A taro stem cellulose-based composite aerogel, a preparation method thereof and application thereof in adsorbing microplastics

By modifying taro stem cellulose as the base material, polypyrrole composite aerogel has solved the problems of low adsorption capacity and limited application range of existing cellulose-based aerogels, realizing efficient adsorption of various microplastics and application in food, and possessing good structural stability and biocompatibility.

CN123148909APending Publication Date: 2026-11-24SOUTH CHINA AGRICULTURAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510656402.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

Smart Images

  • Figure CN123148909A_ABST
    Figure CN123148909A_ABST
Patent Text Reader

Abstract

This invention discloses a taro stem cellulose-based composite aerogel, its preparation method, and its application in the adsorption of microplastics. The TS-MCC / PPy composite aerogel prepared by this invention, using taro stem cellulose as the base material and polypyrrole as a modifier, possesses a honeycomb-like porous structure, exhibiting good structural stability and reusability. It also demonstrates excellent microplastic adsorption performance, showing good adaptability to different pH and aqueous environments, with short adsorption time and high adsorption capacity. It can be used to adsorb a variety of microplastics, making it a safe and reliable biosorbent material. Its preparation process is simple and environmentally friendly. The taro stem cellulose-based composite aerogel provided by this invention overcomes the shortcomings and deficiencies of existing TS-MCC aerogels, such as low adsorption capacity, long adsorption time, and limited adsorption of a single type of microplastic. Furthermore, the aerogel material prepared by this invention has a good effect on the adsorption and enrichment of microplastics in food matrices, which is of great significance for the removal of microplastics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of adsorption materials and plastic pollution treatment technology, and in particular to a taro stem cellulose-based composite aerogel, its preparation method, and its application in adsorbing microplastics. Background Technology

[0002] Plastic products are widely used due to their excellent processing and performance properties. A report released by the European Plastics Association shows that global annual plastic production exceeded 400 million tons in 2022. Large quantities of discarded plastics are gradually broken down into microplastics (MPs) with a particle size of less than 5 mm under the influence of ultraviolet radiation from sunlight, wind erosion, water scouring, and biodegradation. These microplastics can remain environmentally persistent for hundreds of years. Microplastics infiltrate the food chain through atmospheric deposition, irrigation water infiltration, and food processing contact, forming a complete chain of pollution "from production to consumption." The 2023 Global Food Safety Assessment Report by the Food and Agriculture Organization of the United Nations (FAO) shows that microplastics were detected in over 80% of the 23 categories of food sampled. The microplastics detected in the food chain were mainly made of polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), and polystyrene (PS). Microplastics can enter the human body through the ingestion of food containing microplastics, and circulate through the blood and lymphatic system to various organs and parts of the body, causing varying degrees of damage to vital organs such as the heart, liver, spleen, kidneys, and brain. Furthermore, microplastics pose potential health hazards to humans, including neurotoxicity, carcinogenicity, reproductive toxicity, developmental toxicity, and cardiovascular disease.

[0003] Currently, the main methods available for microplastic treatment are: (1) physical methods, including filtration, adsorption, and ion exchange; (2) chemical methods, including catalytic degradation, ozone oxidation, flocculation sedimentation, and pyrolysis; and (3) biological methods, including microbial degradation, enzyme catalysis, and activated sludge processes. Among these, adsorption is based on the abundant active sites of adsorbent materials to achieve efficient capture of target pollutants. Due to its low cost, ease of operation, and wide applicability, it is widely used in the field of microplastic pollution control. Among various adsorbent materials, aerogel materials, with their unique hierarchical porous structure, high specific surface area, abundant functional groups, and easy recovery and separation, have shown strong advantages and broad prospects in the field of microplastic pollution control.

[0004] Compared to synthetic polymers, cellulose-based aerogels not only inherit the low-density and high-porosity structural characteristics of traditional aerogels, but also possess environmental friendliness and functionalizability. In particular, utilizing agricultural waste as a cellulose raw material can not only solve the pollution problem caused by waste generation, but also achieve microplastic remediation, thus realizing a "waste-to-waste" effect. However, the adsorption capacity of existing publicly available aerogel materials for microplastics is relatively low. For example, the biomass aerogel prepared from waste taro stem microcrystalline cellulose (TS-MCC) in previous studies had an adsorption capacity of 418.6 mg / g for microplastics (polystyrene, PS). This TS-MCC aerogel still suffers from low adsorption capacity, long adsorption time, and limited adsorption of specific microplastic types. Furthermore, most existing cellulose-based aerogels focus on the detection of wastewater samples, with few suitable for detecting microplastics in food, thus limiting their application. Therefore, there is an urgent need to develop more safe and efficient cellulose-based aerogels to further improve the adsorption effect on microplastics for microplastic pollution remediation. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing TS-MCC aerogels, such as low adsorption capacity, long adsorption time and limited adsorption of microplastics, and to provide a taro stem cellulose-based composite aerogel, its preparation method and its application in adsorbing microplastics.

[0006] The purpose of this invention is to provide a method for preparing taro stem cellulose-based composite aerogel.

[0007] Another objective of this invention is to provide the application of taro stem cellulose-based composite aerogels.

[0008] Another object of the present invention is to provide a method for adsorbing / removing microplastics.

[0009] The above-mentioned objective of this invention is achieved through the following technical solution: This invention provides a method for preparing taro stem cellulose-based composite aerogel, comprising the following steps: S1. Preparation of taro stem microcrystalline cellulose: Fresh taro stems were dried, pulverized, sieved, impurities removed, washed, and freeze-dried under vacuum to obtain TS-C powder; the TS-C powder was then acid-hydrolyzed, the precipitate was washed with distilled water until neutral, centrifuged, and freeze-dried to obtain TS-MCC powder. S2. Preparation of Taro Stem Cellulose Aerogel: TS-MCC powder was dissolved in an aqueous solution containing 5-8 wt% NaOH and 10-14 wt% urea, stirred and then frozen. After thawing, a uniform TS-MCC solution was obtained. Then, the cross-linking agent epichlorohydrin was added to the TS-MCC solution, stirred, and unreacted residues were removed by washing with distilled water. The hydrogel was then frozen and then freeze-dried under vacuum to obtain TS-MCC aerogel. S3. Preparation of Taro Stem Cellulose / Polypyrrole Aerogel: TS-MCC aerogel was impregnated in a pyrrole solution, stirred, vacuum dried, degassed, and then 5~20wt% Fe was added. 3+ After stirring the solution, an in-situ oxidative polymerization reaction was carried out. After the reaction was completed, the product was washed with deionized water, and finally the product was freeze-dried under vacuum to obtain TS-MCC / PPy composite aerogel.

[0010] To address the problems of existing TS-MCC aerogels, this invention optimizes and enhances the TS-MCC aerogel prepared in previous studies by using specific modifiers for functional modification. The resulting taro stem cellulose / polypyrrole composite aerogel (TS-MCC / PPy) exhibits significantly improved and expanded adsorption capacity, adsorption time, adsorption types, and application range compared to the unmodified TS-MCC aerogel, and also expands its application in food matrices. The TS-MCC / PPy aerogel of this invention is prepared using taro stem cellulose as the base material and polypyrrole as the modifier. This aerogel possesses a honeycomb-like porous structure, exhibiting good structural stability and reusability. The TS-MCC / PPy aerogel demonstrates excellent adsorption capacity for microplastics, good adaptability to different pH and aqueous environments, reaches adsorption equilibrium quickly, and exhibits excellent adsorption stability and durability. It can be used to adsorb various microplastics such as PS, PP, PE, and PET, and also possesses good cell compatibility and biodegradability, making it a safe and reliable biosorbent material. Its preparation process is simple and environmentally friendly. Compared to TS-MCC aerogel, the adsorption capacity has been increased from 418 mg / g to 800 mg / g, and the adsorption time has been shortened from 42 h to 300 min. The types of microplastics adsorbed cover PS, PP, PE and PET, and it can be better used for adsorption in food. This expands the application range of TS-MCC aerogel, solves the waste caused by taro stem waste, and achieves efficient management of microplastics.

[0011] Specifically, for the purpose of cost control and high-value utilization of waste agricultural products, this invention uses taro stems, a plant by-product, to prepare cellulose. As an agricultural by-product, taro stems have a high weight percentage and high cellulose content. Cellulose from other sources in the art, or commercially available cellulose products, can also be used in this invention. Alternatively, cellulose can be prepared by processing cellulose-rich plant samples using conventional techniques in the art (e.g., using plant materials such as grapefruit peel, orange peel, pineapple peel, sugarcane bagasse, corn stalks, bamboo shoot shells, or rice husks).

[0012] As a preferred embodiment, the present invention provides a specific method for preparing taro stem cellulose: Fresh taro stems are washed clean and cut into small sections, naturally air-dried to remove most of the moisture, and then dried in a forced-air drying oven. The taro stem sections are crushed into powder using a pulverizer and passed through a 60-mesh sieve to obtain taro stem powder. The above powder is mixed with a certain proportion of sodium chlorite solution and stirred evenly, and treated for 1-2 hours to remove lignin, pigments, and other impurities from the powder. The washed filter residue is taken, and a certain proportion of NaOH solution is added, and the mixture is placed in a water bath for 1-2 hours to remove hemicellulose. The washed filter residue is taken and added to a certain proportion of H2O2 + H2SO4 solution, and stirred at 30℃-80℃ for 1-9 hours to remove pectin components. The filter residue is washed until neutral and then eluted with 95% (v / v) ethanol to remove alcohol-soluble impurities. The precipitate is collected by centrifugation and then freeze-dried to obtain taro stem cellulose (TS-C) powder. Then, TS-C is added to dilute hydrochloric acid in a certain proportion, and acidified at 60℃ for 20~80 min. The precipitate is washed with distilled water until neutral, and the precipitate is collected by centrifugation and then freeze-dried to obtain taro stem microcrystalline cellulose (TS-MCC) powder.

[0013] Preferably, the sodium chlorite concentration is 2.5~7.5% (v / v), the NaOH concentration is 5~15% (w / w), the drying temperature is 60℃, the ratio of taro stem powder to reaction solution is 1:(10~50) (g / mL), the volume ratio of H2O2 to H2SO4 is 7~10:1~3 (v / v), the reaction temperature is 60℃, and the centrifugation speed is 4500 rpm.

[0014] More preferably, the ratio of taro stem powder to reaction solution is 1:20 (g / mL). The concentration of sodium chlorite is 5% (v / v), the concentration of NaOH is 8% (w / w), and the volume ratio of H2O2 to H2SO4 is 9:1.

[0015] The taro stem microcrystalline cellulose prepared by the above method has an average length of 32.27 μm and a carboxyl content of 1.474 ± ​​0.081 mmol / g.

[0016] Preferably, the concentration of the TS-MCC solution in step S2 is 1.5~6wt%.

[0017] More preferably, step S2 uses an aqueous solution of 7wt% NaOH and 12wt% urea.

[0018] Preferably, the concentration of the crosslinking agent epichlorohydrin in step S2 is 5~30wt%.

[0019] Preferably, the freezing treatment method in step S2 is as follows: pre-freezing at -20℃ or -80℃, non-directional / directional liquid nitrogen freezing, and freeze-drying time of 6~72h.

[0020] Preferably, the concentration of the pyrrole solution in step S3 is 1~8 wt%.

[0021] Preferably, Fe in step S4 3+ The solution used was FeCl3 solution, and the oxidative polymerization reaction time was 5~24h.

[0022] This invention provides a taro stem cellulose-based composite aerogel, which is prepared by the above method.

[0023] This invention provides the application of taro stem cellulose-based composite aerogel in the adsorption / removal of microplastics.

[0024] Preferably, the microplastic is one or more of polystyrene (PS), polyethylene (PE), polypropylene (PP), and polyethylene terephthalate (PET).

[0025] Preferably, taro stem cellulose-based composite aerogel can be used to enrich or remove microplastics from natural water bodies and food samples.

[0026] This invention provides the application of taro stem cellulose-based composite aerogel in the preparation of products that adsorb / remove microplastics.

[0027] The present invention also provides a method for microplastic adsorption / removal, which uses taro stem cellulose-based composite aerogel to treat the sample to be tested.

[0028] In addition, the present invention provides a microplastic adsorption product containing taro stem cellulose-based composite aerogel prepared by the above preparation method.

[0029] This invention provides a method for microplastic adsorption / removal, which uses the above-mentioned composite aerogel to treat the sample to be tested.

[0030] Preferably, the present invention provides a method for adsorbing / removing microplastics in food.

[0031] Preferably, the processing conditions are: 20~30℃, 3~8h.

[0032] The present invention has the following beneficial effects: To address the problems of existing TS-MCC aerogels, this invention optimizes TS-MCC aerogels prepared in previous studies by using specific modifiers for functional modification. The resulting taro stem cellulose / polypyrrole composite aerogel (TS-MCC / PPy) exhibits significantly improved and expanded adsorption capacity, adsorption time, types of adsorbed microplastics, and application range compared to the unmodified TS-MCC aerogel. This invention uses taro stem cellulose as the basic framework and polypyrrole as the modifier, employing epichlorohydrin etherification crosslinking, freeze-drying technology, and in-situ growth methods to prepare a honeycomb-like porous aerogel material. This aerogel exhibits good structural stability, reusability, adaptability to adsorption in different pH and aqueous environments, low cytotoxicity, applicability to adsorption of microplastics of different sizes and materials, and good biodegradability. Furthermore, the aerogel material provided by this invention demonstrates excellent adsorption and enrichment effects on microplastics in food matrices, showcasing broad application value.

[0033] This invention uses taro stems, an agricultural waste that is widely available and inexpensive, as raw material to extract its cellulose, thus broadening the application field of waste taro stems. Moreover, the substrates used in the preparation of the materials are all derived from natural organisms, which are green, safe, and have low environmental pollution, while also having good biocompatibility and biodegradability. Attached Figure Description

[0034] Figure 1 The effects of different modification methods on the adsorption performance of aerogels.

[0035] Figure 2 SEM images of taro stem cellulose / polypyrrole composite aerogels prepared with different amounts of pyrrole.

[0036] Figure 3 The adsorption capacity of taro stem cellulose / polypyrrole composite aerogels prepared with different pyrrole addition amounts.

[0037] Figure 4 This is a graph showing the effect of pH on the adsorption of aerogels.

[0038] Figure 5 The figure shows the effect of adsorption time on the adsorption of aerogel.

[0039] Figure 6 The figure shows the effect of initial PS concentration and temperature on the adsorption of aerogel.

[0040] Figure 7 This image shows the adsorption effect of aerogel on microplastics under different water conditions.

[0041] Figure 8 This is a graph showing the reusability of aerogels.

[0042] Figure 9This demonstrates the adsorption effect of aerogels on microplastics of different materials and sizes.

[0043] Figure 10 This is a diagram showing the cell compatibility of the aerogel.

[0044] Figure 11 This is a diagram showing the adsorption effect of aerogel on microplastics in food. Detailed Implementation

[0045] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0046] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.

[0047] Example 1: Preparation of Taro Stem Cellulose / Polypyrrole Composite Aerogel 1. Preparation of Taro Stem Microcrystalline Cellulose Fresh taro stems were rinsed clean and cut into 3cm lengths. They were then air-dried to remove most of the moisture, followed by drying in a forced-air drying oven at 70℃ for 24 hours to obtain dried taro stem segments. These segments were then ground into powder using a grinder and passed through a 60-mesh sieve to obtain dried taro stem powder (TS). The powder was mixed with a 5% (v / v) sodium chlorite solution at a 1:20 (g / mL) material-to-liquid ratio and stirred until homogeneous. The mixture was then treated in a water bath at 70℃ with magnetic stirring at 700 rpm for 2 hours to remove lignin, pigments, and other impurities. The residue was separated, washed three times with distilled water, and then added to an 8% (w / w) sodium hydroxide solution at a 1:20 (g / mL) material-to-liquid ratio. The mixture was then heated in a water bath at 90℃ for 2 hours to remove hemicellulose. The filter residue was washed with distilled water until neutral. It was then stirred in a 1:9 mixture of concentrated sulfuric acid and 30% hydrogen peroxide at 60°C for 4.5 hours to remove pectin. The residue was washed again until neutral and then eluted with 95% (v / v) ethanol to remove alcohol-soluble impurities. The precipitate was collected by centrifugation and pre-frozen at -80°C for 8 hours. It was then placed in a vacuum freeze dryer and dried at -60°C and 0.37 bar for 48 hours to obtain TS-C powder. TS-C was then placed in 8% (v / v) hydrochloric acid at a 1:20 (g / mL) ratio and acidified at 60°C for 80 minutes. The precipitate was washed with distilled water until neutral, centrifuged, and then freeze-dried to obtain TS-MCC powder.

[0048] 2. Preparation of Taro Stem Cellulose Aerogel First, TS-MCC powder was dissolved in a pre-cooled aqueous solution containing 7wt% NaOH and 12wt% urea, stirred at 4°C for 8 hours, and then frozen at -25°C for 8 hours. After thawing and stirring, a homogeneous TS-MCC solution was obtained. Subsequently, the cross-linking agent epichlorohydrin (ECH) was added to the solution, and the mixture was stirred at 4°C for 1 hour. The mixture was then transferred to a cylindrical mold and heated to 80°C for 1 hour to prepare TS-MCC hydrogels with different cellulose and cross-linking agent mass fractions (adjusting the mass ratio of taro stem microcrystalline cellulose and cross-linking agent to prepare aerogels with different component concentrations).

[0049] After washing with distilled water to remove unreacted residues, the hydrogel was treated under different conditions (-20℃, -80℃, liquid nitrogen freezing and directional liquid nitrogen freezing) and then vacuum freeze-dried at -60℃ and 0.37 bar for 48 hours to obtain TS-MCC aerogel.

[0050] 3. Preparation of Taro Stem Cellulose / Polypyrrole Aerogel The specific preparation method of TS-MCC / PPy composite aerogel is based on TS-MCC. 2.0 Aerogel (containing 2.0 wt% taro stem microcrystalline cellulose and 15 wt% crosslinking agent epichlorohydrin, pre-frozen at -80℃) was used as a matrix template and functionalized by in-situ oxidative polymerization.

[0051] The specific process is as follows: First, pyrrole monomers (Py, with mass gradients of 0.05, 0.10, 0.15, 0.20, 0.25, and 0.30 g) are mixed with 40 mL of deionized water and magnetically stirred at 200 rpm for 30 min to form a uniform dispersion system. Then, 0.2 g of TS-MCC2.0 aerogel cut into 1 cm × 1 cm × 1 cm pieces is immersed in the above solution and stirred continuously for 30 min. After stirring, the mixture is transferred to a vacuum drying oven and degassed at 30 °C for 4–12 h to remove air from the pores of the aerogel, ensuring thorough wetting by the Py solution. Next, 10 mL of 10 wt% FeCl3 solution is added quantitatively to the system, and an in-situ oxidative polymerization reaction is carried out at a constant temperature of 25 °C and a stirring rate of 200 rpm for 6 h. After the reaction, the composite aerogel is washed three times with deionized water.

[0052] Finally, the product was pre-frozen at -80℃ for 12 hours and then treated in a vacuum freeze dryer (-60℃, 0.37 bar) for 48 hours to obtain a series of TS-MCC / PPy composite aerogels. Based on the gradient increase of Py addition (0.05~0.30 g, corresponding to 1.0~6.0 wt% in the solution), the six samples were named TS-MCC / PPy respectively. 1.0 To TS-MCC / PPy 6.0.

[0053] Example 2: Effect of different modification methods on the adsorption performance of aerogels 1. Aerogel materials prepared by different modification methods (1) The preparation method of TS-MCC aerogel is the same as that in Example 1, except that pyrrole is not used for in-situ modification to obtain TS-MCC aerogel.

[0054] (2) The preparation method of TS-MCC / Lys aerogel is the same as that in Example 1. The only difference is that after the TS-MCC cellulose is dissolved, a certain mass of lysine (Lys) powder (0.5-5wt%) is added and mixed. The subsequent steps are the same to obtain TS-MCC / Lys aerogel.

[0055] (3) The preparation method of TS-MCC / PEI aerogel is the same as that of taro stem cellulose aerogel in Example 1. The only difference is that after TS-MCC cellulose is dissolved, a certain mass of polyethyleneimine (PEI) solution (0.5-5wt%) is added for mixing. The subsequent steps are the same to obtain TS-MCC / PEI aerogel.

[0056] (4) The preparation method of TS-MCC / ZIF-8 aerogel is the same as in Example 1. The only difference is that the prepared TS-MCC is soaked in zinc nitrate hexahydrate solution (0.1-2.0 mol / L) for 1-10 h, and then 2-methylimidazole (0.1-2.0 mol / L) is added for in-situ growth to obtain TS-MCC / ZIF-8 aerogel.

[0057] 2. Determination of adsorption effect Take the TS-MCC / PPy prepared in Example 1 respectively 4.0 10 mg of the aerogel material and 10 mg of the TS-MCC / Lys aerogel, TS-MCC / PEI aerogel, and TS-MCC / ZIF-8 aerogel material prepared by the above method were added to 10 mL of PS solution (concentration of 50 mg / L for all). The aerogels were uniformly adsorbed at 120 rpm for 8 h at room temperature of 25 °C using a magnetic stirrer. The concentration of microplastics after adsorption was measured by a UV-Vis spectrophotometer. The adsorption amount of the aerogel material was calculated by the change in the concentration of microplastics before and after adsorption.

[0058] The measurement results are as follows Figure 1As shown, the adsorption capacity of the unmodified TS-MCC aerogel is 28.93±1.31 mg / g. The adsorption capacities of TS-MCC / Lys aerogel, TS-MCC / PEI aerogel, TS-MCC / ZIF8 aerogel, and TS-MCC / PPy aerogel prepared by functionalization with different modifiers (lysine, polyethyleneimine, ZIF8, and PPy) are 62.33±10.62 mg / g, 46.64±6.29 mg / g, 79.79±4.03 mg / g, and 92.25±0.72 mg / g, respectively, showing significant differences. This indicates that while functionalization can improve the adsorption effect of aerogels on PS microplastics to some extent, the effect varies significantly depending on the modifier used. The experimental results show that functionalization of TS-MCC aerogel with PPy significantly improves its adsorption performance.

[0059] Example 3 Effect of pyrrole addition on the adsorption performance of TS-MCC / PPy aerogel 1. Microscopic pore appearance The morphological changes of the TS-MCC / PPy aerogels and TS-MCC aerogels prepared in Example 1 were observed using SME. SME results for some aerogels are shown below. Figure 2 As shown, all aerogels exhibit a honeycomb-like porous structure, with unmodified TS-MCC showing the most significant difference. 2.0 The aerogel pore walls exhibit a relatively smooth surface. After in-situ polymerization modification with pyrrole (Py), the aerogel pore wall surface was covered with a large amount of irregular particulate matter, confirming the successful grafting of PPy onto the cellulose matrix. This increased internal pore wall roughness is beneficial for increasing the specific surface area and exposing active sites, thus providing favorable conditions for the physical adhesion and chemical binding of pollutants.

[0060] Furthermore, the initial concentration of Py monomer significantly modulates the surface morphology of the aerogel. When the Py solution concentration increased from 2.0 wt% to 6.0 wt%, the PPy particles adhering to the pore walls showed a marked increase in quantity and densification. This is mainly attributed to the higher concentration of Py monomer in the Fe... 3+ During catalytic oxidative polymerization, a denser polymer deposition layer is formed through intermolecular π-π stacking and hydrogen bonding.

[0061] 2. Adsorption performance of PS Take 10 mg of each group of TS-MCC / PPy aerogel and TS-MCC aerogel prepared in Example 1 and add them to 10 mL of PS solution with a concentration of 50 mg / L (prepared with deionized water; unless otherwise specified, the water used to prepare the microplastic solution is deionized water). Under room temperature of 25°C, the aerogel is uniformly adsorbed at 120 rpm on a magnetic stirrer for 8 h. The concentration of microplastics after adsorption is measured by UV-Vis spectrophotometer. The adsorption amount of the aerogel adsorbent material is calculated by the change in the concentration of microplastics before and after adsorption.

[0062] Measurement results Figure 3 As shown, with the increase of Py addition, the adsorption capacity of the aerogel for PS shows a trend of first increasing and then decreasing. The system reaches its maximum adsorption capacity (q) when the addition amount is 4.0 wt%. e =92.26±0.73mg / g), which is about 3.19 times higher than the unmodified aerogel sample, significantly improving the adsorption effect of TS-MCC aerogel on PS microplastics.

[0063] Example 4: PS adsorption conditions of TS-MCC / PPy aerogel pairs 1. Effect of pH on the adsorption of TS-MCC / PPy aerogel Take the TS-MCC / PPy prepared in Example 1 4.0 10 mg of aerogel material was added to 10 mL of PS solutions with pH values ​​of 1, 3, 4, 7, 9, 11, and 13 (all concentrations were 100 mg / L). The aerogels were uniformly adsorbed at 120 rpm for 8 h at room temperature (25 °C) using a magnetic stirrer. The concentration of microplastics after adsorption was measured using a UV-Vis spectrophotometer. The adsorption capacity of the aerogel material was calculated by the change in the concentration of microplastics before and after adsorption.

[0064] The measurement results are as follows Figure 4 As shown, as the pH increases from 1 to 3, TS-MCC / PPy 4.0 The adsorption capacity of the aerogel for PS significantly increased from 178.13±3.27 mg / g to 188.72±3.24 mg / g. It remained relatively stable within the pH range of 5-9. With further increases in pH, the adsorption capacity gradually decreased, reaching only 108.25±3.07 mg / g at pH 13. This indicates that the TS-MCC / PPy aerogel exhibits excellent adsorption capacity under a wide range of pH conditions, demonstrating its promising potential for adsorption applications.

[0065] 2. Effect of adsorption time on the adsorption of TS-MCC / PPy aerogel Take the TS-MCC / PPy prepared in Example 1 4.010 mg of aerogel material was added to 10 mL of PS solution with concentrations of 25, 50, and 100 mg / L, respectively. The mixture was stirred at 120 rpm on a magnetic stirrer at 25 °C for 10, 20, 30, 60, 90, 120, 180, 240, 300, 390, and 480 min, respectively. The concentration of microplastics after adsorption was then measured using a UV-Vis spectrophotometer. The adsorption capacity of the aerogel material was calculated by the change in the concentration of microplastics before and after adsorption.

[0066] The measurement results are as follows Figure 5 As shown, the adsorption capacity of TS-MCC / PPy aerogel for PS increases rapidly in the initial stage, then the growth rate gradually decreases, and reaches adsorption equilibrium within a certain period of time. When the initial PS concentration is 25 mg / L, it tends to reach equilibrium at approximately 390 min. e The value was 47.20 ± 0.89 mg / g. When the initial PS concentration was 50 mg / L and 100 mg / L, equilibrium was reached in approximately 300 minutes. e The adsorption values ​​were 92.34±1.78 mg / g and 186.94±2.84 mg / g, respectively. This indicates that the TS-MCC / PPy aerogel can reach adsorption equilibrium in a relatively short time (30 min), achieving rapid and effective adsorption of PS microplastics. This is significantly shorter than the 42 h adsorption time of the TS-MCC aerogel.

[0067] 3. Effect of temperature on the adsorption of TS-MCC / PPy aerogel Take the TS-MCC / PPy prepared in Example 1 4.0 10 mg of aerogel material was added to PS solutions with initial concentrations of 25, 50, 100, 200, 300, 500, 750, and 1000 mg / L, respectively, and the adsorption was carried out uniformly at 120 rpm for 8 h on a magnetic stirrer at 20℃ (293 K), 25℃ (298 K), and 30℃ (303 K), respectively. Subsequently, the concentration of microplastics after adsorption was measured by UV-Vis spectrophotometer, and the adsorption capacity of the aerogel material was calculated by the change in microplastic concentration before and after adsorption.

[0068] The measurement results are as follows Figure 6 As shown, with the increase of the initial concentration of microplastics, the mass transfer driving force increases, leading to changes in the TS-MCC / PPy... 4.0 The adsorption capacity of aerogels for PS initially showed a rapid increase, followed by a slowdown in the rate of increase as adsorption sites approached saturation. Furthermore, the adsorption capacity of the aerogel for PS slightly increased with increasing temperature from 293 K to 303 K. eThe concentration increased from 758.19±46.95 mg / g to 867.33±42.79 mg / g, indicating that TS-MCC / PPy aerogel is more conducive to the adsorption of microplastics under the condition of 303K (30℃).

[0069] Example 5: Adsorption effect of TS-MCC / PPy aerogel under different environmental conditions Take the TS-MCC / PPy prepared in Example 1 4.0 10 mg of aerogel material was added to 10 mL of 100 mg / L PS solution prepared with deionized water, tap water, lake water, river water, and seawater, respectively. The aerogel material was uniformly adsorbed at 120 rpm for 8 h at room temperature (25 °C). The concentration of microplastics after adsorption was measured by UV-Vis spectrophotometer. The adsorption capacity of the aerogel material was calculated by the change in the concentration of microplastics before and after adsorption.

[0070] The measurement results are as follows Figure 7 As shown, compared to the adsorption capacity of the deionized water group (193.47±1.33 mg / g), the adsorption capacities of tap water, lake water, river water, and seawater for PS decreased significantly to 179.93±3.45 mg / g, 175.58±0.64 mg / g, 174.54±5.94 mg / g, and 164.59±4.72 mg / g, respectively. This is because TS-MCC / PPy aerogel has a certain adsorption effect on interfering substances such as metal ions and soluble organic matter (DOM) in water, thus consuming a large number of active sites. However, the adsorption capacity of TS-MCC / PPy aerogel for PS plastic microspheres in different water bodies still maintains a high level (q). e All values ​​were above 160 mg / g, with an adsorption rate of over 80%, indicating that it has good environmental adaptability and practical application prospects.

[0071] Example 6: Cyclic Adsorption Performance of TS-MCC / PPy Aerogel Take the TS-MCC / PPy prepared in Example 1 4.0 10 mg of aerogel material was immersed in 10 mL of PS solution (pH=7, 50 mg / L) and adsorbed for 8 h until equilibrium was reached. Subsequently, the PS-adsorbed aerogel was immersed three times in ethanol and 0.5 M NaOH solution for 2 h each. The remaining ethanol and NaOH were washed with deionized water until neutral, and then lyophilized to prepare for the next adsorption-desorption cycle. This cycle was repeated a total of 10 times.

[0072] The measurement results are as follows Figure 8As shown, the adsorption efficiency of the TS-MCC / PPy aerogel material remained stable in the first two cycles. However, it showed a gradual decline with the increase of the number of cycles. The adsorption efficiency was 91.55±0.53% in the fifth cycle and dropped to 77.65±1.72% in the tenth cycle, which also showed good adsorption stability and durability.

[0073] Example 7: Adsorption effect of TS-MCC / PPy aerogel on microplastics of different types and sizes Take the TS-MCC / PPy prepared in Example 1 4.0 10 mg of aerogel material was immersed in 10 mL of microplastic solutions with an initial concentration of 50 mg / L, namely 100 nm PS, 500 nm PS, 1000 nm PS, 200 nm PP, 1000 nm PET, and 2000 nm PP. The aerogel was uniformly adsorbed at 120 rpm for 8 h at room temperature (25 °C) using a magnetic stirrer. The concentration of microplastics after adsorption was measured using a UV-Vis spectrophotometer and a continuous wavelength multi-functional microplate detection platform. The adsorption capacity of the aerogel material was calculated by the change in microplastic concentration before and after adsorption.

[0074] The measurement results are as follows Figure 9 As shown, TS-MCC / PPy 4.0 The aerogel showed no significant difference in adsorption capacity for 100 nm PS (95.13±1.89 mg / g) and 500 nm PS (96.26±0.59 mg / g). p >0.05), but as the particle size increases to 1000 nm, q e It decreased to 88.03±0.55 mg / g. Despite TS-MCC / PPy 4.0 The adsorption capacity of the aerogel for 200 nm PP (89.01±0.91 mg / g) and 1000 nm PET (89.65±1.96 mg / g) was not statistically different from that for 1000 nm PS. p >0.05), but its adsorption efficiency for 2000nm PE decreased significantly to 82.81±0.69mg / g. This shows that TS-MCC / PPy aerogel exhibits good adsorption capacity for all the aforementioned microplastics (q...). e All of them reached 80mg / g or more, proving their excellent potential for practical application.

[0075] Example 8: Cell compatibility properties of TS-MCC / PPy aerogel This embodiment uses the CCK-8 (Cell Counting Kit-8) method to evaluate the TS-MCC / PPy prepared in Example 1. 4.0 Aerogel and TS-MCC2.0 The effect of the leachate of aerogel material on the survival rate of human liver cancer HepG2 cells was investigated to verify the cell compatibility of aerogel material.

[0076] The specific method is as follows: HepG2 cells are added at a rate of 100 μL per well (approximately 1 × 10⁻⁶ cells). 4 Cells were added to 96-well plates and cultured at 37°C in a 5% CO2 incubator until a monolayer covered 80%–90% of the bottom area of ​​each well. Then, 100 μL of fresh culture medium (0.5, 1.0, 2.5, 5.0, and 10.0 mg / mL) was added to each well, and the cells were cultured for another 24 h. The cells were washed twice with PBS buffer, and then 100 μL of medium (containing 10% CCK8) was added to each well. The cells were cultured for 30 min, and the absorbance was measured at 450 nm. The absorbance values ​​of the blank group (containing CCK8 and no cells) and the control group (normal cells treated with aerogel extract and then treated with CCK8) were compared. Cell viability (%) was calculated based on the changes in absorbance.

[0077] The measurement results are as follows Figure 10 As shown, neither group of materials exhibited significant differences in cytotoxicity at any concentration gradient. p >0.05). When the leachate concentration reaches 10 g / L, TS-MCC 2.0 With TS-MCC / PPy 4.0 The relative cell viability rates in the two groups were 100.36±6.43% and 104.19±3.11%, respectively, with no statistically significant difference compared to the blank control group. p >0.05). This indicates that the TS-MCC / PPy aerogel material did not induce cell growth inhibition or abnormal proliferation within the experimental concentration range, and it has excellent cell compatibility, making it a safe and reliable adsorbent material.

[0078] Example 9: Application of TS-MCC / PPy aerogel in the adsorption and enrichment of microplastics in food. 1. Adsorption effect on microplastics from food packaging This study simulates the microplastic release phenomenon caused by the daily use of plastic products used in everyday food packaging (such as plastic cling film, tea bags, takeout plastic boxes, disposable plastic cups, and mineral water bottles). Specifically, the following groups were set up: PE (PE plastic cling film / bags and PE tea bags), PS (PS sauce containers and PS disposable plastic cups), PET (PET plastic mineral water bottles and beverage bottles), and PP (PP takeout boxes and tableware). Plastic samples from these groups were cut into 1×1cm pieces, and an appropriate amount of deionized water was added. The samples were then heated in a water bath at 100°C for 1 hour, followed by heating in a microwave oven for 5 minutes. Subsequently, the TS-MCC / PPy sample prepared in Example 1 was...4.0 Aerogel materials are used for adsorption, and the change in plastic concentration in the solution is determined by laser projection (Tyndall effect) to judge the adsorption effect.

[0079] The measurement results are as follows Figure 11 As shown, under simulated real-world usage conditions, all types of plastic packaging exhibited significant microplastic release. After heat treatment and microwave irradiation, the originally clear deionized water showed a significant change in turbidity, and a clear Tyndall effect was observed in the laser scattering experiment, indicating the presence of a large number of submicron-sized suspended particles in the solution. (TS-MCC / PPy) 4.0 After aerogel adsorption treatment, the turbidity of the solution significantly decreased to its initial clear state, and the Tyndall effect completely disappeared, indicating that the aerogel achieved efficient capture and adsorption of the released microplastics. Thus, TS-MCC / PPy aerogel exhibits excellent adsorption performance, providing a new technical approach for the control of microplastic contamination in food contact materials.

[0080] 2. Influence of actual food samples and recovery rate determination To verify the application performance of TS-MCC / PPy aerogel material in the adsorption (enrichment) of microplastics in actual food samples, additive recovery experiments were conducted on food samples including soft drinks, tea bags, soy milk in disposable plastic packaging, and seaweed soup packaged in takeout boxes. 10 mL of the above liquid samples were placed in 20 mL sample bottles, and fluorescent plastic microspheres corresponding to the plastic packaging material, namely PET, PE, PS, and PP, were added respectively. Subsequently, 0.5 g of TS-MCC / PPy from Example 1 was added. 4.0 After the aerogel material reached adsorption equilibrium, a sample was taken to test its fluorescence intensity, and the concentration of microplastics was calculated based on the standard curve. The aerogel material after adsorbing microplastics was then eluted with 0.5M sodium hydroxide, and the concentration of microplastics in the eluent was measured. Finally, the recovery rate was calculated.

[0081] The adsorption capacity and recovery rate of the aerogel in different food matrices are shown in Table 1. The results show that the adsorption capacity of TS-MCC / PPy aerogel for the specified microplastics decreased in all food samples. This may be because the organic components (proteins, carbohydrates) and inorganic salts contained in the samples can competitively occupy the adsorption sites of plastic particles in the aerogel pores, thereby weakening the adsorption effect.

[0082] Recovery data show that the TS-MCC / PPy aerogel material has a recovery rate of over 80% for PS, PET, and PP, and the RSD is less than 6 for all of them. This indicates that the aerogel material has good recovery ability and high accuracy, and is expected to be used as an enrichment material in the sample pretreatment process for microplastic detection in food and as a method for developing detection methods.

[0083] Table 1 TS-MCC / PPy4.0 Adsorption capacity and recovery rate of aerogels in different food matrices

[0084] Note: Adsorbent dosage 0.5 g / L, T = 25℃.

[0085] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing a taro stem cellulose-based composite aerogel, characterized in that, Includes the following steps: S1. Preparation of taro stem microcrystalline cellulose: Fresh taro stems were dried, pulverized, sieved, impurities removed, washed, and freeze-dried under vacuum to obtain TS-C powder; the TS-C powder was then acid-hydrolyzed, the precipitate was washed with distilled water until neutral, centrifuged, and freeze-dried to obtain TS-MCC powder. S2. Preparation of Taro Stem Cellulose Aerogel: TS-MCC powder was dissolved in an aqueous solution containing 5-8 wt% NaOH and 10-14 wt% urea, stirred and then frozen. After thawing, a uniform TS-MCC solution was obtained. Then, the cross-linking agent epichlorohydrin was added to the TS-MCC solution, stirred, and unreacted residues were removed by washing with distilled water. The hydrogel was then frozen and then freeze-dried under vacuum to obtain TS-MCC aerogel. S3. Preparation of Taro Stem Cellulose / Polypyrrole Aerogel: TS-MCC aerogel was impregnated in a pyrrole solution, stirred, vacuum dried, degassed, and then 5~20wt% Fe was added. 3+ After stirring the solution, an in-situ oxidative polymerization reaction was carried out. After the reaction was completed, the product was washed with deionized water, and finally the product was freeze-dried under vacuum to obtain TS-MCC / PPy composite aerogel.

2. The preparation method according to claim 1, characterized in that, The concentration of the TS-MCC solution in step S2 is 1.5~6wt%.

3. The preparation method according to claim 1, characterized in that, In step S2, the concentration of the crosslinking agent epichlorohydrin is 5~30wt%.

4. The preparation method according to claim 1, characterized in that, The freezing treatment method in step S2 is as follows: pre-freezing is performed at -20℃ and -80℃ respectively, and the freeze-drying time is 6~72h.

5. The preparation method according to claim 1, characterized in that, The concentration of the pyrrole solution in step S3 is 1~8 wt%.

6. The preparation method according to claim 1, characterized in that, The oxidative polymerization reaction time in step S4 is 5~24h.

7. A taro stem cellulose-based composite aerogel, characterized in that, It is prepared by the method described in any one of claims 1 to 6.

8. The application of the composite aerogel of claim 7 in the adsorption / removal of microplastics.

9. The use of the composite aerogel of claim 7 in the preparation of products that adsorb / remove microplastics.

10. A method for adsorbing / removing microplastics from food, characterized in that, The composite aerogel described in claim 7 was used to process the sample to be tested.