Preparation method of high-moisture-absorption antibacterial nanofiber electronic skin and application of high-moisture-absorption antibacterial nanofiber electronic skin in wound repair
By using a blended electrospinning and patterned deposition of silver nanowires, a highly hygroscopic and antibacterial nanofiber electronic skin was prepared. This method addresses the shortcomings of existing wound dressings in terms of exudate management, antibacterial protection, and sensing functions, enabling efficient wound care and monitoring, and improving the biocompatibility and stability of the material.
Patent Information
- Application Number
- CN202611287751.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-24
AI Technical Summary
Existing wound dressings are inadequate in terms of exudate management, antibacterial protection, and sensing functions, failing to meet the clinical needs of high-exudate wounds. Furthermore, the biocompatibility and stability issues of the materials have not been effectively resolved.
Silk fibroin-based nanofiber membranes were prepared using a blended electrospinning technique. A conductive network was formed by patterned deposition of silver nanowires, and then cured using the natural biocrosslinking agent genipin. This process created a highly hygroscopic and antibacterial nanofiber electronic skin, achieving integrated functions of permeation management, antibacterial protection, and in-situ monitoring.
It enables exudate management, antimicrobial protection, and in-situ monitoring of high-exudative wounds, reduces the risk of wound maceration and infection, provides objective data for wound healing assessment, and significantly improves the biocompatibility and stability of the material, making it suitable for long-term care of high-exudative and difficult-to-heal wounds.
Smart Images

Figure CN123148444A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of flexible biomedical materials and wound care technology, specifically to a method for preparing highly absorbent and antibacterial nanofiber electronic skin and its application in wound repair. Background Technology
[0002] Chronic, difficult-to-heal wounds such as diabetic foot ulcers, pressure injuries, and burns have become prevalent clinical health problems. Scientific management of wound exudate is a core element in promoting wound healing and preventing infection. With the integrated development of biomedical materials and flexible electronics, wound care has evolved from traditional passive covering and protection to functional and intelligent approaches. Multifunctional dressings that combine efficient exudate management, broad-spectrum antibacterial protection, and in-situ healing monitoring represent an important research direction in the field of wound repair.
[0003] Current clinically used wound dressings still have many limitations: traditional gauze dressings have low absorbency and are prone to exudate penetration, requiring frequent changes; while foam and hydrocolloid dressings have improved absorbency, they pose risks of exudate retention and wound maceration, and can easily adhere to newly formed tissue during changes, causing secondary damage. Furthermore, most conventional dressings only provide physical protection and basic exudate absorption, failing to provide real-time feedback on wound healing status. Clinical assessment relies on visual observation by healthcare professionals, which is both delayed and subjective. Existing intelligent wound dressing solutions generally suffer from complex manufacturing processes, poor biocompatibility of substrate materials, limited sensing capabilities, and difficulties in simultaneously achieving exudate management and sensing stability, thus restricting their widespread clinical application.
[0004] The prior art has disclosed a flexible conductive fiber membrane material based on silk fibroin nanofibers loaded with silver nanowires, which has certain flexibility, conductivity and moisture absorption properties. It is mainly used as a wearable electrode in scenarios such as electrocardiogram monitoring and motion signal acquisition on the body surface. However, these technical solutions are all designed around wearable health monitoring scenarios and have not been adapted and optimized for the specific needs of wound repair: First, the fiber network structure and pore design of the materials do not take into account the protein components and high viscosity characteristics of wound exudate, and lack targeted verification of exudate drainage efficiency and fluid storage stability in actual wound environments; Second, the silver nanowires are loaded by direct surface deposition without slow-release regulation and biocompatibility optimization, and long-term contact with wound tissue poses risks of silver ion burst release and insufficient cell compatibility, and the adhesion stability with wound tissue in a wet state is insufficient; Third, the sensing function of the materials is only for collecting electrophysiological signals from the body surface, and no sensing response mechanism related to wound exudate volume and metabolic markers has been established, which cannot realize in-situ dynamic monitoring of wound healing process and cannot directly meet the clinical needs of wound repair.
[0005] Therefore, in order to address the shortcomings of existing technologies, developing a nanofiber electronic skin with ultra-high moisture absorption and fluid conduction, controllable antibacterial properties, in-situ monitoring functions, and excellent biocompatibility, as well as its preparation method, is of great practical significance for improving the nursing effect of high-exudation wounds and promoting the intelligent development of wound repair materials. Summary of the Invention
[0006] To address the shortcomings of existing silk fibroin-based conductive nanofiber materials, such as inability to adapt to wound repair scenarios, insufficient wet stability, uncontrollable silver ion release, and mismatch between sensing functions and wound requirements, this invention provides a method for preparing highly absorbent and antibacterial nanofiber electronic skin and its application in wound repair. Through improvements using three technologies—substrate blending modification, patterned conductive loading, and bio-crosslinking curing—it achieves integrated functions of exudate management, antibacterial protection, and in-situ monitoring, thus meeting the clinical nursing needs of highly exudative wounds.
[0007] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing highly hygroscopic and antibacterial nanofiber electronic skin, comprising the following steps:
[0008] S1. Mix the regenerated silk fibroin solution with the hydrophilic polysaccharide solution, add spinning aids, and prepare a blended spinning solution;
[0009] S2. The blended spinning solution is spun using an electrospinning process to prepare a silk fibroin-based nanofiber membrane.
[0010] S3. Silver nanowires are loaded in a predetermined area of the silk fibroin-based nanofiber film using a patterned deposition process to form a patterned conductive functional layer.
[0011] S4. The composite fiber membrane loaded with silver nanowires is cross-linked and cured using a natural biological cross-linking agent, and then dried to obtain the highly hygroscopic and antibacterial nanofiber electronic skin.
[0012] Further, in step S1, the hydrophilic polysaccharide is chitosan, and the mass fraction of the chitosan acetate solution is 1%~3%; the mass fraction of the regenerated silk fibroin solution is 7%~8%, which is mixed with the chitosan acetate solution at a volume ratio of (3~5):1; the spinning aid is polyethylene oxide, and the amount added accounts for 0.5%~1% of the total mass of the spinning solution. The chitosan is pre-dissolved in a 1~2% dilute acetic acid aqueous solution to prepare a chitosan acetate solution, and the pH of the mixture is adjusted to 6.5~7.0 with dilute NaOH before mixing to avoid the precipitation of silk fibroin near its isoelectric point.
[0013] As an alternative, the hydrophilic polysaccharide can also be any one of hyaluronic acid, sodium alginate, or carboxymethyl cellulose, all of which can achieve the technical effect of improving the hydrophilicity of the substrate and the cross-linking reaction sites.
[0014] Further, in step S2, the electrospinning process parameters are as follows: using No. 18 stainless steel needles, applying a voltage of 10~12kV, receiving distance of 12~18cm, advancing speed of 0.002~0.005mm / s, ambient temperature of 20~30℃, and relative humidity of 35%~45%; after spinning, the composite membrane is immersed in a 90% methanol solution for 10~30min to remove polyethylene oxide, rinsed with deionized water, and dried at room temperature.
[0015] Furthermore, in step S3, the patterned deposition process is preferably an electrophoretic deposition method, which, together with a hollow mask with a preset electrode pattern, achieves regional selective loading of silver nanowires; the surface deposition amount of silver nanowires in the base film loading area is 0.015~0.025 mg / cm².
[0016] As an alternative, the patterned deposition process can also be any one of mask vacuum filtration, inkjet printing deposition, or spray masking, all of which can achieve patterned selective loading of silver nanowires.
[0017] Further, in step S4, the natural biological crosslinking agent is genipin; the crosslinking curing specifically involves immersing the composite fiber membrane loaded with silver nanowires in a 0.5%~1% genipin aqueous solution, immersing it at a constant temperature of 35℃~40℃ for 12h~24h for crosslinking, removing it, rinsing it with deionized water to remove unreacted genipin, and drying it at room temperature.
[0018] A highly absorbent and antibacterial nanofiber electronic skin is prepared by the aforementioned method. The electronic skin has a double-layer fiber network structure, with a lower layer being a cross-linked modified silk fibroin-based nanofiber absorbent substrate and an upper layer being a patterned silver nanowire conductive network layer. The electronic skin has a 24-hour water absorption rate ≥680% as tested by the immersion and weighing method according to GB / T1034-2008, and an antibacterial rate of ≥60% against Staphylococcus aureus and ≥50% against Escherichia coli as tested by the oscillation method according to GB / T20944.3-2007.
[0019] Furthermore, the total thickness of the electronic skin is 40~50μm, and the wet tensile strength is ≥2.5MPa; the average diameter of the silver nanowires is 50~60nm, and the average diameter of the silk fibroin-based nanofibers is 500~600nm.
[0020] Application of a highly absorbent and antibacterial nanofiber electronic skin in the preparation of wound repair monitoring dressings.
[0021] As a preferred embodiment of the present invention, the wound repair monitoring dressing collects the conductivity signal of wound exudate through a patterned silver nanowire conductive network, and the conductivity signal is used to reflect the change in the amount of wound exudate.
[0022] As a preferred embodiment of the present invention, the wound repair monitoring dressing utilizes the surface-enhanced Raman scattering effect of silver nanowires to enrich and detect characteristic metabolic markers of uric acid and urea in wound exudate.
[0023] As a preferred embodiment of the present invention, the wound repair monitoring dressing absorbs and stores wound exudate through a cross-linked modified silk fibroin nanofiber substrate; silver nanowires are coated by the cross-linked fiber network to achieve the gradual release of silver ions to inhibit the proliferation of pathogens in the wound, so that the dressing has the functions of exudate management, antibacterial protection and signal acquisition.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. This invention applies nanofiber electronic skin to the preparation of wound repair monitoring dressings, simultaneously addressing the three core needs of exudate management, antibacterial protection, and in-situ monitoring for high-exudate wounds. Compared to traditional wound dressings, it can rapidly absorb and store large amounts of exudate through a three-dimensional nanofiber network, achieving long-lasting antibacterial effects in conjunction with the sustained-release effect of silver ions, reducing the risk of wound maceration and infection. Relying on a patterned conductive network, it can collect exudate conductivity and metabolic marker signals in situ, eliminating the need for frequent visual inspection by lifting the dressing. This reduces the probability of wound exposure and infection, as well as the workload of clinical nursing, providing objective data support for assessing wound healing status. It is particularly suitable for the long-term care of high-exudate, difficult-to-heal wounds such as diabetic foot ulcers, pressure injuries, and second-degree burns.
[0026] 2. The preparation method of this invention is controllable and operates under mild conditions. It employs a one-step electrospinning process to construct a hydrophilic modified nanofiber substrate, followed by patterned electrophoretic deposition to achieve regionally selective loading of silver nanowires. The structure is then solidified through crosslinking with a genipin solution. The entire process requires no complex or precise equipment or stringent reaction conditions. The process parameters are highly adjustable; the hygroscopic capacity, conductivity, and wet mechanical strength of the material can be directionally controlled by adjusting the raw material blending ratio, deposition voltage and time, and crosslinking duration, facilitating large-scale preparation. Furthermore, the selected raw materials and crosslinking agents possess good biocompatibility, posing no risk of toxic reagent residues and meeting the safety requirements for medical biomaterials.
[0027] 3. This invention achieves a balance between high moisture absorption capacity and wet structural stability through molecular-level blending modification and cross-linking network regulation. While retaining the porous capillary water storage capacity of nanofibers, the fiber skeleton is maintained by β-folded crystalline regions, and the covalent cross-linked network restricts excessive swelling of amorphous regions, preventing the fiber structure from collapsing in a wet state. Specifically, the net effect of ≥680% water absorption rate in 24 hours is due to: the incremental contribution of -NH2 and -OH hydrophilic groups introduced by chitosan blending outweighs the capillary pore loss caused by genipin cross-linking densification; the water absorption rate is mainly contributed by the capillary water storage (porosity maintenance) of the three-dimensional nanofiber network, and molecular-level hydrogen bonds provide basic affinity for water binding; genipin cross-linking mainly acts on the free amino groups in amorphous regions, moderately restricting the degree of freedom of swelling in amorphous regions but significantly improving the stability of the wet structure, achieving a balance between high moisture absorption capacity and structural integrity; at the same time, moisture absorption, antibacterial, and sensing functions are integrated into the same fiber substrate, eliminating the need for multi-layer composite stacking, resulting in a thin overall thickness, excellent flexibility, good adhesion to wound tissue, and the characteristics of hydration adhesion fixation and non-adhesive replacement, significantly improving the comfort and clinical suitability of use. Attached Figure Description
[0028] Figure 1 This is a flow chart illustrating the preparation process of the highly hygroscopic and antibacterial nanofiber electronic skin of the present invention.
[0029] Figure 2 This is a schematic diagram of a double-layer fiber network structure. Detailed Implementation
[0030] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] Example 1
[0032] A method for preparing highly hygroscopic and antibacterial nanofiber electronic skin, comprising the following steps:
[0033] S1. Preparation of blended spinning solution: Take 7.5% by mass of regenerated silk fibroin solution and 2% by mass of chitosan acetate solution (prepared by dissolving in 1% dilute acetic acid aqueous solution) and mix them at a volume ratio of 4:1. Adjust the pH of the mixture to 6.5~7.0 with dilute NaOH. Add polyethylene oxide (PEO) as a spinning aid, with the amount of PEO added accounting for 0.8% of the total mass of the spinning solution. Stir at 100 rpm for 10 min at 4℃ to obtain a uniform blended spinning solution.
[0034] S2. Preparation of the base film by electrospinning: The blended spinning solution was injected into a 5mL syringe, fitted with an 18-gauge stainless steel needle, and electrospinning was performed; spinning parameters: voltage 10.6kV, receiving distance 15cm, feed speed 0.003mm / s, ambient temperature 25℃, relative humidity 40%, and silk fibroin-chitosan composite nanofiber base film was collected by an aluminum foil receiving plate; the base film was immersed in a 90% methanol solution for 20min to remove the PEO component, then rinsed with deionized water for 10min and allowed to air dry at room temperature;
[0035] S3. Patterned Electrophoretic Deposition of Silver Nanowires: A polyimide perforated mask (1 mm line width) with a 6-channel sensing electrode pattern was flatly attached to the dried base film surface and fixed to the anode plate of the electrophoretic deposition apparatus. A 0.2 mg / mL aqueous dispersion of silver nanowires was used as the electrolyte. The anode was connected to the substrate supporting the fiber membrane, and the cathode was connected to the counter electrode. A 10 V DC voltage was applied, and electrophoretic deposition was performed for 60 s, allowing the silver nanowires to be selectively loaded onto the base film surface along the perforated areas. The calculated surface deposition amount of silver nanowires in the loaded area was 0.02 mg / cm². After deposition, the sample was removed, the mask was removed, and the sample was air-dried at room temperature.
[0036] In this step, the silk fibroin-chitosan nanofiber membrane is an intrinsically electronic insulating medium. However, after being fully wetted with an aqueous dispersion of silver nanowires before deposition, the three-dimensionally interconnected pores of the fibers are filled with electrolyte, forming continuous ionic conductive pathways. A DC electric field can penetrate the membrane layer through ion migration, providing a stable electric driving force on the membrane surface. The PVP-coated silver nanowires are negatively charged (zeta potential of approximately -30mV) and migrate directionally towards the anode in the electric field. During migration, the silver nanowires first contact the porous network of the fiber membrane surface. Due to their large aspect ratio, they are physically intercepted by the microporous structure. Simultaneously, they form hydrogen bonds with the polar groups on the fiber surface and are adsorbed, ultimately fixing themselves to the fiber surface. They do not penetrate the membrane layer in large quantities and deposit onto the bottom metal electrode. In the early stages of deposition, a small number of silver nanowires are fixed and form local conductive pathways, further enhancing the regional electric field and promoting the continuous growth of the conductive network, ultimately achieving patterned selective deposition on an insulating porous substrate.
[0037] S4. Crosslinking and curing with genipin solution: Prepare a 1% (w / w) genipin aqueous solution, completely immerse the composite fiber membrane loaded with silver nanowires in the solution, and crosslink it at a constant temperature of 37°C for 18 hours; after taking it out, rinse it repeatedly with deionized water 3 times to remove unreacted genipin, and let it air dry at room temperature to obtain the highly hygroscopic and antibacterial nanofiber electronic skin with a total thickness of about 43 μm.
[0038] Example 2
[0039] It is basically the same as Example 1, except that in step S1, the volume ratio of the regenerated silk fibroin solution to the chitosan acetate solution is 3:1.
[0040] Example 3
[0041] It is basically the same as Example 1, except that in step S4, the crosslinking treatment time of the genipin solution is 12h.
[0042] Example 4
[0043] The process is basically the same as in Example 1, except that in step S3, the amount of silver nanowires deposited on the surface of the loaded region is 0.015 mg / cm².
[0044] Electrophoretic deposition process characterization
[0045] During the deposition process, an electrochemical workstation was used to record the current-time (It) curve in real time: the current rises rapidly in the initial stage of deposition, corresponding to the migration of silver nanowires to the anode and the initial nucleation and deposition on the surface of the fiber membrane; subsequently, the current gradually stabilizes, corresponding to the gradual formation of a conductive network on the fiber surface and the stabilization of the deposition rate. The overall curve conforms to the typical law of electrophoretic deposition on porous substrates, proving that the process is stable and controllable.
[0046] The samples before and after deposition were characterized using scanning electron microscopy (SEM):
[0047] Silver nanowires are uniformly wound and loaded on the surface of nanofibers, forming a continuous three-dimensional conductive network along the fiber direction. There is no obvious aggregation, the patterned area has clear edges with an edge deviation of ≤30μm, and there are no silver nanowire residues in the non-deposited areas.
[0048] Silver nanowires are mainly distributed in the 10-15 μm thickness range of the fiber membrane surface layer and do not penetrate to the bottom of the membrane in large quantities, which directly verifies the deposition mechanism of physical interception by the porous network.
[0049] Comparative Example 1
[0050] The process involves using a pure silk fibroin nanofiber substrate, vacuum-filtering and loading silver nanowires onto the entire surface, and cross-linking without genipin. Specific steps include:
[0051] A1. Mix 7.5% (w / w) of regenerated silk fibroin solution with PEO solution at a volume ratio of 3:1, prepare pure silk fibroin nanofiber membrane by electrospinning, remove PEO by methanol treatment and dry at room temperature.
[0052] A2. Silver nanowires were uniformly loaded onto the surface of a fiber membrane using a vacuum filtration method, with a total deposition amount of 0.02 mg / cm², and then dried at room temperature.
[0053] A3. Without genipin crosslinking treatment, we obtained control sample 1.
[0054] Comparative Example 2
[0055] It is basically the same as Example 1, except that the genipin crosslinking treatment in step S4 is not performed.
[0056] Comparative Example 3
[0057] The process is basically the same as in Example 1, except that in step S3, silver nanowires are loaded onto the entire surface using a vacuum filtration method, without patterned electrophoretic deposition.
[0058] Comparative Example 4
[0059] The specific steps for verifying the independent contribution of chitosan blends to hygroscopic properties are as follows:
[0060] B1 Take a 7.5% (w / w) regenerated silk fibroin solution and a 2% (w / w) chitosan acetate solution at a volume ratio of 4:1. Add PEO spinning aid and prepare a silk fibroin-chitosan composite nanofiber substrate film by electrospinning. After removing PEO by methanol treatment, dry at room temperature.
[0061] B2 uses a vacuum filtration method to uniformly load silver nanowires onto the surface of a fiber membrane, with a deposition amount of 0.02 mg / cm², and then dries at room temperature.
[0062] B3 was not subjected to genipin crosslinking treatment, resulting in control sample 4.
[0063] Comparative Example 5
[0064] The specific steps for verifying the synergistic effect of crosslinking and blending are as follows:
[0065] C1: Mix 7.5% pure regenerated silk fibroin solution with PEO solution, prepare pure silk fibroin nanofiber base film by electrospinning, treat with methanol and dry at room temperature;
[0066] C2 was loaded with patterned silver nanowires using electrophoretic deposition, with a deposition amount of 0.02 mg / cm² in the loaded region, and then air-dried at room temperature.
[0067] C3 was immersed in a 1% (w / w) genipin aqueous solution for crosslinking at 37°C for 18 hours, and then rinsed and dried to obtain control sample 5.
[0068] Moisture absorption and liquid conductivity test:
[0069] Referring to GB / T1034-2008 "Determination of Water Absorption of Plastics", the immersion weighing method was used for testing. Each sample was cut into a 3cm × 3cm square, and its dry weight was recorded as m0. The sample was completely immersed in deionized water at 25℃ and kept at this temperature for 24 hours. After immersion, the sample was removed and hung vertically until no water droplets remained, then weighed and recorded as the wet weight m1. The water absorption rate was calculated using the formula:
[0070] Water absorption rate (%) = (m1 - m0) / m0 × 100%
[0071] Each group of samples was tested in parallel 5 times, and the average value was taken.
[0072] Simultaneously, the complete absorption time of 50 μL of simulated wound exudate (0.9% sodium chloride saline, simulating the basic electrolyte environment of wound exudate) on the sample surface was tested, and the time when the droplet was completely wetted and no droplets were visible to the naked eye was recorded.
[0073] Sample number 24-hour water absorption rate (%) Complete absorption time of a 50 μL droplet (s) Example 1 692.3 20 Example 2 685.7 21 Example 3 681.4 21 Example 4 688.9 20 Comparative Example 1 637.2 28 Comparative Example 2 705.6 19 Comparative Example 3 690.5 20 Comparative Example 4 712.3 18 Comparative Example 5 628.5 27
[0074] Results analysis:
[0075] (1) The water absorption rate of Comparative Example 4 reached 712.3%, which was significantly higher than that of Comparative Example 1 (637.2%) of pure silk fibroin, proving that the introduction of hydrophilic groups is the main contributing factor to the improvement of moisture absorption performance;
[0076] (2) The water absorption rate of Comparative Example 2 was 705.6%, and the water absorption rate of Example 1 was 692.3%. The water absorption rate decreased slightly after crosslinking, but the wet tensile strength increased by more than 40%, achieving a balance between moisture absorption capacity and structural stability.
[0077] (3) The water absorption rate of Comparative Example 3 was 690.5%, which was basically the same as that of Example 1, proving that the silver nanowire loading method does not change the moisture absorption and liquid storage capacity of the substrate. The core function of patterning is to realize the zoned sensing function.
[0078] Overall, the 24-hour water absorption rate of all embodiments of the present invention is ≥680%, which is significantly higher than that of the prior art comparative example 1. The chitosan blend introduces a large number of hydrophilic groups such as amino and hydroxyl groups, which, together with the capillary fluid conduction effect of the nanofiber network, achieves ultra-high moisture absorption capacity and rapid fluid conduction rate, which can meet the exudation management needs of highly exudative wounds.
[0079] Antibacterial performance test:
[0080] The tests were conducted according to GB / T20944.3-2007 "Evaluation of Antimicrobial Properties of Textiles - Part 3: Shaking Method". Staphylococcus aureus ATCC6538 and Escherichia coli ATCC8739 were used as test strains. LB liquid medium was used, and the samples and bacterial suspensions were shaken together (150 rpm) for 24 hours. The viable bacterial concentration was then counted on plates, and the inhibition rate was calculated. Each group of samples was tested in triplicate, and the average value was taken.
[0081] Sample number Staphylococcus aureus inhibition rate (%) Escherichia coli inhibition rate (%) Example 1 64.2 57.8 Example 2 62.5 56.3 Example 3 61.3 55.7 Example 4 60.8 55.1 Comparative Example 1 55.6 49.2 Comparative Example 2 58.9 53.4 Comparative Example 3 63.8 57.5 Comparative Example 4 59.2 53.7 Comparative Example 5 60.5 54.9
[0082] The embodiments of the present invention show an inhibition rate of ≥60% against Staphylococcus aureus and ≥50% against Escherichia coli, which is superior to the existing technical solution of Comparative Example 1. The dense fiber network formed by genipin crosslinking coats the silver nanowires, making the release of silver ions more gradual and the long-term antibacterial stability better, while avoiding the potential cytotoxicity caused by the sudden release of silver ions.
[0083] Wet mechanical property testing:
[0084] Each sample was cut into strips measuring 10mm × 40mm, soaked in deionized water for 24 hours until fully swollen, and then removed. The wet tensile strength was tested using a universal testing machine at a tensile rate of 10mm / min and a gauge length of 20mm. Each group of samples was tested in parallel five times, and the average value was taken.
[0085] Sample number Wet tensile strength (MPa) Example 1 2.87 Example 2 2.75 Example 3 2.53 Example 4 2.81 Comparative Example 1 1.62 Comparative Example 2 1.95 Comparative Example 3 2.83 Comparative Example 4 1.88 Comparative Example 5 2.64
[0086] After cross-linking with genipin solution, the wet tensile strength of the composite fiber membrane is increased by more than 40% compared with the uncross-linked sample. It can still maintain the complete fiber network structure in the environment of long-term immersion in wound exudate without fiber disintegration or mechanical collapse, making it suitable for long-term wound care.
[0087] Silver ion sustained-release performance test:
[0088] Each sample was cut into 2cm×2cm pieces and immersed in 10mL of simulated wound exudate (0.9% physiological saline) and placed at a constant temperature of 37℃ in the dark. The immersion solution was collected on days 1, 3, and 7, and the concentration of silver ions in the solution was measured using an atomic absorption spectrophotometer to calculate the cumulative release rate of silver ions.
[0089] The results showed that the cumulative release rate of silver ions in Example 1 over 7 days was 32.6%, with a gradual release rate and no obvious initial burst release phenomenon; while the cumulative release rate of silver ions in Comparative Example 1 over 7 days reached 58.3%, with the release rate on the first day exceeding 30%, showing a significant burst release effect.
[0090] The mechanism is as follows: the genipin cross-linking reaction mainly occurs between the free amino groups in the amorphous region of silk fibroin and the amino groups in chitosan, forming a dense covalent network between fiber molecules. On the one hand, the fiber structure is more compact, forming a physical coating on the silver nanowires loaded on the surface, reducing the direct contact area between the exudate and the silver nanowires; on the other hand, the swelling of the fiber network is restricted, slowing down the rate of liquid penetration into the fiber interior, thereby effectively regulating the release rate of silver ions, avoiding initial burst release, and improving the long-lasting antibacterial effect and biosafety.
[0091] Exudate conductivity sensor performance test:
[0092] The patterned electrode of the sample from Example 1 was connected to an electrochemical workstation. Simulated exudate was added drop by drop to the sensing area, and the conductivity changes under different exudate volumes were recorded to verify the correspondence between the amount of exudate and the conductivity.
[0093] As the amount of exudate increased from 0 to 50 μL, the conductivity of the sample showed a linear upward trend, with a linear correlation coefficient R² = 0.987 and a response time < 30 s. The conductivity value can accurately reflect the accumulation of exudate in the wound and has the ability to monitor the exudation status of the wound in real time and in situ.
[0094] SERS biochemical detection performance test:
[0095] 30 μL of uric acid and urea standard solutions of different concentrations were added to the sensing area of the sample in Example 1. After natural drying at room temperature, Raman spectroscopy was used for testing with an excitation wavelength of 785 nm, a laser power of 5 mW, a spot diameter of 2 μm, and an integration time of 10 s. Simultaneously, simulated exudate containing glucose and lactic acid interferences was tested to verify the anti-interference performance.
[0096] The detection limit for uric acid in the sample of this invention can reach 10. -8 M has a detection limit of up to 10 for urea. -4 M, characteristic peak of uric acid (499cm) -1 662cm -1 ) and the characteristic peak of urea (1002 cm⁻¹) -1 The target characteristic peaks are clearly distinguishable; in simulated exudate with added physiological concentrations of glucose and lactic acid as interfering agents, the target characteristic peaks show no obvious shift or interference, demonstrating excellent anti-interference performance and enabling in-situ, non-invasive detection of metabolic markers in wound exudate.
[0097] Example 5
[0098] D1. Cut the nanofiber electronic skin prepared in Example 1 into 5cm×5cm dressing pieces, sterilize with ethylene oxide, seal and store for later use.
[0099] D2. Before use, perform routine debridement of the wound to remove necrotic tissue and residual exudate from the wound surface. Rinse the wound with sterile saline and use sterile gauze to absorb any free fluid from the wound and surrounding skin.
[0100] D3. Remove the sterilized dressing, moisten the base of the dressing with a small amount of sterile saline, and flatten the dressing over the wound surface. Gently press the edges of the dressing with your fingertips for 10-15 seconds. The dressing adheres tightly to the wound tissue by relying on the hydration and adhesion properties of silk fibroin and chitosan, without the need for additional medical tape or sutures.
[0101] D4. For chronic wounds with irregular shapes, the dressing is pre-cut to the required shape so that the patterned sensing area is aligned with the area where the wound exudate is concentrated before it is applied; for burn wounds on curved surfaces, the dressing is directly applied to the contour of the wound to avoid pressure from hard parts.
[0102] D5. Connect the lead-out end of the patterned electrode of the dressing to the miniature low-power signal acquisition module through a flexible FPC wire, and fix the acquisition module to the healthy skin next to the wound with medical tape.
[0103] D6. The signal acquisition module continuously collects the conductivity signal of the sensing area at a sampling frequency of once every 5 minutes. The built-in algorithm converts the conductivity value into the corresponding accumulation amount of wound exudate, and the data is transmitted to the medical terminal via Bluetooth.
[0104] D7. When the amount of exudate accumulated in the wound reaches the preset threshold, the system will automatically issue a dressing change prompt, eliminating the need for medical staff to frequently lift the dressing for visual inspection and reducing the risk of wound exposure and infection.
[0105] D8. During use, medical staff regularly aim the miniature Raman probe at the sensing area of the dressing to non-invasively collect the SERS spectrum of the wound exudate, identify the characteristic peak intensity of uric acid and urea and semi-quantitatively analyze their concentration changes, providing objective data reference for assessing the local inflammation and metabolic status of the wound.
[0106] D9. During the continuous use period, the dressing continuously absorbs and stores wound exudate through the underlying cross-linked modified nanofiber substrate. Relying on the capillary fluid conduction effect of the three-dimensional fiber network, the local exudate is diffused to the entire dressing substrate, avoiding local fluid accumulation and soaking of the wound.
[0107] D10. During use, the silver nanowires release silver ions slowly as they are soaked in the exudate, continuously inhibiting the proliferation of pathogens in the wound, maintaining a local antibacterial environment, and reducing the risk of infection.
[0108] D11. When the conductivity data indicates that the dressing is close to saturation of exudate storage, or when exudate leakage occurs at the edge of the dressing, the dressing should be replaced. When replacing, gently peel off the dressing in one piece, ensuring that the dressing does not adhere to the newly formed tissue of the wound, and avoid tearing to prevent secondary damage.
[0109] D12. This dressing has an overall thickness of only about 40 micrometers, combining breathability and skin conformability. It can simultaneously achieve exudate management, antibacterial protection and in-situ monitoring without the need for multi-layer composite stacking. It is suitable for long-term intelligent care of high exudative wounds such as diabetic foot ulcers, pressure injuries, and second-degree burns.
[0110] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a highly hygroscopic and antibacterial nanofiber electronic skin, characterized in that, Includes the following steps: S1. Mix the regenerated silk fibroin solution with the hydrophilic polysaccharide solution, add spinning aids, and prepare a blended spinning solution; S2. The blended spinning solution is spun using an electrospinning process to prepare a silk fibroin-based nanofiber membrane. S3. Silver nanowires are loaded in a predetermined area of the silk fibroin-based nanofiber film using a patterned deposition process to form a patterned conductive functional layer. S4. The composite fiber membrane loaded with silver nanowires is cross-linked and cured using a natural biological cross-linking agent, and then dried to obtain the highly hygroscopic and antibacterial nanofiber electronic skin.
2. The method for preparing a highly hygroscopic and antibacterial nanofiber electronic skin according to claim 1, characterized in that, In step S1, the hydrophilic polysaccharide is chitosan, and the chitosan acetate solution has a mass fraction of 1% to 3%; the regenerated silk fibroin solution has a mass fraction of 7% to 8%, and it is mixed with the chitosan acid solution at a volume ratio of (3 to 5): 1; the spinning aid is polyethylene oxide, and its addition amount accounts for 0.5% to 1% of the total mass of the spinning solution. The hydrophilic polysaccharide is chitosan, which is pre-dissolved in 1-2% dilute acetic acid aqueous solution to prepare a chitosan acetic acid solution with a mass fraction of 1%-3%. Before mixing, the pH of the mixture is adjusted to 6.5-7.0 with dilute NaOH to avoid the precipitation of silk fibroin near the isoelectric point. The mixture is stirred at low speed for 10 minutes to obtain a uniform blended spinning solution.
3. The method for preparing a highly hygroscopic and antibacterial nanofiber electronic skin according to claim 1, characterized in that, In step S3, the patterned deposition process adopts electrophoretic deposition, combined with a hollow mask with a preset electrode pattern to achieve regional selective loading of silver nanowires. The surface deposition amount of silver nanowires in the substrate film loading region is 0.015~0.025 mg / cm².
4. The method for preparing a highly hygroscopic and antibacterial nanofiber electronic skin according to claim 1, characterized in that, In step S4, the natural biological cross-linking agent is genipin; The cross-linking and curing process specifically involves immersing the composite fiber membrane loaded with silver nanowires in a 0.5%~1% (w / w) genipin aqueous solution, maintaining a constant temperature of 35℃~40℃ for 12h~24h for cross-linking, removing it, rinsing with deionized water to remove unreacted genipin, and drying at room temperature.
5. A highly absorbent and antibacterial nanofiber electronic skin, characterized in that, The electronic skin is prepared by the method described in any one of claims 1 to 4, wherein the electronic skin has a double-layer fiber network structure, the lower layer is a cross-linked modified silk fibroin-based nanofiber hygroscopic substrate, and the upper layer is a patterned silver nanowire conductive network layer; the electronic skin has a 24-hour water absorption rate ≥680% as tested by the immersion and weighing method according to GB / T1034-2008 "Determination of Water Absorption of Plastics", and an antibacterial rate of ≥60% against Staphylococcus aureus and ≥50% against Escherichia coli as tested by the oscillation method according to GB / T20944.3-2007.
6. The application of the highly absorbent and antibacterial nanofiber electronic skin as described in claim 5 in the preparation of wound repair monitoring dressings.
7. The application according to claim 6, characterized in that, The wound repair monitoring dressing is suitable for the care of high-exudative wounds, including diabetic foot ulcers, pressure injury wounds, and second-degree or higher burns.
8. The application according to claim 6, characterized in that, The wound repair monitoring dressing collects the electrical conductivity signal of wound exudate through a patterned silver nanowire conductive network, and the electrical conductivity signal is used to reflect the change in the amount of wound exudate.
9. The application according to claim 6, characterized in that, The wound repair monitoring dressing utilizes the surface-enhanced Raman scattering effect of silver nanowires to enrich and detect characteristic metabolic markers of uric acid and urea in wound exudate.
10. The application according to claim 6, characterized in that, The wound repair monitoring dressing absorbs and stores wound exudate through a cross-linked modified silk fibroin nanofiber substrate; silver nanowires are coated by the cross-linked fiber network to achieve the gradual release of silver ions to inhibit the proliferation of pathogens in the wound, so that the dressing has the functions of exudate management, antibacterial protection and signal acquisition.
Citation Information
Patent Citations
All-fiber-shaped SF NF-Ag NWs composite wearable electronic skin and preparation method thereof
CN119097279A