A dual growth factor-loaded time-controlled release lyophilized amniotic membrane sustained-release film and a preparation method thereof
By setting a bFGF immediate-release layer and a VEGF sustained-release layer in the amniotic membrane sustained-release membrane, and utilizing the amniotic membrane dense layer and microsphere design to achieve time-sequential biphasic release, the problems of uncontrollable growth factor membrane release behavior and easy loss of activity were solved, thus promoting the repair effect of chronic wounds.
Patent Information
- Application Number
- CN202611603722.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-24
AI Technical Summary
Existing growth factor membranes are difficult to supply in a timely manner according to the needs of each stage during wound repair, resulting in uncontrollable release behavior, mutual interference between growth factors and easy loss of activity, which affects the repair effect of chronic wounds.
The bFGF immediate-release layer and VEGF sustained-release layer were respectively placed on both sides of the decellularized amniotic membrane dense layer. Spatial separation was achieved by utilizing the natural barrier of the amniotic membrane dense layer, and time-sequential biphasic release was achieved by the differences in microsphere particle size, carrier material and cross-linking degree. Combined with freeze-drying protectant and micropore design, the activity and release control of growth factors were ensured.
It enables independent and controllable release of growth factors, promotes the matching of physiological needs at different stages of wound repair, improves the retention rate of growth factor bioactivity, and enhances the applicability and stability of the membrane in moist wound environments.
Smart Images

Figure CN123148445A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of biomedical materials technology, and more specifically, to a time-controlled release lyophilized amniotic membrane loaded with dual growth factors and its preparation method. Background Technology
[0002] Wound healing, especially the repair of chronic wounds such as diabetic foot ulcers, is a complex and dynamic process involving multiple stages, including inflammation, proliferation, and remodeling. Basic fibroblast growth factor (bFGF) promotes fibroblast proliferation, granulation tissue formation, and reepithelialization in the late stages of inflammation and early stages of proliferation; while vascular endothelial growth factor (VEGF) continuously promotes vascular endothelial cell proliferation and angiogenesis maturation in the late stages of proliferation and remodeling. These two growth factors play different but complementary roles at different stages of wound repair. Rapidly supplying bFGF in the early stages of repair and continuously supplying VEGF in the later stages could potentially achieve more ideal repair outcomes.
[0003] Currently, there are some reports on the preparation of repair membranes by loading growth factors onto biological scaffold materials. However, such studies typically involve directly mixing, soaking, or co-incubating the scaffold material with a solution containing growth factors, followed by freeze-drying to achieve a uniform distribution of multiple growth factors within the material. This co-loading method leads to mutual diffusion and interference among different growth factors during release, making it difficult to achieve a sequential release behavior that is initially rapid and then slows down. Furthermore, the simultaneous release of multiple growth factors into the wound may reduce their individual biological activity due to mutual physicochemical interactions. Additionally, growth factors lacking effective protection are prone to inactivation during freeze-drying and irradiation sterilization.
[0004] Therefore, existing blended growth factor membranes cannot achieve sequential supply according to the needs of different stages of wound repair, and have limited repair effects on chronic wounds. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors and its preparation method. This membrane has a bFGF rapid-release layer and a VEGF sustained-release layer respectively disposed on both sides of a dense layer of decellularized amniotic membrane. The spatial separation of the two growth factors is achieved by utilizing the natural dense barrier of the decellularized amniotic membrane. Furthermore, the differences between the two layers in microsphere size, carrier material, cross-linking degree, and thickness enable a time-controlled dual-phase release effect, with bFGF rapidly releasing early and VEGF continuously releasing later. Simultaneously, through the synergistic protection of microsphere encapsulation and lyophilization protectant, the membrane maintains high bioactivity of both growth factors after lyophilization and irradiation sterilization. This solves the problems of uncontrollable release behavior, mutual interference between factors, and easy loss of activity in existing blended growth factor membranes, effectively promoting wound repair, especially the repair of chronic wounds such as diabetic foot ulcers.
[0006] The above-mentioned technical objective of the present invention is achieved through the following technical solution: In a first aspect, a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors is provided, comprising a decellularized amniotic membrane dense layer and a bFGF immediate-release layer and a VEGF sustained-release layer located on both sides of the decellularized amniotic membrane dense layer, respectively. The bFGF immediate-release layer contains gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor and an amniotic membrane ECM hydrogel framework. The VEGF sustained-release layer contains PLGA alginate composite microspheres loaded with vascular endothelial growth factor and an amniotic membrane ECM hydrogel framework. The release rate of basic fibroblast growth factor in the bFGF immediate-release layer is greater than that of vascular endothelial growth factor in the VEGF sustained-release layer.
[0007] Preferably, the median volume diameter of the gelatin-chitosan composite microspheres is 1 μm to 3 μm, and the median volume diameter of the PLGA-alginic acid composite microspheres is 5 μm to 15 μm. The drug loading of the gelatin-chitosan composite microspheres is from 0.5 μg / mg to 2.0 μg / mg, and the drug loading of the PLGA-algin composite microspheres is from 1.0 μg / mg to 4.0 μg / mg.
[0008] Preferably, the content of the gelatin-chitosan composite microspheres in the bFGF immediate-release layer is 20 mg / mL to 40 mg / mL, and the content of the PLGA-algin composite microspheres in the VEGF sustained-release layer is 30 mg / mL to 50 mg / mL.
[0009] Preferably, under in vitro release conditions in phosphate buffer, the ratio of the cumulative release rate of basic fibroblast growth factor to the cumulative release rate of vascular endothelial growth factor on day 3 is not less than 2.0, and the cumulative release rate of vascular endothelial growth factor on day 7 is not greater than 70%.
[0010] Preferably, it also includes an asymmetric cross-linking region; The asymmetric cross-linked region is located between the bFGF immediate-release layer and the decellularized amnion dense layer, and between the VEGF sustained-release layer and the decellularized amnion dense layer. The degree of cross-linking in the asymmetric cross-linked region decreases from the VEGF sustained-release layer side to the bFGF immediate-release layer side.
[0011] Preferably, the thickness of the bFGF immediate-release layer is 50 μm to 80 μm, the thickness of the decellularized amnion dense layer is 10 μm to 20 μm, and the thickness of the VEGF sustained-release layer is 50 μm to 100 μm; The degradation time of the membrane in phosphate buffer containing lysozyme with a remaining mass fraction of 50% is 15 to 25 days.
[0012] Preferably, it also contains a lyophilization protectant; The freeze-drying protectant contains trehalose, mannitol, and bovine serum albumin; The freeze-drying protectant contains trehalose at a mass concentration of 1% to 10%, mannitol at a mass concentration of 1% to 5%, and bovine serum albumin at a mass concentration of 0.1% to 1%.
[0013] Preferably, it also includes a single-sided laser micropore; The unilateral laser micropore is opened from one side of the VEGF sustained-release layer to the other side of the decellularized amnion dense layer, penetrates the VEGF sustained-release layer and extends through the asymmetric cross-linking region located between the VEGF sustained-release layer and the decellularized amnion dense layer, and terminates on the surface of the decellularized amnion dense layer without penetrating the decellularized amnion dense layer. The aperture of the single-sided laser micro-aperture is 200μm to 300μm, and the center-to-center distance between adjacent single-sided laser micro-apertures is 1mm to 2mm.
[0014] Secondly, a method for preparing a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors is provided, comprising the following steps: The amnion was decellularized to obtain a decellularized amnion; A portion of the decellularized amnion was used to prepare an amnion ECM hydrogel precursor, while a portion of the decellularized amnion was retained as a dense layer of the decellularized amnion. Prepare gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor and PLGA-algin composite microspheres loaded with vascular endothelial growth factor. The gelatin-chitosan composite microspheres were mixed with the amniotic membrane ECM hydrogel precursor to obtain the bFGF immediate release layer composite solution. The PLGA alginate composite microspheres were mixed with the amniotic membrane ECM hydrogel precursor to obtain a VEGF sustained-release layer composite solution. Using the decellularized amnion dense layer as a separator, the VEGF sustained-release layer composite solution is cast onto the first surface of the decellularized amnion dense layer and gelled, and the bFGF rapid-release layer composite solution is cast onto the second surface of the decellularized amnion dense layer and gelled to obtain a wet film. The wet film is freeze-dried to obtain the film sheet.
[0015] Preferably, the method further includes: The wet membrane was gradient crosslinked in MES buffer using EDC and NHS, such that the degree of crosslinking on the bFGF immediate release layer side was lower than that on the VEGF sustained release layer side. The gradient cross-linked wet film was immersed in a lyophilization protectant solution containing trehalose, mannitol and bovine serum albumin; The freeze-drying process employs programmed cooling freeze-drying. After freeze-drying, micropores are processed by laser from one side of the VEGF sustained-release layer to the other side of the decellularized amnion dense layer. The micropores penetrate the VEGF sustained-release layer and extend through the asymmetric cross-linking region between the VEGF sustained-release layer and the decellularized amnion dense layer, ending at the surface of the decellularized amnion dense layer without penetrating it. After processing, it is sterilized by gamma ray irradiation.
[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention provides a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors. By placing a bFGF immediate-release layer and a VEGF sustained-release layer on opposite sides of a decellularized amniotic membrane dense layer, the decellularized amniotic membrane dense layer forms a continuous, non-porous isolation barrier between the two layers, separating basic fibroblast growth factor and vascular endothelial growth factor within the membrane's internal space. Simultaneously, the rapid release characteristics of the immediate-release layer and the sustained release characteristics of the sustained-release layer function independently, forming a time-sequential biphasic release pattern of rapid early bFGF release and sustained later VEGF release based on spatial isolation. The spatial isolation in this invention prevents the two growth factors from diffusing across layers and interfering with each other, ensuring that their release behavior is independent and controllable. The time-sequential release allows bFGF to promote cell proliferation and granulation tissue formation in the early stages of wound repair, while VEGF promotes angiogenesis and maturation in the later stages, matching the physiological needs of different stages of wound healing.
[0017] 2. This invention provides asymmetric cross-linking regions between the bFGF immediate-release layer and the decellularized amnion dense layer, and between the VEGF sustained-release layer and the decellularized amnion dense layer, with the degree of cross-linking decreasing from the VEGF sustained-release layer side to the bFGF immediate-release layer side. This works in conjunction with the spatial isolation effect of the decellularized amnion dense layer: the network on the side with lower cross-linking degree is loose, allowing water to easily penetrate and reducing the diffusion resistance of bFGF, which is beneficial for immediate release; the network on the side with higher cross-linking degree is dense, extending the VEGF diffusion path and slowing down the membrane degradation rate, which is beneficial for sustained release and prolonging the release period. Simultaneously, a unilateral laser micropore is created from the VEGF sustained-release layer towards the decellularized amniotic membrane dense layer, penetrating the VEGF sustained-release layer and extending through the asymmetric cross-linking region, terminating at the surface of the decellularized amniotic membrane dense layer without penetrating it. One end is exposed on the wound side of the membrane, forming a cavity for exudate retention and redistribution, which can promptly absorb wound exudate and prevent exudate accumulation and maceration of the wound. Because the micropore does not penetrate the dense layer, the spatial isolation effect of the two growth factors is not compromised, and the exudate management function and spatial separation function do not interfere with each other. This invention enables the membrane to maintain its core function of sequential biphasic release while also possessing exudate management capabilities and gradient adaptability to degradation performance, improving the applicability and stability of the membrane in moist wound environments.
[0018] 3. This invention provides a first layer of protection through microsphere encapsulation, isolating growth factors from the external environment and reducing mechanical damage to protein structures caused by ice crystals during freeze-drying. A second layer of protection is provided by a freeze-drying protectant containing trehalose, mannitol, and bovine serum albumin. This protectant replaces water molecules during freeze-drying and gamma-ray irradiation sterilization, forming hydrogen bonds with proteins, maintaining their native conformation, and capturing free radicals. This significantly improves the activity retention rate of bFGF and VEGF, ensuring that the activity retention rate after irradiation sterilization is no less than 80%. The synergistic effect of microsphere encapsulation and the freeze-drying protectant ensures that growth factors maintain high biological activity after freeze-drying and irradiation sterilization. Simultaneously, the decellularized amniotic membrane dense layer retains the complete basement membrane structure and dense collagen network, providing the membrane with high tensile strength and a stable support structure. The degradation time is 15 to 25 days, matching the VEGF sustained-release cycle, ensuring the membrane maintains its integrity and functionality throughout the entire wound repair cycle. Attached Figure Description
[0019] The accompanying drawings, which are included to provide a further understanding of embodiments of the invention and form part of this application, do not constitute a limitation thereof. In the drawings: Figure 1 This is a schematic diagram of the layer structure in Embodiment 1 of the present invention; Figure 2 This is an HE staining result diagram from Example 2 of the present invention; where A is fresh amnion and B is decellularized amnion; Figure 3This is a surface SEM image of the bFGF immediate-release layer in Embodiment 1 of the present invention; Figure 4 This is a SEM image of the membrane morphology after rehydration in Embodiment 1 of the present invention. Detailed Implementation
[0020] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the embodiments and accompanying drawings. The illustrative embodiments and descriptions of the present invention are only used to explain the present invention and are not intended to limit the present invention.
[0021] Example 1: A time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors, such as... Figure 1 As shown, the membrane has a five-layer structure, consisting of a bFGF immediate-release layer, an asymmetric cross-linked region, a decellularized amniotic membrane compact layer, another asymmetric cross-linked region, and a VEGF sustained-release layer. The bFGF immediate-release layer contains gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor and an amniotic membrane ECM hydrogel framework. The VEGF sustained-release layer contains PLGA-algin composite microspheres loaded with vascular endothelial growth factor and an amniotic membrane ECM hydrogel framework. The decellularized amniotic membrane compact layer spatially separates the bFGF immediate-release layer from the VEGF sustained-release layer. The asymmetric cross-linked region is located between the bFGF immediate-release layer and the decellularized amniotic membrane compact layer, and also between the VEGF sustained-release layer and the decellularized amniotic membrane compact layer; the degree of cross-linking decreases from the VEGF sustained-release layer side towards the bFGF immediate-release layer side.
[0022] The membrane is also provided with unilateral laser micropores, which are opened from the VEGF sustained-release layer to the decellularized amnion compact layer. They penetrate the VEGF sustained-release layer and extend through the asymmetric cross-linking region between the VEGF sustained-release layer and the decellularized amnion compact layer, ending at the surface of the decellularized amnion compact layer without penetrating it.
[0023] In this embodiment, the thickness of the bFGF immediate-release layer is 50-80 μm, and the thickness of the VEGF sustained-release layer is 60-100 μm; the drug loading of the bFGF microspheres is 1.0-1.5 μg / mg, and the drug loading of the VEGF microspheres is 2.0-3.5 μg / mg.
[0024] In this invention, bFGF is rapidly released in the early stage to promote cell proliferation and granulation formation, while VEGF is continuously released in the later stage to promote angiogenesis and maturation. By utilizing the natural dense structure of the decellularized amnion, the two growth factors are respectively positioned on both sides of the membrane to avoid mutual diffusion and interference.
[0025] Example 2: Preparation and quality control of decellularized amniotic membrane and amniotic membrane ECM hydrogel precursor.
[0026] 1. Decellularization treatment.
[0027] Amniotic membranes from healthy mothers delivered via cesarean section were repeatedly rinsed with sterile saline to remove blood. The amniotic membrane was then immersed in phosphate-buffered saline (PBRS) containing 4 mol / L NaCl and treated with shaking at 4°C for 12 h to separate the epithelial cells from the basement membrane. Subsequently, it was digested with 0.25% trypsin-EDTA solution at 37°C for 30 min, followed by treatment with 1% Triton X-100 solution at 4°C for 6 h to fully lyse any remaining cells. Finally, it was digested with 50 U / mL DNase I in PBRS at 37°C for 1 h to remove DNA fragments. The membrane was repeatedly rinsed with PBRS for 12 h to remove chemical residues, yielding decellularized amniotic membranes, which were stored at -80°C for later use.
[0028] The decellularization process utilizes a hypertonic saline solution to dehydrate and shrink epithelial cells, separating them from the basement membrane. Trypsin is used to further digest cell junction proteins, Triton X-100 nonionic surfactant is used to dissolve the cell membrane phospholipid bilayer, and DNase I is used to degrade residual DNA fragments. In this way, the collagen fiber network structure in the amniotic extracellular matrix is preserved while removing cellular components.
[0029] 2. Preparation of amniotic membrane ECM hydrogel precursor.
[0030] Take a portion of the decellularized amnion and cut it into 1mm pieces. 3 Next, a 0.5 mol / L acetic acid solution containing 1 mg / mL pepsin was added, and the mixture was shaken and digested at 4°C for 12 h until the decellularized amniotic membrane was completely dissolved. The digestion solution was centrifuged at 12000 rpm for 30 min at 4°C to remove insoluble matter. The supernatant was placed in a dialysis bag and dialyzed with phosphate buffer at 4°C until the pH stabilized to obtain the amniotic membrane ECM hydrogel precursor. The total protein concentration of the amniotic membrane ECM hydrogel precursor was determined by the BCA method, adjusted to 6 mg / mL with phosphate buffer, and stored at 4°C for later use.
[0031] Another portion of the aforementioned decellularized amnion is preserved intact without digestion and used as a dense layer of decellularized amnion in subsequent membrane preparation.
[0032] 3. Quality control of decellularization effect.
[0033] The amount of DNA residue in decellularized amniotic membrane was detected using the PicoGreen dsDNA quantitative kit, the collagen retention rate was determined using the hydroxyproline colorimetric method, the glycosaminoglycan retention rate was determined using the dimethylmethylene blue method, and the tissue structure was observed by HE staining.
[0034] like Figure 2As shown, section A is a fresh amniotic tissue section, revealing a complete and continuous epithelial cell layer with deeply stained blue-purple nuclei. The collagen matrix beneath the basement membrane is densely and uniformly arranged. Section B is a decellularized amniotic tissue section, where the epithelial cell layer has been completely removed, and the nuclei have disappeared, leaving only a dense collagen matrix and a continuous, intact basement membrane structure. The collagen fibers remain densely and orderly arranged, without obvious loosening or breakage. These histological results demonstrate that the decellularization process of this embodiment can effectively remove cellular components while maintaining the structural integrity of the amniotic extracellular matrix.
[0035] The amount of residual DNA is expressed by the formula: ; in, The amount of DNA remaining in the decellularized amnion is expressed in ng / mg. The mass of DNA in the sample is measured in ng. The dry weight of the sample is measured in mg.
[0036] Collagen retention rate is expressed by the formula: ; in, Collagen retention rate; The mass of collagen in the amnion after decellularization; The mass of collagen in fresh amnion before decellularization.
[0037] The glycosaminoglycan retention rate is expressed by the formula: ; in, Glycosaminoglycan retention rate; The mass of glycosaminoglycans in the amnion after decellularization; The mass of glycosaminoglycans in fresh amnion before decellularization.
[0038] The quantitative test results before and after decellularization are shown in Table 1.
[0039] Table 1. Results of quality control of decellularized amnion
[0040] Table 1 shows that the residual DNA level after decellularization was 12.5 ng / mg, significantly lower than the 486.3 ng / mg in fresh amnion and below the safety threshold of 50 ng / mg. The collagen retention rate after decellularization was 94.3%. The glycosaminoglycan retention rate was 87.2%. The above quantitative data are consistent with... Figure 2 The histological observations corroborated each other, indicating that the decellularization process can effectively remove cellular components and DNA residues from the amnion while preserving the main components and structural integrity of the extracellular matrix.
[0041] The decellularized amniotic membrane in this invention retains the complete basement membrane structure and dense collagen network. This dense structure acts as a physical barrier in the final membrane, preventing the translayer diffusion of basic fibroblast growth factor in the bFGF immediate-release layer and vascular endothelial growth factor in the VEGF sustained-release layer. Simultaneously, the amniotic membrane ECM hydrogel precursor prepared from the decellularized amniotic membrane provides the microspheres with a three-dimensional network framework rich in natural extracellular matrix components, which is beneficial for maintaining the bioactivity of growth factors and supporting cell adhesion and proliferation.
[0042] Example 3: Preparation and parameter optimization of dual growth factor microspheres.
[0043] 1. Preparation of gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor.
[0044] A 10% (w / w) gelatin solution was prepared and dissolved in deionized water. Basic fibroblast growth factor (bFGF) was loaded into the gelatin solution at a concentration of 10,000 ng / mL, serving as the inner aqueous phase. Chitosan was dissolved in a 2% (w / w) acetic acid solution to obtain a chitosan solution. This chitosan solution was mixed with liquid paraffin at a volume ratio of 1:5 to form the oil phase. The inner aqueous phase was added dropwise to the oil phase, and the mixture was stirred at 600 rpm for 30 min to emulsify and form a W / O emulsion. Glutaraldehyde was slowly added dropwise to a final concentration of 1.0%, and stirring was continued for 2 h to allow the microspheres to fully cross-link and solidify. The microspheres were collected by centrifugation, washed sequentially with petroleum ether, isopropanol, and deionized water, and then freeze-dried under vacuum to obtain gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor, abbreviated as bFGF microspheres.
[0045] 2. Preparation of PLGA alginate composite microspheres loaded with vascular endothelial growth factor.
[0046] A vascular endothelial growth factor (VEGF) solution containing 2% sodium alginate (5000 ng / mL) was prepared as the inner aqueous phase. PLGA was dissolved in dichloromethane to obtain a 5% PLGA solution, which served as the oil phase. The inner aqueous phase and oil phase were mixed at a volume ratio of 1:10 and ultrasonically emulsified to form a W / O primary emulsion. The primary emulsion was added to an outer aqueous phase containing 1% polyvinyl alcohol (PVA), and the mixture was stirred at high speed to form a W / O / W complex emulsion. The mixture was magnetically stirred for 4 hours to evaporate the dichloromethane and solidify the microspheres. The microspheres were collected by centrifugation, washed three times with deionized water, and freeze-dried to obtain PLGA-algin composite microspheres loaded with VEGF, abbreviated as VEGF microspheres.
[0047] 3. Single-factor optimization of microsphere preparation parameters.
[0048] Single-factor investigations were conducted on gelatin mass fraction, final glutaraldehyde concentration, oil-water phase volume ratio, PLGA mass fraction, internal water-to-oil phase volume ratio, and ultrasonic power. Optimal preparation conditions were determined using microsphere size, drug loading, encapsulation efficiency, and in vitro release T50 as evaluation indicators. The investigation ranges and optimal values for each factor are shown in Table 2.
[0049] Table 2 Results of single-factor investigation in microsphere preparation
[0050] 4. Microsphere quality characterization.
[0051] Drug loading capacity is expressed by the formula: ; in, The drug loading capacity of the microspheres is expressed in μg / mg. The mass of growth factors contained in the microspheres is expressed in μg; mms is the total mass of the microspheres, expressed in mg.
[0052] Encapsulation efficiency is expressed by the formula: ; in, Encapsulation ratio; The actual mass of growth factors encapsulated in the microspheres; This refers to the total mass of growth factors added during preparation.
[0053] In in vitro release experiments, the cumulative release rate is expressed by the formula: ; in, for Cumulative release rate at any given time; for The cumulative quality of growth factors released over time; This represents the total mass of growth factors in the microspheres.
[0054] Method for determining in vitro release T50: Microspheres were compounded with amniotic membrane ECM hydrogel precursor according to a specified ratio, and after programmed temperature freeze-drying and irradiation with 25 kGy γ-rays, the time to reach a cumulative release rate of 50% was measured in phosphate buffer containing 1% bovine serum albumin at 37°C and 50 rpm shaking conditions. The obtained T50 is the release half-life of the microspheres in the actual membrane structure.
[0055] The mass parameters of the two types of microspheres under optimal conditions are shown in Table 3.
[0056] Table 3 Microsphere mass parameters
[0057] The distribution morphology of the two types of microspheres in the final membrane was observed by scanning electron microscopy. In the cross-section of the bFGF immediate release layer, the bFGF microspheres were small in size and uniformly distributed, embedded in the pores of the amniotic membrane ECM hydrogel network. In the cross-section of the VEGF sustained release layer, the VEGF microspheres were significantly larger in size than the bFGF microspheres, with a volume approximately 3 to 4 times that of the bFGF microspheres, and were uniformly distributed in the pores of the amniotic membrane ECM hydrogel network. The decellularized amniotic membrane dense layer had a uniform and dense structure with no visible pores, and neither of the microspheres from either side penetrated into the interior of this dense layer.
[0058] The bFGF microspheres of this invention utilize gelatin and chitosan as carriers, both of which are natural hydrophilic polysaccharides and proteins with good swelling properties and enzyme degradation sensitivity, facilitating rapid release of bFGF in the early stages of implantation. The VEGF microspheres employ PLGA and alginate as a composite carrier. PLGA, a hydrophobic polyester material, has a relatively long degradation cycle, significantly prolonging the release time of VEGF compared to the hydrophilic gelatin-chitosan carrier. The alginate hydrogel network forms an additional diffusion barrier on the microsphere surface, synergistically achieving sustained release of VEGF relative to bFGF with PLGA. The significant difference in particle size between the two types of microspheres further enhances the difference in release rates, providing a microstructural basis for time-sequential biphasic release.
[0059] Example 4: Preparation of freeze-dried amniotic membrane sustained-release membrane and verification of its in vitro release behavior.
[0060] 1. Membrane preparation steps.
[0061] The bFGF microspheres prepared in Example 3 were mixed with the amniotic membrane ECM hydrogel precursor prepared in Example 2 in a specific ratio to obtain a bFGF microsphere concentration of 30 mg / mL, thus yielding a bFGF immediate-release layer composite solution. VEGF microspheres were also mixed with the amniotic membrane ECM hydrogel precursor in a specific ratio to obtain a VEGF microsphere concentration of 40 mg / mL, thus yielding a VEGF sustained-release layer composite solution. Both composite solutions were kept liquid at 4°C for later use.
[0062] Using the intact, dense decellularized amniotic membrane as a separator, a VEGF sustained-release composite solution is first cast onto the first surface of the dense decellularized amniotic membrane and gelled at 37°C for 30 minutes to form the VEGF sustained-release layer. Then, a bFGF rapid-release composite solution is cast onto the second surface of the dense decellularized amniotic membrane and gelled at 37°C for 30 minutes to form the bFGF rapid-release layer. This invention first sets the slower-curing VEGF sustained-release composite solution before casting the bFGF rapid-release composite solution, avoiding cross-layer mixing when the two composite solutions come into contact in their ungelled state. This results in a wet film.
[0063] The wet membrane was subjected to gradient crosslinking using EDC and NHS as crosslinking agents. A MES buffer solution containing 50 mmol / L EDC and 25 mmol / L NHS was prepared. The VEGF sustained-release layer side of the wet membrane was immersed in the crosslinking solution for 20 min, followed by immersion of the entire wet membrane in the solution for 10 min. This resulted in a higher degree of crosslinking on the VEGF sustained-release layer side compared to the bFGF immediate-release layer side, forming an asymmetric crosslinked region. The crosslinking reaction mechanism involved EDC activating the carboxyl groups on collagen and gelatin molecules in the ECM, forming amide bonds with the amino groups on adjacent molecules. NHS improved the reaction efficiency, and the MES buffer provided a stable, weakly acidic reaction environment. After crosslinking, residual crosslinking agents were removed by rinsing with phosphate buffer.
[0064] The gradient-crosslinked wet membrane was immersed in a lyophilization protectant solution containing 5% trehalose, 2.5% mannitol, and 0.5% bovine serum albumin (BSA) at 4°C for 2 hours to allow the protectant to fully penetrate the membrane's internal pores and the surface of the microspheres. Subsequently, a programmed freeze-drying process was performed, including: cooling from room temperature to -40°C and holding at that temperature for 2 hours; a first drying process, heating from -40°C to -10°C and maintaining under vacuum for 12 hours to remove the main moisture; and a second drying process, heating from -10°C to 25°C and maintaining under vacuum for 6 hours for further dehydration. After freeze-drying, a freeze-dried amniotic membrane sustained-release membrane was obtained.
[0065] After freeze-drying, single-sided laser micropores were created using a laser drilling device, moving from the VEGF sustained-release layer to the decellularized amniotic membrane compact layer. The micropores penetrated the VEGF sustained-release layer and extended through the asymmetric cross-linking region between the VEGF sustained-release layer and the decellularized amniotic membrane compact layer, ending at the surface of the decellularized amniotic membrane compact layer without penetrating it. Each micropore had a diameter of 250 μm, and the center-to-center distance between adjacent micropores was 1.5 mm. After laser drilling, thermally damaged debris was removed by compressed air purging, followed by sterilization using gamma irradiation at a dose of 25 kGy to obtain the final membrane product.
[0066] 2. Verification of the macroscopic and microscopic structure of the membrane.
[0067] The prepared membrane has a smooth and flat surface, a light yellow and semi-transparent color, and uniformly distributed and regularly arranged laser micropores. When viewed from the side, the upper and lower layers of the membrane are clearly separated. The upper layer, the bFGF immediate release layer, is about 65 μm thick, and the lower layer, the VEGF sustained release layer, is about 80 μm thick. In the middle, a dense linear structure formed by the decellularized amnion is visible.
[0068] Scanning electron microscopy of the membrane cross-section revealed that the bFGF immediate-release layer had a porous and loose structure, with small and uniformly distributed bFGF microspheres, and thin walls in the amniotic membrane ECM hydrogel network. The decellularized amniotic membrane dense layer was uniform and dense, with no visible pores or microsphere intrusion, forming a continuous physical barrier interface. The VEGF sustained-release layer had a porous structure with pore sizes significantly larger than those in the bFGF immediate-release layer, and VEGF microspheres were densely distributed within the network. The edges of the laser micropores penetrating the pore walls of the VEGF sustained-release layer were smooth, with no molten debris residue.
[0069] like Figure 3 As shown, the surface of the bFGF immediate-release layer exhibits a porous and loose structure with uniform pore size distribution. The amniotic membrane ECM hydrogel network is continuous and intact, with bFGF microspheres embedded in the network pores. The microsphere surfaces are smooth, without aggregation or breakage. Scanning electron microscopy observation of the membrane surface shows that the micropore openings on the usable side of the membrane, i.e., the surface of the VEGF sustained-release layer, are regularly circular with uniform pore size and neat edges. The non-usable side of the membrane, i.e., the surface of the bFGF immediate-release layer, has a dense porous structure, and no laser penetration damage was found, indicating that the unilateral laser-induced micropores did not damage the surface integrity of the bFGF immediate-release layer.
[0070] 3. In vitro release experimental methods and results.
[0071] The membrane prepared in Example 4 was cut into 1cm × 1cm pieces and immersed in phosphate buffer containing 1% bovine serum albumin. An in vitro release experiment was conducted at 37°C and 50 rpm with shaking. Samples were taken at preset time points, and an equal volume of fresh release medium was added. The bFGF and VEGF contents in the samples were detected using an ELISA kit.
[0072] The 24-hour burst release rate is expressed by the formula: ; in, The 24-hour burst release rate; This represents the cumulative mass of growth factors released within 24 hours. This represents the total content of the corresponding growth factor in the membrane.
[0073] The fast-slow release ratio is expressed by the formula: ; in, The fast-to-slow release ratio on day 3; This represents the cumulative release rate of bFGF on day 3. This represents the cumulative release rate of VEGF on day 3.
[0074] In vitro release experiments showed that bFGF was rapidly released from day 1, with a cumulative release rate of 22.4% on day 1, 80.8% on day 3, 92.5% on day 7, and 98.2% on day 14. VEGF exhibited a sustained release characteristic, with a cumulative release rate of 8.8% on day 1, 38.1% on day 3, 67.4% on day 7, 90.5% on day 14, and 98.7% on day 28. The two release curves showed a clear separation around day 3, indicating successful staggered release.
[0075] The 24-hour burst release rate comparison showed that the 24-hour burst release rate of the membrane of the present invention was 31.2%, significantly lower than that of Comparative Example 1 (55.8%) and Comparative Example 2 (63.4%). Comparative Example 1 was a uniformly mixed monolayer amniotic membrane prepared by lyophilizing decellularized amniotic membrane, co-incubating it with a mixed solution of bFGF and VEGF for adsorption, and then freeze-drying it, wherein bFGF and VEGF were uniformly distributed in the same layer. Comparative Example 2 was a membrane prepared by directly immersing decellularized amniotic membrane in a mixed solution of bFGF and VEGF for adsorption.
[0076] When the fast and slow release ratio on day 3 Not less than 2.0, and the cumulative VEGF release rate on day 7. When the percentage is no more than 70%, the membrane is considered to have achieved sequential biphasic release.
[0077] The release data at different time points are shown in Table 4.
[0078] Table 4 In vitro release data
[0079] In this invention, the decellularized amniotic membrane dense layer acts as a physical separation barrier, positioning the two growth factors on opposite sides of the membrane. The bFGF microspheres, with their small size and location within a loose, hydrophilic gelatin-chitosan carrier, allow for easy water penetration and a short diffusion path, thus enabling rapid bFGF release. In the VEGF sustained-release layer, the larger VEGF microspheres, with a median volume diameter of 5 μm to 15 μm, have a longer internal diffusion path. Furthermore, the PLGA carrier is a hydrophobic polyester material that requires gradual hydrolysis and degradation, resulting in slow and sustained VEGF release. The difference in particle size between the two types of microspheres, along with the difference in carrier materials, constitutes the microscopic basis for the time-sequential biphasic release.
[0080] The decellularized amniotic membrane dense layer maintains the intact basement membrane structure and dense collagen network, forming a continuous, non-porous physical barrier between the bFGF immediate-release layer and the VEGF sustained-release layer. This structure allows the two growth factors to be positioned on opposite sides of the membrane, preventing bFGF from diffusing into the VEGF sustained-release layer and vice versa, thus avoiding interference between the two growth factors in the same space. Spatial separation is a prerequisite for time-sequential release.
[0081] The unilateral laser-guided micropores extend from the VEGF sustained-release layer towards the decellularized amniotic membrane compact layer, penetrating the VEGF sustained-release layer and extending through the asymmetric cross-linking region, terminating at the surface of the decellularized amniotic membrane compact layer without penetrating it. This microporous structure is only exposed on the wound side of the membrane, serving to temporarily store and redistribute wound exudate while improving membrane adhesion compliance. Exudate entering the micropores is contained within the pore cavities, preventing exudate accumulation and wound maceration. Because the micropores do not penetrate the decellularized amniotic membrane compact layer, the spatial isolation effect of the growth factors on both sides is not compromised, and the exudate management and spatial separation functions do not interfere with each other. The unilateral nature of the micropores allows for functional differentiation on both sides of the membrane: the VEGF sustained-release layer can temporarily contain exudate when applied to the wound, while the bFGF immediate-release layer maintains its surface integrity when facing outwards.
[0082] Example 5: Effects of freeze-drying protectants and irradiation sterilization on growth factor activity.
[0083] 1. Experimental design.
[0084] To investigate the effects of lyophilization protectants and irradiation sterilization on the bioactivity of growth factors in the membranes, three experimental groups were set up using the wet membranes prepared in Example 4. Group A contained no lyophilization protectant; the wet membranes were directly subjected to programmed cooling lyophilization with an irradiation dose of 0 kGy. Group B contained lyophilization protectant; the wet membranes were immersed in the lyophilization protectant solution from Example 4 and then subjected to programmed cooling lyophilization with an irradiation dose of 0 kGy. Group C contained lyophilization protectant and was sterilized by 25 kGy γ-ray irradiation. Growth factors were extracted from all three groups of membranes by reconstitution with phosphate buffer, and the activity concentrations of bFGF and VEGF were detected by ELISA.
[0085] The activity retention rate is expressed by the formula: ; Where A is the retention rate of growth factor activity; The concentration of growth factor activity after freeze-drying and irradiation treatment; The initial concentration of growth factor activity before treatment.
[0086] 2. Appearance and rehydration morphology of freeze-dried membranes.
[0087] After freeze-drying, the membrane is white to pale yellow, with a smooth surface free of cracks, no warping at the edges, and no collapse or deformation. Lateral observation reveals a clear boundary between the bFGF immediate-release layer and the VEGF sustained-release layer, with the decellularized amniotic membrane dense layer located between the two layers, forming a continuous, dense linear structure.
[0088] After immersing the lyophilized membrane in phosphate buffer and rehydrating it at 37°C for 30 min, the amniotic membrane ECM hydrogel network absorbs water and swells, the pore walls thicken, and the originally interconnected pores shrink into closed or semi-closed micropores. The microspheres, after absorbing water and swelling, form circular protrusions on the pore walls. For example... Figure 4 As shown, high-magnification observation reveals that both bFGF microspheres and VEGF microspheres maintain a complete spherical shape, with no breakage, aggregation, or obvious collapse on the surface, indicating that the freeze-drying and rehydration processes did not damage the integrity of the microsphere structure.
[0089] 3. Results of activity retention rate.
[0090] The results of the activity retention rate test for each group are shown in Table 5.
[0091] Table 5. Effects of freeze-drying protectants and irradiation sterilization on the retention rate of growth factor activity.
[0092] The bFGF activity retention rate in the group containing the lyophilization protectant was 91.2%, an increase of approximately 29 percentage points compared to the 62.3% in the group without the protectant; the VEGF activity retention rate was 89.6%, an increase of approximately 31 percentage points compared to the 58.7% in the group without the protectant. After sterilization with 25 kGy irradiation and containing the lyophilization protectant, the bFGF activity retention rate remained at 86.7%, and the VEGF activity retention rate remained at 83.5%, both remaining above 80%.
[0093] The microsphere encapsulation in this invention forms the first layer of protection, isolating growth factors from the external environment and reducing mechanical damage to protein structures caused by ice crystals during freeze-drying. The freeze-drying protectant forms the second layer of protection; trehalose and mannitol replace water molecules during freeze-drying to form hydrogen bonds with proteins, maintaining their native conformation. Bovine serum albumin, as a stabilizer, competitively adsorbs onto the surface of growth factors, reducing protein aggregation and denaturation. Free radicals generated during irradiation sterilization are a major factor leading to protein inactivation; the freeze-drying protectant can capture free radicals, thus maintaining high activity after sterilization.
[0094] Example 6: Membrane mechanical properties and in vitro degradation behavior.
[0095] 1. Mechanical property testing.
[0096] The freeze-dried membrane prepared in Example 4 was rehydrated and cut into dumbbell-shaped standard specimens. A universal testing machine was used to test the specimens at a tensile speed of 10 mm / min until fracture, and the tensile strength and elongation at break were recorded. The membrane of this invention, the decellularized amnion, and the D1 type membrane were tested separately. The D1 type membrane was prepared by lyophilizing the decellularized amnion, co-incubating it with a mixed solution of bFGF and VEGF, and then freeze-drying it to obtain a uniformly mixed monolayer amnion membrane, wherein bFGF and VEGF were uniformly distributed within the same layer.
[0097] Tensile strength is expressed by the formula: ; in, Tensile strength, in MPa; The maximum tensile force that the specimen could withstand before fracture is expressed in N. The initial cross-sectional area of the sample is in mm. 2 .
[0098] Elongation at break is expressed by the formula: ; in, Elongation at break; This is the gauge length at which the specimen breaks. This is the initial gauge length of the sample.
[0099] The mechanical test results are shown in Table 6.
[0100] Table 6 Comparison of Mechanical Properties
[0101] The tensile strength of the membrane of this invention is 127% higher than that of decellularized amnion and 85% higher than that of D1 membrane; the elongation at break is 77% higher than that of decellularized amnion and 45% higher than that of D1 membrane.
[0102] 2. In vitro degradation behavior test.
[0103] After weighing, the membrane was immersed in phosphate buffer containing lysozyme and degraded by shaking at 37°C. Samples were lyophilized and weighed weekly to calculate the remaining mass fraction. The remaining mass fraction during degradation is expressed by the formula: ; in, for The remaining mass fraction at time t; for The remaining mass after freeze-drying is sampled at regular intervals; This represents the initial mass of the membrane.
[0104] Degradation time Defined as the remaining mass fraction The degradation time corresponding to a reduction to 50%.
[0105] The in vitro degradation data of the membrane of the present invention and the D1 type membrane are shown in Table 7.
[0106] Table 7 Residual mass fraction of in vitro degradation
[0107] Degradation time of the membrane of the present invention The degradation time of the D1 membrane was 18.3 days. The degradation cycle of the membrane of the present invention is 12.5 days, which is about 46% longer than that of the D1 membrane.
[0108] The asymmetric crosslinking in this invention creates a crosslinking gradient between the bFGF immediate-release layer and the decellularized amniotic membrane compact layer, and between the VEGF sustained-release layer and the decellularized amniotic membrane compact layer. The VEGF sustained-release layer side has a high degree of crosslinking, and the collagen network is reinforced by amide bonds, thus resulting in a slow degradation rate. The bFGF immediate-release layer side has a low degree of crosslinking, maintaining a porous and loose structure, which is beneficial for cell ingrowth and substance exchange. The significance of the extended degradation window is that the membrane degradation cycle matches the continuous VEGF release cycle; VEGF is continuously released for 18.3 days, and the membrane degrades by only about 50% within 18.3 days, providing stable scaffold support for VEGF release and angiogenesis ingrowth.
[0109] Example 7: Cell compatibility evaluation.
[0110] 1. Experimental methods.
[0111] Membrane extract was prepared according to ISO 10993-5 standard. The membranes prepared in Example 4 were cut into 1cm × 1cm pieces and placed in serum-free culture medium for extraction at 37°C for 24 hours. The extraction ratio was 3 cm² / cm³ of membrane surface area to culture medium volume. 2 / mL calculation. Extracts were co-cultured with human immortalized epidermal cells (HACAT) and human umbilical vein endothelial cells (HUVEC), respectively. CCK-8 assays were performed on days 1, 3, and 7, with absorbance values measured at 450 nm.
[0112] Relative cell viability is expressed by the formula: ; in, Relative cell viability; The absorbance value of the experimental group at a wavelength of 450 nm; The absorbance value of the blank control group at a wavelength of 450 nm is shown.
[0113] 2. Experimental results.
[0114] The results of the relative cell viability test are shown in Table 8.
[0115] Table 8. Results of Cell Compatibility Evaluation
[0116] The relative cell viability of both cell types increased continuously with prolonged culture time, reaching 122.7% for HACAT and 131.3% for HUVEC on day 7, both exceeding 100% and showing no decreasing trend. These results indicate that the sheet extract is non-cytotoxic, and that the bFGF and VEGF released into the extract maintained their biological activity, exhibiting proliferative effects on both epidermal and endothelial cells. This result is consistent with the sustained release behavior of the two growth factors described in Table 4 of Example 4, demonstrating that the in vitro release process did not lead to the loss of the biological function of the growth factors.
[0117] In this invention, bFGF promotes epidermal cell proliferation and migration, while VEGF promotes endothelial cell proliferation and angiogenesis. Both growth factors in the patch-release system maintain their intact tertiary structure, enabling them to bind to corresponding receptors on the cell membrane surface and activate downstream proliferation signaling pathways. The increasing cell viability over time is consistent with the increasing cumulative release of growth factors, further validating the synergistic relationship between the release process and the maintenance of activity.
[0118] Example 8: Animal model repair experiment of diabetic foot ulcer.
[0119] 1. Modeling and Grouping Thirty New Zealand white rabbits were acclimatized for one week, and then diabetic diabetes was induced by intravenous injection of alloxan 180 mg / kg via the ear vein. Successful modeling was defined as a blood glucose level above 16.7 mmol / L that remained stable for two weeks. A 2.0 cm diameter full-thickness skin defect was created on the rabbit's back. The animals were randomly divided into three groups: Group A (blank control, n=10) had their wounds covered with saline gauze; Group B (D1 type membrane group, n=10) had their wounds treated with D1 type membranes; and Group C (the membrane group of this invention, n=10) had their wounds treated with the membrane of this invention, with the VEGF sustained-release layer of the membrane also applied to the wound.
[0120] The wound closure rate is expressed by the formula: ; in, Wound closure rate; This represents the initial wound area; for The area of the wound at any given time.
[0121] 2. Wound closure rate results.
[0122] The results of wound closure rate detection at each time point are shown in Table 9.
[0123] Table 9 Wound Closure Rate
[0124] On day 28, the wound closure rate of group C was 97.5%, which was about 25 percentage points higher than that of group A (72.3%) and about 9 percentage points higher than that of group B (88.6%). This indicates that the temporal biphasic release strategy of the membrane of the present invention has a better wound repair effect than the uniform mixing single-layer strategy of the D1 membrane.
[0125] 3. Histological evaluation.
[0126] On day 28, wound tissue was taken for HE staining and CD31 immunohistochemical staining. HE staining was used for inflammation scoring and epidermal reepithelialization scoring, while CD31 immunohistochemical staining was used for neovascularization density counting.
[0127] Inflammation scores were calculated on a scale of 0 to 3, with 0 indicating no inflammatory cell infiltration, 1 indicating mild inflammatory cell infiltration, 2 indicating moderate inflammatory cell infiltration, and 3 indicating severe inflammatory cell infiltration. Epidermal re-epithelialization scores were calculated on a scale of 0 to 4, with 0 indicating no re-epithelialization, 1 indicating epidermal hyperplasia at the wound margin, 2 indicating wound coverage less than 50%, 3 indicating wound coverage of 50% to 90%, and 4 indicating complete wound re-epithelialization. CD31-positive vessel density was expressed as the number of CD31-positive vessels per square millimeter of tissue.
[0128] The results of the histological evaluation are shown in Table 10.
[0129] Table 10 Histological evaluation results
[0130] The inflammation score in group C was 0.7, significantly lower than that in group A (2.4) and group B (1.5). The epidermal re-epithelialization score in group C was 3.4, significantly higher than that in group A (1.5) and group B (2.6). The CD31-positive vessel density in group C was 61.5 vessels per square millimeter, 3.4 times that of group A and 1.9 times that of group B. These results indicate that the membrane of this invention can effectively reduce wound inflammation, promote epidermal re-epithelialization, and stimulate angiogenesis.
[0131] In this invention, the bFGF immediate-release layer first releases basic fibroblast growth factor, which promotes fibroblast proliferation and granulation tissue formation in the early stages of wound repair. The VEGF sustained-release layer then continuously releases vascular endothelial growth factor, which promotes vascular endothelial cell proliferation and angiogenesis maturation after granulation tissue formation. The synergistic release of these two growth factors allows the wound repair process to proceed according to the physiological healing sequence. The VEGF sustained-release layer is directly applied to the wound, and the continuously released vascular endothelial growth factor penetrates into the wound bed, promoting angiogenesis. The bFGF immediate-release layer is located on the side away from the wound, and its released basic fibroblast growth factor acts on the wound edge epithelial cells and fibroblasts. The decellularized amniotic membrane acts as a barrier, preventing interference between the release of the two layers, while the unilateral laser micropores create a temporary exudate retention cavity on the wound side, reducing the maceration damage to the wound caused by exudate accumulation.
[0132] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors, characterized in that, It includes a decellularized amnion dense layer and a bFGF immediate-release layer and a VEGF sustained-release layer located on both sides of the decellularized amnion dense layer, respectively; The bFGF immediate-release layer contains gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor and an amniotic membrane ECM hydrogel framework. The VEGF sustained-release layer contains PLGA alginate composite microspheres loaded with vascular endothelial growth factor and an amniotic membrane ECM hydrogel framework. The release rate of basic fibroblast growth factor in the bFGF immediate-release layer is greater than that of vascular endothelial growth factor in the VEGF sustained-release layer.
2. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, The median volume diameter of the gelatin-chitosan composite microspheres is 1 μm to 3 μm, and the median volume diameter of the PLGA-alginic acid composite microspheres is 5 μm to 15 μm. The drug loading of the gelatin-chitosan composite microspheres is from 0.5 μg / mg to 2.0 μg / mg, and the drug loading of the PLGA-algin composite microspheres is from 1.0 μg / mg to 4.0 μg / mg.
3. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, The content of the gelatin-chitosan composite microspheres in the bFGF immediate-release layer is 20 mg / mL to 40 mg / mL, and the content of the PLGA-algin composite microspheres in the VEGF sustained-release layer is 30 mg / mL to 50 mg / mL.
4. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, Under in vitro release conditions in phosphate buffer, the ratio of the cumulative release rate of basic fibroblast growth factor to the cumulative release rate of vascular endothelial growth factor on day 3 was not less than 2.0, and the cumulative release rate of vascular endothelial growth factor on day 7 was not greater than 70%.
5. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, It also includes asymmetric cross-linked regions; The asymmetric cross-linked region is located between the bFGF immediate-release layer and the decellularized amnion dense layer, and between the VEGF sustained-release layer and the decellularized amnion dense layer. The degree of cross-linking in the asymmetric cross-linked region decreases from the VEGF sustained-release layer side to the bFGF immediate-release layer side.
6. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 5, characterized in that, The thickness of the bFGF immediate-release layer is 50 μm to 80 μm, the thickness of the decellularized amnion dense layer is 10 μm to 20 μm, and the thickness of the VEGF sustained-release layer is 50 μm to 100 μm; The degradation time of the membrane in phosphate buffer containing lysozyme with a remaining mass fraction of 50% is 15 to 25 days.
7. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, It also contains a freeze-drying protectant; The freeze-drying protectant contains trehalose, mannitol, and bovine serum albumin; The freeze-drying protectant contains trehalose at a mass concentration of 1% to 10%, mannitol at a mass concentration of 1% to 5%, and bovine serum albumin at a mass concentration of 0.1% to 1%.
8. The time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 1, characterized in that, It also includes unilateral laser micropores; The unilateral laser micropore is opened from one side of the VEGF sustained-release layer to the other side of the decellularized amnion dense layer, penetrates the VEGF sustained-release layer and extends through the asymmetric cross-linking region located between the VEGF sustained-release layer and the decellularized amnion dense layer, and terminates on the surface of the decellularized amnion dense layer without penetrating the decellularized amnion dense layer. The aperture of the single-sided laser micro-aperture is 200μm to 300μm, and the center-to-center distance between adjacent single-sided laser micro-apertures is 1mm to 2mm.
9. A method for preparing a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors, characterized in that, Includes the following steps: The amnion was decellularized to obtain a decellularized amnion; A portion of the decellularized amnion was used to prepare an amnion ECM hydrogel precursor, while a portion of the decellularized amnion was retained as a dense layer of the decellularized amnion. Prepare gelatin-chitosan composite microspheres loaded with basic fibroblast growth factor and PLGA-algin composite microspheres loaded with vascular endothelial growth factor. The gelatin-chitosan composite microspheres were mixed with the amniotic membrane ECM hydrogel precursor to obtain the bFGF immediate release layer composite solution. The PLGA alginate composite microspheres were mixed with the amniotic membrane ECM hydrogel precursor to obtain a VEGF sustained-release layer composite solution. Using the decellularized amnion dense layer as a separator, the VEGF sustained-release layer composite solution is cast onto the first surface of the decellularized amnion dense layer and gelled, and the bFGF rapid-release layer composite solution is cast onto the second surface of the decellularized amnion dense layer and gelled to obtain a wet film. The wet film is freeze-dried to obtain the film sheet.
10. The method for preparing a time-controlled release lyophilized amniotic membrane sustained-release membrane loaded with dual growth factors according to claim 9, characterized in that, The method also includes: The wet membrane was gradient crosslinked in MES buffer using EDC and NHS, such that the degree of crosslinking on the bFGF immediate release layer side was lower than that on the VEGF sustained release layer side. The gradient cross-linked wet film was immersed in a lyophilization protectant solution containing trehalose, mannitol and bovine serum albumin; The freeze-drying process employs programmed cooling freeze-drying. After freeze-drying, micropores are processed by laser from one side of the VEGF sustained-release layer to the other side of the decellularized amnion dense layer. The micropores penetrate the VEGF sustained-release layer and extend through the asymmetric cross-linking region between the VEGF sustained-release layer and the decellularized amnion dense layer, ending at the surface of the decellularized amnion dense layer without penetrating it. After processing, it is sterilized by gamma ray irradiation.