, skin protection, and fixation of auxiliary instruments. The materials must be able to block external liquid water, contaminants, and external irritants during use, while allowing water vapor from the skin surface to escape, reducing stuffiness and maintaining good fit and comfort. Traditional gauze dressings have some breathability, but the gaps between their fibers allow liquid water to easily penetrate, making it difficult to provide stable waterproof protection in scenarios requiring bathing, moisture protection, or isolation from external contaminants.
[0003] Polyurethane films, due to their flexibility, transparency, and good adhesion, have been used as substrates for medical dressings. However, conventional polyurethane films have relatively smooth surfaces. If waterproofing is achieved solely through a continuous, dense film layer, issues such as surface reflection, a sticky feel, and insufficient breathability and comfort can easily arise. Existing technologies also include adding matting agents to improve the film's surface appearance. However, if the particle size and distribution of the matting agent are not properly controlled in relation to the film thickness, problems can easily arise, such as particles being completely embedded with insufficient surface microstructure, or particles disrupting the film's continuity and affecting liquid water barrier properties. Therefore, in existing medical polyurethane dressing films, when the particle size and distribution of the matting agent are not properly controlled in relation to the film thickness, complete particle embedding leads to insufficient surface microstructure, while particle disruption of the film's continuity reduces liquid water barrier properties, making it difficult to simultaneously achieve waterproofing, breathability, and a matte finish. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a breathable microporous medical polyurethane dressing film and its preparation method, thereby solving the problem that existing medical polyurethane dressing films cannot simultaneously achieve liquid water barrier, breathability, and a matte finish. This film uses a continuous polyurethane matrix as its main body, incorporating silica matting powder to create a non-penetrating microporous structure and a non-penetrating micro-uneven structure on the exposed surface, while maintaining a continuous and dense polyurethane surface on the back side.
[0005] To achieve this objective, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a moisture-permeable microporous medical polyurethane dressing film, the moisture-permeable microporous medical polyurethane dressing film comprising a continuous polyurethane matrix and silica matting powder dispersed in the continuous polyurethane matrix;
[0007] The continuous polyurethane matrix is formed from a reactant comprising polytetramethylene ether glycol and isocyanate components;
[0008] The breathable microporous medical polyurethane dressing film has an exposed surface and a back surface. The exposed surface has a non-penetrating surface microporous structure and a non-penetrating micro-protrusion structure formed by the silica matting powder. The back surface is a continuous and dense polyurethane surface.
[0009] Preferably, the number-average molecular weight of the polytetramethylene ether glycol is 1000-3000.
[0010] Preferably, the isocyanate component is hexamethylene diisocyanate or isophorone diisocyanate.
[0011] Preferably, the D50 of the silica matting agent is 5-7 μm.
[0012] Preferably, the ratio of the median particle size D50 of the silica matting powder to the finished film thickness of the moisture-permeable microporous medical polyurethane dressing film is 0.20-0.90.
[0013] Preferably, the finished film thickness of the moisture-permeable microporous medical polyurethane dressing film is 8-25 μm.
[0014] Secondly, the present invention provides a method for preparing the moisture-permeable microporous medical polyurethane dressing film described in the first aspect, the method comprising:
[0015] S1, polytetramethylene ether glycol, isocyanate component, prepolymer organic solvent and tin catalyst are prepolymerized, then diol chain extender and chain extender organic solvent are added for chain extension reaction, after the chain extension reaction is completed, end-capping agent is added for end-capping reaction to obtain polyurethane resin solution.
[0016] S2, mix and disperse silica matting powder, medical-grade color paste, polyurethane resin solution and coating organic solvent to obtain coating liquid;
[0017] S3, apply the coating liquid to the surface of the release substrate to form a wet film;
[0018] S4, the wet film is dried and cured in sections to obtain a breathable microporous medical polyurethane dressing film.
[0019] Preferably, in S1, the mass ratio of polytetramethylene ether glycol, isocyanate component, diol chain extender, organic solvent and capping agent is 100:(12-35):(1-10):(80-250):(0.05-2.0), wherein the organic solvent is composed of organic solvent for prepolymerization and organic solvent for chain extension.
[0020] Preferably, in S1, the mass ratio of the organic solvent for prepolymerization to the organic solvent for chain extension is (30-70):(30-70); the temperature of the prepolymerization reaction is 75-85℃ and the time is 2-4h; the temperature of the chain extension reaction is 60-75℃ and the time is 1-3h; the temperature of the end-capping reaction is 50-70℃ and the time is 0.5-2h.
[0021] Preferably, in S1, the tin-free catalyst is an organobismuth catalyst or an organozinc catalyst, and the mass of the tin-free catalyst is 0.01%-0.05% of the total mass of polytetramethylene ether glycol, isocyanate component and diol chain extender.
[0022] Preferably, in S1, the diol chain extender is one of ethylene glycol, 1,4-butanediol, and 1,6-hexanediol; and the end-capping agent is one of ethanol, isopropanol, and n-butanol.
[0023] Preferably, in S1, the organic solvent for prepolymerization and the organic solvent for chain extension are each independently one or more of butanone, ethyl acetate, and butyl acetate.
[0024] Preferably, in S2, the mass ratio of the polyurethane resin solution, silica matting powder, and medical-grade pigment is 100:(1-5):(0.05-2.0), the organic solvent for coating is one or more of butanone, ethyl acetate, and butyl acetate, and the solid content of the coating liquid is 25%-40%.
[0025] Preferably, in S4, the segmented drying film formation includes a first drying, a second drying, and a third drying performed sequentially; the temperature of the first drying is 50-65℃, and the time is 1-5 min; the temperature of the second drying is 80-100℃, and the time is 1-6 min; the temperature of the third drying is 110-130℃, and the time is 1-8 min; the temperature of the curing is 50-60℃, and the time is 24-48 h.
[0026] The terminal hydroxyl groups of polytetramethylene ether glycol undergo an addition reaction with the isocyanate groups in the isocyanate component to form urethane bonds, creating a polyurethane chain with polyether segments as soft segments and urethane segments as hard segments. The metal center in the tin catalyst can coordinate with hydroxyl or isocyanate groups, facilitating nucleophilic attack of hydroxyl oxygen on isocyanate carbon, thereby promoting prepolymerization and chain extension reactions. The diol chain extender continues to react with the isocyanate groups in the prepolymer, causing the polyurethane chain to grow and form a film-forming resin solution. After the chain extension reaction, the hydroxyl groups in the end-capping agent react with the residual isocyanate groups, converting them into urethane structures and reducing the risk of migration of residual isocyanate groups in the finished film.
[0027] The polytetramethylene ether glycol segments contain ether oxygen atoms, which can form dipole interactions and hydrogen bonds with water molecules, enabling water vapor molecules to adsorb, dissolve, and diffuse within the continuous polyurethane phase. The isocyanate component and the diol chain extender form a urethane structure containing carbonyl and amino groups. The carbonyl groups can form interchain hydrogen bonds with the amino groups. The hydrogen bonding between urethane segments restricts excessive flow of polyurethane segments, ensuring the film maintains a continuous polyurethane matrix after film formation. The polyether segments provide water vapor diffusion channels, while the urethane segments provide interchain bonding points. Together, they allow water vapor to pass through the polyurethane phase, while liquid water cannot easily pass directly through the continuous polyurethane surface.
[0028] The surface of the silica matting powder contains silanol groups, which can form hydrogen bonds with the urethane carbonyl and amino groups in the polyurethane segments and the ether oxygen groups in the polyether segments. This allows the silica particles to be wetted by the polyurethane matrix and embedded in the film-forming system. When the particle size of the silica matting powder is within the matching range of the finished film thickness, the particles can form local protrusions and non-penetrating depressions around the particles on the exposed surface. The exposed part of the particles changes the geometry of the exposed surface of the film, while the embedded part of the particles remains bonded to the continuous polyurethane matrix and does not form channels that penetrate the film layer. During the drying process, the polyurethane segments around the silica particles shrink, creating a non-penetrating surface microporous structure at the interface between the particles and the polyurethane matrix. This microporous structure terminates in the surface area and does not extend to the back side.
[0029] After the coating liquid is applied to the release substrate, the side closest to the release substrate is constrained by the substrate surface, causing the coating liquid to level and form a continuous polyurethane surface in contact with the substrate. The side furthest from the release substrate is exposed to air, and the organic solvent evaporates from this side. The solvent content in the exposed surface area first decreases, while the polyurethane resin concentration increases, and the silica matting powder is gradually fixed at the exposed surface. During the segmented drying and film formation process, the low-temperature drying stage maintains the flow of the coating liquid, allowing the silica matting powder to form a particle-involved surface morphology on the exposed surface. Subsequently, as the temperature increases, the viscosity of the polyurethane resin solution increases and film formation is completed, fixing the embedded state of the particles on the exposed surface. Subsequent drying and curing continue to remove organic solvents and promote residual reactions, maintaining a continuous and dense polyurethane surface on the back side, while the exposed surface retains a non-penetrating surface microporous structure and a non-penetrating micro-uneven structure.
[0030] Compared with existing technologies, the beneficial effects of this invention are as follows: The breathable microporous medical polyurethane dressing film of this invention uses a continuous polyurethane matrix as the main body, maintaining a continuous and dense polyurethane surface on the back of the film, which is beneficial for blocking external liquid water and contaminants from contacting the wound area. Silica matte powder is dispersed in the continuous polyurethane matrix and participates in the formation of non-penetrating microporous structures and non-penetrating micro-protrusion structures on the exposed surface, preventing the formation of through-holes on the exposed surface of the film. This maintains liquid water barrier while improving water vapor expulsion and a matte surface feel. The polyether segments formed by polytetramethylene ether glycol impart flexibility and conformability to the film, while the polyurethane segments formed by the isocyanate component and the diol chain extender improve the continuity of film formation. The use of a tin-free catalyst and end-capping agent during the preparation process helps promote the isocyanate group reaction and reduces the risk of residual isocyanate migration; the segmented drying and curing process helps stabilize the microstructure of the exposed surface and remove residual organic solvents, making the resulting film suitable for medical dressing substrates. Attached Figure Description
[0031] Figure 1 The flowchart illustrates the preparation method provided by this invention. Detailed Implementation
[0032] The technical solutions of the present invention will be described in detail below with reference to specific embodiments and accompanying drawings. The embodiments described herein are specific implementations of the present invention, used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary, and should not be construed as limiting the implementation methods or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can employ other obvious technical solutions based on the content disclosed in the claims and specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.
[0033] The chemical reagents used in the embodiments and comparative examples of this invention are all commercially available products and have not undergone any further purification treatment.
[0034] Example 1
[0035] This embodiment provides a breathable microporous medical polyurethane dressing film and its preparation method. The preparation method is as follows: Figure 1 As shown, the preparation method specifically includes the following steps:
[0036] S1, polytetramethylene ether glycol (number average molecular weight 1000), hexamethylene diisocyanate, a prepolymerization organic solvent, and an organobismuth catalyst are subjected to a prepolymerization reaction. The prepolymerization organic solvent is butanone (MEK), and the mass of the organobismuth catalyst is 0.01% of the total mass of polytetramethylene ether glycol, hexamethylene diisocyanate, and diol chain extender. Ethyl glycol and an organic solvent for chain extension are then added to carry out a chain extension reaction. The chain extension organic solvent is ethyl acetate. After the chain extension reaction is completed, ethanol is added to carry out a capping reaction to obtain polytetramethylene ether glycol (MEG). The solution contains an urethane resin; wherein the mass ratio of polytetramethylene ether glycol, hexamethylene diisocyanate, ethylene glycol, organic solvent, and ethanol is 100:12:1:80:0.05; the organic solvent consists of a prepolymer organic solvent and a chain extender organic solvent, with a mass ratio of 30:70; the prepolymerization reaction temperature is 75℃ for 2 hours; the chain extension reaction temperature is 60℃ for 1 hour; and the end-capping reaction temperature is 50℃ for 0.5 hours.
[0037] S2, a coating solution is prepared by mixing and dispersing silica matting powder with a D50 of 5 μm, medical-grade pigment, polyurethane resin solution, and coating organic solvent; wherein, the coating organic solvent is methyl ethyl ketone (MEK), the mass ratio of polyurethane resin solution, silica matting powder, and medical-grade pigment is 100:1:0.05, and the solid content of the coating solution is 25%.
[0038] S3, apply the coating liquid to the surface of the release substrate to form a wet film;
[0039] S4, the wet film is dried and cured in stages to obtain a moisture-permeable microporous medical polyurethane dressing film with a thickness of 25 μm; wherein, the staged drying and film formation includes a first drying, a second drying and a third drying in sequence, the first drying temperature is 50℃ and the time is 1 min, the second drying temperature is 80℃ and the time is 1 min, the third drying temperature is 110℃ and the time is 1 min, and the curing temperature is 50℃ and the time is 24 h; the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished moisture-permeable microporous medical polyurethane dressing film is 0.20.
[0040] Example 2
[0041] This embodiment provides a breathable microporous medical polyurethane dressing film and its preparation method, the preparation method specifically including the following steps:
[0042] S1, a prepolymerization reaction was carried out on polytetramethylene ether glycol (number average molecular weight 1600), isophorone diisocyanate, a prepolymerization organic solvent, and an organozinc catalyst. The prepolymerization organic solvent was butyl acetate, and the mass of the organozinc catalyst was 0.02% of the total mass of polytetramethylene ether glycol, isophorone diisocyanate, and diol chain extender. Then, 1,4-butanediol and a chain extender organic solvent (butanone) were added to carry out a chain extension reaction. After the chain extension reaction was completed, isopropanol was added to carry out a capping reaction to obtain a polyurethane resin. The mixture is a lipid solution in which the mass ratio of polytetramethylene ether glycol, isophorone diisocyanate, 1,4-butanediol, organic solvent, and isopropanol is 100:20:4:135:0.70. The organic solvent consists of a prepolymer organic solvent and a chain extender organic solvent, with a mass ratio of 45:55. The prepolymerization reaction is carried out at 78°C for 2.6 h, the chain extension reaction at 65°C for 1.6 h, and the end-capping reaction at 56°C for 1.0 h.
[0043] S2, a coating solution is prepared by mixing and dispersing silica matting agent with a D50 of 5.6 μm, medical-grade pigment, polyurethane resin solution, and coating organic solvent; wherein, the coating organic solvent is ethyl acetate, the mass ratio of polyurethane resin solution, silica matting agent, and medical-grade pigment is 100:2.3:0.70, and the solid content of the coating solution is 30%.
[0044] S3, apply the coating liquid to the surface of the release substrate to form a wet film;
[0045] S4, the wet film is dried and cured in stages to obtain a moisture-permeable microporous medical polyurethane dressing film with a thickness of 18 μm; wherein, the staged drying and film formation includes a first drying, a second drying and a third drying in sequence, the first drying temperature is 55℃ and the time is 2.3 min, the second drying temperature is 87℃ and the time is 2.5 min, the third drying temperature is 116℃ and the time is 3.2 min, and the curing temperature is 53℃ and the time is 32 h; the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished moisture-permeable microporous medical polyurethane dressing film is 0.31.
[0046] Example 3
[0047] This embodiment provides a breathable microporous medical polyurethane dressing film and its preparation method, the preparation method specifically including the following steps:
[0048] S1, polytetramethylene ether glycol (number average molecular weight 2300), hexamethylene diisocyanate, a prepolymerization organic solvent, and an organobismuth catalyst were subjected to a prepolymerization reaction. The prepolymerization organic solvent was ethyl acetate, and the mass of the organobismuth catalyst was 0.035% of the total mass of polytetramethylene ether glycol, hexamethylene diisocyanate, and diol chain extender. Then, 1,6-hexanediol and a chain extender organic solvent (butyl acetate) were added to carry out a chain extension reaction. After the chain extension reaction, n-butanol was added for end-capping to obtain polyurethane. An ester resin solution was prepared, wherein the mass ratio of polytetramethylene ether glycol, hexamethylene diisocyanate, 1,6-hexanediol, organic solvent, and n-butanol was 100:28:7:190:1.30. The organic solvent consisted of a prepolymer organic solvent and a chain extender organic solvent, with a mass ratio of 55:45. The prepolymerization reaction was carried out at 82°C for 3.3 h; the chain extension reaction was carried out at 70°C for 2.4 h; and the end-capping reaction was carried out at 64°C for 1.5 h.
[0049] S2, a coating solution is prepared by mixing and dispersing silica matting agent with a D50 of 6.3 μm, medical-grade pigment, polyurethane resin solution, and coating organic solvent; wherein, the coating organic solvent is butyl acetate, the mass ratio of polyurethane resin solution, silica matting agent, and medical-grade pigment is 100:3.7:1.30, and the solid content of the coating solution is 35%.
[0050] S3, apply the coating liquid to the surface of the release substrate to form a wet film;
[0051] S4, the wet film is dried and cured in stages to obtain a moisture-permeable microporous medical polyurethane dressing film with a thickness of 12 μm; wherein, the staged drying and film formation includes a first drying, a second drying and a third drying in sequence, the temperature of the first drying is 60℃ and the time is 3.7 min, the temperature of the second drying is 94℃ and the time is 4.5 min, the temperature of the third drying is 124℃ and the time is 5.5 min, and the curing temperature is 56℃ and the time is 40 h; the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished moisture-permeable microporous medical polyurethane dressing film is 0.53.
[0052] Example 4
[0053] This embodiment provides a breathable microporous medical polyurethane dressing film and its preparation method, the preparation method specifically including the following steps:
[0054] S1, a prepolymerization reaction is carried out on polytetramethylene ether glycol (3000 number average molecular weight), isophorone diisocyanate, a prepolymerization organic solvent, and an organozinc catalyst. The prepolymerization organic solvent is methyl ethyl ketone (MEK) and butyl acetate, with a mass ratio of MEK to butyl acetate of 1:1. The mass of the organozinc catalyst is 0.05% of the total mass of polytetramethylene ether glycol, isophorone diisocyanate, and diol chain extender. Then, 1,4-butanediol and an organic solvent for chain extension are added to carry out a chain extension reaction. The organic solvent for chain extension is ethyl acetate. After the chain extension reaction is completed, isopropyl... An alcohol was used for end-capping to obtain a polyurethane resin solution; wherein the mass ratio of polytetramethylene ether glycol, isophorone diisocyanate, 1,4-butanediol, organic solvent, and isopropanol was 100:35:10:250:2.0, and the organic solvent consisted of a prepolymer organic solvent and a chain extender organic solvent, with a mass ratio of prepolymer organic solvent to chain extender organic solvent of 70:30; the prepolymerization reaction was carried out at 85℃ for 4 hours; the chain extension reaction was carried out at 75℃ for 3 hours; and the end-capping reaction was carried out at 70℃ for 2 hours.
[0055] S2, a coating solution is prepared by mixing and dispersing silica matting powder with a D50 of 7 μm, medical-grade pigment, polyurethane resin solution, and coating organic solvent; wherein the coating organic solvent is methyl ethyl ketone (MEK) and ethyl acetate, with a mass ratio of MEK to ethyl acetate of 1:1; the mass ratio of polyurethane resin solution, silica matting powder, and medical-grade pigment is 100:5:2.0; and the solid content of the coating solution is 40%.
[0056] S3, apply the coating liquid to the surface of the release substrate to form a wet film;
[0057] S4, the wet film is dried and cured in stages to obtain a breathable microporous medical polyurethane dressing film with a thickness of 8 μm; wherein, the staged drying and film formation includes a first drying, a second drying and a third drying in sequence, the first drying temperature is 65℃ and the time is 5 min, the second drying temperature is 100℃ and the time is 6 min, the third drying temperature is 130℃ and the time is 8 min, and the curing temperature is 60℃ and the time is 48 h; the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished breathable microporous medical polyurethane dressing film is 0.875.
[0058] Comparative Example 1
[0059] This comparative example provides a breathable microporous medical polyurethane dressing film and its preparation method. The difference from Example 1 is that silica matting powder is not added in S2. Instead, the color paste and polyurethane resin solution are mixed and dispersed to obtain the coating liquid. Other process parameters and operating conditions are exactly the same as in Example 1.
[0060] Comparative Example 2
[0061] This comparative example provides a breathable microporous medical polyurethane dressing film and its preparation method. The difference from Example 1 is that silica matting powder with a D50 of 3 μm is used in S2, and the thickness of the finished breathable microporous medical polyurethane dressing film is 25 μm, so that the ratio of the median particle size D50 of silica matting powder to the thickness of the finished film is less than 0.20. Other process parameters and operating conditions are exactly the same as in Example 1.
[0062] Comparative Example 3
[0063] This comparative example provides a breathable microporous medical polyurethane dressing film and its preparation method. The difference from Example 1 is that silica matting powder with a D50 of 25 μm is used in S2, and the thickness of the finished breathable microporous medical polyurethane dressing film is 25 μm, so that the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished film is higher than 0.90. Other process parameters and operating conditions are exactly the same as in Example 1.
[0064] Comparative Example 4
[0065] This comparative example provides a breathable microporous medical polyurethane dressing film and its preparation method. The difference from Example 1 is that no end-capping agent is added after the chain extension reaction in S1 to carry out the end-capping reaction, and a polyurethane resin solution is obtained directly. Other process parameters and operating conditions are exactly the same as those in Example 1.
[0066] Performance testing:
[0067] The MVTR (water vapor transmission rate) test method refers to YY / T 0471.2-2004;
[0068] Hydrostatic pressure resistance test: The obtained breathable microporous medical polyurethane dressing film was cut into circular samples with a diameter of not less than 80 mm. Before testing, the samples were placed in an environment with a temperature of 23℃ and a relative humidity of 50% for 24 hours. The hydrostatic pressure was tested using a hydrostatic pressure tester at a water temperature of 23℃ and a test area of 20 cm². 2 The exposed surface of the film faces the side where the water pressure is applied, and the back side faces the observation side. The clamping edges are sealed with rubber sealing rings. During the test, the pressure is continuously increased at a rate of 1.0 kPa / s, and the appearance of water droplets or seepage points on the back of the sample is observed. When a third water droplet appears on the back of the sample, the corresponding pressure is recorded as the hydrostatic pressure resistance value.
[0069] Surface gloss test: The obtained breathable microporous medical polyurethane dressing film was cut into 80mm×80mm samples and placed in an environment of 23℃ and 50% relative humidity for 24 hours before testing. The gloss of the exposed surface of the film was tested using a gloss meter at a test angle of 60°. During the test, the sample was placed flat on a black non-reflective substrate with the exposed surface facing upwards, avoiding air bubbles, creases, scratches, and edge areas.
[0070] Test for residual free isocyanate: The obtained breathable microporous medical polyurethane dressing film was cut into small pieces, and 1.000 g of the sample was placed in a sealed glass sample bottle. 20 mL of acetonitrile was added, and the mixture was ultrasonically extracted for 30 min, then allowed to stand for 10 min. The supernatant was used as the extract. 1-(2-pyridyl)piperazine acetonitrile solution was added to the extract for derivatization at 25 °C for 30 min. After the reaction, the sample solution was filtered through a 0.22 μm organic filter membrane and detected by high-performance liquid chromatography (HPLC). The chromatographic column was a C18 reversed-phase column, the mobile phase was acetonitrile and water, the detection wavelength was 254 nm, the column temperature was 30 °C, and the injection volume was 10 μL. A standard curve was established using the corresponding isocyanate monomer standard after the same derivatization treatment, and the residual free isocyanate in the film was calculated based on the peak area of the sample.
[0071] The test results are shown in Table 1.
[0072] Table 1. Test results of moisture-permeable microporous medical polyurethane dressing films of Examples 1-4 and Comparative Examples 1-4
[0073]
[0074] As shown in Table 1, compared with Example 1, Comparative Example 1 showed a decrease in MVTR, an increase in hydrostatic pressure resistance, an increase in surface gloss, and an increase in the amount of free isocyanate residue; Comparative Example 2 showed a decrease in MVTR, an increase in hydrostatic pressure resistance, an increase in surface gloss, and an increase in the amount of free isocyanate residue; Comparative Example 3 showed an increase in MVTR, a decrease in hydrostatic pressure resistance, a decrease in surface gloss, and an increase in the amount of free isocyanate residue; and Comparative Example 4 showed a decrease in MVTR and hydrostatic pressure resistance, and an increase in surface gloss and the amount of free isocyanate residue.
[0075] This is because, in Comparative Example 1, no silica matting powder was added, and the exposed surface lacked the non-penetrating microporous structure and non-penetrating micro-uneven structure formed by the silica matting powder. This reduced the water vapor exchange interface and increased surface reflectivity. At the same time, the continuous polyurethane matrix was not affected by the silica matting powder, thus increasing the liquid water barrier capacity. In Comparative Example 2, the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished film was lower than the range specified in this invention. The silica matting powder was more easily embedded in the continuous polyurethane matrix, resulting in insufficient formation of microstructures on the exposed surface, which reduced MVTR and increased surface gloss.
[0076] In Comparative Example 3, the ratio of the median particle size D50 of the silica matting powder to the thickness of the finished film is higher than the range specified in this invention. The silica matting powder particles are relatively large relative to the thickness of the finished film, resulting in an increase in the micro-uneven structure of the exposed surface, which increases MVTR and decreases surface gloss. However, the local integrity of the continuous polyurethane matrix decreases, which reduces hydrostatic pressure resistance. In Comparative Example 4, no end-capping reaction was performed, and the residual isocyanate groups after the chain extension reaction were not consumed by the end-capping agent, thus increasing the amount of free isocyanate residue. The uncapped residual isocyanate groups continue to react with trace amounts of moisture or active hydrogen in the polyurethane segments during the curing and pre-testing process, causing changes in the surface structure and segment activity of the polyurethane. Therefore, MVTR and hydrostatic pressure resistance decrease, while surface gloss increases.
[0077] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A breathable microporous medical polyurethane dressing film, characterized in that, The breathable microporous medical polyurethane dressing film comprises a continuous polyurethane matrix and silica matting powder dispersed in the continuous polyurethane matrix; The continuous polyurethane matrix is formed from a reactant comprising polytetramethylene ether glycol and isocyanate components; The breathable microporous medical polyurethane dressing film has an exposed surface and a back surface. The exposed surface has a non-penetrating surface microporous structure and a non-penetrating micro-protrusion structure formed by the silica matting powder. The back surface is a continuous and dense polyurethane surface.
2. The breathable microporous medical polyurethane dressing film according to claim 1, characterized in that, The number-average molecular weight of the polytetramethylene ether diol is 1000-3000.
3. The breathable microporous medical polyurethane dressing film according to claim 1, characterized in that, The isocyanate component is hexamethylene diisocyanate or isophorone diisocyanate.
4. The breathable microporous medical polyurethane dressing film according to claim 1, characterized in that, The D50 of the silica matting agent is 5-7 μm.
5. The breathable microporous medical polyurethane dressing film according to claim 1, characterized in that, The ratio of the median particle size D50 of the silica matting powder to the finished film thickness of the moisture-permeable microporous medical polyurethane dressing film is 0.20-0.
90.
6. The breathable microporous medical polyurethane dressing film according to claim 1, characterized in that, The finished film thickness of the breathable microporous medical polyurethane dressing film is 8-25 μm.
7. A method for preparing a breathable microporous medical polyurethane dressing film as described in any one of claims 1-6, characterized in that, The preparation method includes: S1, polytetramethylene ether glycol, isocyanate component, prepolymer organic solvent and tin catalyst are prepolymerized, then diol chain extender and chain extender organic solvent are added for chain extension reaction, after the chain extension reaction is completed, end-capping agent is added for end-capping reaction to obtain polyurethane resin solution. S2, mix and disperse silica matting powder, medical-grade color paste, polyurethane resin solution and coating organic solvent to obtain coating liquid; S3, apply the coating liquid to the surface of the release substrate to form a wet film; S4, the wet film is dried and cured in sections to obtain a breathable microporous medical polyurethane dressing film.
8. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S1, the mass ratio of polytetramethylene ether glycol, isocyanate component, diol chain extender, organic solvent and end-capping agent is 100:(12-35):(1-10):(80-250):(0.05-2.0), and the organic solvent is composed of organic solvent for prepolymerization and organic solvent for chain extension.
9. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S1, the mass ratio of the organic solvent for prepolymerization to the organic solvent for chain extension is (30-70):(30-70); the temperature of the prepolymerization reaction is 75-85℃ and the time is 2-4h; the temperature of the chain extension reaction is 60-75℃ and the time is 1-3h; the temperature of the end-capping reaction is 50-70℃ and the time is 0.5-2h.
10. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S1, the tin-free catalyst is an organobismuth catalyst or an organozinc catalyst, and the mass of the tin-free catalyst is 0.01%-0.05% of the total mass of polytetramethylene ether glycol, isocyanate component and diol chain extender.
11. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S1, the diol chain extender is one of ethylene glycol, 1,4-butanediol, and 1,6-hexanediol; the end-capping agent is one of ethanol, isopropanol, and n-butanol.
12. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S1, the organic solvent for prepolymerization and the organic solvent for chain extension are each independently one or more of butanone, ethyl acetate, and butyl acetate.
13. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S2, the mass ratio of the polyurethane resin solution, silica matting powder, and medical-grade pigment is 100:(1-5):(0.05-2.0), the organic solvent for coating is one or more of butanone, ethyl acetate, and butyl acetate, and the solid content of the coating liquid is 25%-40%.
14. The method for preparing a breathable microporous medical polyurethane dressing film according to claim 7, characterized in that, In S4, the segmented drying film formation includes a first drying, a second drying, and a third drying performed sequentially; the temperature of the first drying is 50-65℃, and the time is 1-5 min; the temperature of the second drying is 80-100℃, and the time is 1-6 min; the temperature of the third drying is 110-130℃, and the time is 1-8 min; the temperature of the curing is 50-60℃, and the time is 24-48 h.