Degradable embolic agents for intracranial aneurysms and methods of making and using the same

By combining lipoic acid and lipoic acid-N-hydroxysuccinimide ester in the polyethylene glycol 400 solvent system with PEG block copolymer, a biodegradable intracranial aneurysm embolizing agent is formed, which solves the problems of high viscosity, uncontrollable curing and poor biocompatibility of existing embolizing agents, and achieves a safe and dense embolization effect.

CN123148447APending Publication Date: 2026-11-24ZHUJIANG HOSPITAL OF SOUTHERN MEDICAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611655500.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing intracranial aneurysm embolizing agents have high viscosity, are difficult to inject, have uncontrollable solidification, poor tissue adhesion, poor biocompatibility, and are non-degradable, resulting in a high risk of complications and making it difficult to achieve dense and safe embolization.

Method used

Using polyethylene glycol 400 as a solvent, thioctic acid and thioctic acid-N-hydroxysuccinimide ester are combined with PEG block copolymer to form a biodegradable embolic agent through dynamic disulfide bonds and covalent bonds. Combined with a developer, it achieves rapid curing and adhesion, and leaves no toxic residue after degradation.

Benefits of technology

It has developed a low-toxicity, biodegradable embolic agent that can be injected through a microcatheter, solidify into a block, and adhere tightly to the blood vessel wall, reducing the risk of complications and making it suitable for minimally invasive treatment of intracranial aneurysms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148447A_ABST
    Figure CN123148447A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of medical materials technology, specifically relating to a biodegradable embolizing agent for intracranial aneurysms, its preparation method, and its application. The biodegradable embolizing agent for intracranial aneurysms is prepared from the following components: per 1 mL of polyethylene glycol 400 (by volume), 0.1-0.3 g of thioctic acid, 0.007-0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.1-0.3 g of PEG block copolymer, and 0.4-0.5 g of contrast agent. The biodegradable embolizing agent for intracranial aneurysms provided by this invention has the advantages of being non-toxic, non-drifting, biodegradable, and highly safe, effectively embolizing intracranial aneurysms and providing a novel solution for intracranial aneurysm embolization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of medical materials technology, specifically relating to a biodegradable embolizing agent for intracranial aneurysms, its preparation method, and its application. Background Technology

[0002] Intracranial aneurysms are abnormal bulges in the walls of intracranial arteries and are the leading cause of subarachnoid hemorrhage. Currently, endovascular interventional therapy has become the first-line treatment for intracranial aneurysms. Endovascular interventional techniques mainly include coil embolization, stent-assisted coil embolization, and dense-mesh stent implantation. However, these mechanical treatments have limitations: they cannot achieve immediate and complete occlusion of the aneurysm cavity, there is a possibility of recanalization or delayed rupture after the procedure, and the procedures are complex and expensive. In contrast, liquid embolic agents can conform to the irregular shape of the aneurysm cavity, achieving more uniform and denser occlusion, thus possessing irreplaceable advantages in the treatment of complex aneurysms.

[0003] Currently, the main liquid embolizing agents used in clinical practice include n-butyl N-cyanoacrylate (NBCA) and Onyx (ethylene-vinyl alcohol copolymer, EVOH). While NBCA provides strong embolization, it suffers from drawbacks such as difficulty in precisely controlling the polymerization rate, a high risk of "tube adhesion," and stringent technical requirements. Onyx, on the other hand, faces safety challenges due to the use of dimethyl sulfoxide (DMSO) as an organic solvent—DMSO injection into blood vessels can induce severe vasospasm, local vascular wall necrosis, and its volatility can lead to systemic toxicity, even causing serious complications such as arrhythmia and pulmonary edema. Previous experiments in a porcine wide-necked aneurysm model showed that when experienced interventional neurologists used Onyx for embolization, all animals experienced leakage of the liquid embolizing material from the aneurysm into the parent artery and downstream vessels, resulting in non-targeted embolization. Furthermore, none of the above-mentioned embolizing agents are biodegradable, and long-term retention in the body may induce chronic inflammatory responses. Therefore, the development of a novel, low-toxicity, biodegradable liquid embolizing agent has significant clinical value.

[0004] In recent years, novel liquid embolization agents for intracranial aneurysms have become a research hotspot. Jensen et al. (Jensen, MM, et al., Protein-based polymer liquid embolics for cerebral aneurysms. Acta Biomaterialia, 2022, 151: p. 174-182.) developed a temperature-responsive liquid embolization agent based on a silk fibroin-elastin composite polymer (SELP815K), achieving an occlusion rate of over 90% in a rabbit elastase aneurysm model. However, there is a risk of partial recanalization due to embolism contraction or aneurysm dilation. Baidya et al. (Baidya, A., et al., ACohesive Shear-Thinning Biomaterial for Catheter-Based Minimally Invasive Therapeutics. ACS Applied Materials & Interfaces, 2022. 14(38): p. 42852-42863.) prepared cohesive shear-thinning biomaterials (pGLs) by enhancing electrostatic interactions and demonstrated their integrity under physiological pulsatile flow in a patient-derived intracranial aneurysm model, providing a new approach to resolving the contradiction between "injectability and mechanical integrity" in shear-thinning hydrogels. However, the aforementioned shear-thinning gels all rely on single physical interactions such as hydrogen bonding, electrostatic interaction, and temperature response to construct networks, resulting in insufficient mechanical stability under dynamic blood flow impact; their high viscosity makes them difficult to pass through 1.7F neurointerventional microcatheters, limiting their application in neurointerventional therapy. Summary of the Invention

[0005] The purpose of this invention is to provide a biodegradable embolizing agent for intracranial aneurysms, its preparation method and application, to solve the technical problems of high viscosity, difficulty in injection, uncontrollable solidification, poor tissue adhesion, poor biocompatibility and non-degradability of existing intracranial aneurysm embolizing agents, so as to achieve dense and safe embolization of intracranial aneurysms, reduce the risk of complications and meet the needs of clinical treatment.

[0006] According to a first aspect of the invention, a biodegradable embolizing agent for intracranial aneurysms is provided, which is prepared from the following components: based on the volume of polyethylene glycol 400, per 1 mL of polyethylene glycol 400, 0.1-0.3 g of thioctic acid, 0.007-0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.1-0.3 g of PEG block copolymer, and 0.4-0.5 g of contrast agent.

[0007] In some embodiments, the biodegradable embolizing agent for intracranial aneurysms is prepared from the following components: per 1 mL of polyethylene glycol 400, 0.1-0.2 g of thioctic acid, 0.007-0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.2-0.3 g of PEG block copolymer, and 0.4-0.5 g of contrast agent.

[0008] In some embodiments, the biodegradable embolizing agent for intracranial aneurysms is prepared from the following components: per 1 mL of polyethylene glycol 400, 0.2 g of thioctic acid, 0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.2 g of PEG block copolymer, and 0.45 g of contrast agent.

[0009] In some embodiments, the PEG block copolymer is selected from PLGA-PEG-PLGA triblock copolymers and / or PDLLA-PEG-PDLLA triblock copolymers. When the PEG block copolymer is selected from PLGA-PEG-PLGA triblock copolymers, the molar ratio of lactide to glycolide in the PLGA segments is 50:50, the number average molecular weight of the PLGA segments is 3000-10000, and the number average molecular weight of the PEG segments is 1000-2000; preferably, PLGA4000-PEG1500-PLGA4000.

[0010] In some embodiments, the developer is tantalum powder that can be dispersed in an organic solvent or PEG400 labeled with iodine at both ends; when the developer is tantalum powder, the particle size of the tantalum powder is 60-80 nm.

[0011] Polyethylene glycol 400 is the only organic solvent used in the preparation of biodegradable embolic agents. It does not use any of the following solvents: dimethyl sulfoxide, ethanol, N-methylpyrrolidone, dimethylformamide, and dimethylacetamide, thus fundamentally avoiding the risk of vascular toxicity.

[0012] When the biodegradable embolic agent provided by this invention comes into contact with blood, the PEG block copolymer diffuses into the blood through polyethylene glycol 400 and rapidly solidifies into a strip shape; polythioctic acid imparts flexibility and self-fusion ability to the strip colloid through dynamic disulfide bonds, and the strips fuse into a block after contact, and further infiltrate with polyethylene glycol 400 to complete deep curing; thioctic acid-N-hydroxysuccinimide ester inhibits the depolymerization of polythioctic acid chains and enhances the adhesion between the embolization body and the blood vessel wall by activating ester groups to form covalent bonds with amino groups of blood vessel wall tissue.

[0013] The core innovation of this invention lies in its two-component synergistic design: lipoic acid / lipoic acid-NHS ester provides tissue reactive adhesion and dynamic disulfide bond-mediated chemical cross-linking and self-fusion, endowing the embolic body with flexibility and dense packing ability; the PEG block copolymer achieves rapid physical curing through solvent exchange to form mechanical support, solidifying into strips upon contact with blood after exiting the catheter, effectively overcoming the defect of embolic agents being easily broken under blood flow. This invention is the first to integrate physical phase transformation into strips and dynamic chemical cross-linking into the same embolization system. Combining the low toxicity of PEG400 solvent with the convenient operation of glycerol-assisted delivery, it achieves comprehensive performance of non-toxic solvent, non-drift, degradable, dense packing, and high safety, effectively embolizing intracranial aneurysms and providing a novel solution for intracranial aneurysm embolization.

[0014] According to a second aspect of the present invention, a method for preparing the above-described biodegradable embolic agent for intracranial aneurysms is provided, comprising the following steps: S1. Dissolve lipoic acid and lipoic acid-N-hydroxysuccinimide ester in polyethylene glycol 400, and heat and stir at 80-120°C for 1-4 hours to obtain the first mixture; S2. Cool the first mixture to 60-70°C, add the PEG block copolymer, and stir for 0.5-2 hours to obtain the second mixture; S3. Cool the second mixture to room temperature, add the developer, mix well, and the biodegradable embolic agent is obtained.

[0015] According to a third aspect of the invention, the use of the above-described biodegradable embolic agent as a medical device for intracranial aneurysms is provided.

[0016] According to a fourth aspect of the present invention, a method for delivering the above-described biodegradable embolic agent is provided, comprising the following steps: (1) Before injecting the biodegradable embolic agent through the microcatheter, rinse the inner wall of the microcatheter with a biocompatible liquid to isolate moisture and reduce pushing resistance, and prevent premature solidification. (2) The biodegradable embolic agent was injected into the target aneurysm cavity through a microcatheter at an injection rate of 0.4 mL / min; (3) After contact with blood, the biodegradable embolic agent solidifies in situ through solvent exchange mechanism to form an embolus that adheres to the blood vessel wall.

[0017] In some embodiments, the biocompatible liquid in step (1) refers to one or more organic solvents that are non-irritating to blood vessels, do not cause hemolysis, and are soluble in blood, preferably glycerol or polyethylene glycol 400, and the amount used is 20 to 100 μL.

[0018] In some embodiments, the outer diameter of the microcatheter in step (1) is 1.7F-2.7F, preferably 1.7F.

[0019] The biodegradable embolic agent prepared by this invention has low viscosity and low injection resistance, making it easy to pass through microcatheters and avoiding catheter blockage, thus meeting the minimally invasive requirements of interventional treatment for intracranial aneurysms. Upon contact with blood, it undergoes stepwise solidification, first rapidly forming strip-shaped polymers, then fusing into blocks and further solidifying, ensuring uniform filling of the aneurysm cavity for dense embolization and preventing distal drift. The embolic agent has good tissue adhesion, adhering tightly to the vessel wall and reducing the risk of detachment. All core components exhibit excellent biocompatibility, with no significant inflammatory response, and can slowly degrade in vivo. The degradation products are metabolized and excreted by the body, avoiding residual substances that could cause complications. Combined with a specialized contrast agent, the injection process and embolization area can be clearly visualized via DSA digital subtraction angiography, facilitating precise clinical operation. Attached Figure Description

[0020] Figure 1 This is a schematic diagram illustrating the composition, preparation process, and application mechanism of the biodegradable embolic agent of the present invention. Among them, Figure 1 The diagram shows the preparation process of thioctic acid, thioctic acid-N-hydroxysuccinimide ester, PLGA-PEG-PLGA triblock copolymer, PEG400 and developer for the embolization agent. Figure 1 B in the diagram represents the application mechanism of the embolic agent being delivered to the aneurysm cavity via a microcatheter, where it undergoes in-situ strip formation, inter-strip fusion, and the formation of a block-shaped embolism in an aqueous environment.

[0021] Figure 2 The graph shows the injection performance test results of different formulations of embolic agents when injected through a microcatheter.

[0022] Figure 3 The figures show the test results of tube formation, self-fusion, and stepwise curing properties of different embolic agents in PBS at 37°C. Figure 3 In the figure, A represents the strip formation effect of Example 1 at the moment of tube exit, 3 seconds, 10 seconds, 30 seconds, and 60 seconds. Figure 3 B in the text represents comparative photographs of the strips and their morphology from Example 1, Example 2, Example 3, Example 4, Comparative Example 1, and Comparative Example 2. Figure 3 C in the image is a photograph of the intermittent injection test process in Example 1, used to show the status of the catheter orifice and the continuous ejection of material when injection is resumed after a pause. Figure 3 In this context, D represents the development results of Example 1, Example 2, Example 3, Example 4, Comparative Example 1, and Comparative Example 2 under DSA.

[0023] Figure 4 The graph shows the DSA development performance test results of the biodegradable embolic agent of the present invention under different developer conditions.

[0024] Figure 5 This image shows the in vitro embolization performance test results of the biodegradable embolic agent of this invention in a 3D-printed aneurysm model. (The image likely shows the results of the in vitro embolization performance test.) Figure 5 In the figure, A represents the photographs of Comparative Example 2, Example 3, Example 4, and Example 1 after embolization, used to show the dispersion or loss of the material in a fluid environment when different masses of PLGA-PEG-PLGA triblock copolymer are added to embolize lateral wall narrow carotid aneurysms (neck: 3.5 mm, length × width × height: 6.0 × 6.0 × 6.2 mm); Figure 5 B in the figure represents photographs of Comparative Examples 2, 3, 4, and 1 after embolization, used to show the dispersion or loss of materials in a fluid environment when different masses of PLGA-PEG-PLGA triblock copolymer are added to embolize wide carotid aneurysms at the base tip or bifurcation (neck: 5.5 mm, length 7.0 mm × width 7.0 mm × height 7.2 mm). Figure 5 In the figure, C represents the imaging result under DSA after embolization in Example 1 group.

[0025] Figure 6 This image shows the morphological stability test results of the biodegradable embolic agent of the present invention after continuous fluid flushing in a 3D printed aneurysm model.

[0026] Figure 7 This is a graph showing the in vitro biocompatibility evaluation results of the biodegradable embolic agent of the present invention. Among them, Figure 7 In the figure, A represents the results of the hemolysis experiment, and the groups include the positive control group, the negative control group, the Example 1 group, and the Example 4 group; Figure 7 B in the figure represents the results of the cytotoxicity experiment, and the groups include the positive control group, the negative control group, the extract of Example 1, and the extract of Example 4.

[0027] Figure 8 The graph shows the in vitro degradation performance test results of the biodegradable embolic agent of this invention.

[0028] Figure 9 This image shows the early local tissue compatibility evaluation results of the biodegradable embolic agent of this invention after subcutaneous application in rats. Figure 9 In Figure A, there are gross observation photos of the skin tissue of the Example 1 group and the blank surgical control group 3 and 7 days after subcutaneous injection; Figure 9 B in the image represents H&E staining photographs of skin tissue from the Example 1 group and the blank surgical control group 3 and 7 days after subcutaneous injection; Figure 9 C in the figure represents the H&E staining images of major organs in the Example 1 group and the blank surgical control group on the 3rd and 7th day after surgery. Detailed Implementation

[0029] The present invention will be further described in detail below with reference to specific embodiments. It is worth noting that the following embodiments are only for better explaining the content of the present invention and do not limit the scope of protection of the present invention. Process steps not disclosed in the embodiments are prior art. Unless otherwise specified, all raw materials are commercially available.

[0030] Unless otherwise specified, all raw materials used in the following examples are commercially available products or can be prepared by conventional methods in the art. The polyethylene glycol 400 is abbreviated as PEG400; the thioctic acid is abbreviated as LA; the thioctic acid-N-hydroxysuccinimide ester is abbreviated as LA-NHS; the PLGA-PEG-PLGA triblock copolymer is preferably PLGA4000-PEG1500-PLGA4000, wherein the number average molecular weight of the PLGA segments is approximately 4000, and the number average molecular weight of the PEG segments is approximately 1500.

[0031] Example 1 The formulation of the biodegradable embolic agent is as follows: Based on 1 mL of PEG400, the amounts of each component in this example are as follows: 0.20 g of lipoic acid, 0.014 g of lipoic acid-N-hydroxysuccinimide ester (LA-NHS), 0.20 g of PLGA4000-PEG1500-PLGA4000 triblock copolymer, 0.45 g of tantalum powder, and 1 mL of PEG400. The preferred particle size of the tantalum powder is 60-80 nm.

[0032] The preparation method of the biodegradable embolic agent is as follows: (1) Preparation of thioctic acid prepolymer: Weigh 0.20g thioctic acid and 0.014g LA-NHS, add them to 1mL PEG400, heat to 120℃ under inert gas protection and light protection, stir for 2 hours to allow thioctic acid to undergo ring-opening polymerization and form a polythioctic acid prepolymer solution containing dynamic disulfide bonds.

[0033] (2) Composition of block copolymers: Cool the mixture obtained in step (1) to 70°C, add 0.20g of PLGA4000-PEG1500-PLGA4000 triblock copolymer, and continue stirring for 1 hour to fully dissolve it and form a homogeneous composite system with the polythioctic acid prepolymer.

[0034] (3) Dispersion of developer: Cool the mixture obtained in step (2) to room temperature, add 0.45g of tantalum powder, and mix by mechanical stirring, vortex oscillation or homogenization to make the tantalum powder evenly dispersed, thus obtaining the biodegradable embolic agent of the present invention.

[0035] The embolic agent obtained in Example 1 is a black, flowable system at room temperature. Tantalum powder is relatively uniformly dispersed in the system, with no obvious agglomeration observed. This embolic agent can be dispensed through a microcatheter and rapidly forms flexible, strip-shaped colloids upon contact with 37°C PBS and anticoagulated blood. Multiple strip-shaped colloids can fuse at the interface upon contact, further forming a block-shaped embolus. This embolus maintains its integral morphology in an aqueous medium, and the injection path and occlusion area can be visualized under X-ray or DSA. The embolic agent obtained in Example 1 exhibits good overall performance in terms of injectability, strip-forming ability, inter-strip fusion, imaging effect, and erosion resistance.

[0036] Example 2: Low Thiooctanoic Acid Feed Formulation The difference between this embodiment and Example 1 is that the amount of thioctic acid added is 0.10g, the amount of LA-NHS added is 0.007g, and the remaining components and amounts are as follows: PLGA4000-PEG1500-PLGA4000 triblock copolymer 0.20g, tantalum powder 0.45g, PEG400 1mL.

[0037] The preparation method is the same as in Example 1.

[0038] The embolic agent obtained in Example 2 exhibited better flowability and lower microcatheter injection resistance at room temperature compared to Example 1. Upon contact with an aqueous medium, the strips formed a viscous colloid (non-strip-shaped), but the colloid's flexibility and self-supporting properties were lower than those of Example 1, resulting in slower inter-strip fusion and weaker mechanical support in the formed blocky embolic body. In a simulated aneurysm model, this formulation can be used for filling low-flow-rate or small-volume cavities, but its morphology retention under strong fluid scouring conditions is inferior to that of Example 1. These results indicate that when the amount of thioctic acid added is too low, the polythioctic acid dynamic network is insufficient, affecting inter-strip fusion and the overall stability of the embolic body.

[0039] Example 3: Low PLGA-PEG-PLGA Feed Rate Formulation The difference between this embodiment and Example 1 is that the amount of PLGA4000-PEG1500-PLGA4000 triblock copolymer fed is 0.10 g, and the remaining components and their amounts are as follows: 0.20 g of thioctic acid, 0.014 g of LA-NHS, 0.45 g of tantalum powder, and 1 mL of PEG400.

[0040] The preparation method is the same as in Example 1.

[0041] The embolic agent obtained in Example 3 can be injected via a microcatheter, with injection resistance similar to or slightly lower than that in Example 1. Upon contact with an aqueous medium, it forms a strip-like colloid, but its hardness and support are lower than in Example 1, resulting in a more porous internal structure of the embolus. In a 3D-printed aneurysm model, this formulation can achieve initial occlusion, but after continuous flushing, slight morphological depression or insufficient support may appear at the aneurysm neck. This result indicates that when the PLGA-PEG-PLGA dosage is reduced, the physical support network formed by solvent exchange curing is insufficient, affecting the erosion resistance of the embolus.

[0042] Example 4: Formulation with high PLGA-PEG-PLGA feed rate The difference between this embodiment and Example 1 is that the amount of PLGA4000-PEG1500-PLGA4000 triblock copolymer fed is 0.30g, and the remaining components and their amounts are as follows: 0.20g thioctic acid, 0.014g LA-NHS, 0.45g tantalum powder, and 1mL PEG400.

[0043] The preparation method is basically the same as in Example 1. However, due to the increase in the amount of PLGA-PEG-PLGA, the stirring time in step (2) can be appropriately extended to 1 to 2 hours to ensure that the block copolymer is fully dissolved.

[0044] The embolic agent obtained in Example 4 forms a relatively hard strip-shaped colloid upon contact with the aqueous medium. After curing, the embolus is denser than that of Example 1, exhibiting enhanced erosion resistance. However, due to the increased PLGA-PEG-PLGA dosage, the system viscosity and microcatheter injection resistance increase accordingly, resulting in a slight decrease in strip flexibility and rapid inter-strip fusion ability compared to Example 1. This formulation is suitable for cavity filling scenarios requiring high mechanical support, but Example 1 offers a more balanced approach between injectability and post-curing support.

[0045] Example 5: Formulation using iodinated polyethylene glycol as a developer The difference between this embodiment and Embodiment 1 is that iodinated polyethylene glycol is used instead of tantalum powder as the developer.

[0046] Based on 1 mL of PEG400, the amounts of each component in this example are as follows: 0.20 g of lipoic acid, 0.014 g of LA-NHS, 0.20 g of PLGA4000-PEG1500-PLGA4000 triblock copolymer, 0.45 g of iodinated polyethylene glycol, and 1 mL of PEG400.

[0047] The preparation method is basically the same as in Example 1, wherein the iodinated polyethylene glycol can be added at room temperature in step (3) or added together with the block copolymer in step (2).

[0048] The embolic agent obtained in Example 5 can be injected via a microcatheter. Upon contact with an aqueous medium, it forms a strip-shaped colloid and further fuses into a block. Due to the good compatibility between iodinated polyethylene glycol and the PEG400 system, this group of developing agents disperses relatively uniformly and is not prone to solid particle sedimentation after standing. However, this embolic agent does not have long-term developing capability under X-ray or DSA and is only used for short-term real-time observation of the injection path and embolization range. This example illustrates that, in addition to tantalum powder, iodine-containing developing polymers can also be used as developing components of the embolic agent of this invention. Iodine-containing developing polymers can be used as alternative developing components to tantalum powder and are suitable for scenarios requiring reduced risk of solid particle sedimentation. However, the developing time is short, and it is not used for long-term developing scenarios of the embolic agent.

[0049] Example 6: Formulation using PDLLA-PEG-PDLLA instead of PLGA-PEG-PLGA The difference between this embodiment and Example 1 is that the PLGA4000-PEG1500-PLGA4000 triblock copolymer is replaced with PDLLA4000-PEG1500-PDLLA4000 triblock copolymer. The remaining components and amounts are as follows: 0.20g lipoic acid, 0.014g LA-NHS, 0.20g PDLLA4000-PEG1500-PDLLA4000 triblock copolymer, 0.45g tantalum powder, and 1mL PEG400.

[0050] The preparation method is the same as in Example 1.

[0051] The embolic agent obtained in Example 6 can be injected via a microcatheter. Upon contact with an aqueous medium, it forms a strip-shaped colloid and further solidifies into a block. Compared to Example 1, the hydrophobic degradation segment of PDLLA-PEG-PDLLA exhibits a slower degradation rate, resulting in a relatively longer morphological retention time of the embolus in in vitro degradation experiments. This example illustrates that the biodegradable block copolymer in the system of this invention can adjust the mechanical retention time and degradation rate of the embolus by changing the type of hydrophobic segment.

[0052] Comparative Example 1: Formula without LA-NHS The difference between this comparative example and Example 1 is that LA-NHS is not added.

[0053] Based on 1 mL of PEG400, the amounts of each component in this comparative example are as follows: 0.20 g of lipoic acid, 0.20 g of PLGA4000-PEG1500-PLGA4000 triblock copolymer, 0.45 g of tantalum powder, and 1 mL of PEG400.

[0054] The preparation method is the same as in Example 1, but LA-NHS is not added in step (1).

[0055] The system obtained in Comparative Example 1 exhibits a certain viscosity shortly after preparation, but its storage stability and post-curing morphology retention are lower than those in Example 1. Upon contact with an aqueous medium, it forms a gel-like substance, but inter-strip fusion and subsequent morphological stability are poor; after continuous incubation or fluid flushing, it rapidly shows edge loosening or local dissociation. These results indicate that LA-NHS helps improve the stability of polythiooctanoic acid prepolymers and the morphology retention of emboli by inhibiting LA depolymerization.

[0056] Comparative Example 2: Formulation without PLGA-PEG-PLGA The difference between this comparative example and Example 1 is that the PLGA4000-PEG1500-PLGA4000 triblock copolymer is not added.

[0057] Based on 1 mL of PEG400, the amounts of each component in this comparative example are as follows: 0.20 g of lipoic acid, 0.014 g of LA-NHS, 0.45 g of tantalum powder, and 1 mL of PEG400.

[0058] The preparation method is the same as in Example 1, but only the steps of preparing the thioctic acid prepolymer and dispersing the developer are performed.

[0059] The system obtained in Comparative Example 2 exhibits localized gelation upon contact with an aqueous medium, but it is difficult to form a continuous strip-shaped colloid with self-supporting capabilities. In a fluid environment, it tends to flow or disperse in fragments, failing to stably accumulate and form a dense embolus. This result indicates that the PLGA-PEG-PLGA triblock copolymer is the key component for achieving the rapid strip formation and self-supporting embolus formation of the embolic agent of this invention upon contact with an aqueous medium.

[0060] Comparative Example 3: Formula with excessive lipoic acid dosage The difference between this comparative example and Example 1 is that the amount of thioctic acid added is 0.30g, the amount of LA-NHS added is 0.021g, and the remaining components and amounts are as follows: PLGA4000-PEG1500-PLGA4000 triblock copolymer 0.20g, tantalum powder 0.45g, PEG400 1mL.

[0061] The preparation method is the same as in Example 1.

[0062] The viscosity of the system obtained in Comparative Example 3 was significantly higher than that in Example 1, its fluidity at room temperature decreased, and the delivery resistance of the microcatheter increased significantly. In some cases, it became difficult to continuously inject or deliver smoothly through the microcatheter. This result indicates that excessive thioctic acid dosage can lead to excessive viscosity or excessive cross-linking of the system, thereby affecting the delivery performance of the microcatheter.

[0063] Comparative Example 4: Formulation with excessive PLGA-PEG-PLGA dosage The difference between this comparative example and Example 1 is that the amount of PLGA4000-PEG1500-PLGA4000 triblock copolymer fed is 0.40g, and the remaining components and amounts are as follows: lipoic acid: 0.20g, LA-NHS 0.014g, tantalum powder 0.45g, PEG400 1mL.

[0064] The preparation method is the same as in Example 1, but because the amount of PLGA-PEG-PLGA added is relatively high, the stirring time in step (2) can be extended to 1.5 to 2 hours to promote its full dissolution.

[0065] The embolic agent obtained in Comparative Example 4 forms a hard strip-shaped or block-shaped colloid upon contact with the aqueous medium. It exhibits strong support after curing, but significantly increases injection resistance, reducing the operability of manual injection via a microcatheter. Larger diameter catheters or mechanical injection devices are required when necessary. This result indicates that while excessive PLGA-PEG-PLGA dosage can improve post-curing support, it weakens the delivery performance of the microcatheter and is therefore not a preferred formulation in this invention.

[0066] Comparative Example 5: Formulation with excessively large tantalum powder particle size The difference between this comparative example and Example 1 is that the tantalum powder has a particle size of 1-6 μm and an amount of 0.45 g. The other components and their amounts are as follows: 0.20 g of thioctic acid; 0.014 g of LA-NHS; 0.20 g of PLGA4000-PEG1500-PLGA4000 triblock copolymer; and 1 mL of PEG400.

[0067] The preparation method is the same as in Example 1. However, due to the high particle size of tantalum powder, the stirring time in step (2) can be extended to 1.5 to 2 hours to promote its full dispersion.

[0068] The embolic agent obtained in Comparative Example 5 showed obvious sedimentation after being placed in a syringe for half an hour, and obvious tantalum powder aggregation was observed under X-ray or DSA. This comparative example illustrates that excessively large tantalum powder particle size weakens the uniformity of the embolic adhesive and increases the risk of solid particle sedimentation; therefore, it is not a preferred formulation of this invention.

[0069] Comparative Example 6: Formula without any developer The difference between this comparative example and Example 1 is that tantalum powder and iodinated polyethylene glycol and other developers are not added. The remaining components and amounts are as follows: 0.20 g of thioctic acid, 0.014 g of LA-NHS, 0.20 g of PLGA4000-PEG1500-PLGA4000 triblock copolymer, and 1 mL of PEG400.

[0070] The preparation method is the same as in Example 1.

[0071] The embolic agent obtained in Comparative Example 6 did not exhibit imaging ability under X-ray or DSA and was only used to compare the imaging effects of tantalum powder and iodine-containing imaging polymers. This comparative example illustrates that without the addition of tantalum powder and iodine-containing imaging polymers, the imaging effect of the embolic agent of the present invention is weak, and therefore it is not considered a preferred formulation of the present invention.

[0072] Experimental Example 1: Microcatheter Injection Performance Test This experiment was conducted to evaluate the injectability of different formulations of embolic agents delivered via neurointerventional microcatheters and to screen for preferred formulations that combine low injection resistance and post-curing support.

[0073] Experimental Groups: G1: Example 1, the amount of lipoic acid added was 0.20 g / mL PEG400; G2: Example 2, the amount of lipoic acid added was 0.10 g / mL PEG400; G3: Example 3, PLGA-PEG-PLGA feed amount is 0.10 g / mL PEG400; G4: Example 4, PLGA-PEG-PLGA feed amount is 0.30 g / mL PEG400; G5: Comparative Example 3, with lipoic acid dosage of 0.30 g / mL PEG400; G6: Comparative Example 4, PLGA-PEG-PLGA feed amount is 0.40 g / mL PEG400.

[0074] Experimental Method: Each group of embolic agents was taken and placed into a 1mL syringe, which was then connected to a neurointerventional microcatheter for injection force testing. The outer diameter of the microcatheter could be selected from 1.7F to 2.7F, preferably 1.7F; the length of the microcatheter could be selected from 100 to 150cm; and the injection rate could be selected from 0.2 to 1.0mL / min, preferably 0.4mL / min. The curve of the injection force changing with time during the injection process was recorded using a universal testing machine or a push force testing device. The results are as follows: Figure 2 As shown.

[0075] The results show that the formulation in Example 1 can be continuously injected via a microcatheter without significant blockage during injection, and the injection force is within the range suitable for manual or conventional mechanical injection. In Example 2, due to the lower amount of thioctic acid, the injection resistance is low, but the subsequent curing support is insufficient. In Example 3, due to the lower amount of PLGA-PEG-PLGA, the injection resistance is low, but the support after curing is insufficient. In Example 4, due to the higher amount of PLGA-PEG-PLGA, the injection resistance is increased compared to Example 1, but the support after curing is enhanced. In Comparative Example 3, due to the excessively high amount of thioctic acid, the system fluidity is significantly reduced, making it unsuitable for delivery via a microcatheter. In Comparative Example 4, due to the excessively high amount of PLGA-PEG-PLGA, the injection resistance is significantly increased, making it unsuitable for delivery via a microcatheter. These results indicate that the formulation in Example 1 achieves a good balance between injectability and post-curing support.

[0076] Test Example 2: Test of tube forming, self-fusion and step-by-step curing performance This experiment is used to evaluate whether the embolic agent of the present invention can rapidly form strips, fuse between strips, and form an integral embolus after contact with an aqueous medium.

[0077] Experimental Groups: G1: Example 1 group, preferred formulation; G2: Example 2 group, low thioctic acid feed dosage formulation; G3: Example 3, low PLGA-PEG-PLGA feed formulation; G4: Example 4, high PLGA-PEG-PLGA feed formulation; G5: Comparative Example 1, LA-NHS-free formula; G6: Comparative group 2, PLGA-PEG-PLGA-free formulation.

[0078] Experimental Method: The sample from Example 1 was loaded into a syringe and pushed into 37°C PBS via a microcatheter. The morphological changes after contact with the aqueous medium were observed. The state was recorded at the instant of dispensing, 3 seconds, 10 seconds, 30 seconds, and 60 seconds. The results are as follows: Figure 3 As shown in A in the figure. A comparison of the strip formation and morphology of Example 1, Example 2, Example 3, Example 4, Comparative Example 1, and Comparative Example 2 is shown below. Figure 3 As shown in B in the figure. Another example, Group 1, underwent intermittent injection testing: injection was administered via the microcatheter for 10 seconds, paused for 30 seconds, and then continued, observing for catheter blockage. Figure 3 As shown in C. The development effect under DSA was verified by immersion in PBS solution, as shown in Figure C. Figure 3 As shown in D in the diagram.

[0079] The results showed that in Example 1, a flexible strip-shaped colloid quickly formed after exiting the tube. Multiple strip-shaped colloids could fuse at the interface upon contact, further forming a monolithic block plug. Example 2 formed a softer semi-strip-shaped colloid, but the inter-strip fusion speed and post-curing support were lower than in Example 1, and it gradually dispersed upon contact with the aqueous medium. Example 3 formed strips, but the strip hardness and support were insufficient. Example 4 formed a harder strip-shaped colloid, but its flexibility and rapid fusion ability were slightly lower than in Example 1. Comparative Example 1 formed a certain gel-like structure, but its self-fusion ability was weak, and it quickly dispersed or broke apart upon contact with the aqueous medium. Comparative Example 2 struggled to form a stable, self-supporting strip-shaped colloid and easily deformed upon contact with the aqueous medium. Intermittent injection tests showed that Example 1 did not exhibit significant tube blockage after a pause and subsequent injection, indicating its potential suitability for intermittent delivery operations.

[0080] Experimental Example 3: Development Performance Test This experiment was used to evaluate the imaging ability of the embolic agent of the present invention under X-ray or DSA under different imaging conditions.

[0081] Experimental Groups: G1: Blank control group, with no liquid added; G2: Comparative Example 6, without developer added; G3: Example 1, the developer is nano tantalum powder; G4: Comparative Example 5, developer is micron-sized tantalum powder; G5: Example 5, the developer is iodinated polyethylene glycol; Experimental Method: Materials from each group were taken and loaded into syringes, and the development effect was observed under DSA. For further static observation of Group 1 (Example), Group 5 (Comparative Example), and Group 5 (Example), DSA development was preferably performed after 6 hours of standing to observe whether the developer showed significant sedimentation, aggregation, or uneven development. Results are as follows: Figure 4 As shown.

[0082] The results showed that comparative example group 6 exhibited weak development under DSA, making it difficult to clearly determine the material distribution. Example group 1, containing nano-tantalum powder, showed better developability and strip formation. Comparative example group 5 used micron-sized tantalum powder, which had a larger particle size and was difficult to disperse; after standing, it settled and aggregated, potentially leading to tube blockage. Example group 5, containing iodinated polyethylene glycol, also had good developability, and the developer had good compatibility with the PEG400 system, resulting in better development uniformity after standing. However, due to the good water solubility of iodinated polyethylene glycol, the developer might escape during solvent replacement, gradually reducing the developing effect over time. These results indicate that the preferred formulation of the embolic agent of this invention can achieve visualized delivery using nano-tantalum powder.

[0083] Experimental Example 4: Embolization Performance Testing in a 3D-Printed Aneurysm Model This experiment was used to evaluate the in-situ packing ability, tumor channel protection ability, and material loss prevention ability of the embolizing agent of the present invention in simulated aneurysm cavities.

[0084] Experimental Groups: G1: Blank model group, no embolic agent injected; G2: Example 1, preferred formulation; G3: Example 3, low PLGA-PEG-PLGA feed formulation; G4: Example 4, formulation with high PLGA-PEG-PLGA feed rate; G5: Comparative Example 2, PLGA-PEG-PLGA-free formulation.

[0085] Experimental Methods: A 3D-printed aneurysm model containing a tumor-bearing channel and a lateral wall aneurysm cavity was constructed and connected to a circulation pump system. Physiological saline was used as the circulation medium, and the flow rate was adjusted to 300–900 mL / min, preferably 900 mL / min, to simulate a high fluid scouring environment. A microcatheter was inserted into the aneurysm cavity, and each group of embolic agents was slowly injected. The distribution of the embolic agent within the aneurysm cavity, the degree of aneurysm cavity occlusion, and the patency of the tumor-bearing channel were observed under visualization conditions. Results are as follows: Figure 5 As shown.

[0086] The results showed that the blank model group demonstrated that the aneurysm cavity could be filled with circulating fluid. In Example 1, after delivery into the aneurysm cavity via a microcatheter, the emboli could be formed in situ within the cavity and accumulated, subsequently fusing to form a monolithic embolic body. After embolization, the aneurysm cavity visualization was significantly reduced or disappeared, while the aneurysm-carrying channel remained patent. Example 3 achieved preliminary embolization, but the embolic body support was lower than in Example 1, and due to insufficient PLGA-PEG-PLGA dosage, it was easily dispersed by blood flow. In Example 4, due to the higher colloid hardness, the support force was higher than in Example 1, supporting the spatial spacing between the colloid strips and forming a looser embolic body. However, due to excessive hardness and insufficient inter-strip adhesion, there was a risk of the colloid strips dislodging from the aneurysm cavity when used in wide-necked aneurysms. In Comparative Example 2, lacking the rapid PLGA-PEG-PLGA-mediated strip-forming effect, the curing speed was slow, making it prone to loss in a fluid environment and being flushed out of the aneurysm cavity by blood flow, resulting in difficulty in stably filling the aneurysm cavity. The above results indicate that the preferred formulation of this invention has good in-situ embolization capability within the aneurysm cavity.

[0087] Example 5: In vitro erosion stability test This test was used to evaluate the morphology retention and anti-fracture ability of the embolic agent of the present invention under continuous fluid scouring conditions.

[0088] Experimental group: G1, i.e. Example 1 group, preferred formulation.

[0089] Experimental Method: After embolization in the 3D-printed aneurysm model described in Experimental Example 4, the model was continuously flushed with circulating fluid. The flushing time was set at 24 hours. The gross morphology of the embolized body within the aneurysm cavity was observed, and whether fragmentation, detachment, loss, or significant deformation occurred. The results are as follows: Figure 6 As shown.

[0090] The results showed that the emboli obtained in Example 1 exhibited good stability in both wide and narrow neck aneurysms, maintaining their overall morphology under continuous flushing conditions without significant fragmentation or large-scale detachment, with only partial swelling observed, presumably due to water absorption during solvent exchange. These results indicate that PLGA-PEG-PLGA-mediated solvent exchange and the dynamic polythiooctanoic acid network together contribute to improving the morphological stability of the emboli in a fluid environment.

[0091] Experimental Example 6: In vitro biocompatibility evaluation This experiment was used to evaluate the in vitro blood compatibility and cell compatibility of the embolic agent of the present invention.

[0092] Experimental Groups: G1: Positive control group, using deionized water; G2: Negative control group, using physiological saline; G3: Example 1; G4: Example 4.

[0093] The cytotoxicity assay was set up with the following groups: G1: Positive control group; G2: Negative control group; G3: Extract from Example 1; G4: Extract from Example 4; Experimental method: Take each group of materials or their extracts and incubate them together with anticoagulated rabbit blood or other experimental blood samples. After incubation, centrifuge and collect the supernatant. Observe the color of the supernatant and measure the absorbance. Calculate the hemolysis rate. The results are as follows: Figure 7 As shown in A in the figure. Extracts were prepared from each group of materials according to the method for extracting medical materials. The extracts were co-cultured with HUVEC vascular endothelial cells for 24–72 hours. Cell viability was evaluated by cell morphology and CCK-8 assay. The results are shown in Figure A. Figure 7 As shown in B in the diagram.

[0094] The results showed that the positive control group was clearly red, indicating significant hemolysis; the supernatant of the negative control group was relatively clear; no obvious red hemolysis was observed in the supernatant of the Example 1 and Example 4 groups, and the hemolysis rate was at a low level, indicating that the embolic agent of the present invention did not cause significant hemolysis under the experimental conditions. In the cytotoxicity experiment, the cell viability of the positive control group was significantly decreased; the cell morphology of the negative control group was good. The cell morphology of the Example 1 and Example 4 groups was relatively intact, and the cell viability remained within an acceptable range.

[0095] Experimental Example 7: In vitro degradation performance test This experiment was used to evaluate the in vitro degradation trend of the embolic agent of the present invention in an aqueous environment and to compare the degradation differences under different degradable block copolymers or developer conditions.

[0096] Experimental Groups: G1: Example 1, PLGA-PEG-PLGA / tantalum powder formulation; G2: Example 6, PDLLA-PEG-PDLLA / tantalum powder formulation.

[0097] Experimental Method: Embolic agents from each group were pre-cured in PBS at 37°C to form emboli, and then incubated in PBS at 37°C. Samples were taken at 0, 7, 14, and 28 days to observe the gross morphology, volume changes, and mass changes of the emboli. Results are as follows: Figure 8 As shown.

[0098] The results showed that in Example 1, softening, volume reduction, or mass decrease gradually occurred with prolonged incubation time, indicating that it exhibits gradual degradation characteristics in an aqueous environment. In Example 6, due to the use of PDLLA-PEG-PDLLA instead of PLGA-PEG-PLGA, the degradation rate was relatively slower, and the retention time of the embolic body morphology was relatively prolonged. These results demonstrate that the embolic agent of the present invention can have its degradation behavior controlled by adjusting the type of degradable block copolymer and the type of developer.

[0099] Example 8: Evaluation of early local tissue compatibility of subcutaneous implantation in rats This experiment was used to evaluate the early local tissue compatibility of the embolic agent of the present invention after implantation.

[0100] Experimental Groups: G1: Blank surgical control group, only a subcutaneous implantation cavity was created, and no material was implanted; G2: Example 1, subcutaneous injection of the embolic agent of Example 1.

[0101] Experimental Methods: The biodegradable embolic agent prepared in Example 1 was sterilized and used for later use. Healthy SD rats were selected, and an implantation cavity was prepared subcutaneously on the back under anesthesia. In the blank surgical control group, only the subcutaneous implantation cavity was established and the incision was sutured; in the control group, 200 μL of the embolic agent from Example 1 was injected subcutaneously and the incision was sutured. Rats were sacrificed on postoperative days 3 and 7, respectively, and tissue samples were collected to observe the gross morphology of the implantation site. The implantation area and surrounding tissues were fixed, dehydrated, embedded, sectioned, and stained with H&E. The results are as follows: Figure 9 As shown.

[0102] The results showed that no obvious suppuration or tissue necrosis was observed in the incision area at 3 and 7 days postoperatively in the blank surgical control group. In the Example 1 group, no obvious suppuration, tissue necrosis, or severe foreign body reaction was observed grossly at the implantation site at 3 and 7 days postoperatively; H&E staining showed a certain degree of early inflammatory cell infiltration and tissue repair reaction around the material, but no extensive necrosis was observed. Compared with the blank surgical control group, the Example 1 group showed a typical early tissue reaction after material implantation, and no severe local tissue damage was observed. These results indicate that the preferred embolic agent of the present invention has good early local tissue compatibility.

[0103] In summary, the above examples, comparative examples, and experimental cases demonstrate that the biodegradable embolic agent of the present invention, using PEG400 as a solvent system, combined with the solvent exchange curing effect of PEG block copolymers, the self-fusion effect of the dynamic disulfide bond network of polythiooctanoic acid, and the visualization effect of the contrast agent, can achieve microcatheter delivery, rapid strip formation in an aqueous environment, inter-strip fusion, in-situ filling of tumor cavities, visualization, in vitro degradation, and good early biocompatibility. Compared with comparative examples without PLGA-PEG-PLGA or without LA-NHS, the preferred formulation of the present invention exhibits better overall performance in terms of injectability, strip formation stability, embolization morphology retention, and erosion resistance.

[0104] The above descriptions are merely some specific embodiments of the present invention. For those skilled in the art, various modifications and improvements can be made without departing from the inventive concept of the present invention, and all such modifications and improvements fall within the scope of protection of the present invention.

Claims

1. A biodegradable embolizing agent for intracranial aneurysms, characterized in that, It is prepared from the following components: per 1 mL of polyethylene glycol 400, 0.1-0.3 g of thioctic acid, 0.007-0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.1-0.3 g of PEG block copolymer, and 0.4-0.5 g of developer.

2. The biodegradable embolizing agent for intracranial aneurysms according to claim 1, characterized in that, It is prepared from the following components: per 1 mL of polyethylene glycol 400, 0.1-0.2 g of thioctic acid, 0.007-0.014 g of thioctic acid-N-hydroxysuccinimide ester, 0.2-0.3 g of PEG block copolymer, and 0.4-0.5 g of developer.

3. The biodegradable embolizing agent for intracranial aneurysms according to claim 1 or 2, characterized in that, The PEG block copolymer is selected from PLGA-PEG-PLGA triblock copolymer and / or PDLLA-PEG-PDLLA triblock copolymer.

4. The biodegradable embolizing agent for intracranial aneurysms according to claim 1 or 2, characterized in that, The developer is tantalum powder that can be dispersed in organic solvents or PEG400 labeled with iodine at both ends.

5. The biodegradable embolizing agent for intracranial aneurysms according to claim 4, characterized in that, The tantalum powder has a particle size of 60-80 nm.

6. The method for preparing the biodegradable embolizing agent for intracranial aneurysms according to any one of claims 1-5, characterized in that, Includes the following steps: S1. Dissolve lipoic acid and lipoic acid-N-hydroxysuccinimide ester in polyethylene glycol 400, and heat and stir at 80-120°C for 1-4 hours to obtain the first mixture; S2. Cool the first mixture to 60-70°C, add the PEG block copolymer, and stir for 0.5-2 hours to obtain the second mixture; S3. Cool the second mixture to room temperature, add the developer, and mix to obtain the biodegradable embolic agent.

7. Use of the biodegradable embolizing agent for intracranial aneurysms according to any one of claims 1-5 as a medical device for intracranial aneurysms.

8. The method for delivering the biodegradable embolic agent for intracranial aneurysms according to any one of claims 1-5, characterized in that, Includes the following steps: (1) Before injecting the biodegradable embolic agent through the microcatheter, rinse the inner wall of the microcatheter with a biocompatible liquid; (2) The biodegradable embolizing agent is injected into the target aneurysm cavity through a microcatheter; (3) After contact with blood, the biodegradable embolic agent solidifies in situ through solvent exchange mechanism to form an embolus that adheres to the blood vessel wall.

9. The delivery method according to claim 8, characterized in that, The biocompatible liquid mentioned in step (1) refers to one or more organic solvents that are non-irritating to blood vessels, do not cause hemolysis, and are soluble in blood.

10. The delivery method according to claim 8, characterized in that, The outer diameter of the microcatheter mentioned in step (1) is 1.7F-2.7F.