A hydrogel adhesive with photothermal performance and a preparation method and application thereof
By preparing a composite hydrogel of polyvinyl alcohol, gelatin, boric acid, tannic acid, gallic acid and polydopamine, the problem of strong adhesion and easy removal of hydrogel dressings at body temperature was solved. It achieved a synergistic enhancement of strong adhesion, rapid hemostasis and multiple functions, and is suitable for immediate repair and infection prevention of complex wounds.
Patent Information
- Application Number
- CN202611065781.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-17
- Publication Date
- 2026-11-24
AI Technical Summary
Existing hydrogel dressings adhere firmly at body temperature but are prone to causing secondary trauma when removed. There is a lack of systems that can intelligently adjust the adhesion strength, resulting in limited hemostatic efficiency. Furthermore, they are insufficient in terms of temperature response, photothermal-assisted hemostasis, antibacterial or self-healing functions, making it difficult to meet the requirements for immediate repair and infection prevention of complex wounds.
A dual-network composite hydrogel was prepared by chemical crosslinking and hydrogen bond physical crosslinking. A combination of polyvinyl alcohol, gelatin, boric acid, tannic acid, gallic acid and polydopamine was used to form a multi-network system, which achieved temperature-sensitive adhesion and photothermal properties, and enhanced adhesion strength and hemostatic ability.
It achieves strong adhesion at body temperature and painless detachment under cold compress, possesses excellent mechanical properties and multiple synergistic enhancements, can rapidly coagulate blood, promote tissue regeneration, and has antibacterial and photothermal therapy capabilities.
Smart Images

Figure CN123148446A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically relating to a hydrogel adhesive with photothermal properties, its preparation method, and its application. Background Technology
[0002] Skin trauma, especially extensive burns, diabetic ulcers, and traumatic bleeding, often poses a clinical challenge due to infection, excessive inflammation, and slow healing. Traditional dressings such as gauze and sponges only provide a physical barrier and lack adhesion, hemostasis, and active anti-infection capabilities, making them unsuitable for repairing complex wounds. Ideal medical dressings should achieve immediate and strong adhesion in a moist and dynamic environment, while also possessing multiple functions such as antibacterial, antioxidant, and tissue regeneration promotion.
[0003] Hydrogels, with their three-dimensional network structure, high water content, and extracellular matrix-like properties, have become an ideal platform for wound repair. However, existing hydrogel dressings still face the following key challenges in practical applications: the contradiction between adhesion and on-demand detachment—most strongly adhesive hydrogels adhere firmly at body temperature but are prone to causing secondary trauma upon removal, and there is a lack of systems capable of intelligently adjusting adhesion strength; limited hemostatic efficiency—traditional dressings or existing hydrogels mainly rely on physical adsorption, which cannot rapidly coagulate blood proteins or provide on-demand hemostasis; and insufficient performance of existing hydrogels in terms of temperature response, photothermal-assisted hemostasis, antibacterial properties, or self-healing functions, making it difficult to meet the requirements for immediate repair and infection prevention of complex wounds.
[0004] Therefore, developing a hydrogel adhesive that can simultaneously achieve strong adhesion at body temperature, painless detachment under cold compresses, and synergistic enhancement of multiple functions remains a technical challenge that urgently needs to be solved in this field. Summary of the Invention
[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.
[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a hydrogel adhesive with photothermal properties, its preparation method, and its application.
[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solutions, including: Polyvinyl alcohol and deionized water are mixed to obtain solution A; gelatin and deionized water are mixed to obtain solution B. Boric acid and deionized water are mixed evenly to obtain solution C; tannic acid and gallic acid are mixed evenly with deionized water to obtain solution D. Dopamine hydrochloride was dissolved in a buffer solution and stirred at room temperature; the sample was centrifuged, washed with deionized water, and then freeze-dried to obtain polydopamine particles, which were then mixed with deionized water and sonicated to obtain solution E. Solution A and solution B are mixed and stirred until homogeneous to obtain solution F. Solution C, solution D and solution E are added dropwise to solution F in sequence and stirred to form a homogeneous solution. After standing, the solution is frozen and then thawed at room temperature. The freeze-thaw cycle is repeated twice to obtain a hydrogel adhesive with photothermal properties.
[0009] In a preferred embodiment of the preparation method of the hydrogel adhesive with photothermal properties described in this invention, the mass fraction of polydopamine in the solution E is 1.5~1.6%.
[0010] In a preferred embodiment of the preparation method of the photothermal hydrogel adhesive of the present invention, the following is provided: the mass fraction of polyvinyl alcohol in solution A is 17-18%; the mass fraction of gelatin in solution B is 8-9%; the mass fraction of boric acid in solution C is 0.7-0.8%; and the mass fraction of tannic acid and gallic acid in solution D is 1-2%.
[0011] In a preferred embodiment of the preparation method of the hydrogel adhesive with photothermal properties described in this invention, the stirring is carried out at a speed of 250-300 rpm, a temperature of 40-50°C, and a time of 30-40 min.
[0012] In a preferred embodiment of the preparation method of the hydrogel adhesive with photothermal properties described in this invention, the freezing time is 12-13 hours and the thawing time is 0.5-1 hour.
[0013] Another object of the present invention is to overcome the shortcomings of the prior art and provide a temperature-sensitive hydrogel adhesive with photothermal properties.
[0014] As a preferred embodiment of the photothermal hydrogel adhesive of the present invention, the hydrogel adhesive has a tensile strength of 111~181 kPa and an elongation at break of 327.94~414.62%. The hydrogel adhesive exhibits an adhesion strength of 7.3~9.2 kPa at 25°C and 11.5~16.0 kPa at 37°C. The hydrogel adhesive can raise its temperature to 72.4°C within five minutes, and the equilibrium temperature remains stable at 57.3°C throughout five cycles.
[0015] The third objective of this invention is to overcome the shortcomings of the prior art and provide an application of a temperature-sensitive hydrogel adhesive with photothermal properties in medical dressings.
[0016] Beneficial effects of this invention: This invention creatively prepares a dual-network composite hydrogel through chemical crosslinking and hydrogen bond physical crosslinking. The method is simple to operate, and the hydrogel obtained has excellent mechanical properties: tensile strength not less than 0.1 MPa and elongation at break not less than 300%; the adhesion properties are adjustable: at 37℃, the adhesion strength on pigskin can reach 16.0 kPa; at 25℃, the adhesion strength decreases, which can achieve non-damaging and painless peeling. Attached Figure Description
[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 These are scanning electron microscope (SEM) images of Examples 1-5 and Comparative Example 1 of the present invention, wherein... Figure 1 (a) is Comparative Example 1; Figure 1 (b) to (e) are scanning electron microscope images of Examples 1 to 5.
[0018] Figure 2 The bar chart shows the tensile strength-elongation at break of the composite hydrogels in Examples 1-5 and Comparative Example 1 of this invention.
[0019] Figure 3 This is a schematic diagram of the adhesion of the present invention on different substrates in Embodiment 3.
[0020] Figure 4 The above are bar charts showing the adhesion strength of Examples 1-5 and Comparative Example 1 of the present invention, wherein... Figure 4 (a) A bar chart showing the adhesion strength of the composite hydrogels of Comparative Example 1 and Examples 1-5 at 25°C and 37°C; Figure 4 (b) is a bar chart of the adhesion strength of Example 3 on different substrates.
[0021] Figure 5 This is a bar chart showing the adhesion strength of Embodiment 3 of the present invention after ten cycles of adhesion to different substrates at 25°C and 37°C.
[0022] Figure 6 These are near-infrared radiation data graphs for Embodiments 1-5 and Comparative Example 1 of the present invention. Figure 6(a) is the heating rate curve of the composite hydrogels of Comparative Example 1 and Examples 1-5 under near-infrared light source irradiation at 808 nm; Figure 6 (b) represents five cycles of heating and cooling under near-infrared radiation in Example 3.
[0023] Figure 7 This is a schematic diagram showing the temperature rise of the composite hydrogels of Comparative Example 1 and Examples 1-5 of the present invention under near-infrared light source irradiation at 808nm for 0s, 150s, and 300s.
[0024] Figure 8 The diagram shows the heating rate curve of the composite hydrogel of Comparative Example 2 of this invention under near-infrared light irradiation at 808nm, as well as heating diagrams at 0s, 150s, and 300s. Detailed Implementation
[0025] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0026] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0027] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0028] Unless otherwise specified, all raw materials used in this invention are commercially available.
[0029] The abbreviations of the substances in this invention are as follows: Polyvinyl alcohol (PVA), gelatin, boric acid (B), tannic acid (TA), gallic acid (GA), polydopamine (PDA).
[0030] The raw materials and specifications used in the embodiments of the present invention are shown in Table 1 below: Table 1
[0031] The materials obtained in the embodiments of the present invention were subjected to performance testing according to the following method: Scanning electron microscopy (SEM): The prepared hydrogels were grouped, pre-frozen at -40℃, and then freeze-dried. The dried samples were quenched with liquid nitrogen and their morphological characteristics were recorded using SEM. Gold was sputtered evenly and the accelerating voltage was 3.0 kV.
[0032] Tensile stress-strain performance testing: For tensile testing, the hydrogel sample was cut into dumbbell-shaped pieces. Following the testing standard GB1040-79, the tensile rate was set to 50 mm / min, and the stress-strain relationship of the hydrogel was recorded using a universal testing machine. Strain is the ratio of the sample length at the end of the test to the initial sample length, and stress is expressed as the ratio of force to the sample's cross-sectional area. Three replicate specimens were prepared for each group of samples.
[0033] Adhesion performance testing: Overlap shear tests were conducted using a universal testing machine (GOTECHAI-3000-U, China) to test adhesive strength. First, the substrates (glass plate, metal plate, rubber sheet, wood chip, pigskin) were cleaned three times with ethanol and deionized water and thoroughly dried at room temperature. The hydrogel was cut into 30mm × 25mm × 5mm samples. The hydrogel adhesive was then attached between two identical substrates and pressed with a 1kg weight for 5 minutes. The samples were then fixed on the universal testing machine and stretched at a speed of 5mm / min until the samples separated or broke. Each hydrogel was tested three times on different substrates. The adhesion strength was calculated by dividing the maximum load by the initial contact area.
[0034] Photothermal performance testing: Different samples were tested using a near-infrared photothermal imaging system, employing a near-infrared laser light source (808nm, 1W / cm²). 2 The hydrogel was irradiated for 300 seconds, and images were taken using a thermal imager to record the temperature changes in the photothermal response. The effects of near-infrared laser (808 nm, 1 W / cm²) on the hydrogel in Example 3 were also investigated. 2 The hydrogel was irradiated for 2 minutes, followed by a 2-minute rest period, and this process was repeated for 5 photothermal cycles to study its photothermal stability.
[0035] Example 1 This embodiment provides a method for preparing a hydrogel adhesive with photothermal properties, specifically as follows: 1) Preparation of solution A: Add 9g of polyvinyl alcohol to 41g of deionized water and stir at 90℃ for 3h to mix evenly to obtain a polyvinyl alcohol solution with a mass fraction of 18%, denoted as solution A; 2) Preparation of Solution B: Add 4.5g of gelatin to 45.5g of deionized water, stir at 50℃ for 1 hour to mix evenly, and obtain a gelatin solution with a mass fraction of 9%, denoted as Solution B; 3) Preparation of solution C: Add 0.072g of boric acid to 9.928g of deionized water and mix well to obtain a boric acid solution with a mass fraction of 0.72%, which is denoted as solution C; 4) Preparation of solution D: Add 1.2g of tannic acid and 0.6g of gallic acid to 8.2g of deionized water, mix well to obtain a polyphenol solution with a mass fraction of 1.8%, and the ratio of tannic acid to gallic acid is 2:1, which is denoted as solution D; 5) Preparation of solution E: Dissolve dopamine hydrochloride at a concentration of 0.5 mg / mL in Tris buffer (10 mM, pH 8.5) and stir the solution at room temperature for 48 hours. Centrifuge the sample, wash it three times with deionized water, and then freeze-dry it to obtain polydopamine (PDA) particles. Add 0.156 g of PDA to 9.844 g of deionized water and sonicate for 10 min to obtain solution E.
[0036] 6) Preparation of solution F: Mix 5g of solution A and 5g of solution B, stir and mix evenly at 45℃. The mass fraction of PVA in the solution is 9% and the mass fraction of gelatin is 4.5%. This solution is denoted as solution F. 7) Then, 1g of solution C, 1g of solution D, 333μL of solution E and 667μL of deionized water were added dropwise to solution F to make the PDA content in the final hydrogel 0.04wt%. The reaction was carried out at 45℃ for 40min to obtain Gel-PVA-B-T2G1 / 0.04PDA gel solution. The gel solution was poured into a petri dish and frozen at -20℃ for 12h. Then, it was thawed at 20℃ for 0.5h. The freeze-thaw cycle was repeated twice to obtain Gel-PVA-B-T2G1 / 0.04PDA hydrogel (abbreviated as GPB-T2G1 / 0.04PDA).
[0037] Example 2 The difference between this embodiment and Example 1 is that the volume of solution E in step 7) is adjusted to 500 μL and the volume of deionized water is adjusted to 500 μL. The rest of the preparation process is the same as in Example 1, so that the content of PDA in the final hydrogel is 0.06 wt%, and Gel-PVA-B-T2G1 / 0.06PDA hydrogel (abbreviated as GPB-T2G1 / 0.06PDA) is obtained.
[0038] Example 3 The difference between this embodiment and Example 1 is that the volume of solution E in step 7) is adjusted to 667 μL and the volume of deionized water is adjusted to 333 μL. The rest of the preparation process is the same as in Example 1, so that the content of PDA in the final hydrogel is 0.08 wt%, and Gel-PVA-B-T2G1 / 0.08PDA hydrogel (abbreviated as GPB-T2G1 / 0.08PDA) is obtained.
[0039] Example 4 The difference between this embodiment and Example 1 is that the volume of solution E in step 7) is adjusted to 833 μL and the volume of deionized water is adjusted to 167 μL. The rest of the preparation process is the same as in Example 1, so that the content of PDA in the final hydrogel is 0.1 wt%, and Gel-PVA-B-T2G1 / 0.1PDA hydrogel (abbreviated as GPB-T2G1 / 0.1PDA) is obtained.
[0040] Example 5 The difference between this embodiment and Example 1 is that the volume of solution E in step 7) is adjusted to 1000 μL and the volume of deionized water is 0 μL. The rest of the preparation process is the same as in Example 1, so that the content of PDA in the final hydrogel is 0.12 wt%, and Gel-PVA-B-T2G1 / 0.12PDA hydrogel (abbreviated as GPB-T2G1 / 0.12PDA) is obtained.
[0041] Comparative Example 1 The difference between this embodiment and Example 1 is that the volume of solution E in step 7) is adjusted to 0 μL and the deionized water is 1000 μL. The rest of the preparation process is the same as in Example 1, and GPB-T2G1 / OPDA hydrogel (abbreviated as GPB-T2G1) is obtained.
[0042] Comparative Example 2 The difference between this embodiment and embodiment 3 is that 1g of solution D in step 7) is replaced with an equal amount of deionized water. The rest of the preparation process is the same as in embodiment 3, and Gel-PVA-B / 0.08PDA hydrogel (abbreviated as GPB-0.08PDA) is obtained.
[0043] Comparative Example 3 The difference between this embodiment and Example 1 is that in step 7), 1g of solution D is replaced with an equal amount of deionized water, and 0μL of solution E and 1000μL of deionized water are added. The rest of the preparation process is the same as in Example 1, and Gel-PVA-B hydrogel (abbreviated as GPB) is obtained.
[0044] The microstructure of the hydrogels prepared in the above examples and Comparative Example 1 was characterized, and the results are as follows: Figure 1 As shown.
[0045] Figure 1 (a) to (f) are Comparative Example 1 and Examples 1 to 5, respectively. Figure 1 (a) It can be seen that the pure GPB-T2G1 hydrogel exhibits a three-dimensional porous network structure with uniform pore size and thin pore walls. From Figure 1(b) It can be seen that after adding PDA, the pore size of the hydrogel becomes smaller, the pore walls become thicker, the surface roughness gradually increases, and the network becomes denser. This proves that PDA, as an additional crosslinking point and rigid filler, increases the crosslinking density of the network, and the hydrogen bonding between PDA and gelatin and PVA enhances the degree of crosslinking of the hydrogel. Figure 1 As can be seen from (b) to (e), the internal structure of the composite hydrogels in Examples 1 to 5 also has a similar typical honeycomb structure. When PDA is added to 0.12%, the hydrogel exhibits a denser but potentially brittle morphology.
[0046] The mechanical properties of the hydrogels prepared in the above embodiments and comparative examples were tested, and the results are shown in Table 2 below.
[0047] Table 2
[0048] Figure 2 The effect of different PDA concentrations on the tensile properties of composite hydrogels; From Table 2 and Figure 3 As can be seen, the tensile properties of the examples are improved compared to Comparative Example 1. This is because the addition of PDA increases the tensile strength of the hydrogel, reaching 181 kPa when the PDA content is 0.1%, while the elongation at break decreases. As a nanofiller, PDA affects the movement of polymer chain segments. Its abundant phenolic hydroxyl groups are tightly cross-linked with PVA and gelatin through strong hydrogen bonds and hydrophobic interactions, enhancing the degree of cross-linking of the hydrogel and thus improving the tensile properties. Table 2 shows that Comparative Example 2, without the addition of TA / GA, has weaker mechanical properties compared to the examples. This is because TA / GA can fill the network and form a uniform high-density physical cross-linking, while PDA nanoparticles and borate ester bonds alone may not achieve the same reinforcing effect. Meanwhile, Comparative Example 3 has the lowest mechanical properties. This proves that PVA crystallization, gelatin chain entanglement, and borate dynamic ester bonds alone can form a soft and stretchable basic network, but the mechanical properties do not yet meet the requirements of medical dressings. It is through the subsequent gradual introduction of TA / GA and PDA that the synergistic enhancement of mechanical properties is achieved.
[0049] The adhesion properties of the hydrogels prepared in Examples 1-3 and Examples 1-5 were tested at different temperatures using a universal testing machine. The adhesion strength results on pigskin are shown in Table 3 below.
[0050] Table 3
[0051] Figure 3 This is a schematic diagram illustrating the adhesion of hydrogel adhesives on different substrates. Figure 3As can be seen, the hydrogel adhesive prepared by this invention can adhere to substrates such as wood, plastic, rubber, iron sheet, glass, and pigskin. Figure 4 (a) is a bar chart of the adhesion strength of Comparative Examples 1 and Examples 1-5 at 25°C and 37°C. (From Table 3 and...) Figure 4 It was found that all hydrogel adhesives exhibited stronger adhesion at 37°C than at 25°C. This indicates that when the temperature approaches body temperature, due to the temperature-responsiveness of gelatin, the triple helix structure of gelatin unfolds, exposing more amino, hydroxyl, and carboxyl groups. These groups form ionic and hydrogen bonds with amino and carboxyl groups on the substrate surface, thereby improving the adhesion performance of the hydrogel adhesive. When the temperature decreases (25°C), the gelatin chains re-entangle, weakening the interfacial bonding with the skin surface. The number of active groups in the hydrogel decreases, resulting in weaker adhesion and easier removal of the hydrogel adhesive. Meanwhile, compared to Comparative Example 1, the addition of PDA improved the adhesion of the hydrogel adhesive. This is because the addition of PDA increases the crosslinking density and cohesive energy of the hydrogel; it also introduces more phenolic hydroxyl groups, increasing surface adhesion and thus improving the adhesion performance of the hydrogel. When the PDA concentration was 0.08%, the adhesion to wood in Example 3 was optimal, at 18.7 kPa. Table 3 shows that the absence of TA / GA in Comparative Example 2 affects the adhesion strength of the hydrogel. The adhesion strength of the examples is higher than that of Comparative Example 2. This is because the phenolic hydroxyl groups of TA / GA synergistically form denser hydrogen bonds and hydrophobic interactions with the catechol of PDA at the tissue interface, significantly enhancing the interfacial adhesion energy. Meanwhile, the adhesion strength of Comparative Example 3 is the lowest. This indicates that without the interfacial hydrogen bonds and hydrophobic interactions provided by polyphenolic substances (TA / GA / PDA), the adhesion force relying solely on the hydroxyl / amino groups of gelatin and PVA is very limited. The above performance comparison demonstrates that the technical solution of this invention is not a simple superposition of existing components, but rather significantly enhances the cohesive strength and adhesion performance of the hydrogel by forming a synergistic polyphenol cross-linking functional network through TA / GA and PDA.
[0052] Figure 5 This is a bar chart showing the adhesion strength of Example 3 after ten cycles of adhesion to different substrates at 25°C and 37°C. Figure 5 It is known that the adhesion strength of GPB-T2G1 / 0.08PDA hydrogel to all materials is relatively stable. This is attributed to the multiple reversible hydrogen bonds formed between the abundant catechol groups in PDA and TA / GA and the surface proteins of the tissue, which dissociate during peeling and can be rapidly rebuilt upon re-contact.
[0053] Figure 6 (a) is at 1W / cm 2 Heating rate curves of hydrogels with different PDA contents under near-infrared light irradiation at 808 nm, from Figure 6 , Figure 7It can be seen that, under 808 nm near-infrared laser irradiation, the temperature of Comparative Example 1 (GPB-T2G1, without PDA) remained almost stable at 20.7℃ within five minutes, exhibiting almost no photothermal conversion capability. Compared to Comparative Example 1, with the addition of PDA, the temperature rise increased and the heating rate accelerated with increasing PDA concentration. Example 3 could raise its temperature to 72.4℃ within five minutes. This is attributed to the increased density of light-absorbing groups within the hydrogel, thereby converting more photon energy into heat energy. This proves that PDA is the key component for achieving efficient photothermal performance in the hydrogel of this invention. Figure 8 The photothermal performance of Comparative Example 2 shows that the temperature of Comparative Example 2 rises to 62.1°C within five minutes. Compared with Example 3, the temperature rise is lower. The phenolic hydroxyl groups of TA / GA form π-π stacks with PDA, which improves the dispersion state of PDA and reduces light scattering loss caused by agglomeration. This photothermal synergistic effect is a technical effect beyond the inherent performance of PDA. Figure 6 (b) shows five cycles of heating and cooling under near-infrared radiation for 2 minutes and 2 minutes respectively in Example 3. The results show that the equilibrium temperature of the hydrogel remained stable at 57.3°C throughout the five cycles without significant decrease. This excellent cyclic stability can be attributed to the high robustness of the PDA covalent cross-linked network. This photothermal conversion property is expected to enable rapid coagulation. For active bleeding wounds, the thermal effect generated after irradiation can rapidly coagulate the blood proteins exudated from the wound, forming a physical barrier and assisting in hemostasis.
[0054] In summary, this invention creatively prepares interpenetrating network composite hydrogels through chemical crosslinking and electrostatic physical crosslinking. First, aqueous solutions of tannic acid, gallic acid, polydopamine, and boric acid of specific concentrations are prepared for later use. Then, a mixed solution of polyvinyl alcohol and gelatin in a specific ratio is prepared. Next, a certain proportion of tannic acid, gallic acid, polydopamine, and boric acid solutions are added dropwise. Finally, the solution is transferred to a petri dish, allowed to stand, and then frozen in a -20°C freezer. It is then thawed at room temperature (20°C) and the freeze-thaw cycle is repeated twice to obtain Gel-PVA-B-T2G1 / PDA hydrogel.
[0055] This hydrogel adhesive constructs a multi-network system synergistically integrated with dynamic covalent bonds, supramolecular physical interactions, and biomimetic interfacial bonding. Polyvinyl alcohol and gelatin form the basic mechanical framework through hydrogen bonds and interchain entanglement. Boric acid forms reversible boronic acid ester dynamic covalent bonds with the cis-diol structures of polyvinyl alcohol and polyphenolic components, endowing the material with self-healing capabilities and shear-thinning properties, while also acting as sacrificial bonds to effectively dissipate energy during interfacial peeling. Tannic acid / gallic acid and polydopamine construct a high-density physical cross-linking network through dense hydrogen bonds, π-π stacking, and hydrophobic association, further enhancing the cohesive strength of the hydrogel. When the hydrogel comes into contact with tissue, the catechol groups of polydopamine are oxidized to highly reactive quinones, which undergo Michael addition and Schiff base reactions with the amino or thiol groups of proteins on the tissue surface, forming irreversible covalent anchoring. Simultaneously, unoxidized catechol also assists adhesion through hydrogen bonds and hydrophobic interactions, thereby achieving strong wet adhesion even under the flushing of blood and tissue fluid. It is worth noting that the chemical adhesion reaction rate exhibits a significant temperature dependence, accelerating markedly at body temperature (37°C), thus ensuring good handling convenience at room temperature, while the adhesion strength spontaneously increases in physiological environments. Furthermore, the highly conjugated structure of polydopamine endows the hydrogel with broad-spectrum near-infrared absorption capabilities. Under 808nm laser irradiation, it efficiently generates a localized thermal field through non-radiative relaxation, which can not only rapidly coagulate blood proteins for synergistic hemostasis but also kill bacteria through thermal effects, enabling on-demand and controllable photothermal therapy. In summary, this system integrates strong wet adhesion, dynamic energy dissipation, temperature-sensitive response, and photothermal function through multiple synergistic mechanisms, and is expected to overcome the limitations of traditional medical adhesives in humid and dynamic environments.
[0056] This invention has found that in the process of preparing polyvinyl alcohol-gelatin-boric acid-tannic acid / gallic acid / polydopamine composite hydrogel based on the aforementioned optimized conditions of polyvinyl alcohol-gelatin solution, when the PDA concentration is 0.08wt%, the resulting GPB-T2G1 / 0.08PDA composite hydrogel can simultaneously achieve the following properties: (1) good adhesion performance, reaching a maximum of 18.7kPa; (2) excellent mechanical properties: tensile strength can reach 166KPa, and elongation at break can reach 400.96%. At the same time, due to the temperature responsiveness of gelatin, the hydrogel adhesive can achieve good adhesion to the skin at body temperature when the temperature drops from 37℃ to 25℃, and can be easily and non-damagingly peeled off by means of cold compresses and ice packs.
[0057] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a hydrogel adhesive with photothermal properties, characterized in that: include, Polyvinyl alcohol and deionized water are mixed to obtain solution A; gelatin and deionized water are mixed to obtain solution B. Boric acid and deionized water are mixed evenly to obtain solution C; tannic acid and gallic acid are mixed evenly with deionized water to obtain solution D. Dopamine hydrochloride was dissolved in a buffer solution and stirred at room temperature; the sample was centrifuged, washed with deionized water, and then freeze-dried to obtain polydopamine particles, which were then mixed with deionized water and sonicated to obtain solution E. Solution A and solution B are mixed and stirred until homogeneous to obtain solution F. Solution C, solution D and solution E are added dropwise to solution F in sequence and stirred to form a homogeneous solution. After standing, the solution is frozen and then thawed at room temperature. The freeze-thaw cycle is repeated twice to obtain a hydrogel adhesive with photothermal properties.
2. The preparation method according to claim 1, characterized in that: The mass fraction of polydopamine in solution E is 1.5-1.6%.
3. The method for preparing the hydrogel adhesive with photothermal properties as described in claim 1, characterized in that: The mass fraction of polyvinyl alcohol in solution A is 17-18%; the mass fraction of gelatin in solution B is 8-9%; the mass fraction of boric acid in solution C is 0.7-0.8%; and the mass fraction of tannic acid and gallic acid in solution D is 1-2%.
4. The preparation method according to claim 1, characterized in that: The stirring process includes a stirring speed of 250-300 rpm, a stirring temperature of 45-50℃, and a stirring time of 30-40 min.
5. The preparation method according to claim 1, characterized in that: The freezing time in each of the two freeze-thaw cycles is 12-13 hours, and the thawing time is 0.5-1 hour.
6. A hydrogel adhesive prepared by any one of the preparation methods described in claims 1 to 5.
7. The hydrogel adhesive as described in claim 6, characterized in that: The hydrogel adhesive has a tensile strength of 111~181 kPa and an elongation at break of 327.94~414.62%.
8. The hydrogel adhesive as described in claim 6, characterized in that: The hydrogel adhesive exhibits an adhesion strength of 7.3~9.2 kPa at 25°C and 11.5~16.0 kPa at 37°C.
9. The hydrogel adhesive as described in claim 6, characterized in that: The hydrogel adhesive can maintain a stable equilibrium temperature of 57.3°C throughout 5 cycles.
10. The application of the hydrogel adhesive as described in claim 6 in medical dressings.