Infection-responsive nanoparticle multifunctional hydrogel dressing and preparation method thereof

By integrating photothermal, NO gas therapy, and nanozyme catalysis, the infection-responsive nanoparticle multifunctional hydrogel dressing solves the problem of balancing infection sensing, antibacterial and repair promotion in wound dressings. It achieves effective biofilm disruption and wound healing, adapts to different wound shapes, and has magnetic responsiveness and safety.

CN123148455APending Publication Date: 2026-11-24HAINAN MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611624964.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing wound dressings lack active infection sensing capabilities, have a single antibacterial mode, struggle to achieve a balance between antibacterial and repair-promoting effects, and are difficult to effectively remove biofilms.

Method used

A multifunctional hydrogel dressing with infection-responsive nanoparticles is used. The hydrogel matrix is ​​constructed through Schiff base reaction and combined with magnetic composite nanoparticles to integrate photothermal effect, NO gas therapy and nanozyme catalytic activity. The HA-PBA gated layer is designed to activate the antibacterial function on demand, and the Fe₃O₄ magnetic core is combined to facilitate recycling.

Benefits of technology

It significantly reduces the survival rate of planktonic bacteria, disrupts the biofilm of multidrug-resistant bacteria, promotes wound healing, avoids tissue toxicity, adapts to irregular wounds, is easy to operate, and has high safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148455A_ABST
    Figure CN123148455A_ABST
Patent Text Reader

Abstract

This invention discloses an infection-responsive nanoparticle multifunctional hydrogel dressing and its preparation method. The hydrogel dressing comprises a hydrogel matrix and magnetic composite nanoparticles. The hydrogel matrix is ​​constructed by a Schiff base reaction of QCS-Cat and OHA. The magnetic composite nanoparticles have Fe3O4 as the magnetic core, Prussian blue PB as the photothermal / catalytic intermediate layer, and cerium dioxide (CeO) containing oxygen vacancies as the composite nanoparticles. 2‑x The surface-active layer is loaded with a NO donor and then capped with HA-PBA as a gating layer. This invention combines mild photothermal effect (Prussian blue component, 808 nm near-infrared response), NO gas therapy, and CeO2. 2‑x The nanozyme-catalyzed ROS triple antibacterial mechanism is integrated into a single dressing. The three mechanisms work synergistically to not only significantly reduce the survival rate of planktonic bacteria, but also effectively destroy the biofilm structure of multidrug-resistant bacteria, including Staphylococcus aureus. This overcomes the shortcomings of single antibacterial modes, such as poor biofilm permeability and easy induction of drug resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of biomaterials technology, specifically to an infection-responsive nanoparticle multifunctional hydrogel dressing and its preparation method. Background Technology

[0002] Bacterial wound infections, especially chronic wounds involving multidrug-resistant bacteria, pose a significant challenge to clinical wound healing. The mutually reinforcing relationship between bacterial proliferation, persistent biofilms, excessive inflammatory responses, and delayed tissue regeneration makes effective healing difficult with conventional treatments.

[0003] Currently, functional hydrogel dressings are considered promising wound repair matrices. Dynamic polysaccharide hydrogels based on hyaluronic acid and chitosan derivatives have attracted widespread attention due to their injectability, self-healing properties, and wet adhesion. However, existing hydrogel dressings generally suffer from the following shortcomings: First, they lack the ability to actively detect and respond to infection. Most hydrogels only act as passive barriers or drug reservoirs, and cannot autonomously upregulate their antibacterial activity after infection occurs. If high concentrations of antibacterial agents are continuously released, although they can inhibit bacteria, they often have toxicity to regenerating tissues, making it difficult to balance the relationship between antibacterial and repair.

[0004] Secondly, single antibacterial modalities are insufficient to effectively remove biofilms. Traditional dressings often use single antibiotics or silver ions as antibacterial agents, but the presence of biofilm barriers significantly weakens their penetration and killing efficiency and easily induces drug resistance.

[0005] Furthermore, existing systems struggle to integrate multiple therapeutic functions. The integration of photothermal effects, gas therapy (such as nitric oxide release), nanozyme catalytic activity with tissue adhesion and recyclability into a single dressing, and its on-demand activation in response to the infection microenvironment, is not adequately disclosed in current technologies.

[0006] Therefore, there is an urgent need in this field to develop a novel hydrogel dressing that combines responsiveness to the infection microenvironment, multiple synergistic antibacterial properties (photothermal / NO / nanozymes), biofilm disruption capabilities, and tissue regeneration promotion functions. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention aims to provide an infection-responsive nanoparticle multifunctional hydrogel dressing and its preparation method, thereby solving the technical problems of existing wound dressings lacking active infection sensing capabilities, having a single antibacterial mode, and being unable to achieve a balance between antibacterial and repair-promoting effects.

[0008] To achieve this objective, the present invention adopts the following technical solution: A first aspect of the present invention is to provide an infection-responsive nanoparticle multifunctional hydrogel dressing, the hydrogel dressing comprising a hydrogel matrix and magnetic composite nanoparticles loaded in the hydrogel matrix; the hydrogel matrix is ​​constructed by a Schiff base reaction of catecholized quaternized chitosan (QCS-Cat) and oxidized hyaluronic acid (OHA); the magnetic composite nanoparticles are configured with Fe3O4 as a magnetic core, Prussian blue (PB) as a photothermal / catalytic intermediate layer, and cerium dioxide (CeO) containing oxygen vacancies. 2-x The surface-active layer forms a ternary carrier, on which a NO donor is loaded, and then the hyaluronic acid HA-PBA modified with phenylboronic acid is used as a gating layer for end-capping.

[0009] In one optional embodiment, the magnetic composite nanoparticles are prepared as follows: S1. Preparation of magnetic core: The iron source was reduced in a polyol solvent in the presence of a dispersant and a precipitant using a solvothermal method. The magnetic precipitate obtained after the reaction was collected and washed with anhydrous ethanol and deionized water alternately to remove impurities. The washed precipitate was dried to obtain magnetic iron(III) oxide (Fe3O4) nanoparticles. S2, Intermediate layer coating: The Fe3O4 nanoparticles are dispersed in an aqueous medium. After adjusting the pH, a ferricyanide precursor solution is added sequentially. A Prussian blue PB coating layer is formed on the surface of the Fe3O4 nanoparticles through in-situ coordination reaction, resulting in Fe3O4@PB composite particles. S3. External functionalization modification: The Fe3O4@PB composite particles are dispersed in a precursor solution containing cerium salt and an alkaline source. Through low-temperature aqueous in-situ hydrolysis, cerium dioxide (CeO) containing oxygen vacancies is formed on the surface of the Fe3O4@PB composite particles. 2-x Layers were formed to obtain FPBC composite particles; S4. Active substance loading: The FPBC composite particles are mixed with nitric oxide (NO) donor molecules under low temperature and light-protected conditions, so that the NO donor is loaded into the pores and / or surface of the FPBC composite particles to obtain FPBC / NO composite particles. S5. Assembly of the intelligent gated layer: Prepare FPBC / NO composite particle dispersion and hyaluronic acid (HA-PBA) solution modified with phenylboronic acid respectively. Add the HA-PBA solution dropwise to the FPBC / NO composite particle dispersion. Induce cross-linking of HA-PBA molecular chains by pH control to form a microporous HA-PBA gated layer on the surface of the FPBC / NO composite particles, and obtain the target magnetic composite nanoparticles FPBC / NO@HP.

[0010] In an optional embodiment, in step S1, the iron source is ferric chloride hexahydrate, the polyol is ethylene glycol, the dispersant is polyethylene glycol, the precipitant is anhydrous sodium acetate, and the mass ratio of ferric chloride hexahydrate, polyethylene glycol, and anhydrous sodium acetate is 1:(0.5-1):(2-3); the reduction reaction is carried out at a temperature of 180-220°C for 6-12 hours.

[0011] In one optional embodiment, the ferricyanide precursor comprises ferric chloride hexahydrate and potassium ferrocyanide K4[Fe(CN)6]·3H2O, with the ferric chloride hexahydrate solution added first, followed by potassium ferrocyanide K4[Fe(CN)6]·3H2O. The concentration ratio of the Fe3O4 nanoparticle solution, the ferric chloride hexahydrate solution, and the potassium ferrocyanide K4[Fe(CN)6]·3H2O is 1:5:5. The pH of the aqueous medium is adjusted to 3.5–4.0.

[0012] In one optional embodiment, the cerium salt is cerium nitrate, the alkali source is hexamethylenetetramine, and the mass ratio of the Fe3O4@PB composite particles, cerium nitrate, and hexamethylenetetramine is 1:(0.7-1):(0.3-0.7); the temperature of the low-temperature aqueous in-situ hydrolysis reaction is 70-90°C, and the time is 3-6 h.

[0013] In an optional embodiment, in step S5, the concentration ratio of the FPBC / NO composite particle dispersion to the HA-PBA solution is 1:2; the pH adjustment specifically involves: first, allowing HA-PBA to adsorb onto the particle surface at pH 7.0–7.6, then adjusting the pH to 7.8–8.2 to induce the formation of borate ester crosslinking bonds, and finally adjusting the pH back to 7.4 after the reaction is complete.

[0014] In an optional embodiment, in step S4, the NO donor is S-nitrosoglutathione (GSNO), and the loading process is carried out at 0–10°C under light-protected conditions for 10–15 h. The preparation process of S-nitrosoglutathione (GSNO) is as follows: glutathione is dissolved in an acidic medium, and nitrite solution is slowly added under low temperature and light-protected conditions to carry out a nitrosation reaction. After the reaction is completed, the pH is adjusted to 5.5–6.5 with an alkaline solution to obtain the GSNO solution. The mass ratio of glutathione to nitrite is (4–5):1.

[0015] In an optional embodiment, in step S5, the preparation method of phenylboronic acid modified hyaluronic acid HA-PBA is as follows: hyaluronic acid HA is dissolved in a weakly acidic buffer solution, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide are added to activate the carboxyl group, 3-aminophenylboronic acid is added to the activation system, and an amidation reaction is carried out under pH 6.0-6.5 conditions. After the reaction is completed, the hyaluronic acid is dialyzed, purified, and freeze-dried to obtain phenylboronic acid modified hyaluronic acid HA-PBA; wherein, the mass ratio of hyaluronic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-hydroxysuccinimide, and 3-aminophenylboronic acid is 1:(0.5-0.7):(0.1-0.4):(0.5-0.7).

[0016] In one optional embodiment, the preparation method of the catecholized quaternized chitosan QCS-Cat includes the following steps: (1) Synthesis of quaternized chitosan QCS Chitosan powder was dispersed in deionized water and then 0.1-5 wt% dilute acetic acid solution was added to prepare an aqueous solution of 0.1-1 wt%. Then 0.025-0.10 g / mL glycidyl trimethylamine chloride was added to carry out the reaction. The reaction product was dialyzed to remove small molecule impurities and then freeze-dried to obtain purified quaternized chitosan QCS material. (2) Synthesis of catecholized quaternized chitosan QCS-Cat Quaternized chitosan QCS material was dissolved in deionized water to prepare a 0.1–1 wt% aqueous solution. 0.001–0.005 g / mL of 3-(2,4-dihydroxy)phenylpropionic acid and 0.001–0.005 g / mL of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added sequentially to the solution. The reaction was carried out at pH 4–5.5 for 12 h. The resulting product was dialyzed and lyophilized to obtain catecholized quaternized chitosan QCS-Cat.

[0017] A second aspect of the present invention is to provide a method for preparing the infection-responsive nanoparticle multifunctional hydrogel dressing, comprising the following steps: Magnetic composite nanoparticles were dispersed in a phosphate buffer solution at pH 7.4. The dispersion was then mixed with a QCS-Cat precursor solution to obtain a QCS-Cat precursor solution containing magnetic composite nanoparticles. This precursor solution was then mixed with an OHA precursor solution at a volume ratio of 1:1. After mixing, the mixture was allowed to stand for 10–18 minutes at 20–25°C and pH 7.2–7.6 to obtain a hydrogel dressing.

[0018] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention combines mild photothermal effect (Prussian blue component, 808 nm near-infrared response), NO gas therapy, and CeO2. 2-x The nanozyme-catalyzed ROS triple antibacterial mechanism is integrated into a single dressing. The three mechanisms work synergistically to not only significantly reduce the survival rate of planktonic bacteria, but also effectively destroy the biofilm structure of multidrug-resistant bacteria, including Staphylococcus aureus. This overcomes the shortcomings of single antibacterial modes, such as poor biofilm permeability and easy induction of drug resistance.

[0019] 2. This invention utilizes a HA-PBA gated layer design to enable the hydrogel dressing to sense signals characteristic of the infection microenvironment (acidic pH, elevated H2O2, and bacterial enzymes). Under normal physiological conditions, the gated layer is stable, limiting premature NO release and excessive exposure of nanozymes. Once in an infection microenvironment, the gated structure responsively opens, exposing internal active sites and accelerating NO release, achieving "on-demand activation" of the antibacterial function. This mechanism effectively avoids the toxicity and delayed healing problems caused by traditional continuous high-concentration antibacterial agents to regenerating tissues.

[0020] 3. This invention constructs a hydrogel matrix based on dynamic Schiff base crosslinking between OHA and QCS-Cat, endowing the material with solid-like rheological behavior, repeated strain recovery ability, swelling / degradation balance characteristics, and macroscopic self-healing properties. At the same time, the catechol groups in QCS-Cat endow the material with good adhesion to moist biological substrates, enabling the hydrogel dressing to adapt to wounds of different shapes and depths, resist mechanical disturbance, and remain stably in the local area for a long time, solving the problem that traditional dressings are difficult to adhere to irregular wounds and are easy to fall off.

[0021] 4. The hydrogel dressing of this invention can significantly reduce local bacterial load in infected wound models, while promoting collagen deposition, vascularization, and re-epithelialization, accelerating the transition of the wound from the infection control stage to the tissue remodeling stage. This sequential functional design of "controlling bacteria first, then promoting healing" aligns with the pathophysiological process of infected wound healing. Furthermore, due to the presence of the Fe3O4 magnetic core, this invention exhibits excellent magnetic responsiveness. After treatment or when dressing replacement is required, the material can be recovered using an external magnetic field, reducing long-term residue of nanoparticles in the body and further enhancing application safety.

[0022] 5. The hydrogel precursor solution of this invention can rapidly crosslink into a gel at room temperature without the need for external crosslinking agents or ultraviolet irradiation. This characteristic endows the material with good injectability, making it easy to fill deep or irregular infected wounds by injection. The operation is simple and suitable for clinical application. Attached Figure Description

[0023] Figure 1 This is a schematic diagram of the synthesis route for the magnetic composite nanoparticles FPBC / NO@HP.

[0024] Figure 2 TEM and HRTEM images of the magnetic composite nanoparticles FPBC / NO@HP.

[0025] Figure 3 This is a STEM-EDS elemental mapping of the magnetic composite nanoparticles FPBC / NO@HP.

[0026] Figure 4 The XRD pattern of the magnetic composite nanoparticles FPBC / NO@HP is shown.

[0027] Figure 5 The image shows the zeta potential analysis of the magnetic composite nanoparticles FPBC / NO@HP.

[0028] Figure 6 The DLS particle size distribution diagram of the magnetic composite nanoparticles FPBC / NO@HP.

[0029] Figure 7 XPS spectra of magnetic composite nanoparticles FPBC / NO@HP.

[0030] Figure 8 The image shows the hysteresis loop and UV-vis-NIR absorption spectrum of the magnetic composite nanoparticles FPBC / NO@HP.

[0031] Figure 9 This is a schematic diagram illustrating the formation of the hydrogel dressing FPBC / NO@HP-Gel.

[0032] Figure 10 Frequency scan rheology results for the hydrogel dressing FPBC / NO@HP-Gel.

[0033] Figure 11 The graph shows the step strain self-healing properties of the hydrogel dressing FPBC / NO@HP-Gel.

[0034] Figure 12 The graph shows the swelling and degradation properties of the hydrogel dressing FPBC / NO@HP-Gel.

[0035] Figure 13 This is a graph showing the adhesion properties of the hydrogel dressing FPBC / NO@HP-Gel on different substrates.

[0036] Figure 14 This is a diagram showing the macroscopic self-healing properties of the hydrogel dressing FPBC / NO@HP-Gel.

[0037] Figure 15 This is a diagram showing the extrusion molding and rapid sol-gel transition of the hydrogel dressing FPBC / NO@HP-Gel.

[0038] Figure 16 Macroscopic color response diagram of hydrogel dressing FPBC / NO@HP-Gel under different infection simulation conditions.

[0039] Figure 17 The diagram shows the reversible pH response and color change of the hydrogel dressing FPBC / NO@HP-Gel.

[0040] Figure 18 This is a schematic diagram illustrating the opening / closing mechanism of the HA-PBA gating layer in normal and infected microenvironments.

[0041] Figure 19 This figure shows the relative nanozyme exposure of the hydrogel dressing FPBC / NO@HP-Gel under different microenvironmental conditions.

[0042] Figure 20 NO release curves of hydrogel dressing FPBC / NO@HP-Gel under different infection-related stimuli.

[0043] Figure 21 TMB oxidation activity of hydrogel dressing FPBC / NO@HP-Gel under infection simulation conditions.

[0044] Figure 22 This is a schematic diagram of a three-dimensional bacterial model showing the gating structure response to enzyme-related stimuli.

[0045] Figure 23 Photothermal temperature rise curves of hydrogel dressing FPBC / NO@HP-Gel under 808 nm irradiation with different nanoparticle loadings.

[0046] Figure 24 Infrared thermographic image of hydrogel dressing FPBC / NO@HP-Gel under 808 nm irradiation.

[0047] Figure 25 Photothermal heating curves of hydrogel dressing FPBC / NO@HP-Gel under different 808 nm laser power densities.

[0048] Figure 26 The DCFH-DA fluorescence images generated by ROS under different treatment conditions.

[0049] Figure 27 The graph shows the cumulative NO release curves under normal, infected response, and infected response combined 808 nm irradiation conditions.

[0050] Figure 28 The graph shows the cumulative NO release results of NO@HP-Gel and FPBC / NO@HP-Gel using the Griess method.

[0051] Figure 29 The image shows the validation of the free radical scavenger and its effect in killing E. coli.

[0052] Figure 30 This is a schematic diagram illustrating the synergistic anti-infection mechanism of mild photothermal activity, ROS regulation, and NO release.

[0053] Figure 31 Escherichia coli in different treatment groups Escherichia coli ( E. coli Staphylococcus aureus Staphylococcus aureus ( S. aureus ) and methicillin-resistant Staphylococcus aureus Methicillin- resistance Staphylococcus aureus (MRSA) colony plate diagram.

[0054] Figure 32 Log10 CFU quantification chart of bacterial survival in different treatment groups.

[0055] Figure 33 Crystal violet staining images of bacterial biofilms from different treatment groups.

[0056] Figure 34 This is a graph showing the quantitative analysis of biofilm biomass in different treatment groups.

[0057] Figure 35 Escherichia coli in different treatment groups Escherichia coli ( E. coli ) and methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus (MRSA) Live / Dead fluorescence staining image.

[0058] Figure 36 Escherichia coli in different treatment groups Escherichia coli ( E. coli ) and methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus (MRSA) Quantitative analysis chart of mortality rate.

[0059] Figure 37 Three-dimensional Live / Dead fluorescence reconstruction images of bacterial biofilms from different treatment groups.

[0060] Figure 38 This is a graph showing the quantitative analysis of biofilm thickness and biomass in different treatment groups.

[0061] Figure 39 Escherichia coli in different treatment groups Escherichia coli ( E. coli ) and methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus SEM image of (MRSA) morphology.

[0062] Figure 40 Staphylococcus aureus in different treatment groups Staphylococcus aureus ( S. aureus Methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus (MRSA) and Pseudomonas aeruginosa Pseudomonas aeruginosa ( p.aeruginosa Colony plate diagram of ).

[0063] Figure 41 Staphylococcus aureus in different treatment groups Staphylococcus aureus ( S. aureus Methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus (MRSA) and Pseudomonas aeruginosa Pseudomonas aeruginosa ( p.aeruginosa Log10 CFU quantitative analysis chart of survival rate.

[0064] Figure 42 Representative photographs of infected wounds from different treatment groups at different time points.

[0065] Figure 43 This is a quantitative analysis chart showing the area and closure status of infected wounds in different treatment groups.

[0066] Figure 44 Figures showing the bacterial colony and bacterial load analysis of wound tissue homogenates from different treatment groups.

[0067] Figure 45 H&E staining and histological quantitative analysis of wound tissues from different treatment groups.

[0068] Figure 46 Masson's trichrome staining and collagen area analysis of wound tissues from different treatment groups.

[0069] Figure 47 This diagram illustrates the magnetic recovery of hydrogel dressings and shows the analysis of residual Fe and Ce content in the wound.

[0070] Figure 48 The graph shows the serum ALT, AST, BUN, and Cr levels in the PBS group and the group receiving FPBC / NO@HP-Gel hydrogel dressing combined with 808 nm irradiation.

[0071] Figure 49 The image shows a comparison of blood biochemical indicators ALT and CREA on day 14 between the PBS group and the group receiving FPBC / NO@HP-Gel combined with 808 nm irradiation. Detailed Implementation

[0072] To enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present application, and not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present application.

[0073] Example An infection-responsive nanoparticle multifunctional hydrogel dressing, the preparation method of which includes the following steps: I. Preparation of magnetic composite nanoparticles FPBC / NO@HP (I) Preparation of magnetic iron(III) oxide nanoparticles (Fe3O4) 1.35 g of ferric chloride hexahydrate (FeCl3·6H2O) was weighed and added to 40 mL of ethylene glycol. The mixture was magnetically stirred at 500 r / min for 20 min at room temperature until the ferric chloride hexahydrate was completely dissolved, yielding a clear, orange-yellow iron salt solution. Subsequently, 3.60 g of anhydrous sodium acetate and 1.00 g of polyethylene glycol (PEG-2000) were added sequentially to the iron salt solution, and stirring was continued for 30 min until no obvious solid particles remained in the system. The resulting mixture was transferred to a 50 mL polytetrafluoroethylene-lined reactor, sealed, and placed in a constant temperature oven at 200 °C for 10 h. After the reaction was complete, the heating device was turned off, and the reactor was allowed to cool naturally to room temperature. The reactor was then opened, and the resulting black magnetic precipitate was collected using an external permanent magnet. The collected magnetic precipitate was washed alternately with anhydrous ethanol and deionized water, 30 mL of washing solution added each time. After ultrasonic dispersion for 5 min, the precipitate was separated using a magnet. This washing process was repeated 3 times each to remove unreacted iron salts, sodium acetate, ethylene glycol, and free polyethylene glycol. The washed precipitate was then dried in a vacuum drying oven at 50 °C for 12 h to obtain magnetic iron(III) oxide nanoparticles (Fe3O4).

[0074] (II) Preparation of Prussian Blue Coated Magnetic Nanoparticles Fe3O4@PB Weigh 100 mg of the Fe3O4 nanoparticles obtained in step (I) and add them to 100 mL of deionized water. Simultaneously, add 100 mg of polyvinylpyrrolidone (PVP). Disperse the Fe3O4 nanoparticles using a probe-type ultrasonic instrument under ice bath conditions for 10 min, with the ultrasonic power controlled at 80–100 W. Then continue ultrasonication in a water bath for another 10 min to ensure uniform dispersion of Fe3O4 in the aqueous phase. Adjust the pH of the dispersion to 3.5–4.0 using 0.1 mol / L hydrochloric acid and stir at room temperature for 20 min.

[0075] A 5 mg / mL solution of ferric chloride hexahydrate and a 5 mg / mL solution of potassium ferrocyanide K4[Fe(CN)6]·3H2O were prepared. First, 10 mL of the ferric chloride hexahydrate solution was added dropwise to the Fe3O4 dispersion at a rate of approximately 0.5 mL / min, while stirring at 600 r / min during the addition. After the addition was complete, stirring was continued for 30 min to allow the Fe3O4 dispersion to settle. 3+ The Prussian blue adsorbs onto the surface of Fe3O4 particles. Then, 10 mL of potassium ferrocyanide solution is slowly added dropwise to the system at the same rate. During the addition process, excessively high local concentrations are avoided to reduce the formation of free Prussian blue particles.

[0076] After the addition was complete, the reaction was carried out at 25°C in the dark for 4 hours to allow Fe to react. 3+ With [Fe(CN)6] 4- A coordination reaction occurs on the Fe3O4 surface, forming a Prussian blue coating in situ. After the reaction is complete, the blue-black precipitate is collected using an external magnetic field, washed three times with deionized water, and then once with anhydrous ethanol. The washed product is dried under vacuum at 40°C to obtain Fe3O4@PB powder.

[0077] (III) Preparation of oxygen-vacancy cerium dioxide-modified composite particles FPBC Weigh 100 mg of Fe3O4@PB obtained in step (II) and add it to 80 mL of deionized water. Add 50 mg of polyvinylpyrrolidone (PVP) and sonicate in an ice bath for 15 min. Then add 86.8 mg of cerium nitrate hexahydrate (Ce(NO3)3·6H2O) and 56 mg of hexamethylenetetramine to the dispersion and stir magnetically for 20 min to ensure that the cerium salt and hexamethylenetetramine are evenly distributed around the Fe3O4@PB particles.

[0078] The reaction system was heated to 80℃ and stirred continuously at 500 r / min for 4 h. Hexamethylenetetramine slowly hydrolyzed under heating conditions, gradually releasing basic groups, causing the pH of the reaction system to slowly rise to 7.5–8.2. This allowed the cerium precursor to preferentially undergo hydrolysis, nucleation, and low-temperature oxidation on the Fe3O4@PB surface, forming a Ce-containing... 3+ / Ce 4+ CeO with mixed valence states and oxygen vacancies 2-x Layer. High-temperature calcination is not performed during the reaction to prevent structural damage to the Prussian blue layer, while retaining CeO₂. 2-x The defective structure in the precipitate was investigated. After the reaction was completed and allowed to cool naturally to room temperature, the precipitate was collected using an external magnetic field and washed four times with deionized water. Each wash involved low-power ultrasonic dispersion for 3 minutes followed by magnetic separation to remove free cerium ions, hexamethylenetetramine, and unbound CeO₂. 2-x Particles.

[0079] The cleaned composite particles were dried under vacuum at 40°C to obtain Fe3O4@PB / CeO 2-x The composite material is denoted as FPBC. The FPBC material possesses an Fe3O4 magnetic core, a Prussian blue photothermal and catalytic functional layer, and oxygen-containing CeO2 vacancies. 2-x Surface active layer.

[0080] (iv) Preparation of hyaluronic acid-phenylboronic acid coupling compound HA-PBA Weigh 500 mg of hyaluronic acid (HA), preferably with a molecular weight of 50–100 kDa, and add it to 100 mL of 0.1 mol / L MES buffer at pH 5.5. Stir overnight at room temperature to fully dissolve the hyaluronic acid, obtaining a homogeneous and transparent hyaluronic acid solution. Add 287 mg of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC·HCl) and 173 mg of N-hydroxysuccinimide (NHS) to the hyaluronic acid solution and stir at room temperature for 30 min to activate the carboxyl groups on the hyaluronic acid molecular chain.

[0081] Weigh 260 mg of 3-aminophenylboronic acid salt and dissolve it in 10 mL of MES buffer. Slowly add the resulting solution dropwise to an activated hyaluronic acid solution. Adjust the pH of the reaction system to 6.0–6.5 using a 0.1 mol / L sodium hydroxide solution. Continue the reaction at room temperature and in the dark for 18 h to allow the amino group of 3-aminophenylboronic acid to undergo an amidation reaction with the activated carboxyl group of hyaluronic acid.

[0082] After the reaction was completed, the reaction solution was placed in a dialysis bag with a molecular weight cutoff of 3500 Da and dialyzed with deionized water for 72 hours. The dialysate was changed every 6 hours for the first 24 hours and every 8–12 hours for the next 48 hours to remove unreacted 3-aminophenylboronic acid, EDC, NHS, and their byproducts. After dialysis, the resulting solution was pre-frozen at -80°C for 12 hours and then freeze-dried to obtain a white or off-white spongy hyaluronic acid-phenylboronic acid conjugate HA-PBA, denoted as HP.

[0083] (v) Preparation of nitric oxide donor GSNO Weigh 307 mg of reduced glutathione (GSH) and dissolve it in 5 mL of pre-cooled 0.5 mol / L hydrochloric acid solution. Place the reaction vessel in an ice bath at 0–4 °C and stir in the dark. Separately, weigh 69 mg of sodium nitrite (NaNO2) and dissolve it in 5 mL of pre-cooled deionized water. Slowly add the sodium nitrite solution dropwise to the glutathione solution over 10 min, stirring continuously in the dark during the addition. After the addition is complete, continue the reaction at 0–4 °C for 40 min to induce nitrosation of glutathione, generating S-nitrosoglutathione (GSNO). After the reaction is complete, slowly adjust the pH of the system to approximately 6.0 using pre-cooled 1 mol / L sodium hydroxide solution to obtain a freshly prepared GSNO solution.

[0084] (vi) Preparation of nitric oxide donor-supported composite particles FPBC / NO Weigh 100 mg of the FPBC obtained in step (III) and add it to 20 mL of a 5 mg / mL GSNO solution. Place the mixture in an ice bath and sonicate at a low power of less than 80 W for 3 min to avoid premature decomposition of GSNO due to prolonged sonication. Then transfer the mixture to a brown reaction flask and react for 12 h at 4°C, in the dark, and with stirring at 300 r / min. Utilize the porous structure of Prussian blue and CeO2... 2-x The adsorption sites on the surface, as well as the electrostatic and coordination interactions on the surface of FPBC particles, allow GSNO to enter the pores of the composite particles and adsorb onto the particle surface.

[0085] After loading was completed, particles were rapidly collected using an external magnetic field, and the supernatant was discarded. The particles were then rapidly washed once with 10 mL of pre-cooled pH 6.5 phosphate buffer for no more than 2 min to remove weakly adsorbed free GSNO from the particle surface and minimize the loss of the loaded GSNO. The resulting NO donor-loaded composite particles were designated FPBC / NO. The entire separation and washing process was performed at 4°C under light-protected conditions.

[0086] (vii) HA-PBA infection response gating layer coating and preparation of FPBC / NO@HP Weigh 100 mg of the FPBC / NO obtained in step (VI) and add it to 20 mL of pre-cooled pH 7.4 phosphate buffer. Disperse the solution by low-power sonication for 3 min under ice bath conditions. Separately weigh 100 mg of the HA-PBA prepared in step (IV) and dissolve it in 10 mL of deionized water to prepare a 10 mg / mL HA-PBA solution.

[0087] The HA-PBA solution was slowly added dropwise to the FPBC / NO dispersion at a rate of 0.5 mL / min, while maintaining stirring at 300 r / min during the addition. After the addition was complete, stirring was continued for 2 h at room temperature and in the dark to allow the HA-PBA molecular chains to bind with CeO through the carboxyl groups. 2-x The cerium ions on the surface are adsorbed onto the FPBC / NO surface through coordination, hydrogen bonding, and electrostatic interactions.

[0088] The pH of the system was then slowly adjusted to 7.8–8.2 using a 0.1 mol / L sodium hydroxide solution, and stirring continued for 4 h. This allowed the phenylboronic acid groups in the HA-PBA molecule to form reversible borate ester bonds with the vicinal diol structure on the hyaluronic acid sugar chain, resulting in a continuous HA-PBA gating layer with a small-pore structure on the FPBC / NO surface. After the reaction was complete, the pH of the system was adjusted back to 7.4.

[0089] The coated composite particles were collected using an external magnetic field and gently washed twice with pre-cooled pH 7.4 phosphate buffer. Prolonged sonication and strong agitation were avoided during washing to reduce gating layer detachment and premature NO donor release. Finally, the obtained particles were dispersed in sterile pH 7.4 phosphate buffer to a final concentration of 10 mg / mL, yielding the infection microenvironment responsive magnetic composite material FPBC / NO@HP dispersion.

[0090] The obtained FPBC / NO@HP dispersion was stored in a brown sealed bottle at 4°C in the dark. Under normal physiological conditions, the HA-PBA gating layer remains relatively dense, limiting the rapid leakage of NO donors. In the weakly acidic environment of the infected area, with increased hydrogen peroxide, or in the bacteria-associated microenvironment, the borate ester bonds dissociate or oxidatively break, gradually loosening the gating layer, exposing the active surface of FPBC and promoting NO release, thereby achieving responsive activation in the infected microenvironment.

[0091] II. Preparation of Nanoparticle Multifunctional Hydrogel Dressing FPBC / NO@HP-Gel (I) Synthesis of Catechol-Modified Quaternized Chitosan QCS-Cat Chitosan powder was dispersed in deionized water and then 0.1-5 wt% dilute acetic acid solution was added to prepare an aqueous solution of 0.1-1 wt%. Then 0.025-0.10 g / mL glycidyl trimethylamine chloride was added to carry out the reaction. The reaction product was dialyzed to remove small molecule impurities and then freeze-dried to obtain purified quaternized chitosan QCS material. Quaternized chitosan QCS material was dissolved in deionized water to prepare a 0.1–1 wt% aqueous solution. 0.001–0.005 g / mL of 3-(2,4-dihydroxy)phenylpropionic acid and 0.001–0.005 g / mL of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added sequentially to the solution. The reaction was carried out at pH 4–5.5 for 12 h. The resulting product was dialyzed and lyophilized to obtain catecholized quaternized chitosan QCS-Cat.

[0092] (II) Preparation of OHA precursor solution Weigh 200 mg of oxidized hyaluronic acid (OHA) and add it to 5 mL of sterile pH 7.4 phosphate-buffered saline (PBS). Stir magnetically at 300–500 r / min for 2–4 h at room temperature to fully hydrate the OHA and form a homogeneous, transparent, or slightly milky white solution, yielding a 4% (w / v) OHA precursor solution. If the OHA dissolves slowly, allow it to stand at 4°C for approximately 2 h to hydrate, then return to room temperature and continue stirring. Avoid vigorous shaking and the generation of large amounts of bubbles during dissolution. Allow the obtained OHA precursor solution to stand for 10–20 min to remove bubbles. Before use, maintain the pH of the system at 7.2–7.6. For cell or animal experiments, sterilize by filtration through a 0.22 μm filter before gelation.

[0093] (III) Preparation of QCS-Cat precursor solution Weigh 200 mg of QCS-Cat and add it to 5 mL of sterile pH 7.4 PBS. Stir magnetically at 300–500 r / min for 2–4 h at room temperature until fully dissolved to obtain a 4% (w / v) QCS-Cat precursor solution. Before use, allow the QCS-Cat precursor solution to stand for 10–20 min to defoam, maintaining the pH at 7.2–7.6. No additional small molecule chemical cross-linking agents or free radical initiators are added during preparation, and no ultraviolet light is applied to preserve the free amino and catechol groups in QCS-Cat.

[0094] (iv) Predispersion of FPBC / NO@HP nanoparticles Take the aforementioned FPBC / NO@HP stock dispersion, with a material concentration of 10 mg / mL. Before use, gently invert the stock solution at 4°C in the dark to mix thoroughly. If slight sedimentation occurs, it can be dispersed by low-power ultrasonication (no higher than 80 W) for 30–60 s under ice bath conditions to allow the particles to redisperse uniformly. To reduce premature decomposition of GSNO and shedding of the HA-PBA gated layer, prolonged probe ultrasonication, strong vortexing, or heating treatment should be avoided.

[0095] (v) Mixing of FPBC / NO@HP and QCS-Cat precursor fluid Take 4.5 mL of the above 4% (w / v) QCS-Cat precursor solution and place it in a light-protected container. Slowly add 0.5 mL of FPBC / NO@HP stock dispersion with a concentration of 10 mg / mL. During the addition process, gently stir at 200–300 r / min. After the addition is complete, continue mixing for about 5 min to ensure that FPBC / NO@HP is uniformly dispersed in the QCS-Cat precursor solution, thus obtaining a QCS-Cat precursor solution containing FPBC / NO@HP. According to the above formulation, the concentration of FPBC / NO@HP in the particulate QCS-Cat precursor solution is approximately 1 mg / mL; after crosslinking with an equal volume of OHA precursor solution, the final concentration of FPBC / NO@HP in the hydrogel is approximately 0.5 mg / mL.

[0096] (vi) OHA / QCS-Cat dynamic Schiff base crosslinking and in-situ gelation Take 5 mL of the above-mentioned QCS-Cat precursor solution containing FPBC / NO@HP and rapidly mix it with 5 mL of 4% (w / v) OHA precursor solution at a volume ratio of 1:1. During mixing, a double-barreled syringe with a 1:1 static mixing connector can be used for simultaneous dispensing, or a pipette can be used in a sterile container for rapid reciprocating pipetting 8–12 times. After mixing, the aldehyde groups on the OHA molecular chain and the free amino groups on the QCS-Cat molecular chain undergo a dynamic Schiff base reaction, gradually forming a three-dimensional dynamic covalent cross-linked network, while simultaneously embedding the FPBC / NO@HP nanoparticles uniformly within the network pores. Under conditions of 20–25℃ and pH 7.2–7.6, the mixture typically transforms from a flowable precursor into a shape-maintaining gel within approximately 30–120 seconds. After initial gelation, continue to allow it to stand at room temperature in the dark for 10–15 minutes to further stabilize the cross-linked network, thus obtaining the FPBC / NO@HP-Gel hydrogel dressing.

[0097] Test case I. Construction and Physicochemical Characterization of FPBC / NO@HP The construction process of FPBC / NO@HP was characterized by multiple dimensions, including synthesis schematic, morphology, composition, crystal structure, surface chemistry, magnetic response, and light absorption.

[0098] The synthetic route for FPBC / NO@HP is as follows: Figure 1 As shown, this synthetic route utilizes Fe3O4 to derive a magnetic core, Prussian blue-related optical / catalytic framework, and CeO2. 2-x Redox active components, NO loading, and HA-PBA-gated chemistry are integrated into the same nanoparticle architecture, rather than being dispersed in separate materials.

[0099] TEM and HRTEM images of FPBC / NO@HP confirm as follows Figure 2As shown, after stepwise assembly and surface modification, the final FPBC / NO@HP formulation still retains the Fe-containing dark region within the composite particle structure.

[0100] STEM-EDS element mapping for FPBC / NO@HP as follows Figure 3 As shown, the elemental mapping reveals that the Fe, Ce, N, and O signals overlap within the same particle region, supporting the view that it is an integrated inorganic / nitrogen-containing complex rather than a simple mixture of isolated phases.

[0101] The XRD pattern of FPBC / NO@HP is as follows Figure 4 As shown in the figure, the main crystal diffraction peaks were still retained after gradual modification, indicating that NO loading and surface coating did not destroy the inorganic structural domains.

[0102] Zeta potential analysis and DLS of FPBC / NO@HP are as follows: Figure 5 and Figure 6 As shown, Zeta potential analysis revealed a change in surface charge after the formation of the composite structure, while DLS confirmed that the hydrated particle size gradually increased from Fe3O4 to FPBC and then to FPBC / NO@HP.

[0103] XPS plots for FPBC / NO@HP are as follows Figure 7 As shown in the figure, Fe 2p, Ce 3d, N 1s and O 1s signals were further detected, and the chemical state characteristics of Fe and mixed valence Ce were shown in the accessible area of ​​the surface.

[0104] The hysteresis loop of FPBC / NO@HP is as follows Figure 8 As shown in Figure A, the figure demonstrates that despite the reduction in mass-normalized magnetization due to nonmagnetic coating and functionalization, FPBC / NO@HP retains its magnetic response to changes in the external magnetic field.

[0105] The UV-vis-NIR spectrum of FPBC / NO@HP is as follows: Figure 8 As shown in Figure B, the figure shows that FPBC / NO@HP has a wider and stronger absorption, providing an optical basis for subsequent near-infrared assisted experiments.

[0106] II. Formation and Overall Performance of Dynamic Hydrogel Dressing FPBC / NO@HP-Gel in Wound Adaptability After the nanoparticles were constructed, FPBC / NO@HP were introduced into the dynamic hydrogel matrix. A schematic diagram of the formation is shown below. Figure 9As shown in the figure, OHA and QCS-Cat form a cross-linked network through dynamic Schiff base chemistry, while FPBC / NO@HP particles are uniformly embedded in the gel, resulting in the hydrogel dressing FPBC / NO@HP-Gel. The performance of this hydrogel dressing FPBC / NO@HP-Gel was then tested.

[0107] (a) Elasticity and self-healing properties test of hydrogel dressing FPBC / NO@HP-Gel The results of the elasticity and self-healing performance tests are as follows: Figure 10 and Figure 11 As shown, frequency scanning rheology ( Figure 10 This confirms that the hydrogel dressing FPBC / NO@HP-Gel exhibits solid-like behavior: within the tested frequency range, the storage modulus G' is consistently higher than the loss modulus G''. Step strain rheology ( Figure 11 Further analysis shows that the hydrogel dressing FPBC / NO@HP-Gel can repeatedly recover after high-strain damage, with a recovery rate of over 80% for three consecutive cycles (approximately 90%, 86%, and 82%, respectively). This property endows the hydrogel dressing with good structural stability and injectable self-healing ability, which facilitates its rapid recovery of complete coverage after being subjected to external deformation (such as injection or wound compression), thereby adapting to irregular dynamic wounds and maintaining local barrier function for a long time.

[0108] (II) Swelling and Degradation Performance Tests of Hydrogel Dressing FPBC / NO@HP-Gel The results of the swelling and degradation performance tests are as follows: Figure 12 As shown in Figures A and B, Figure 12 Figure A shows that swelling increases rapidly during the early incubation period and then plateaus. The degree of swelling in deionized water is higher than that in PBS, indicating that the gel has significant water absorption capacity while maintaining network integrity. Figure 12 Figure B shows that in PBS (pH 7.4), the remaining mass gradually decreases over time rather than disintegrates abruptly, indicating that the gel undergoes progressive degradation. The swelling and degradation behavior described above demonstrates that the hydrogel of this invention possesses both excellent hydrophilic and absorbent properties and structural stability, enabling it to continuously absorb exudate and maintain its intact dressing shape during the wound healing cycle, thereby providing a stable moist healing environment for tissue regeneration.

[0109] (III) Adhesion performance test of hydrogel dressing FPBC / NO@HP-Gel Adhesion performance test results are as follows Figure 13 As shown, from Figure 13As shown in Figures A and B, the hydrogel exhibits measurable adhesion strength on glass, porcine skin, wet porcine skin, and liver tissue. Representative photographs also demonstrate its stable adhesion without detachment after being flipped across different substrates. This broad-spectrum adhesion is attributed to the multiple interactions (including hydrogen bonding, π-π stacking, and metal coordination) between the catechol groups provided by the QCS-Cat component in the hydrogel matrix and the substrate surface groups. These properties enable the hydrogel dressing to adhere firmly to tissue surfaces of varying properties, including moist, irregular, and dynamic wound beds, providing long-term, stable local coverage and therapeutic support for infected wounds.

[0110] (iv) Self-healing performance test of hydrogel dressing FPBC / NO@HP-Gel The self-healing performance test results are as follows: Figure 14 As shown, from Figure 14 The results show that the gel can undergo visible reconnection after being cut and reattached, indicating its macroscopic self-healing ability.

[0111] Extrusion molding and rapid sol-gel transition are respectively as follows Figure 15 As shown in Figures A and B, the hydrogel can maintain a preset shape (such as the letter "GEL") through extrusion and can complete the sol-gel transformation in a short time at room temperature. These properties indicate that the hydrogel dressing of this invention possesses both self-healing and plasticity. It can be pre-shaped according to the wound shape before use, or it can be injected to fill irregular defects and then gel in situ. Furthermore, it can autonomously restore network continuity after cracking under stress, which helps simplify clinical procedures and ensure the integrity of the local dressing coverage.

[0112] III. Infection Response Gating and Release of Chemical Effectors in Hydrogel Dressing FPBC / NO@HP-Gel The infection response behavior of FPBC / NO@HP-Gel was evaluated using color readout, pH response, gating analysis, nanozyme exposure, NO release, and TMB oxidation.

[0113] like Figure 16 As shown, macroscopically, the gel appears dark green / black under normal conditions, gradually turning brown and reddish under more intense infection simulation conditions. This macroscopic color change indicates that the hydrogel can produce a direct visual response to environmental acidification and increased oxidative stress levels, suggesting that it possesses the ability to perceive the infection microenvironment and can preliminarily determine the local infection status through visual color changes.

[0114] like Figure 17As shown, pH cycling experiments revealed reversible color and ΔE changes in the material, indicating its ability to respond to environmental acidification and return to its initial state after repeated cycles. These results demonstrate that the hydrogel of this invention possesses reversible pH-responsive characteristics and good response stability, enabling it to repeatedly sense infection-related acid fluctuations without losing its function, thus facilitating its continued effectiveness in the complex and dynamic pH environment of infected wounds.

[0115] like Figure 18 As shown, the proposed activation model posits that neutral and low H2O2 conditions maintain the gating closed state, while acidic pH, elevated H2O2, and conditions rich in bacterial enzymes can open the network structure, expose the catalytic domains, and promote NO release. This model reveals the "normal-state inert, infected-state activated" response mechanism of the hydrogel described in this invention.

[0116] Functional experiments further support this model: like Figure 19 As shown, compared with normal conditions, the relative nanozyme exposure of the hydrogel was significantly increased under infection simulation conditions. This result validates the above activation model, indicating that the infection microenvironment signal can effectively trigger structural changes in the HA-PBA gating layer, leading to an increase in the internal CeO₂ content. 2-x The Prussian blue-related catalytic sites are exposed, providing a material basis for subsequent antibacterial activity.

[0117] like Figure 20 As shown, infection-related stimuli (acidic pH, H2O2, and bacterial enzymes) significantly accelerated the release rate and cumulative release of NO in the hydrogel, while NO release was effectively inhibited under normal physiological conditions. This behavior confirms that the responsive opening of the HA-PBA gating layer to infection signals can regulate the NO release kinetics, enabling "on-demand delivery" of antibacterial gas molecules. This facilitates achieving effective therapeutic concentrations at the infection site while minimizing impact on surrounding normal tissues.

[0118] like Figure 21 As shown, the hydrogel material activated under infection simulation conditions exhibited an increased TMB oxidation reading, indicating a significant enhancement of its nanozyme activity. This result further supports the mechanism of catalytic domain exposure after gating, confirming that the hydrogel of this invention can restore or enhance its oxidase / peroxidase-like activity in an infection microenvironment, providing enzymatic catalytic support for synergistic antibacterial activity.

[0119] like Figure 22As shown, the reconstructed 3D bacterial model further visualized and verified the bacterial enzyme-related response behavior. In the presence of bacterial enzymes, the gating structure opens, consistent with the aforementioned microenvironment triggering mechanism. This result confirms the responsiveness of the hydrogel of this invention to bacterial metabolites in a 3D bacterial system that more closely resembles a real infection scenario, providing more convincing experimental evidence for its application in infected wounds.

[0120] IV. Near-infrared assisted photothermal activation, ROS generation, and NO release of hydrogel dressing FPBC / NO@HP-Gel Since photothermal input is expected to synergistically catalyze ROS generation and NO release, the near-infrared activation behavior will be evaluated next.

[0121] like Figure 23 As shown, under 808 nm near-infrared irradiation, PBS and the blank hydrogel without nanoparticles (HP-Gel) only showed slight temperature increases, while the FPBC / NO@HP-Gel hydrogel dressing exhibited a concentration-dependent temperature increase, with the temperature rise significantly increasing with increasing nanoparticle content. These results indicate that the photothermal effect of the hydrogel described in this invention originates from the photothermal conversion capability of the Prussian blue component embedded in the FPBC / NO@HP nanoparticles, and that controllable temperature rise can be achieved by adjusting the nanoparticle loading.

[0122] Figure 24 Infrared thermal imaging results under 808nm laser irradiation further confirmed that, under the same irradiation conditions, the FPBC / NO@HP-Gel hydrogel produced a significantly stronger heating effect than water and the blank hydrogel, visually demonstrating the excellent photothermal conversion performance of the hydrogel of this invention. This imaging data, along with... Figure 23 The quantitative temperature results corroborated each other, confirming the effective photothermal response of the Prussian blue component in the hydrogel network.

[0123] like Figure 25 As shown, the heating behavior of the hydrogel is power density dependent; the equilibrium temperature increases accordingly with the increase of the 808 nm laser output power density. This characteristic indicates that the photothermal heating of the hydrogel of the present invention can be flexibly controlled by adjusting the irradiation power density, providing an operational window for setting photothermal intensity differently according to the severity of infection and treatment needs.

[0124] While photothermal therapy has been widely used for local antibacterial applications, excessively high temperatures (typically >50°C) can damage surrounding normal tissue and delay wound healing. The hydrogel described in this invention belongs to a mild photothermal system, which, under optimized irradiation conditions, can control the local temperature within a suitable mild antibacterial range (e.g., 45–50°C). This temperature range is sufficient to enhance antibacterial activity while avoiding thermal damage to regenerating tissue. These mild photothermal properties allow the hydrogel of this invention to achieve a balance between enhanced antibacterial efficacy and ensure tissue compatibility, facilitating safe and effective thermo-assisted therapy in infected wounds.

[0125] like Figure 26 As shown, in the ROS generation test results, PBS and the control group under simple near-infrared irradiation both showed only weak DCFH-DA fluorescence signals, indicating no significant ROS generation; while the hydrogel containing FPBC nanoparticles showed a significant increase in fluorescence signal after near-infrared irradiation, with the FPBC / NO@HP-Gel combined with near-infrared irradiation showing the strongest signal. These results indicate that Prussian blue and CeO₂ in the hydrogel described in this invention... 2-x The component exhibits enhanced activity in catalyzing ROS generation under near-infrared excitation, and the presence of NO donors further amplifies this effect, providing a reactive oxygen species basis for the photothermal / NO / nanozyme synergistic antibacterial mechanism.

[0126] Figure 27 as well as Figure 28 The results show that the near-infrared photothermal effect can not only induce accelerated NO release on its own, but also synergistically work with infection microenvironment signals to jointly promote structural perturbation of the HA-PBA gating layer, achieving on-demand and controllable NO release. This photothermal combined NO release characteristic is beneficial for achieving synergistic antibacterial concentrations at the infection site, while avoiding premature depletion of NO under normal physiological conditions.

[0127] The above results indicate that near-infrared irradiation can simultaneously activate the dual antibacterial pathways of ROS generation and NO release in the hydrogel of this invention, providing a spatiotemporally matched triggering mechanism for photothermal / nanozyme / gas synergistic therapy.

[0128] Depend on Figure 29 As shown in Figure A, the relative ·OH fluorescence signal in the system was approximately 100% without the addition of a scavenger. After adding the NO scavenger cPTIO, the signal decreased to approximately 55%; after adding the ROS scavenger NAC, it decreased to approximately 62%; and after adding the H2O2 scavenger Catalase, it decreased to approximately 77%, all showing significant differences compared to the group without scavengers. Among these, cPTIO and NAC caused the most significant inhibition, while Catalase also produced some inhibitory effect.

[0129] The above results indicate that the active species signal generated by the hydrogel dressing FPBC / NO@HP-Gel does not originate from a single reaction, but is related to a coupled reaction involving NO, ROS, and H2O2. NO and ROS may be important factors in generating oxidative / nitrification stress and exerting antibacterial effects in this system, while H2O2 participates in the generation of active species as an upstream reaction substrate.

[0130] Depend on Figure 29 As shown in Figure B, the viable E. coli counts in the PBS combined with laser group, the HP-Gel combined with laser group, and the FPBC / NO@HP-Gel unirradiated group were approximately 8.0, 7.1, and 6.9 log, respectively. 10 CFU / mL, with little difference between groups. After FPBC / NO@HP-Gel combined with laser irradiation, the viable bacterial count decreased to approximately 2.8 log. 10 The CFU / mL level was approximately 4 log units lower than that of the unirradiated group, a statistically significant difference.

[0131] The results indicate that laser irradiation alone or HP-Gel alone is unlikely to produce a significant bactericidal effect, and FPBC / NO@HP-Gel only shows a limited antibacterial effect in the unirradiated state; the bactericidal ability is significantly enhanced after combined light irradiation, proving that 808nm irradiation can effectively activate the antibacterial function of the composite hydrogel.

[0132] A schematic diagram of the combined pathway of photothermal, ROS, and NO is shown below. Figure 30 As shown.

[0133] V. In vitro antibacterial and antibiofilm properties of hydrogel dressing FPBC / NO@HP-Gel The antimicrobial effects of multi-stimuli activation were evaluated using planktonic bacteria and biofilm models.

[0134] like Figure 31 As shown in the representative colony plates, Escherichia coli in the PBS and HP-Gel groups... Escherichia coli ( E. coli Staphylococcus aureus Staphylococcus aureus ( S. aureus ) and methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus Dense bacterial growth was observed in both (MRSA) samples, indicating that the blank gel matrix itself has limited activity.

[0135] like Figure 32 As shown, the active formulation reduces colony formation, and the combination of FPBC / NO@HP-Gel and 808 nm irradiation produces the strongest bacterial inhibition effect. (Quantitative log) 10 CFU analysis confirmed the presence of the same hierarchical trend across different strains. (See figure). E. coli Represents Escherichia coli Escherichia coli , S. aureus Represents Staphylococcus aureus Staphylococcus aureus MRSA stands for methicillin-resistant Staphylococcus aureus. Methicillin-resistance Staphylococcus aureus .

[0136] like Figure 33 and Figure 34 As shown, the anti-biofilm experiment revealed similar hierarchical structures. Crystal violet staining showed dense biofilm biomass in the PBS and blank gel groups, with staining weakening after treatment with the active component, while the FPBC / NO@HP-Gel + 808 nm group exhibited the lowest residual biomass. Among these, the figures show… S. aureus Represents Staphylococcus aureus Staphylococcus aureus MRSA stands for methicillin-resistant Staphylococcus aureus. Methicillin-resistance Staphylococcus aureus , E. coli Represents Escherichia coli Escherichia coli .

[0137] Figures 35 to 38 The Live / Dead fluorescence imaging results showed that the PBS control group and the blank gel group exhibited predominantly green viable bacterial fluorescence signals, indicating intact biofilm structure and high bacterial activity. After treatment with FPBC / NO@HP-Gel alone, the green fluorescence signal weakened while the red dead bacterial fluorescence signal increased, indicating that the hydrogel's infection-responsive antibacterial function can exert a certain bactericidal effect under conditions without external light. The FPBC / NO@HP-Gel combined with near-infrared irradiation group showed the most significant red fluorescence signal and the lowest green viable bacterial signal, indicating that the near-infrared photothermal effect and the synergistic antibacterial effect of NO / nanozyme jointly enhanced the killing efficiency of bacteria within the biofilm. These results demonstrate that the hydrogel dressing described in this invention, under near-infrared assistance, can effectively penetrate and disrupt the bacterial biofilm structure, killing bacteria embedded within the membrane, overcoming the technical obstacle of traditional antibiotics' inability to penetrate the biofilm barrier. Figure 35 and Figure 36 middle, E. coli Represents Escherichia coli Escherichia coli MRSA stands for methicillin-resistant Staphylococcus aureus. Methicillin-resistance Staphylococcus aureus .

[0138] Figure 39 The SEM images shown indicate that the bacteria in the control group had intact morphology and a dense biofilm structure; while the bacteria in the FPBC / NO@HP-Gel combined with near-infrared irradiation group showed significant morphological damage, cell wall collapse, and fragmented, disintegrating biofilms. (The image shows...) E. coli Represents Escherichia coli Escherichia coli MRSA stands for methicillin-resistant Staphylococcus aureus. Methicillin-resistance Staphylococcus aureus This result is consistent with Live / Dead fluorescent staining ( Figures 35-38Together, these findings confirm the anti-biofilm activity of the hydrogel of this invention.

[0139] Depend on Figure 40 It can be seen that Staphylococcus aureus in the control group Staphylococcus aureus ( S. aureus Methicillin-resistant Staphylococcus aureus Methicillin-resistance Staphylococcus aureus ( MRSA ) and Pseudomonas aeruginosa Pseudomonas aeruginosa ( p.aeruginosa All three treatments resulted in a large number of dense colonies. After treatment with HP-Gel, NO-Gel, FPBC / HP-Gel, and FPBC / NO-Gel, the number of bacterial colonies decreased to varying degrees. Among them, the FPBC / NO@HP-Gel combined with 808 nm irradiation group had the fewest colonies, with only a few scattered colonies remaining on some plates, and the antibacterial effect was significantly better than the other treatment groups.

[0140] The results showed that FPBC / NO@HP-Gel had good inhibitory effects on Gram-positive bacteria, drug-resistant bacteria, and Gram-negative bacteria. Irradiation at 808 nm further enhanced its bactericidal ability, indicating that NO release, FPBC-related catalytic activity, and photoresponse effect in the composite hydrogel can produce a synergistic antibacterial effect and have certain broad-spectrum antibacterial potential.

[0141] Depend on Figure 41 It can be seen that the colony count results are consistent with... Figure 40 The plate culture results were largely consistent. The viable cell count in the control group for the three bacteria was approximately 7.5–8.0 log₂O₅. 10 CFU / mL; the number of viable bacteria gradually decreased after treatment with different hydrogels. Staphylococcus aureus was significantly reduced after FPBC / NO@HP-Gel combined with 808 nm irradiation. Staphylococcus aureus ( S. aureus ), MRSA Methicillin-resistance Staphylococcus aureus (MRSA) and Pseudomonas aeruginosa Pseudomonas aeruginosa ( p.aeruginosa The viable bacterial counts decreased to approximately 4.3, 3.6, and 3.4 log, respectively. 10 The CFU / mL level was reduced by approximately 3.7 to 4.1 log units compared to the corresponding control group, and there was a significant difference compared to the relevant control treatment group.

[0142] These results further demonstrate that the combination of FPBC / NO@HP-Gel and 808 nm irradiation can significantly reduce the survival levels of different types of bacteria, while maintaining a strong bactericidal effect against MRSA, suggesting that its antibacterial effect is independent of traditional antibiotic sensitivity. The various functional components of the material exhibit progressive antibacterial effects, while the complete composite system combined with phototreatment demonstrates the strongest bactericidal ability.

[0143] VI. Hydrogel dressing FPBC / NO@HP-Gel: In vivo wound repair, bacterial clearance, magnetic recovery, and preliminary biosafety. Staphylococcus aureus Staphylococcus aureus ( S. aureus The in vivo performance of FPBC / NO@HP-Gel was evaluated in a full-thickness infected wound model. Evaluation metrics included wound monitoring, bacterial load analysis, histology, magnetic recovery, and biosafety assessment.

[0144] like Figure 42 As shown in the representative wound photographs, the PBS control group and the blank gel group without nanoparticles had larger wound areas and slower healing processes during the follow-up observation period; while the FPBC / NO@HP-Gel treatment group showed significantly accelerated wound closure, with the FPBC / NO@HP-Gel combined with near-infrared irradiation group showing the most significant wound contraction, indicating that the hydrogel of the present invention can effectively promote the healing of infected wounds under near-infrared assistance.

[0145] Figure 43 The quantitative wound area analysis results further confirmed that the FPBC / NO@HP-Gel combined with near-infrared irradiation group showed significantly faster wound closure at each time point than other control groups (PBS group, blank gel group, and FPBC / NO@HP-Gel without irradiation group), and the difference was statistically significant. This quantitative data and representative photographs ( Figure 43 The results corroborated each other, confirming the effectiveness of the hydrogel of this invention in repairing infected wounds under near-infrared synergy.

[0146] Figure 44 The images of wound tissue homogenate colonies and the results of quantitative analysis of bacterial load showed that the PBS control group and the blank gel group had a large number of colonies, indicating that the infection model was successfully established and that bacteria proliferated extensively without effective treatment. In contrast, the FPBC / NO@HP-Gel treatment group showed a significant reduction in colony count, with the group receiving combined near-infrared irradiation showing the most significant decrease. These results demonstrate that the hydrogel dressing described in this invention, under near-infrared irradiation assistance, can achieve highly efficient sterilization at the site of infected wounds, effectively reducing the bacterial load and creating a favorable microbial environment for wound healing. This reduction partially explains the improvement in macroscopic wound healing, as a sustained bacterial load would prolong inflammation and delay re-epithelialization.

[0147] Figure 45 and Figure 46 The histological analysis results shown further support the promoting effect of the combined treatment strategy described in this invention on tissue regeneration. H&E staining shows ( Figure 45 In the FPBC / NO@HP-Gel combined with near-infrared irradiation group, the epidermal and dermal structures of the wound tissue were more intact and orderly, the coverage of newly formed epithelium was larger, and the infiltration of inflammatory cells was significantly reduced; Masson's trichrome staining showed that ( Figure 46 The collagen deposition in this group was denser and more regularly arranged, indicating improved maturity of the newly formed tissue. This was particularly evident in the FPBC / NO@HP-Gel + 808 nm group. These results demonstrate that the hydrogel dressing described in this invention, based on its responsive release of antibacterial factors in the infection microenvironment and combined with near-infrared photothermal synergistic therapy, can not only effectively control local infection but also create a favorable microenvironment for wound tissue regeneration, promoting epidermal re-epithelialization and dermal collagen remodeling, thus accelerating the transition of the wound from the repair phase to the maturation phase.

[0148] Figure 47 Figures A and B illustrate how the Fe3O4 magnetic core of the hydrogel dressing of this invention imparts excellent magnetic responsiveness, allowing it to be quickly retrieved from the wound area under the influence of an external magnetic field. This magnetic retrieval characteristic facilitates non-invasive removal of the material after treatment, reduces the risk of nanoparticle residue in the body, and provides a convenient magnetically controlled means for on-demand replacement or removal of the wound dressing.

[0149] Figure 48 AD chart and Figure 49 Preliminary biosafety assessment showed that no significant abnormalities were observed in the major organ tissue structures after treatment with the hydrogel dressing FPBC / NO@HP-Gel described in this invention. Figure 48 ), hematological indicators ( Figure 49 No significant deviations from the normal range were observed. This result indicates that the hydrogel of the present invention has good biocompatibility and safety in vivo.

[0150] The applicant declares that the technical solution of this invention is illustrated by the above embodiments, but this invention is not limited to the above embodiments, that is, it does not mean that this invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the products of this invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of this invention.

Claims

1. An infection-responsive nanoparticle multifunctional hydrogel dressing, characterized in that, The hydrogel dressing comprises a hydrogel matrix and magnetic composite nanoparticles loaded in the hydrogel matrix; the hydrogel matrix is constructed by Schiff base reaction of catechol quaternized chitosan QCS-Cat and oxidized hyaluronic acid OHA; the magnetic composite nanoparticles are prepared by taking Fe3O4 as a magnetic core, taking Prussian blue PB as a photo-thermal / catalytic intermediate layer, and taking oxygen vacancy-containing cerium dioxide CeO 2-x The surface active layer is a ternary carrier, on which a NO donor is loaded, and the obtained product is capped and coated by a gate layer of hyaluronic acid HA-PBA modified by phenylboronic acid.

2. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 1, characterized in that, The preparation process of the magnetic composite nanoparticles is as follows: S1. Preparation of magnetic core: The iron source was reduced in a polyol solvent in the presence of a dispersant and a precipitant using a solvothermal method. The magnetic precipitate obtained after the reaction was collected and washed with anhydrous ethanol and deionized water alternately to remove impurities. The washed precipitate was dried to obtain magnetic iron(III) oxide (Fe3O4) nanoparticles. S2, Intermediate layer coating: The Fe3O4 nanoparticles are dispersed in an aqueous medium. After adjusting the pH, a ferricyanide precursor solution is added sequentially. A Prussian blue PB coating layer is formed on the surface of the Fe3O4 nanoparticles through in-situ coordination reaction, resulting in Fe3O4@PB composite particles. S3. External functionalization modification: The Fe3O4@PB composite particles are dispersed in a precursor solution containing cerium salt and an alkaline source. Through low-temperature aqueous in-situ hydrolysis, cerium dioxide (CeO) containing oxygen vacancies is formed on the surface of the Fe3O4@PB composite particles. 2-x Layers were formed to obtain FPBC composite particles; S4. Active substance loading: The FPBC composite particles are mixed with nitric oxide (NO) donor molecules under low temperature and light-protected conditions, so that the NO donor is loaded into the pores and / or surface of the FPBC composite particles to obtain FPBC / NO composite particles. S5. Assembly of the intelligent gated layer: Prepare FPBC / NO composite particle dispersion and hyaluronic acid (HA-PBA) solution modified with phenylboronic acid respectively. Add the HA-PBA solution dropwise to the FPBC / NO composite particle dispersion. Induce cross-linking of HA-PBA molecular chains by pH control to form a microporous HA-PBA gated layer on the surface of the FPBC / NO composite particles, and obtain the target magnetic composite nanoparticles FPBC / NO@HP.

3. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S1, the iron source is ferric chloride hexahydrate, the polyol is ethylene glycol, the dispersant is polyethylene glycol, the precipitant is anhydrous sodium acetate, and the mass ratio of ferric chloride hexahydrate, polyethylene glycol, and anhydrous sodium acetate is 1:(0.5-1):(2-3); the reduction reaction is carried out at a temperature of 180-220°C for 6-12 hours.

4. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S2, the ferricyanide precursor includes ferric chloride hexahydrate and potassium ferrocyanide K4[Fe(CN)6]·3H2O. The ferric chloride hexahydrate solution is added first, followed by the potassium ferrocyanide K4[Fe(CN)6]·3H2O. The concentration ratio of the Fe3O4 nanoparticle solution, the ferric chloride hexahydrate solution, and the potassium ferrocyanide K4[Fe(CN)6]·3H2O is 1:5:

5. The pH value of the aqueous medium is adjusted to 3.5-4.

0.

5. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S3, the cerium salt is cerium nitrate, the alkali source is hexamethylenetetramine, and the mass ratio of the Fe3O4@PB composite particles, cerium nitrate, and hexamethylenetetramine is 1:(0.7-1):(0.3-0.7). The temperature of the low-temperature aqueous phase in-situ hydrolysis reaction is 70-90℃, and the time is 3-6 h.

6. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S5, the concentration ratio of the FPBC / NO composite particle dispersion to the HA-PBA solution is 1:2; the pH adjustment is specifically as follows: first, HA-PBA is adsorbed onto the particle surface under pH conditions of 7.0 to 7.6, then the pH is adjusted to 7.8 to 8.2 to induce the formation of borate ester crosslinking bonds, and after the reaction is completed, the pH is adjusted back to 7.

4.

7. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S4, the NO donor is S-nitrosoglutathione (GSNO), and the loading process is carried out at 0–10°C under light-protected conditions for 10–15 h. The preparation process of S-nitrosoglutathione (GSNO) is as follows: glutathione is dissolved in an acidic medium, and nitrite solution is slowly added under low temperature and light-protected conditions to carry out the nitrosation reaction. After the reaction is completed, the pH is adjusted to 5.5–6.5 with an alkaline solution to obtain the GSNO solution. The mass ratio of glutathione to nitrite is (4–5):

1.

8. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 2, characterized in that, In step S5, the preparation method of phenylboronic acid modified hyaluronic acid HA-PBA is as follows: hyaluronic acid HA is dissolved in a weakly acidic buffer solution, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide are added to activate the carboxyl group, 3-aminophenylboronic acid is added to the activation system, and an amidation reaction is carried out under pH 6.0-6.5 conditions. After the reaction is completed, the hyaluronic acid modified hyaluronic acid HA-PBA is obtained by dialysis, purification and freeze drying; wherein, the mass ratio of hyaluronic acid, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, N-hydroxysuccinimide and 3-aminophenylboronic acid is 1:(0.5-0.7):(0.1-0.4):(0.5-0.7).

9. The infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 1, characterized in that, The preparation method of the catecholized quaternized chitosan QCS-Cat includes the following steps: (1) Synthesis of quaternized chitosan QCS Chitosan powder was dispersed in deionized water and then 0.1-5 wt% dilute acetic acid solution was added to prepare an aqueous solution of 0.1-1 wt%. Then 0.025-0.10 g / mL glycidyl trimethylamine chloride was added to carry out the reaction. The reaction product was dialyzed to remove small molecule impurities and then freeze-dried to obtain purified quaternized chitosan QCS material. (2) Synthesis of catecholized quaternized chitosan QCS-Cat Quaternized chitosan QCS material was dissolved in deionized water to prepare a 0.1–1 wt% aqueous solution. 0.001–0.005 g / mL of 3-(2,4-dihydroxy)phenylpropionic acid and 0.001–0.005 g / mL of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride were added sequentially to the solution. The reaction was carried out at pH 4–5.5 for 12 h. The resulting product was dialyzed and lyophilized to obtain catecholized quaternized chitosan QCS-Cat.

10. A method for preparing the infection-responsive nanoparticle multifunctional hydrogel dressing according to claim 1, characterized in that, Includes the following steps: Magnetic composite nanoparticles were dispersed in a phosphate buffer solution at pH 7.

4. The dispersion was then mixed with a QCS-Cat precursor solution to obtain a QCS-Cat precursor solution containing magnetic composite nanoparticles. This precursor solution was then mixed with an OHA precursor solution at a volume ratio of 1:

1. After mixing, the mixture was allowed to stand for 10–18 minutes at 20–25°C and pH 7.2–7.6 to obtain a hydrogel dressing.