An artificial blood vessel matrix and a method for preparing and using the same

By embedding selenium-containing ether segments into artificial blood vessel materials, a continuous nanofiber network structure was constructed, which solved the problems of oxidative stress and inflammatory microenvironment, enabled endothelial cell adhesion and migration, and improved the interfacial integration and long-term service capability of artificial blood vessels.

CN123148459APending Publication Date: 2026-11-24RESEARCH INSTITUTE OF TRANSVASCULAR IMPLANTATION EQUIPMENT ZHEJIANG MEDICAL SECOND HOSPITAL BINJIANG DISTRICT HANGZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611591260.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing artificial blood vessel materials are susceptible to oxidative stress and inflammatory microenvironment after implantation, resulting in insufficient endothelial cell adhesion, migration, and interfacial integration. Furthermore, the uniform distribution and long-term stability of selenium-containing polymer materials in the nanofiber matrix are insufficient.

Method used

A continuous nanofiber network structure was constructed by embedding a polymer compound containing selenium ether segments into the polymer backbone, forming a continuous distribution of selenium-containing structures inside, on the surface and at the interface of the fiber. This was then combined with electrospinning technology to prepare an artificial blood vessel matrix.

Benefits of technology

It improves the functional stability of the material under oxidative stress and enhances its ability to adhere to and spread endothelial cells, promotes endothelial repair and interfacial integration, and strengthens the long-term service potential of artificial blood vessels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148459A_ABST
    Figure CN123148459A_ABST
Patent Text Reader

Abstract

This application relates to an artificial vascular matrix, its preparation method, and its application. The artificial vascular matrix is ​​a continuous nanofiber network structure formed by a polymer material. The polymer material includes a polymer compound containing selenium ether segments, which contains a -R-Se-R′- structure, wherein R and R′ are the same or different, and are independently selected from C2-C12 alkylene groups, polyether segments, or polyester segments. The artificial vascular matrix obtained in this application has a continuous fiber network structure, suitable pore morphology, and flexible mechanical characteristics. Through the synergistic construction of the selenium-containing ether segments and the nanofiber structure, the selenium-containing structure is continuously distributed within the fibers, on the fiber surface, and at the interfiber interfaces. This provides interfacial stability and oxidative stress regulation capabilities in the oxidative stress environment associated with artificial vascular implantation, and promotes endothelial cell adhesion, spreading, and migration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of biomedical polymer materials technology, and in particular to an artificial blood vessel matrix, its preparation method and application. Background Technology

[0002] Artificial blood vessels are important implantable materials in surgical reconstruction and vascular replacement therapy for vascular diseases, commonly used in scenarios such as vascular bypass, vascular replacement, and vascular access construction. Currently, the artificial blood vessel materials commonly used in clinical practice and research mainly include polytetrafluoroethylene (PTFE), polyester polymers, and some biodegradable polymers. These materials can provide the mechanical support and luminal structure required for vascular replacement to a certain extent, but their surfaces are mostly relatively bioinert. During long-term implantation, problems such as insufficient endothelialization, inadequate tissue integration, persistent inflammatory response, intimal hyperplasia, and thrombosis may still occur, especially in small-diameter artificial blood vessels, which are more likely to affect vascular patency and long-term service stability.

[0003] Following implantation of artificial blood vessels, factors such as surgical trauma, hemodynamic changes, foreign body reactions, and local inflammatory responses can lead to increased oxidative stress levels at the implantation site, accompanied by the accumulation of reactive oxygen species (ROS) and free radicals. Excessive ROS not only affect the survival, adhesion, migration, and functional maintenance of endothelial cells but may also exacerbate inflammatory responses and abnormal smooth muscle cell proliferation, thus hindering early endothelial repair and subsequent tissue integration of the artificial blood vessel. Traditional polymeric artificial blood vessel materials typically lack the ability to actively regulate the local oxidative stress microenvironment, making it difficult to provide a continuously stable functional interface for endothelial cell repair in complex implantation environments. Electrospun nanofiber materials, due to their high specific surface area, tunable pore structure, and extracellular matrix-like fibrous morphology, have been widely used in the construction of artificial blood vessels and vascular repair materials. Nanofiber structures facilitate cell adhesion, spreading, and migration, and also help regulate interfacial reactions between materials and tissues. However, if nanofiber materials are still primarily composed of conventional inert polymers, their role in regulating the antioxidant microenvironment, alleviating inflammation, and repairing endothelial function remains limited, failing to fully meet the functional requirements of the complex biological interface after artificial blood vessel implantation.

[0004] Selenium is an important element in various antioxidant enzyme systems in the body, and selenium-containing polymers have potential applications in scavenging reactive oxygen species, regulating the redox microenvironment, and promoting tissue repair. Existing research and patents have attempted to introduce selenium-containing structures into artificial blood vessel materials, for example, using diselenyl polyurethane as an elastic inner layer, combined with an outer support structure, support ring, or heparin anticoagulant coating to improve the mechanical properties and blood compatibility of artificial blood vessels. However, existing selenium-containing polymers often employ side-chain modification or local physical blending, resulting in problems such as excessively deep embedding of selenium-containing active sites or easy loss. The uniform distribution within the nanofiber matrix, the stability during long-term wet service, and the sustained regulation of endothelial cell repair behavior under oxidative stress still require further improvement. In particular, the antioxidant kinetics and wet stability of selenium-containing ether segments with different specific structures embedded in the main chain have not yet been fully and systematically studied and optimized.

[0005] Therefore, it is necessary to develop a novel artificial blood vessel matrix material with a well-defined structure, which is stably introduced into the polymer backbone through specific raw material selection and embedding. This material can maintain the flexibility and structural stability required for artificial blood vessel matrix, while possessing a superior ability to regulate the oxidative stress microenvironment and providing a suitable interface for endothelial cell adhesion, migration and repair, thereby significantly improving the interface integration and long-term service potential of artificial blood vessels after implantation. Summary of the Invention

[0006] To address the aforementioned technical problems, this application provides an artificial vascular matrix, its preparation method, and its application. The artificial vascular matrix provided in this application solves the problem that existing artificial vascular materials are susceptible to oxidative stress and inflammatory microenvironment after implantation, leading to insufficient endothelial cell adhesion, migration, functional maintenance, and interfacial integration.

[0007] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, this application provides an artificial blood vessel matrix, wherein the artificial blood vessel matrix is ​​a continuous nanofiber network structure formed of a polymer material; the polymer material includes a polymer compound containing selenium ether segments, the polymer compound containing selenium ether segments comprising a -R-Se-R′- structure, wherein R and R′ are the same or different, and are each independently selected from C2-C12 (e.g., C2, C4, C6, C8, C10, C12, etc.) alkylene segments, polyether segments, or polyester segments.

[0008] Unlike existing artificial blood vessels that rely on outer / inner composite walls, external support rings, or heparin anticoagulant coatings to achieve comprehensive performance, this application introduces selenium ether segments into polymer segments via embedding. This allows selenium to exist stably within the polymer segments through chemical bonds (rather than relying solely on surface coating or post-modification to introduce functional components), and further constructs a monolithic nanofiber matrix. This results in a continuous distribution of selenium-containing structures within the fibers, on the fiber surface, and at the interfiber interfaces. While maintaining flexible structural support and suitable pore morphology, this matrix provides excellent interfacial stability and reactive oxygen species scavenging capacity in the oxidative stress environment associated with artificial blood vessel implantation, and provides a suitable nanofiber interface for endothelial cell adhesion, spreading, and migration.

[0009] In some embodiments, the polymeric compound containing selenium ether segments is prepared by reacting a difunctional compound with a selenium ether structure, a polyester glycol, and a diisocyanate.

[0010] In some embodiments, the difunctional compound containing a selenium ether structure has the following structure: HO-R-Se-R′-OH, wherein R and R′ are the same or different, and are each independently selected from C2-C12 (e.g., C2, C4, C6, C8, C10, C12, etc.) alkylene, polyether, or polyester segments.

[0011] In some embodiments, the difunctional compound containing a selenium ether structure is selected from bis(2-hydroxyethyl)selenoether or bis(3-hydroxypropyl)selenoether.

[0012] In some embodiments, the polyester diol is selected from any one or a combination of at least two of polycaprolactone diol, polylactic acid diol, polylactic-hydroxyacetic acid diol, or polyethylene glycol-b-polycaprolactone diol.

[0013] In some embodiments, the number-average molecular weight Mn of the polyester diol is 1000-3000 g / mol (e.g., 1000 g / mol, 1500 g / mol, 2000 g / mol, 2500 g / mol, 3000 g / mol, etc.).

[0014] In some embodiments, the diisocyanate is selected from any one or a combination of at least two of hexamethylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, or diphenylmethane diisocyanate.

[0015] In some embodiments, the molar ratio of the selenium-containing difunctional compound, polyester glycol, and diisocyanate is 1:x:(1+x), where x is 0.5-2.0 (e.g., 0.5, 0.8, 1.0, 1.2, 1.5, 2.0, etc.), preferably 1:1:2.

[0016] In some preferred embodiments, the difunctional compound containing a selenium ether structure is bis(2-hydroxyethyl)selenoether, the polyester diol is polycaprolactone diol with a number-average molecular weight Mn of 1800-2200 g / mol (preferably 2000 g / mol), and the diisocyanate is hexamethylene diisocyanate. The molar ratio of the three is 1:x:(1+x), where x is 0.8-1.2, preferably 1:1:2.

[0017] In this application, the above reaction can regularly introduce the selenium ether structure into the polymer chain segment in the form of chemical bonds, thereby obtaining a polymer compound containing selenium ether segments with excellent fiber forming ability and antioxidant stability.

[0018] In some embodiments, the weight-average molecular weight (Mw) of the polymer containing the selenium ether segment is 100,000-150,000 g / mol (e.g., 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, etc.).

[0019] In some embodiments, the polymer containing selenium ether segments has the following structure: ; m represents the number of repeating caprolactone structural units in the polycaprolactone segment, and n represents the number of repeating polyurethane structural units containing selenium ether segments; m is an integer from 8 to 26 (e.g., 8, 10, 12, 17, 20, 22, 26, etc.), preferably 15-20, and more preferably 17; n is an integer from 20 to 100 (e.g., 20, 40, 50, 60, 80, 100, etc.), preferably 40-60.

[0020] In some embodiments, the diameter of the nanofibers in the artificial blood vessel matrix is ​​50-800 nm (e.g., 50 nm, 100 nm, 200 nm, 500 nm, 800 nm, etc.), preferably 100-600 nm.

[0021] In some embodiments, the polymeric material further includes any one or a combination of at least two of polycaprolactone, polylactic acid, polylactic acid-glycolic acid copolymer, polyurethane, polycarbonate, gelatin, collagen, chitosan, or derivatives thereof.

[0022] In this application, the polymer compound containing selenium ether segments can also be blended with the other polymer materials mentioned above to adjust the fiber formability, mechanical properties, degradation behavior, and flexibility of the material. The blending ratio can be adjusted according to the requirements of spinning stability and artificial blood vessel matrix performance.

[0023] In some embodiments, the artificial blood vessel matrix is ​​membranous, layered, or tubular.

[0024] In a second aspect, this application provides a method for preparing an artificial blood vessel matrix according to the first aspect, the method comprising: dissolving a polymeric material in a solvent to obtain a spinning solution; and forming a continuous nanofiber network structure in the spinning solution by electrospinning to obtain the artificial blood vessel matrix.

[0025] In some embodiments, the solvent includes any one or a combination of at least two of hexafluoroisopropanol, chloroform, dichloromethane, dimethylformamide, or tetrahydrofuran.

[0026] In some embodiments, the mass concentration of the spinning solution is 8-15 wt% (e.g., 8 wt%, 10 wt%, 12 wt%, 14 wt%, 15 wt%, etc.).

[0027] In some embodiments, the electrospinning voltage is 10-25 kV (e.g., 10 kV, 15 kV, 20 kV, 25 kV, etc.), the spinning solution flow rate is 0.5-2.0 mL / h (e.g., 0.5 mL / h, 1.0 mL / h, 1.5 mL / h, 2.0 mL / h, etc.), and the receiving distance is 10-18 cm (e.g., 10 cm, 12 cm, 14 cm, 16 cm, 18 cm, etc.).

[0028] In some embodiments, when preparing a membrane or layered artificial blood vessel matrix, a flat plate or roller receiver is used for receiving.

[0029] In some embodiments, when preparing the tubular artificial blood vessel matrix, a rotating rod-shaped receiver is used for receiving the material. The diameter of the rotating rod-shaped receiver is 1-6 mm (e.g., 1 mm, 2 mm, 3 mm, 4 mm, 6 mm, etc.), and the rotation speed is 300-1500 rpm (e.g., 300 rpm, 500 rpm, 800 rpm, 1000 rpm, 1200 rpm, 1500 rpm, etc.).

[0030] In this application, the inner diameter, wall thickness, pore structure, fiber orientation, and flexibility of the resulting matrix can be controlled by adjusting the receiver diameter, rotation speed, spinning time, and fiber deposition amount.

[0031] In some embodiments, the electrospinning process further includes a solvent removal operation, such as drying the material in a ventilated environment or under vacuum conditions.

[0032] In some embodiments, the electrospinning process further includes thermal stabilization treatment, physical crosslinking, or chemical crosslinking to improve the structural stability of the material in a humid environment.

[0033] Thirdly, this application provides the use of the artificial blood vessel matrix according to the first aspect in the preparation of artificial blood vessel materials.

[0034] In some embodiments, the artificial blood vessel material is a small-diameter artificial blood vessel material, an artificial blood vessel inner surface interface layer material, an artificial blood vessel wall matrix layer material, or a blood vessel repair matrix material.

[0035] Compared with the prior art, this application has at least the following beneficial effects: (1) In this application, selenium-containing ether segments are embedded into the polymer backbone or side chain, so that the selenium-containing structure no longer depends solely on adsorption, coating or post-modification on the material surface, but is stably distributed in the polymer segments and the nanofiber as a whole. As a result, the selenium-containing structure can be continuously presented inside the fiber, on the fiber surface and at the fiber interface, which is beneficial to improving the functional stability and continuity of the material in a wet service environment.

[0036] (2) The high molecular weight compound containing selenium ether segments obtained in this application is electrospun into a continuous nanofiber network structure, which has a high specific surface area, suitable pore morphology and flexible mechanical characteristics. This structure has certain similarities with the natural extracellular matrix, which can provide more contact sites and suitable interfaces for endothelial cell adhesion, spreading and migration, which is beneficial to the early cell response and interface integration after artificial blood vessel implantation.

[0037] (3) This application utilizes the synergistic design of selenium-containing ether segments and nanofiber structures to enable the material to possess redox regulation capabilities in the oxidative stress environment associated with artificial blood vessel implantation. This material can be used to reduce local reactive oxygen species levels, mitigate the adverse effects of oxidative stress on endothelial cell survival, adhesion, migration, and functional maintenance, thereby promoting the endothelial repair process on the surface of the artificial blood vessel matrix.

[0038] (4) This application differs from artificial blood vessel solutions that primarily rely on an outer / inner composite wall or heparin anticoagulant coating to achieve comprehensive performance. This application uses an integral selenium-containing ether segment nanofiber matrix as its core, integrating the selenium-containing structure with the fiber matrix body, without requiring a heparin anticoagulant coating or external support rings as essential components. Therefore, this material can be used as an inner surface interface layer, a wall matrix layer, or an integral tubular scaffold for artificial blood vessels, providing a new functionalized matrix solution for small-diameter artificial blood vessels and vascular repair materials. Attached Figure Description

[0039] Figure 1 This is an energy dispersive spectroscopy (EDS) analysis chromatogram of the selenium-containing ether segment polyurethane polymer obtained in Example 1, in which a selenium element signal can be detected.

[0040] Figure 2 This is a photograph of the polyurethane polymer containing selenium ether segments prepared in Example 1.

[0041] Figure 3 This is a photograph of the tubular artificial blood vessel matrix in Example 1.

[0042] Figure 4 This is a scanning electron microscope image of the membranous artificial blood vessel matrix in Example 1.

[0043] Figure 5 The image shows the Fourier transform infrared spectra of the membrane-like and tubular artificial blood vessel matrix obtained in Example 1.

[0044] Figure 6 This is a tensile stress-strain curve of the membrane-like artificial blood vessel matrix obtained in Example 1.

[0045] Figure 7 The image is a scanning electron microscope image of the polyurethane nanofiber matrix without selenium ether segments in Test Example 1 after treatment with H2O2 solution for 24 h, denoted as PU / H2O2 group.

[0046] Figure 8 The image is a scanning electron microscope image of the polyurethane nanofiber matrix containing selenium ether segments in Test Example 1 after treatment with H2O2 solution for 24 h, denoted as Se-PU / H2O2 group.

[0047] Figure 9 This is a tensile stress-strain curve of three parallel specimens of the Se-PU / H2O2 group after being treated with H2O2 solution for 24 h in Test Example 1 (Note: the black, red and blue curves represent the three parallel specimens of the Se-PU / H2O2 group respectively).

[0048] Figure 10 This is a diagram showing the cell morphology, cytoskeleton, and CD31 expression of HUVECs in the blank group, PU group, and Se-PU group in test example 2 (Blank represents the blank control group without material, PU represents the polyurethane nanofiber matrix group without selenide segments, and Se-PU represents the polyurethane nanofiber matrix group containing selenide segments). Detailed Implementation

[0049] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments. However, the examples below are merely simplified examples of this application and do not represent or limit the scope of protection of this application. The scope of protection of this application shall be determined by the claims.

[0050] Preparation Example 1 Preparation of polyurethane polymers containing selenium ether segments 10.0 g (5.0 mmol) of vacuum-dried polycaprolactone diol (PCL-diol, Mn = 2000 g / mol) was weighed and added to 50 mL of anhydrous tetrahydrofuran, and stirred until completely dissolved. Under nitrogen protection, 1.68 g (10.0 mmol) of hexamethylene diisocyanate (HDI) and stannous octoate catalyst were added, with the amount of stannous octoate being 0.1 wt% of the total mass of the reactants. The mixture was stirred at 70 °C for 2 h to obtain an isocyanate-terminated prepolymer. Subsequently, 0.78 g (5.0 mmol) of selenium-containing diol HO—CH2CH2—Se—CH2CH2—OH was added, and the reaction was continued at 85 °C for 6 h. After the reaction was completed, the reaction solution was cooled to room temperature and slowly added dropwise to excess cold diethyl ether to precipitate. The precipitate was collected and washed three times with diethyl ether, and then vacuum-dried at 40 °C for 48 h to obtain a polyurethane polymer containing selenium ether segments.

[0051] The structural formula of the obtained product is: The molecular weight of the obtained selenium-containing ether segment polyurethane was determined by gel permeation chromatography, and the weight-average molecular weight (Mw) was 128,000 g / mol. The energy dispersive spectroscopy (EDS) results are as follows: Figure 1 As shown, a clear selenium signal was detected in the obtained polymer, indicating that the selenium-containing ether structure was successfully introduced into the polyurethane molecular chain. A photograph of the obtained polyurethane containing selenium ether segments is shown below. Figure 2 As shown.

[0052] Example 1 This embodiment provides a method for preparing an artificial blood vessel matrix: The polymer obtained in Preparation Example 1 was weighed and dissolved in hexafluoroisopropanol. The solution was stirred at room temperature for 6 h to prepare a spinning solution with a mass concentration of 10 wt%. The spinning solution was loaded into a syringe and processed using an electrospinning device. The spinning parameters were set as follows: spinning voltage 15 kV, spinning solution flow rate 1.0 mL / h, distance from the nozzle to the receiver 15 cm, ambient temperature 25℃, and relative humidity 45%. When preparing nanofiber membranes, a flat plate receiver was used for collection; when preparing tubular artificial blood vessel matrix, a rotating rod-shaped receiver with a diameter of 3 mm was used at a rotation speed of 800 rpm. After continuous spinning for 2 h, samples were taken and dried in a vacuum drying oven for 24 h to completely remove residual solvent. Membrane-like artificial blood vessel matrix and tubular artificial blood vessel matrix were obtained, with the tubular artificial blood vessel matrix sample shown below. Figure 3 As shown.

[0053] The resulting membranous artificial blood vessel matrix was observed using a scanning electron microscope. Figure 4As shown, the resulting membranous artificial blood vessel matrix is ​​composed of continuous, overlapping fibers. At least three fields of view were randomly selected, and no fewer than 30 fibers were measured in each field of view. The average diameter of the fibers was 300 ± 50 nm, and the overall structure presented a continuous fiber network.

[0054] Fourier transform infrared spectroscopy analysis was performed on the obtained membranous and tubular artificial blood vessel matrix, and the results are as follows: Figure 5 As shown. The infrared spectra of both the membrane and tubular samples are at approximately 3320 cm⁻¹. -1 An absorption peak for N-H stretching vibrations appears at approximately 2930 cm⁻¹. -1 and 2860 cm -1 An aliphatic C-H stretching vibration absorption peak appears at approximately 1720 cm⁻¹. -1 An absorption peak for the stretching vibration of the C=O group in the urethane group appears at approximately 1100 cm⁻¹. -1 An absorption peak for the C—O—C stretching vibration appears at approximately 2270 cm⁻¹. Simultaneously, an absorption peak for the C—O—C stretching vibration is observed at approximately 2270 cm⁻¹. -1 No obvious free -NCO characteristic absorption peaks were observed, indicating that the isocyanate groups have basically participated in the reaction and formed a polyurethane structure. The main characteristic absorption peaks of the film and tubular samples are basically the same, indicating that the electrospinning method has not significantly changed the main chemical structure of the material.

[0055] The uniaxial tensile properties of the obtained membranous artificial blood vessel matrix were tested. The samples were cut into strips 50 mm long and 10 mm wide, and the thickness was measured using calipers or a thickness gauge. The samples were fixed between the clamps of a universal testing machine with an initial clamp spacing of 20 mm, and uniaxial tension was applied at a tensile speed of 10 mm / min at room temperature until the samples fractured. The tensile stress was calculated based on the initial cross-sectional area of ​​the samples, and the stress-strain curves were recorded. Five parallel samples were used in each group, and the test results are shown below. Figure 6 As shown, the resulting membrane-like artificial blood vessel matrix exhibits a continuous stress-strain response and does not show significant interlayer delamination during stretching, indicating that the continuous nanofiber network formed by electrospinning has a certain load-bearing capacity and tensile deformation capability.

[0056] Comparative Example 1 This comparative example provides a method for preparing a polyurethane artificial blood vessel matrix that does not contain selenium ether segments.

[0057] This comparative example uses commercially available medical-grade thermoplastic polyurethane as a control material free of selenium ether segments. The polyurethane was purchased from Lubrizol, product model Tecoflex™ SG-80A, with a weight-average molecular weight (Mw) of 100,000-150,000 g / mol as determined by gel permeation chromatography. The polyurethane was dissolved in hexafluoroisopropanol and stirred at room temperature for 6 hours to prepare a spinning solution with a mass concentration of 10 wt%. The spinning solution was loaded into a syringe and processed under the same electrospinning conditions as in Example 1: a spinning voltage of 15 kV, a spinning solution flow rate of 1.0 mL / h, a needle-to-receiver distance of 15 cm, an ambient temperature of 25°C, and a relative humidity of 45%. Fibers were collected using a flat plate receiver. After 2 hours of continuous spinning, samples were taken and dried in a vacuum drying oven for 24 hours to remove residual solvent, yielding a PU nanofiber artificial blood vessel matrix free of selenium ether segments.

[0058] Test Example 1 Structural stability test after oxidative environmental treatment The polyurethane nanofiber matrix containing selenium ether segments obtained in Example 1 was designated as the Se-PU group, and the polyurethane nanofiber matrix without selenium ether segments obtained in Comparative Example 1 was designated as the PU group. Both groups of samples were immersed in physiological saline solution containing 1 mmol / L H2O2 and treated at 37°C for 24 h. The treated samples were designated as the Se-PU / H2O2 group and the PU / H2O2 group, respectively.

[0059] After H2O2 treatment for 24 h, the sample was removed and observed using a scanning electron microscope. The results are as follows: Figure 7 and Figure 8 As shown, some nanofibers in the PU / H2O2 group exhibited swelling, adhesion, and blurred fiber boundaries; in contrast, the Se-PU / H2O2 group maintained a relatively clear and continuous nanofiber network structure, with no obvious large-area fusion between fibers. Uniaxial tensile tests were performed on the Se-PU nanofiber matrix after H2O2 treatment for 24 h. The results are as follows... Figure 9 As shown, all three parallel specimens exhibited continuous stress-strain response, with a maximum tensile stress of approximately 3.0-3.5 MPa and an elongation at break of approximately 40%-60%, indicating that the Se-PU nanofiber matrix still maintains a certain load-bearing capacity and tensile deformation capacity after H2O2 treatment.

[0060] Test Example 2 In vitro cell co-culture and evaluation of endothelial cell behavior HUVECs were 2×10 4 pcs / cm 2Cells were seeded at various densities on the surfaces of Se-PU, PU, ​​and unsupported cell culture plates, and cultured for 24 h to allow for full cell adhesion. H2O2 was then added to the culture medium to a final concentration of 200 μmol / L, and cultured for another 24 h. After culture, cells in each group were fixed, their cytoskeleton and CD31 were immunofluorescently stained, and cell morphology, spreading, and CD31 expression were observed using a laser confocal microscope. The Se-PU group used the selenium-ether segment-containing polyurethane nanofiber matrix obtained in Example 1, the PU group used the selenium-ether segment-free polyurethane nanofiber matrix obtained in Comparative Example 1, and the blank group consisted of HUVECs cultured directly on the cell culture plate surface without any polymer material. The seeding density and culture conditions were kept consistent across all groups.

[0061] The results of laser confocal microscopy observation are as follows Figure 10 As shown, under oxidative stress conditions, compared with the PU group, the HUVECs on the surface of the Se-PU group were more fully spread, the cytoskeleton structure was more complete, and CD31 positive expression was observed, indicating that the selenium ether chain segment polyurethane nanofiber matrix is ​​beneficial to the maintenance of endothelial cell morphology and endothelial phenotype under oxidative stress conditions.

[0062] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. An artificial vascular matrix, characterized in that, The artificial blood vessel matrix is ​​a continuous nanofiber network structure formed by polymer materials; the polymer materials include polymer compounds containing selenium ether segments, the polymer compounds containing selenium ether segments contain -R-Se-R′- structures, wherein R and R′ are the same or different, and are each independently selected from C2-C12 alkylene, polyether segments or polyester segments.

2. The artificial vascular matrix according to claim 1, characterized in that, The high molecular weight compound containing selenium ether segments is prepared by reacting a difunctional compound with a selenium ether structure, a polyester diol, and a diisocyanate.

3. The artificial blood vessel matrix according to claim 2, characterized in that, The difunctional compound containing a selenium ether structure has the following structure: HO-R-Se-R′-OH, wherein R and R′ are the same or different, and are each independently selected from C2-C12 alkylene, polyether segment or polyester segment, preferably bis(2-hydroxyethyl)selenoether or bis(3-hydroxypropyl)selenoether. And / or, the polyester diol is selected from any one or a combination of at least two of polycaprolactone diol, polylactic acid diol, polylactic-hydroxyacetic acid diol or polyethylene glycol-b-polycaprolactone diol, preferably a polyester diol with a number average molecular weight Mn of 1000-3000 g / mol; And / or, the diisocyanate is selected from any one or a combination of at least two of hexamethylene diisocyanate, isophorone diisocyanate, lysine diisocyanate or diphenylmethane diisocyanate; Preferably, the molar ratio of the selenium-containing difunctional compound, polyester diol, and diisocyanate is 1:x:(1+x), where x is 0.5-2.0; Preferably, the difunctional compound containing a selenium ether structure is bis(2-hydroxyethyl)selenoether, the polyester diol is polycaprolactone diol with a number-average molecular weight Mn of 1800-2200 g / mol, the diisocyanate is hexamethylene diisocyanate, and the molar ratio of the three is 1:x:(1+x), where x is 0.8-1.

2.

4. The artificial vascular matrix according to any one of claims 1-3, characterized in that, The weight-average molecular weight (Mw) of the high molecular weight compound containing selenium ether segments is 100,000-150,000 g / mol.

5. The artificial vascular matrix according to any one of claims 1-4, characterized in that, The polymeric compound containing selenium ether segments has the following structure: ; Where m is an integer from 8 to 26, and n is an integer from 20 to 100; preferably, m is an integer from 15 to 20, and n is an integer from 40 to 60.

6. The artificial vascular matrix according to any one of claims 1-5, characterized in that, The diameter of the nanofibers in the artificial blood vessel matrix is ​​50-800 nm, preferably 100-600 nm; And / or, the polymeric material further includes any one or a combination of at least two of polycaprolactone, polylactic acid, polylactic acid-glycolic acid copolymer, polyurethane, polycarbonate, gelatin, collagen, chitosan or its derivatives; And / or, the artificial blood vessel matrix is ​​membranous, lamellar, or tubular.

7. A method for preparing an artificial vascular matrix according to any one of claims 1-6, characterized in that, The preparation method includes: dissolving a polymer material in a solvent to obtain a spinning solution; and forming a continuous nanofiber network structure in the spinning solution by electrospinning to obtain the artificial blood vessel matrix.

8. The preparation method according to claim 7, characterized in that, The solvent includes any one or a combination of at least two of hexafluoroisopropanol, chloroform, dichloromethane, dimethylformamide, or tetrahydrofuran; And / or, the mass concentration of the spinning solution is 8-15 wt%; And / or, the voltage of the electrospinning is 10-25 kV, the flow rate of the spinning solution is 0.5-2.0 mL / h, and the receiving distance is 10-18 cm; And / or, when preparing a membrane or layered artificial blood vessel matrix, a flat plate or roller receiver is used for receiving; And / or, when preparing a tubular artificial blood vessel matrix, a rotating rod-shaped receiver is used for receiving, the rotating rod-shaped receiver having a diameter of 1-6 mm and a rotation speed of 300-1500 rpm.

9. The use of an artificial blood vessel matrix according to any one of claims 1-6 in the preparation of artificial blood vessel materials.

10. The application according to claim 9, characterized in that, The artificial blood vessel material is a small-diameter artificial blood vessel material, an artificial blood vessel inner surface interface layer material, an artificial blood vessel wall matrix layer material, or a blood vessel repair matrix material.