A multiscale composite functional interface of Ti6Al4V artificial joint and a preparation method and application thereof
By constructing a multi-scale composite interface on the surface of Ti6Al4V artificial joints and combining thermal oxidation, laser texturing, and hyaluronic acid grafting, the problems of high load-bearing capacity, low wear, and long-term antibacterial properties of Ti6Al4V artificial joints were solved, achieving a synergistic improvement in high load-bearing capacity, stable lubrication, and antibacterial performance.
Patent Information
- Application Number
- CN202611006665.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-07
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to achieve a synergistic design of high load-bearing capacity, low wear, and long-term antibacterial properties on the surface of Ti6Al4V artificial joints, and single functional modifications are insufficient to maintain stability and effectiveness under complex physiological friction environments.
By constructing a multi-scale composite interface on the surface of Ti6Al4V consisting of a "high-hardness thermal oxidation layer, biomimetic micro-nano texture, and HA functional lubrication layer," and combining thermal oxidation strengthening, laser surface texturing, and hyaluronic acid covalent grafting, a synergistic improvement in load-bearing capacity, lubrication regulation, and antibacterial properties is achieved.
It significantly improves the load-bearing capacity, wear resistance, and antibacterial properties of Ti6Al4V artificial joints, reduces the risk of friction and wear and bacterial colonization, and extends the service life of artificial joints.
Smart Images

Figure CN123148463A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of biomedical material surface engineering and biotribology, specifically involving a multi-scale functionalization construction method and application of titanium alloy (Ti6Al4V) artificial joint surface, specifically involving a method for preparing a friction-reducing and antibacterial composite interface combining thermal oxidation strengthening, laser surface texturing and hyaluronic acid covalent grafting, and the surface constructed thereby with synergistic friction-reducing and antibacterial functions. Background Technology
[0002] Artificial joint replacement surgery is one of the most effective surgical treatments for end-stage osteoarthritis, widely used in the clinical treatment of osteoarthritis, rheumatoid arthritis, and femoral head necrosis. Titanium alloy (Ti6Al4V), due to its excellent corrosion resistance, high specific strength, low density, and good biocompatibility, has become an important candidate material for artificial joint implants and is widely used in orthopedic implants such as hip and knee joints. Despite decades of development in artificial joint technology, implants still face two core problems during long-term in-body service: interfacial wear and bacterial infection, severely limiting their service life and clinical efficacy. Periprosthetic joint infection (PJI) is one of the most serious complications after artificial joint replacement surgery. Studies show that the incidence of PJI after primary total hip replacement is approximately 0.5%–2.0%, after primary total knee replacement is approximately 0.4%–2.0%, and the infection rate after revision surgery can even reach 5%–15%. PJI treatment is lengthy, costly, and has a poor prognosis, placing a significant burden on patients and the healthcare system. Besides infection issues, friction and wear are also a significant cause of long-term failure in artificial joints, accounting for approximately 25% to 40% of revision surgeries. The interface of an artificial joint is subjected to high loads, complex sliding, and boundary lubrication environments for extended periods, resulting in extremely harsh tribological conditions: peak contact pressures in the hip joint can reach 5–10 MPa, and even higher in the knee joint; relative sliding speeds during the gait cycle typically vary between 0 and 60 mm / s; the lubricating medium within the joint cavity is primarily synovial fluid containing hyaluronic acid and phospholipids, but its lubrication performance is far lower than that of engineered lubrication systems. During long-term cyclic friction, interface wear generates a large number of wear particles, triggering inflammatory responses and bone resorption, ultimately leading to aseptic loosening and failure of the implant. Furthermore, in the early stages of artificial joint service, the lubricating film has not yet stabilized, making the interface more susceptible to boundary lubrication or even localized dry friction. Therefore, developing a Ti6Al4V surface that combines initial friction reduction and antibacterial functions is crucial for improving the early stability and long-term reliability of artificial joints.
[0003] Currently, the main methods for functional modification of Ti6Al4V artificial joint surfaces include thermal oxidation strengthening, laser surface texturing, and bio-lubricating molecule modification. (1) Thermal oxidation (TO) is a commonly used and low-cost surface strengthening method. This method involves oxidizing Ti6Al4V under certain temperature conditions to form a composite structure on its surface consisting of a dense TO layer and an oxygen diffusion layer. The rutile TiO2 oxide film formed has high hardness, good chemical stability, and corrosion resistance, which can effectively improve the hardness, wear resistance, and interfacial load-bearing capacity of the Ti6Al4V surface, thereby improving the tribological properties of the artificial joint implant. (2) Laser surface texturing (LST) is a surface control technology based on ultrafast laser micro-nano processing. This technology uses picosecond or femtosecond lasers to construct a regular micro-texture array on the material surface to achieve control over interfacial contact behavior and lubrication state. Studies have shown that rationally designed microtextures can reduce the actual contact area, capture wear particles, regulate local contact stress, and form a local hydrodynamic pressure effect, thereby reducing interfacial friction and improving wear stability. In addition, inspired by the natural hierarchical structure of the elytra of the Oriental dragonfly, biomimetic microtextures have shown good application potential in liquid retention and interfacial friction reduction. (3) Hyaluronic acid (HA) is a naturally occurring anionic glycosaminoglycan in the extracellular matrix and synovial fluid of joints, with excellent biocompatibility, hydrophilicity and lubrication properties. HA can form a stable hydration layer at the friction interface, thereby reducing interfacial shear resistance; at the same time, its negative charge properties can also inhibit protein adsorption and initial bacterial adhesion to a certain extent, so it is widely used in the biolubrication and functional modification of artificial joint surfaces.
[0004] Existing research indicates that combining thermal oxidation with laser texturing can improve the tribological properties of Ti6Al4V surfaces to some extent. Furthermore, studies have used biolubricating molecules such as HA to functionalize implant surfaces, enhancing their lubrication and biocompatibility. However, a multi-scale composite interface design scheme that synergistically integrates TO strengthening, LST regulation, and HA biolubricating functions onto the Ti6Al4V surface is currently lacking.
[0005] Although existing technologies such as TO, LST, and HA functionalization can improve the tribological properties or biological functions of Ti6Al4V artificial joint implants to a certain extent, the following shortcomings still exist: (1) Although single TO treatment can improve the surface hardness and load-bearing capacity of Ti6Al4V, it mainly relies on the high-hardness oxide layer to achieve wear resistance and has limited interfacial lubrication capacity. Under complex physiological friction environment and high load conditions, the interface is still prone to large shear stress and adhesive wear, making it difficult to maintain a stable low-friction state for a long time. (2) Although LST can improve the interfacial lubrication state and reduce friction, it is difficult to effectively inhibit bacterial adhesion and biofilm formation by relying solely on surface texturing. In addition, under long-term high-load sliding conditions, stress concentration and structural damage may occur in local textured areas, affecting its long-term stability. (3) Although HA has good lubrication performance, biocompatibility, and antibacterial initial adhesion ability, the mechanical strength of the HA functional layer is low. It is prone to wear, detachment, or loss during long-term sliding friction, resulting in rapid decay of its lubrication and antibacterial functions, making it difficult to play a stable role for a long time. (4) Most existing technologies are optimized for a single function and lack synergistic design for interface load-bearing enhancement, friction regulation, biological lubrication and antibacterial functions. It is difficult to meet the comprehensive requirements of artificial joint implants for high load-bearing capacity, low wear and long-term antibacterial stability in complex service environments. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a multi-scale composite interface structure of Ti6Al4V based on the synergistic construction of TO, biomimetic laser texture and HA grafting, and its preparation method. By constructing a synergistic system of "high-hardness thermal oxidation layer - biomimetic micro-nano texture - HA functional lubrication layer" on the surface of Ti6Al4V, the interface bearing capacity, friction reduction and wear resistance and antibacterial properties are simultaneously improved.
[0007] This invention further utilizes laser-guided microtextured pits to store and mechanically protect the HA functional layer, reducing wear and shedding of HA during sliding and improving its long-term lubrication and antibacterial stability. Simultaneously, through multi-scale interface synergy, the thermal oxidation layer provides load-bearing support, the microtexture regulates interface contact behavior and stores lubricating media, and HA forms a stable hydrated lubricating layer and inhibits bacterial adhesion, thereby improving the interface stability and long-term service life of the artificial joint implant in the early stages of service.
[0008] This invention is achieved through the following technical solution: A method for preparing a multi-scale synergistic friction-reducing and antibacterial composite interface for the surface of a Ti6Al4V artificial joint includes the following steps: (1) The surface of the Ti6Al4V matrix is pretreated and a load-bearing reinforcement layer is constructed on its surface; (2) A textured surface layer with micro-nano scale structural features is constructed on the surface of the bearing reinforcement layer, the textured surface layer including microstructure units for storing lubricating medium; (3) A molecular functional layer with biological lubrication and antibacterial functions is constructed on the textured surface layer and fixed by chemical bonding.
[0009] The textured surface layer provides spatial confinement, storage and replenishment, and shear protection during friction for the molecular functional layer through microstructural units, so that the molecular functional layer maintains a continuous hydration and lubrication state and inhibits structural failure during sliding contact. The load-bearing reinforcement layer, textured surface layer, and molecular functional layer work together to enable the interface to simultaneously achieve high load-bearing support, low friction lubrication, and antibacterial adhesion properties under load.
[0010] Furthermore, the load-bearing reinforcement layer is an oxide layer or hard coating formed by thermal oxidation, micro-arc oxidation or physical vapor deposition.
[0011] Furthermore, the textured surface layer is constructed using any one of picosecond laser processing, femtosecond laser processing, nanosecond laser processing, chemical etching, electrochemical etching, or microimprinting methods.
[0012] Furthermore, the microstructure unit includes one or more combinations of micropit structures, microgroove structures, or periodic array structures, and is used to store lubricating media and molecular functional layer materials.
[0013] Furthermore, the molecular functional layer is a polymer or biomolecular layer with biolubricating properties and antibacterial adhesion capabilities. The molecular functional layer is fixed to the textured surface layer through amide bonding, silane coupling, or self-assembly.
[0014] Specifically, This invention provides a multi-scale composite functional interface for Ti6Al4V artificial joints synergistically constructed with TO, LST, and HA. It features a multi-level functional structure on the Ti6Al4V surface, consisting of a thermally oxidized hard load-bearing layer, a biomimetic laser microtextured layer, and an HA hydration lubrication and antibacterial layer. This achieves a synergistic improvement in the high load-bearing capacity, stable lubrication, and antibacterial and anti-adhesion performance of the artificial joint implant during its early service phase.
[0015] This composite functional interface is mainly suitable for the functional modification of the surface of high-load sliding contact implanted components such as artificial hip joints and artificial knee joints, and is especially suitable for artificial joint friction pairs with risks of interface wear, boundary lubrication failure and bacterial adhesion.
[0016] A method for preparing a multi-scale composite functional interface for Ti6Al4V artificial joints synergistically constructed with TO, LST, and HA is disclosed. The overall technical route includes: Ti6Al4V substrate pretreatment → thermal oxidation strengthening → laser microtexturing construction → surface hydroxylation treatment → silanization amino modification → HA activation → HA covalent grafting → construction of OCT-HA multi-scale composite functional interface. Specific steps are as follows: Step 1: Pretreatment of Ti6Al4V substrate The Ti6Al4V titanium alloy was ground and polished, and then ultrasonically cleaned with anhydrous ethanol and deionized water to remove residual particles, oil and impurities from the surface. Finally, it was dried with high-purity nitrogen for later use. Step 2: Construction of the thermal oxidation reinforcement layer The Ti6Al4V titanium alloy pretreated in step 1 was placed in a muffle furnace, heated and calcined, and then naturally cooled to room temperature with the furnace to obtain a thermally oxidized sample. Furthermore, the calcination process involves raising the temperature from room temperature to 550-700℃ at a rate of 3-10℃ / min, then holding the temperature at 550-700℃ for 6-24 hours, and finally cooling.
[0017] Step 3: Laser Microtexture Construction In step 2, the sample surface was laser-processed using a picosecond laser processing system with the following parameters: laser pulse width: 5~20 ps; focused spot diameter: approximately 20~50 μm; output power: 35%~55%; scanning speed: 200~800 mm / s; number of repeated scans: 3~8. By repeatedly scanning along a preset trajectory, a regularly arranged composite microtexture structure was formed on the thermally oxidized surface, resulting in a thermally oxidized microtextured sample, denoted as OCT (Oxidized Composite Titanium).
[0018] The constructed microtextures mainly have the following functions: (a) Reduce the actual contact area and decrease solid-solid direct contact; (b) Capture wear particles to reduce third-body wear; (c) It creates a local hydrodynamic effect, improving lubrication stability; (d) As a HA and lubricating fluid storage unit, it improves the durability of interfacial lubrication; (e) Provides mechanical protection for the subsequent HA hydrogel layer, reducing the risk of the HA layer being directly damaged by shear during the sliding process.
[0019] Step 4: Surface hydroxylation and amination modification First, the OCT sample was immersed in a 2-8 M NaOH solution at 40-80℃ for 1-4 h to form a large number of hydroxyl (–OH) active sites on the TiO2 surface. Then, the sample was immersed in a 2-8% (v / v) ethanol solution of 3-aminopropyltriethoxysilane (APTES) and reacted at room temperature for 3-8 h to form a silanized functional layer rich in amino (–NH2) on the surface, thus obtaining the OCT-NH2 sample.
[0020] This step serves the following purpose: (a) Improve surface chemical reactivity; (b) To provide amino reaction sites for subsequent HA grafting; (c) Enhance the bonding strength between the HA functional layer and the Ti6Al4V matrix.
[0021] Step 5: Covalent grafting of hyaluronic acid (HA) First, HA was dissolved in 0.05-0.2 M MES buffer (pH=5.5-6.5) at a concentration of 1-5 g / L. Then, ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS) were added. The OCT-NH2 sample was then immersed in the activated HA solution and reacted at room temperature for 12-24 h.
[0022] The total concentration of EDC / NHS was 2.5 mg / mL, with a mass ratio of EDC to NHS of 4:1.
[0023] The EDC / NHS system first activates the carboxyl groups (–COOH) in HA to form a highly reactive NHS ester intermediate. Then, the OCT-NH2 sample is immersed in the activated HA solution. During the reaction, the activated carboxyl groups of HA undergo an amidation reaction with the surface amino groups (–NH2) to form stable amide bonds (–CONH–), thereby achieving covalent fixation of HA on the textured thermal titanium dioxide surface. Finally, a composite interface with friction-reducing and antibacterial functions is formed, namely the OCT-HA multi-scale composite functional interface.
[0024] The multi-scale composite interface of Ti6Al4V artificial joint constructed in this invention consists of an HA hydration lubrication and antibacterial layer, a laser microtexture layer, a thermally oxidized TiO2 reinforcement layer, and a Ti6Al4V matrix. The functional layers form a synergistic enhancement mechanism, thereby achieving simultaneous improvement in the interface's load-bearing capacity, lubrication performance, and antibacterial performance.
[0025] in: The HA functional layer is responsible for forming a stable hydrated lubricating film and inhibiting bacterial adhesion; The microtextured layer is responsible for storing lubricating media, forming hydrodynamic pressure, and providing mechanical protection for the HA (hydraulic hydride). The thermal oxidation layer is responsible for improving the interface hardness and load-bearing capacity; The Ti6Al4V matrix provides overall structural support.
[0026] During sliding contact: (a) The thermally oxidized layer provides high-hardness support and reduces interfacial plastic deformation; (b) Microtextures reduce solid-solid direct contact through local hydrodynamic pressure effects; (c) Textured pits can store HA and lubricating fluid, improving the continuous lubrication supply capability; (d) HA forms a stable hydration layer and inhibits bacterial adhesion and biofilm formation.
[0027] The aforementioned multi-layered structure works together to achieve the integration of interface functions such as "high load-bearing capacity, stable lubrication, and antibacterial and anti-adhesion".
[0028] Experimental results show that the multi-scale composite interface constructed in this invention can significantly reduce the theoretical friction coefficient and achieve an antibacterial rate of 93.5% against Staphylococcus aureus.
[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) This invention not only significantly improves the load-bearing capacity and wear resistance of the Ti6Al4V artificial joint interface, but also effectively reduces the risk of friction and wear and bacterial colonization, and has good prospects for long-term service of artificial joints.
[0030] (2) Synergistic Mechanism of Multi-Scale Composite Interface: Compared with existing single TO, single LST, or single HA lubrication coating technologies, this invention forms a multi-scale composite functional interface on the surface of Ti6Al4V artificial joints through the synergistic construction of a thermal oxidation strengthening layer, a biomimetic laser microtexture layer, and an HA hydration lubrication and antibacterial layer, achieving simultaneous improvement in load-bearing capacity, lubrication performance, and antibacterial performance. Among them, the thermal oxidation layer can significantly improve the interface hardness and wear resistance; the laser microtexture can reduce the actual contact area, form a local hydrodynamic pressure effect, and store the lubricating medium; the HA layer reduces the interfacial shear resistance by forming a stable hydration film, while inhibiting bacterial adhesion and biofilm formation. The synergistic effect of the three effectively solves the problem of difficulty in achieving high load-bearing capacity, stable lubrication, and long-term antibacterial properties in existing technologies.
[0031] (3) This invention is the first to utilize laser microtexturing to form a mechanical protection and storage effect on the HA functional layer, reducing the problem of HA detachment and failure caused by shearing during sliding friction, thereby significantly improving the continuous stability of lubrication and antibacterial functions. Experimental results show that the composite interface constructed by this invention can significantly reduce the coefficient of friction and achieve an antibacterial rate of 93.5%, showing good prospects for clinical application of artificial joints. Attached Figure Description
[0032] Figure 1 This is a flowchart illustrating the overall fabrication process of the multi-scale composite functional interface of the Ti6Al4V artificial joint of the present invention.
[0033] Figure 2 This is a SEM topography image of the UT surface in an embodiment of the present invention.
[0034] Figure 3 This is a SEM image of the OT surface in an embodiment of the present invention.
[0035] Figure 4 This is a SEM and EDS line scan analysis diagram of the OT section in an embodiment of the present invention.
[0036] Figure 5 This is a SEM image of the OCT in an embodiment of the present invention.
[0037] Figure 6 This is a schematic diagram of the HA activation and covalent grafting process in an embodiment of the present invention.
[0038] Figure 7 This is a SEM image of the surface of the HA functional layer in an embodiment of the present invention.
[0039] Figure 8 This is an XPS analysis image of the surface of OCT-NH2 and OCT-HA samples in an embodiment of the present invention.
[0040] Figure 9 These are XRD patterns of different sample surfaces in embodiments of the present invention.
[0041] Figure 10 This is a graph showing the change of friction coefficient over time for different samples in the embodiments of the present invention under the conditions of a load of 19.6 N (corresponding to a contact stress of approximately 2.75 MPa) and a linear velocity of 0.01 m / s.
[0042] Figure 11 This is a SEM image of the wear morphology on the pin disk surface of the UT sample.
[0043] Figure 12 This is a SEM image of the wear morphology on the pin plate surface of the OT sample.
[0044] Figure 13This is a SEM image of the wear morphology on the pin plate surface of the OCT sample.
[0045] Figure 14 SEM image of the wear morphology on the pin plate surface of the OCT-HA sample.
[0046] Figure 15 The results show the antibacterial performance of different samples in the embodiments of the present invention.
[0047] Figure 16 The antibacterial rate of different samples against Staphylococcus aureus after in vitro culture for 24 h in the embodiments of the present invention. Detailed Implementation
[0048] The specific implementation of the present invention will be further described below with reference to the accompanying drawings and embodiments, but the implementation and protection of the present invention are not limited thereto. It should be noted that any processes not specifically described in detail below are those that can be implemented or understood by those skilled in the art by referring to the prior art. Reagents or instruments whose manufacturers are not specified are considered to be conventional products that can be purchased commercially.
[0049] Figure 1 This is a flowchart illustrating the overall fabrication process of the multi-scale composite functional interface of the Ti6Al4V artificial joint of the present invention. The flowchart sequentially includes steps such as thermal oxidation strengthening of the Ti6Al4V substrate, laser microtexturing construction, surface hydroxylation treatment, silanization amino modification, and HA covalent grafting, ultimately forming the OCT-HA multi-scale composite functional interface.
[0050] The specific implementation method includes the following steps: I. Pretreatment of Ti6Al4V substrate In both the embodiments and comparative examples of this invention, a Ti6Al4V titanium alloy disk was used as the experimental substrate. The sample had a diameter of 30 mm, a thickness of 6 mm, and a through hole structure with a diameter of 5 mm in the center.
[0051] First, the sample was mechanically polished step by step using 400#, 800#, 1200#, 1500# and 2000# wet sandpaper to remove original processing defects and surface oxide contamination layers. Then, the sample was mechanically polished with diamond polishing paste to achieve a mirror finish, obtaining an untreated titanium alloy sample, denoted as UT (Untreated Titanium).
[0052] After mechanical polishing, the samples were ultrasonically cleaned with anhydrous ethanol and deionized water for 15 minutes each time to remove residual particles, oil and impurities on the surface. Finally, they were dried with high-purity nitrogen gas for later use.
[0053] After pretreatment, the surface of the UT sample is relatively flat, with only shallow grooves distributed along the grinding direction, providing a stable substrate for subsequent thermal oxidation and laser texturing.
[0054] II. Construction of Thermal Oxidation Reinforcement Layer To improve the surface hardness, load-bearing capacity, and wear resistance of Ti6Al4V, the present invention further subjected the sample to thermal oxidation treatment.
[0055] The specific process is as follows: The pretreated UT sample was placed in a muffle furnace and heated from room temperature to 550-700℃ at a heating rate of 3-10℃ / min. It was then held at 550-700℃ for 6-24 h and then naturally cooled to room temperature with the furnace to obtain the thermally oxidized sample, denoted as OT (Oxidized Titanium).
[0056] During the thermal oxidation process, Ti reacts with oxygen at high temperatures to form a composite structure on the Ti6Al4V surface, consisting of a dense oxide layer and an oxygen diffusion layer. The rutile-TiO2 ceramic layer formed on the surface exhibits high hardness and excellent chemical stability, significantly improving interfacial wear resistance and load-bearing capacity. Simultaneously, the oxygen diffusion layer formed between the oxide layer and the Ti6Al4V substrate enhances the bonding strength between the oxide layer and the substrate, reducing the risk of interfacial plastic deformation and adhesive wear under high load conditions.
[0057] Scanning electron microscopy (SEM) results showed that after thermal oxidation, the original wear marks gradually blurred or even disappeared, and a large number of nano-TiO2 particles and island-like structures were formed on the surface, indicating that the oxide layer underwent a formation process of "nucleation-growth-aggregation".
[0058] Energy Dispersive Spectroscopy (EDS) line scan results showed that an oxide layer with a thickness of about 0.8 μm was formed on the surface of the OT sample.
[0059] X-ray diffraction (XRD) analysis results show that a stable rutile TiO2 structure is mainly formed on the sample surface after thermal oxidation.
[0060] III. Construction of Bionic Laser Microtexture Based on thermal oxidation strengthening, this invention further employs picosecond laser processing technology to construct a biomimetic microtexture structure on the OT surface.
[0061] The structural design is inspired by the hierarchical structure of the elytra surface of the oriental water beetle, whose natural surface has excellent fluid retention and friction control capabilities.
[0062] The laser processing parameters are as follows: laser pulse width: 5~20 ps; focused spot diameter: approximately 20~50 μm; output power: 35%~55%; scanning speed: 200~800 mm / s; number of repeated scans: 3~8 times.
[0063] By repeatedly scanning along a preset trajectory, a regularly arranged composite microtexture structure is formed on the thermally oxidized surface, and a thermally oxidized microtexture sample is obtained, denoted as OCT (Oxidized Composite Titanium).
[0064] The laser microtexture parameters constructed in this invention are as follows: the depth of the circular pit texture is about 6 μm; the depth of the hexagonal texture is about 3 μm; and the period of the laser-induced periodic surface structures (LIPSS) nanostripes is about 600 nm.
[0065] SEM results show that after laser processing, a regularly arranged composite texture structure is formed on the surface, and obvious nano-interference fringes are formed at the bottom of the texture, indicating that the ultrafast laser induces the formation of a hierarchical micro-nano structure.
[0066] The microtexture constructed in this invention mainly has the following functions: (1) Reduce the actual contact area and reduce solid-solid direct contact; (2) Capture wear particles and reduce third-body wear; (3) It creates a local hydrodynamic effect, improving lubrication stability; (4) As a HA and lubricating fluid storage unit, it improves the durability of interfacial lubrication; (5) It provides mechanical protection for the subsequent HA hydrogel layer, reducing the risk of the HA layer being directly damaged by shear during the sliding process.
[0067] IV. Surface hydroxylation and amination modification To achieve stable fixation of HA on the Ti6Al4V surface, the present invention further performs hydroxylation and amination treatment on the surface of the OCT sample.
[0068] First, the OCT sample is immersed in a 2-8 M NaOH solution at 40-80℃ for 1-4 h to form a large number of hydroxyl (–OH) active sites on the TiO2 surface.
[0069] The sample was then immersed in a 2%–8% (v / v) ethanol solution of 3-aminopropyltriethoxysilane (APTES) and reacted at room temperature for 3–8 h to form an amino-rich (–NH2) silanized functional layer on the surface, thus obtaining the OCT-NH2 sample.
[0070] This step mainly serves the following purposes: (1) Improve surface chemical reactivity; (2) Provides amino reaction sites for subsequent HA grafting; (3) Enhance the bonding strength between the HA functional layer and the Ti6Al4V matrix.
[0071] V. Covalent grafting of hyaluronic acid (HA) After surface amination, the present invention further employs an EDC / NHS activation system to achieve covalent fixation of HA on the Ti6Al4V surface.
[0072] Hyaluronic acid (HA) is a naturally occurring anionic glycosaminoglycan found in synovial fluid, possessing excellent hydrophilicity, biocompatibility, and lubricating properties. HA can reduce interfacial shear stress by forming a stable hydration layer, while simultaneously inhibiting protein adsorption and initial bacterial adhesion, thereby achieving friction reduction and antibacterial functions.
[0073] First, dissolve HA in 0.05–0.2 M MES buffer (pH = 5.5–6.5) to a concentration of 1–5 g / L. Then add ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS).
[0074] The total EDC / NHS concentration was 2.5 mg / mL, with an EDC to NHS mass ratio of 4:1.
[0075] The EDC / NHS system first activates the carboxyl group (–COOH) in HA to form a highly reactive NHS ester intermediate. Then, the OCT-NH2 sample is immersed in the activated HA solution and reacted at room temperature for 12–24 h.
[0076] During the reaction, the activated carboxyl groups of HA undergo amidation with the surface amino groups (–NH2) to form stable amide bonds (–CONH–), thereby achieving covalent fixation of HA on the textured thermal titanium oxide surface, ultimately forming a composite interface with friction-reducing and antibacterial functions, denoted as OCT-HA.
[0077] X-ray photoelectron spectroscopy (XPS) results showed that the C content on the surface increased significantly after HA grafting, and a distinct amide bond characteristic peak appeared. At the same time, the intensity of the Ti–O peak decreased, proving that HA had been successfully grafted and covered the TiO2 surface.
[0078] Example 1 (UT) This example uses a UT sample, which is an untreated sample.
[0079] Figure 2 The images show the SEM morphology of the UT surface in this embodiment of the invention. The left image is a low-magnification SEM morphology image, showing that the sample surface is generally flat, with strip-shaped scratches distributed along the mechanical polishing direction. The right image is a SEM morphology image, further characterizing the local microscopic morphology features of the polished surface, indicating that the sample surface still retains certain polishing traces. Figure 11 It can be seen that the surface of the friction disk after UT treatment ( Figure 11 (Left and Middle) Numerous parallel and continuous deep furrows and obvious micro-cutting marks can be observed, with localized spalling pits and wear debris, exhibiting typical abrasive wear characteristics. (Matching pin surface) Figure 11 The right side also shows many deep friction scratches, indicating that the two contact surfaces of the friction pair experienced relatively intense mechanical action during the friction process, and the material wear was relatively severe.
[0080] Example 2 (OT) The UT sample was subjected to thermal oxidation treatment to obtain the OT sample.
[0081] Figure 3 The SEM morphology images of the OT surface in this embodiment of the invention are shown in the following: the left image is a low-magnification SEM morphology image, showing that a uniformly distributed oxide structure is formed on the sample surface after thermal oxidation treatment; the right image is a high-magnification SEM morphology image, showing that the surface is composed of a large number of nanoscale TiO2 particles and island structures, indicating that the oxide layer underwent nucleation, growth and aggregation processes during thermal oxidation. Figure 4 The SEM and EDS line scan analysis images of the OT cross-section in this embodiment of the invention are shown. The left image is a cross-sectional morphology image of the OT sample, showing the formation of a thermal oxide layer on the surface of the Ti6Al4V substrate. The right image is a distribution curve of Ti, Al, and O elements along the scan line direction, used to characterize the oxide layer thickness and elemental distribution. The results show that an oxide layer structure of approximately 0.8 μm thick is formed on the surface. Figure 12 It can be seen that, compared with UT, the surface of the friction disk after OT treatment ( Figure 12 (Left and Middle) The wear marks are significantly reduced, the furrow depth is decreased, the wear area is smoother, and large-area peeling is significantly reduced. This indicates that after thermal oxidation treatment, the wear resistance of the material surface is improved, and the degree of wear is reduced. The corresponding mating pin surface ( Figure 12 (Right) The friction scratches are also significantly reduced, with only finer scratches visible.
[0082] Example 3 (OCT) A biomimetic microtexture structure was constructed on the surface of the OT sample using picosecond laser processing technology to obtain the OCT sample.
[0083] Figure 5 These are SEM images of the OCT in this embodiment of the invention. The left image is a low-magnification SEM image, showing a regularly arranged array of biomimetic hexagonal microtextures on the surface; the middle image is a magnified partial image, showing the edges of the texture units and the micro-pit structure; the right image is a high-magnification SEM image, showing the formation of laser-induced periodic surface structure (LIPSS) nanostripes on the textured surface after laser processing. Figure 13 It can be seen that after OCT treatment, a composite biomimetic texture consisting of hexagonal grooves and circular micro-pits was formed on the surface of the friction disk. Figure 13 (Left). After the friction and wear test, the main body of the texture remained intact, with only slight wear in some areas, indicating that the texture has good structural stability. (Medium magnification image) Figure 13 The image shows a clear boundary between the textured and untextured regions, with only slight wear marks in the untextured areas. The constructed composite texture can store wear debris and promote lubricant retention during friction, thereby reducing abrasive wear. The corresponding mating pin surface ( Figure 13 (Right) Only shallow and uniform friction scratches were observed, indicating that the composite texture can effectively improve the wear condition of the friction pair.
[0084] Example 4 (OCT-HA) The surface of the OCT sample was subjected to hydroxylation and amination treatment, and then the HA was covalently fixed on the Ti6Al4V surface using an EDC / NHS activation system to obtain the OCT-HA sample.
[0085] Figure 6 This diagram illustrates the HA activation and covalent grafting process. The upper part shows the process of HA forming an active ester intermediate of HA-NHS under the action of the EDC / NHS system. The lower part shows the process of activated HA undergoing an amidation reaction with the amino groups on the surface of OCT-NH2 to form a covalent graft layer, ultimately obtaining the OCT-HA composite functional interface. Figure 7 The image shows the SEM morphology of the HA functional layer surface, which reveals that a continuously cross-linked porous network structure is formed on the surface after HA grafting, indicating that the HA functional layer is successfully covered on the Ti6Al4V surface.
[0086] Figure 8The images shown are XPS analysis images of the surfaces of OCT-NH2 and OCT-HA samples in this embodiment of the invention. The top row shows the high-resolution spectra of C 1s, N 1s, and O 1s of the OCT-NH2 sample, and the bottom row shows the corresponding high-resolution spectra of the OCT-HA sample. The results show that obvious amide bond-related characteristic peaks appear on the surface after HA grafting, while the intensity of the Ti–O peak decreases, indicating that HA has been successfully covalently fixed to the surface.
[0087] from Figure 14 It can be seen that after OCT-HA treatment, the composite biomimetic texture on the surface of the friction disc remains intact. Figure 15 (Left), wear marks are further reduced. Medium magnification ( Figure 14 The data (in the middle section) shows that the surface of the wear area is relatively smooth, with no obvious spalling or severe plastic deformation observed. Compared with the first three groups, the surface of the mating pin ( Figure 14 The friction scratches on the right side are the shallowest and most uniformly distributed, indicating that the OCT-HA sample has the best friction-reducing and wear-resistant properties. After HA grafting, the hydrophilicity of the sample surface is improved, and together with the composite texture, it facilitates lubricant retention and interfacial lubrication during friction, thereby further reducing friction and wear. The composite texture can store wear debris and reduce three-body wear, while the HA layer further improves the lubrication state of the friction interface. The synergistic effect of both gives the sample excellent wear resistance.
[0088] Figure 9 The XRD patterns of different sample surfaces in Examples 1-4 of the present invention are shown, where UT is the untreated titanium matrix, OT is the thermally oxidized titanium surface, OCT is the thermally oxidized microtextured titanium surface, and OCT-HA is the composite functional interface after hyaluronic acid grafting. The results show that a stable rutile TiO2 structure is formed on the sample surface after thermal oxidation, and the subsequent laser texturing and HA grafting treatments do not destroy the crystal structure of the oxide layer.
[0089] Figure 10 The graphs show the friction coefficient versus time curves of the four samples in Examples 1-4 of this invention under a load of 19.6 N (corresponding to a contact stress of approximately 2.75 MPa) and a linear velocity of 0.01 m / s. The results show that, compared to the UT, OT, and OCT samples, the OCT-HA composite functional interface exhibits the best friction reduction performance, with its stable friction coefficient reduced to as low as approximately 0.04. This indicates that the constructed multi-scale synergistic structure of "thermal oxidation layer—microtexture—HA lubrication layer" can effectively reduce interfacial shear resistance and improve lubrication stability.
[0090] Example 5 (Antibacterial Experiment) from Figure 15As can be seen, a large number of colonies were observed in the UT group; the number of colonies decreased in the OT group; the number of colonies further decreased in the OCT group; and only a very small number of colonies were observed in the OCT-HA group, with a significantly lower colony count than the other groups, indicating that the OCT-HA sample had the best antibacterial performance. This is because the laser-constructed composite microtexture reduces the effective contact area of bacteria on the material surface and inhibits initial bacterial adhesion; simultaneously, the grafting of hyaluronic acid increases surface hydrophilicity, forming a stable hydration layer on the material surface, which is unfavorable for bacterial adhesion and biofilm formation. The synergistic effect of the composite texture and the hyaluronic acid layer results in high antibacterial activity in the sample.
[0091] from Figure 16 It can be seen that, compared with UT, OT and OCT samples, the OCT-HA composite functional interface exhibits the best antibacterial performance, with an antibacterial rate of 93.5%. This indicates that the synergistic effect of the HA functional layer combined with the microtexture and thermal oxidation structure can effectively inhibit bacterial adhesion and proliferation, thereby reducing the risk of biofilm formation on the implant surface.
Claims
1. A method for preparing a multiscale synergistic friction-reducing and antibacterial composite interface of a Ti6AI4V artificial joint surface, characterized in that, Includes the following steps: (1) The surface of the Ti6Al4V matrix is pretreated and a load-bearing reinforcement layer is constructed on its surface; (2) A textured surface layer with micro-nano scale structural features is constructed on the surface of the bearing reinforcement layer, the textured surface layer including microstructure units for storing lubricating medium; (3) A molecular functional layer with biological lubrication and antibacterial functions is constructed on the textured surface layer and fixed by chemical bonding.
2. The preparation method according to claim 1, characterized in that, The load-bearing reinforcement layer is an oxide layer or hard coating formed by thermal oxidation, micro-arc oxidation or physical vapor deposition.
3. The preparation method according to claim 1, characterized in that, The textured surface layer is constructed using any one of picosecond laser processing, femtosecond laser processing, nanosecond laser processing, chemical etching, electrochemical etching, or microimprinting.
4. The preparation method according to claim 1, characterized in that, The microstructure unit includes one or more combinations of micropit structures, microgroove structures, or periodic array structures, and is used to store lubricating media and molecular functional layer materials.
5. The preparation method according to claim 1, characterized in that, The molecular functional layer is a polymer or biomolecular layer with biolubricating properties and antibacterial adhesion capabilities.
6. The preparation method according to claim 1, characterized in that, The molecular functional layer is fixed to the textured surface layer by amide bonding, silane coupling, or self-assembly.
7. The preparation method according to claim 1, characterized in that, A method for preparing a multi-scale composite functional interface of Ti6Al4V artificial joint synergistically constructed from TO, LST, and HA includes the following steps: Step 1: Pretreatment of Ti6Al4V substrate The Ti6Al4V titanium alloy was ground and polished, and then ultrasonically cleaned with anhydrous ethanol and deionized water to remove residual particles, oil and impurities from the surface. Finally, it was dried with high-purity nitrogen for later use. Step 2: Construction of the thermal oxidation reinforcement layer The Ti6Al4V titanium alloy pretreated in step 1 was placed in a muffle furnace, heated and calcined, and then naturally cooled to room temperature with the furnace to obtain a thermally oxidized sample. Step 3: Laser Microtexture Construction In step 2, the sample surface is laser-processed using a picosecond laser processing system. By repeatedly scanning along a preset trajectory, a regularly arranged composite microtexture structure is formed on the thermally oxidized surface, thus obtaining a thermally oxidized microtexture sample. Step 4: Surface hydroxylation and amination modification The thermally oxidized microtextured sample was immersed in NaOH solution to form a large number of hydroxyl active sites on the TiO2 surface. Then the sample was immersed in APTES ethanol solution and reacted at room temperature to form an amino-rich silanized functional layer on the surface, thus obtaining the OCT-NH2 sample. Step 5: Covalent grafting of hyaluronic acid (HA) HA was dissolved in MES buffer, followed by the addition of EDC and NHS. The OCT-NH2 sample was then immersed in the activated HA solution and reacted at room temperature to finally construct the OCT-HA multiscale composite functional interface.
8. The preparation method according to claim 7, characterized in that, In step 3, the laser processing parameters are as follows: laser pulse width 5~20ps; focused spot diameter 20~50μm; output power 35%~55%; scanning speed 200~800mm / s; number of repeated scans 3~8; In step 4, the OCT sample is immersed in a 2-8 M NaOH solution at 40-80°C for 1-4 h; then it is reacted in APTES ethanol solution at room temperature for 3-8 h. In step 5, the HA concentration is 1~5 g / L, the total EDC / NHS concentration is 2.5 mg / mL, the mass ratio of EDC to NHS is 4:1, and the reaction is carried out at room temperature for 12~24 h.
9. A multi-scale composite functional interface of Ti6Al4V artificial joint synergistically constructed from TO, LST and HA, obtained by the preparation method according to any one of claims 7-8.
10. The application of the Ti6Al4V artificial joint multi-scale composite functional interface synergistically constructed by TO, LST and HA as described in claim 9 in the preparation of contact implants for artificial hip joints and artificial knee joints.