Process and equipment for producing sodium metasilicate pentahydrate
By improving the production equipment and process for sodium metasilicate pentahydrate, and utilizing a combination of heat exchange coils and stirring frames, the problem of poor temperature control was solved, achieving high-efficiency production and uniform crystallization, thus improving production efficiency and product quality.
Patent Information
- Application Number
- CN202410600326.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2026-11-24
AI Technical Summary
In the existing sodium metasilicate pentahydrate production process, the temperature control system is ineffective, resulting in low production efficiency.
The production equipment includes water glass storage tanks, caustic soda storage tanks, metering tanks, crystallizing tanks, automatic centrifuges, and steam tanks. The mixing and processing of raw materials are controlled by connecting pipes and valves. Heat exchange coils are used to concentrate and cool the slurry. Combined with a motor-driven stirring frame, uniform stirring and temperature control are achieved.
This technology enables the efficient production of sodium metasilicate pentahydrate, improving production efficiency and product quality, and ensuring the uniformity of crystals and the effectiveness of solid-liquid separation.
Smart Images

Figure CN123148917A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical processing technology, and in particular to a production process and equipment for sodium metasilicate pentahydrate. Background Technology
[0002] Sodium metasilicate pentahydrate is an inorganic compound with the molecular formula H10Na2O8Si and a molecular weight of 212.14. It is a slightly green or white powder used in ultra-concentrated laundry detergent, washing agents, metal cleaning agents, food industry cleaning agents, as well as paper bleaching, cotton yarn cooking, and porcelain clay dispersion.
[0003] There are three main production processes for sodium metasilicate pentahydrate: granulation, crystallization and pulverization, and mother liquor circulation. Among them, the mother liquor circulation process is relatively simple, and the crystallization tank is the main equipment.
[0004] However, while existing production methods can produce sodium metasilicate pentahydrate, they still have many drawbacks: 1. Chinese Patent No. CN113955764A discloses a continuous production process and apparatus for sodium metasilicate pentahydrate, specifically disclosing that when the liquid cools to a certain temperature, a valve is automatically opened to transfer the cooled liquid. This invention provides the following technical solution: including a main body of equipment, a temperature control and detection device fixedly installed in the inner cavity of the main body, an energy storage mechanism set at the top of the inner wall of the main body, a heat dissipation structure set at the bottom of the energy storage mechanism, a central block fixedly installed inside the main body, a valve mechanism movably installed on the right side of the inner cavity of the main body, and a discharge port set inside the main body. The temperature control system of this patent is not effective, resulting in low production efficiency of sodium metasilicate pentahydrate.
[0005] Based on the aforementioned technical deficiencies, this application urgently requires a production process and equipment for sodium metasilicate pentahydrate. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and to improve the efficient production process and equipment for sodium metasilicate pentahydrate.
[0007] The objective of this invention is achieved through the following technical solution: a production equipment for sodium metasilicate pentahydrate, comprising a water glass storage tank, a caustic soda storage tank, a metering tank, a crystallization tank, an automatic centrifuge, and a steam tank, wherein a first connecting pipe is provided between the water glass storage tank and the metering tank, and a second connecting pipe is provided between the caustic soda storage tank and the metering tank; The first connecting pipe is equipped with a valve and a mud pump. The second connecting pipe is equipped with a valve and a mud pump. The top of the water glass storage tank is equipped with a detachable cover plate. The top of the caustic soda storage tank is equipped with a detachable cover plate. The side walls of both the water glass storage tank and the caustic soda storage tank are equipped with detachable auxiliary feed pipes. The interiors of the water glass storage tank and the caustic soda storage tank are respectively equipped with detachable mesh plates. The bottoms of both mud pumps are equipped with detachable movable support plates. The metering tank includes a movable support metering plate. The top of the movable metering plate is equipped with a metering tank. The metering tank and the crystallization tank are connected by a third connecting pipe.
[0008] In the sodium metasilicate pentahydrate production equipment of the present invention, valve 3 and mud pump 3 are provided on the connecting pipe 3, connecting pipe 4 is provided between the crystallization tank and the automatic centrifuge, and valve 8 is provided on the connecting pipe 4, connecting pipe 5 is provided between the automatic centrifuge and the steam tank, and valve 12 is provided on the connecting pipe 5, and pipe 1 and pipe 2 are provided at the upper part of the crystallization tank.
[0009] In the sodium metasilicate pentahydrate production equipment of the present invention, the lower part of the crystallization tank is provided with pipe three and pipe four, pipe one is provided with valve four, pipe two is provided with valve five, pipe three is provided with valve six, pipe four is provided with valve seven, the steam tank is provided with mother liquor tank, and the side wall of the steam tank is provided with discharge pipe one, the discharge pipe one is provided with valve nine and sludge pump, and the other side of the sludge pump is provided with discharge branch pipe one and discharge branch pipe two.
[0010] In the sodium metasilicate pentahydrate production equipment of the present invention, valve 10 and valve 11 are respectively provided on the discharge branch pipe 1 and discharge branch pipe 2, heating pipe is provided on the bottom of the steam tank, and steam inlet and steam outlet are provided on the top of the steam tank. Heat exchange coil is provided inside the crystallization tank. The heat exchange coil includes an annular plate 1. Several through-hole threads 1 are provided on the side wall of the annular plate 1, and a detachable annular placement plate 1 is provided on the through-hole threads 1.
[0011] In the sodium metasilicate pentahydrate production equipment of the present invention, a motor is provided on the top of the crystallization tank. The output shaft of the motor is provided with a first part, a second part, a third part, a fourth part, a fifth part, and a sixth part. The length of the fifth part is greater than the lengths of the first part, the second part, the third part, the fourth part, and the fifth part. The sixth part and the fifth part are detachably connected. The crystallization tank is composed of a straight cylindrical section and a head. The height of the heat exchange coil is 20 mm lower than the height of the straight cylindrical section, and the diameter is 30 mm smaller than the diameter of the straight cylindrical section. The coil must be reliably fixed to the tank wall. The distance between the two outer sides of the heat exchange coil and the inner side of the tank wall must be the same. The distance between the bottom and top of the coil and the head and the tank opening must be the same.
[0012] In the sodium metasilicate pentahydrate production equipment of the present invention, the upper end of the heat exchange coil is welded to the upper end of the straight section of the tank body and passes through the tank body, with a flange installed. The lower end is welded to the lower end of the straight section of the tank body and passes through the tank body, with a flange installed. A tee is connected at the upper flange, one end of which connects to a steam pipe (pipe one) and the other end connects to a cooling water outlet pipe (pipe two). A tee is connected at the lower flange, one end of which is a steam outlet pipe (pipe three) and the other end is a cooling water inlet pipe (pipe four). A water glass injection pipe and a liquid alkali injection pipe, along with corresponding valves, are installed on the crystallization tank. When 5 0% sodium hydroxide and 50Be water glass are fed into the crystallization tank in a certain proportion. After the motor is started and the mixture is evenly mixed, a sample is taken for testing. When the solid content does not meet the requirements, the cooling water inlet valve is closed and the condensate valve is opened. Then the steam inlet valve is opened, and the steam enters the heat exchange coil to concentrate the slurry. After the specified value is reached, the steam inlet valve is closed and the cooling water inlet valve is opened to start cooling the slurry. The cooling is carried out according to the cooling curve to ensure that the quality of the crystals meets the requirements. The cooling water after heat exchange enters the circulation tank, is cooled by the cooling tower, and is reused.
[0013] In the sodium metasilicate pentahydrate production equipment of the present invention, a stirring frame is provided on the output shaft of the motor, and the stirring frame includes a horizontal stirring frame one and a horizontal stirring frame two, and the horizontal stirring frame one and the horizontal stirring frame two are staggered. The horizontal stirring frame one and the horizontal stirring frame two each include a horizontal stirring plate and a vertical stirring plate, and the horizontal stirring plate and the vertical stirring plate are connected by bolts. The horizontal stirring plate and the vertical stirring plate are provided with a fixed through hole thread two.
[0014] A process for preparing equipment for producing sodium metasilicate pentahydrate includes the following steps: S11. 50Be water glass and 50% caustic soda that have passed the test shall be sent to the storage tank for storage. S12. Based on the production of 8 tons of sodium metasilicate pentahydrate per batch, 8 tons of 50Be water glass and 8 tons of 50% caustic soda are required. The operation method is as follows: Open valve one and start mud pump one to first draw the required water glass into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve one and mud pump one, open valve three and start mud pump three to transfer the water glass in the metering tank to the crystallization tank. Open valve two and start mud pump two to draw the required caustic soda into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve two and mud pump two, open valve three and start mud pump three to transfer the 50% caustic soda in the metering tank to the crystallization tank. S13. Start motor one on the crystallizer and stir continuously for 30 minutes. After the slurry is evenly mixed, take a sample for testing. The required Beaufort concentration is 51±1Be and the modulus M=0.58-0.6. If the above requirements are not met, fine-tuning is required. The method is as follows: S131, (1) Modulus adjustment: The content of SiO2 and Na2O in the slurry is detected. Based on the content and the weight of the slurry, the amount of water glass or caustic soda required is calculated. The addition method in the second part of the working principle is used. After the addition is completed, the mixture is stirred continuously for 30 minutes and then a sample is taken for testing. If the sample fails to meet the requirements, the process is repeated until the modulus is qualified. S132, (2) Concentration Adjustment Before adjustment, ensure that the modulus of the slurry meets the requirements. If the concentration is lower than the Poisson concentration of 51±1Be, close valves five and seven, and open valves four and six. Steam enters the heat exchange coil through valve four to heat and concentrate the slurry. Take multiple samples to test the concentration during the process. Once the concentration meets the requirements, close valve four. The remaining steam is discharged into the recovery water system through valve six. If the concentration is higher than the Poisson concentration of 51±1Be, water needs to be added to reduce the concentration in order to ensure smooth discharge. The amount added is controlled by a quantitative water meter and is calculated based on the initial concentration. S14. After the slurry concentration and modulus meet the requirements, the cooling and crystallization stage begins. The specific operating method is as follows: Open valves seven and five, and cool water should be introduced from high temperature to low temperature to cool the material in the crystallizer through the heat exchange coil. To ensure the quality of the crystallized particles, the cooling gradient needs to be controlled. Depending on the ambient temperature, the cooling should continue for 1-2 hours, and the slurry temperature should be 60℃-70℃. To induce crystallization, seed crystals (sodium metasilicate pentahydrate) should be added at a ratio of 0.15%. The time for the temperature to drop to around 50℃ should be controlled at 7-8 hours, and uniform cooling is required. After the requirement is met, add sodium dodecylbenzene sulfonate P70 at a ratio of 0.075%, stir evenly, and then cool to 46℃-47℃ before discharging for solid-liquid separation. S15. When the slurry temperature reaches 46℃-47℃, start the automatic centrifuge and open valve eight. The mixture of sodium metasilicate pentahydrate and mother liquor in the crystallization tank enters the automatic centrifuge. The feeding speed should be determined according to the discharge of sodium metasilicate pentahydrate. If the feeding speed is too fast, the solid-liquid separation will be incomplete, and more mother liquor will be adsorbed on the surface of the sodium metasilicate pentahydrate particles, making the product prone to agglomeration. If the feeding speed is too low, it will affect the output. S16. The granular sodium metasilicate pentahydrate from the centrifuge falls into the screw conveyor, where it is manually bagged, weighed, and sewn at the discharge end of the screw conveyor. S17. The mother liquor produced after solid-liquid separation contains more than 30% caustic soda and 5% silica. In order to prevent the mother liquor falling into the mother liquor tank from crystallizing due to the low temperature, a heating coil needs to be installed in the mother liquor tank to heat the mother liquor with steam. S18. There are two ways to use the mother liquor. One is to use it as a raw material for sodium metasilicate pentahydrate and then use it for secondary batching. However, due to its low concentration, the cost of subsequent concentration is high. The other is to use it for the production of wet water glass. It is mixed with 50% caustic soda and quartz sand in a certain proportion and then sent to the reactor to produce 50Be water glass.
[0015] The present invention has the following advantages: 1. The mother liquor circulation method of the present invention involves adding 50% sodium hydroxide and 50Be water glass to a crystallization tank in a certain proportion, and obtaining the product through concentration, cooling, crystallization and solid-liquid separation. At the same time, the crystallization tank of the present invention can realize the concentration, cooling and crystallization of the feed liquid separately, and realize convenient temperature control.
[0016] 2. The present invention includes a water glass storage tank, a caustic soda storage tank, a metering tank, a crystallizing tank, an automatic centrifuge, and a steam tank. A connecting pipe is provided between the water glass storage tank and the metering tank, and a connecting pipe is provided between the caustic soda storage tank and the metering tank, so that the incoming raw materials can be conveniently weighed. A valve and a mud pump are installed on connecting pipe 1, and a valve and a mud pump are installed on connecting pipe 2. A removable cover plate 1 is installed on the top of the water glass storage tank, and a removable cover plate 2 is installed on the top of the caustic soda storage tank. A removable auxiliary feed pipe 1 is installed on the side wall of both the water glass storage tank and the caustic soda storage tank. A removable mesh plate 1 and a removable mesh plate 2 are installed inside the water glass storage tank and the caustic soda storage tank, respectively. A removable movable support plate is installed at the bottom of both mud pump 1 and mud pump 2. The metering tank includes a movable support metering plate, and a metering tank is installed on the top of the movable metering plate. A connecting pipe 3 is installed between the metering tank and the crystallization tank, so that processing can be carried out sequentially. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the structure of the present invention; Figure 2 This is a schematic diagram of the setup structure of the automatic centrifuge in this invention; Figure 3 This is a schematic diagram of the stirring frame in this invention; Figure 4 This is a schematic diagram showing the positional relationship between the first transverse stirring frame and the second transverse stirring frame in this invention; Figure 5 This is a schematic diagram of the structure of an output shaft of the motor in this invention; Figure 6 This is a schematic diagram of the detachable annular placement plate in this invention; Figure 7 This is a schematic diagram of the structure of the annular plate one in this invention; Figure 8 for Figure 1 A magnified view of a portion of point A in the middle; Figure 9 for Figure 3 A magnified view of a portion of point B in the middle.
[0018] In the diagram, the components are: 1. Water glass storage tank; 2. Caustic soda storage tank; 3. Metering tank; 4. Crystallization tank; 5. Automatic centrifuge; 6. Steam tank; 7. Connecting pipe 1; 8. Connecting pipe 2; 9. Valve 1; 10. Mud pump 1; 11. Valve 2; 12. Mud pump 2; 13. Removable cover plate 1; 14. Removable cover plate 2; 15. Removable auxiliary feed pipe 1; 16. Removable mesh plate 1; 17. Removable mesh plate 2; 18. Mobile metering plate; 19. Connecting pipe 3; 20. Connecting pipe 4; 21. Connecting pipe 5; 22. Pipe 1; 23. Pipe 2; 24. Pipe 3; 25. Pipe 4; 26. Pipe 5; 27. Pipe 6; 28. Pipe 7; 29. Pipe 8; 20. Connecting pipe 9; 21. Pipe 1; 22. Pipe 2; 23. Pipe 3; 24. Pipe 5; 25. Pipe 6; 26. Pipe 7; 27. Pipe 8; 28. Pipe 9; 29. Pipe 1; 20. Pipe 1; 21. Pipe 2 ...8; 25. Discharge branch pipe 1; 26. Discharge branch pipe 2; 27. Steam inlet; 28. Steam outlet; 29. Heat exchange coil; 30. Annular plate 1; 31. Through hole thread 1; 32. Detachable annular placement plate 1; 33. Motor 1; 34. First part; 35. Second part; 36. Third part; 37. Fourth part; 38. Fifth part; 39. Sixth part; 40. Stirring frame; 41. Horizontal stirring frame 1; 42. Horizontal stirring frame 2; 43. Horizontal stirring plate; 44. Vertical stirring plate; 45. Fixed through hole thread 2; 46. Detailed Implementation
[0019] The present invention will be further described below with reference to the accompanying drawings. The scope of protection of the present invention is not limited to the following description: like Figures 1-9 As shown, a production equipment for sodium metasilicate pentahydrate includes a water glass storage tank 1, a caustic soda storage tank 2, a metering tank 3, a crystallization tank 4, an automatic centrifuge 5, and a steam tank 6. A connecting pipe 7 is provided between the water glass storage tank 1 and the metering tank 3, and a connecting pipe 8 is provided between the caustic soda storage tank 2 and the metering tank 3. A valve 9 and a mud pump 10 are provided on the connecting pipe 7, and a valve 11 and a mud pump 12 are provided on the connecting pipe 8. A detachable cover plate 13 is provided on the top of the water glass storage tank 1, and a detachable cover plate 14 is provided on the top of the caustic soda storage tank 2. Detachable auxiliary feed pipes 15 are provided on the side walls of both the water glass storage tank 1 and the caustic soda storage tank 2. Detachable mesh plates 16 and 17 are provided on the interior of the water glass storage tank 1 and the caustic soda storage tank 2, respectively. Detachable movable support plates are provided on the bottom of both the mud pump 10 and the mud pump 12. The metering tank 3 includes a movable support metering plate 18. The metering tank 3 is located on the top of the movable metering plate 18. A connecting pipe 3 19 is provided between the metering tank 3 and the crystallization tank 4.
[0020] A valve and a mud pump are provided on the connecting pipe 319. A connecting pipe 420 is provided between the crystallizing tank 4 and the automatic centrifuge 5, and a valve 8 is provided on the connecting pipe 420. A connecting pipe 521 is provided between the automatic centrifuge 5 and the steam tank 6, and a valve 12 is provided on the connecting pipe 521. Pipe 12 and pipe 23 are provided on the upper part of the crystallizing tank 4.
[0021] The lower part of the crystallization tank 4 is equipped with pipe 3 24 and pipe 4 25. Pipe 1 22 is equipped with valve 4, pipe 2 23 is equipped with valve 5, pipe 3 24 is equipped with valve 6, and pipe 4 25 is equipped with valve 7. The steam tank 6 is equipped with a mother liquor tank, and the side wall of the steam tank 6 is equipped with discharge pipe 1. The discharge pipe 1 is equipped with valve 9 and a sludge pump, and the other side of the sludge pump is equipped with discharge branch pipe 1 26 and discharge branch pipe 2 27.
[0022] The discharge branch pipe 1 26 and the discharge branch pipe 27 are respectively equipped with valve 10 and valve 11. The bottom of the steam tank 6 is equipped with a heating pipe, and the top of the steam tank 6 is equipped with a steam inlet 28 and a steam outlet 29. The interior of the crystallization tank 4 is equipped with a heat exchange coil 30. The heat exchange coil 30 includes an annular plate 31. The side wall of the annular plate 31 is equipped with several through-hole threads 32, and the through-hole threads 32 are equipped with a detachable annular placement plate 33.
[0023] The top of the crystallization tank 4 is equipped with a motor 34. The output shaft of the motor 34 has a first part 35, a second part 36, a third part 37, a fourth part 38, a fifth part 39, and a sixth part 40. The length of the fifth part 39 is greater than the lengths of the first part 35, the second part 36, the third part 37, the fourth part 38, and the fifth part 39. The sixth part 40 is detachably connected to the fifth part 39. The crystallization tank 4 consists of a straight section and a head. The height of the heat exchange coil 30 is 20 mm lower than the height of the straight section, and the diameter is 30 mm smaller than the diameter of the straight section. The coil must be reliably fixed to the tank wall. The distance between the two outer sides of the heat exchange coil 30 and the inner side of the tank wall must be the same. The distance between the bottom and top of the coil and the head and the tank opening must be the same.
[0024] The upper end of heat exchange coil 30 is welded to the upper end of the straight section of the tank body and passes through the tank body, with a flange installed. The lower end is welded to the lower end of the straight section of the tank body, passes through the tank body, and is fitted with a flange. A tee is connected at the upper flange, one end to the steam pipe (pipe 1 22) and the other end to the cooling water outlet pipe (pipe 2 23). A tee is connected at the lower flange, one end to the steam outlet pipe (pipe 3 24) and the other end to the cooling water inlet pipe (pipe 4 25). A water glass injection pipe and a liquid alkali injection pipe, along with corresponding valves, are installed on crystallizing tank 4. When 50% sodium hydroxide and 5... 0Be water glass is fed into crystallization tank 4 in a certain proportion. After the motor 34 is started and the mixture is evenly mixed, a sample is taken for testing. When the solid content does not meet the requirements, the cooling water inlet valve is closed, the condensate valve is opened, and then the steam inlet valve is opened. Steam enters the heat exchange coil 30 to concentrate the slurry. After reaching the specified value, the steam inlet valve is closed, the cooling water inlet valve is opened, and the slurry is cooled down. The cooling is carried out according to the cooling curve to ensure that the quality of the crystals meets the requirements. The cooling water after heat exchange enters the circulation tank, is cooled by the cooling tower, and is reused.
[0025] The output shaft of motor 34 is equipped with a stirring frame 41 to ensure high stirring efficiency. The stirring frame 41 includes a first horizontal stirring frame 42 and a second horizontal stirring frame 43, which are staggered. Both the first horizontal stirring frame 42 and the second horizontal stirring frame 43 include a horizontal stirring plate 44 and a vertical stirring plate 45, which are connected by bolts. The horizontal stirring plate 44 and the vertical stirring plate 45 are provided with a second threaded fixing hole 46.
[0026] A process for preparing equipment for producing sodium metasilicate pentahydrate includes the following steps: S11. 50Be water glass and 50% caustic soda that have passed the test shall be sent to the storage tank for storage. S12. Based on the production of 8 tons of sodium metasilicate pentahydrate per batch, 8 tons of 50Be water glass and 8 tons of 50% caustic soda are required. The operation method is as follows: Open valve one and start mud pump one to first draw the required water glass into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve one and mud pump one, open valve three and start mud pump three to transfer the water glass in the metering tank to the crystallization tank. Open valve two and start mud pump two to draw the required caustic soda into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve two and mud pump two, open valve three and start mud pump three to transfer the 50% caustic soda in the metering tank to the crystallization tank. S13. Start motor one on the crystallizer and stir continuously for 30 minutes. After the slurry is evenly mixed, take a sample for testing. The required Beaufort concentration is 51±1Be and the modulus M=0.58-0.6. If the above requirements are not met, fine-tuning is required. The method is as follows: S131, (1) Modulus adjustment: The content of SiO2 and Na2O in the slurry is detected. Based on the content and the weight of the slurry, the amount of water glass or caustic soda required is calculated. The addition method in the second part of the working principle is used. After the addition is completed, the mixture is stirred continuously for 30 minutes and then a sample is taken for testing. If the sample fails to meet the requirements, the process is repeated until the modulus is qualified. S132, (2) Concentration Adjustment Before adjustment, ensure that the modulus of the slurry meets the requirements. If the concentration is lower than the Poisson concentration of 51±1Be, close valves five and seven, and open valves four and six. Steam enters the heat exchange coil through valve four to heat and concentrate the slurry. Take multiple samples to test the concentration during the process. Once the concentration meets the requirements, close valve four. The remaining steam is discharged into the recovery water system through valve six. If the concentration is higher than the Poisson concentration of 51±1Be, water needs to be added to reduce the concentration in order to ensure smooth discharge. The amount added is controlled by a quantitative water meter and is calculated based on the initial concentration. S14. After the slurry concentration and modulus meet the requirements, the cooling and crystallization stage begins. The specific operating method is as follows: Open valves seven and five, and cool water should be introduced from high temperature to low temperature to cool the material in the crystallizer through the heat exchange coil. To ensure the quality of the crystallized particles, the cooling gradient needs to be controlled. Depending on the ambient temperature, the cooling should continue for 1-2 hours, and the slurry temperature should be 60℃-70℃. To induce crystallization, seed crystals (sodium metasilicate pentahydrate) should be added at a ratio of 0.15%. The time for the temperature to drop to around 50℃ should be controlled at 7-8 hours, and uniform cooling is required. After the requirement is met, add sodium dodecylbenzene sulfonate P70 at a ratio of 0.075%, stir evenly, and then cool to 46℃-47℃ before discharging for solid-liquid separation. S15. When the slurry temperature reaches 46℃-47℃, start the automatic centrifuge and open valve eight. The mixture of sodium metasilicate pentahydrate and mother liquor in the crystallization tank enters the automatic centrifuge. The feeding speed should be determined according to the discharge of sodium metasilicate pentahydrate. If the feeding speed is too fast, the solid-liquid separation will be incomplete, and more mother liquor will be adsorbed on the surface of the sodium metasilicate pentahydrate particles, making the product prone to agglomeration. If the feeding speed is too low, it will affect the output. S16. The granular sodium metasilicate pentahydrate from the centrifuge falls into the screw conveyor, where it is manually bagged, weighed, and sewn at the discharge end of the screw conveyor. S17. The mother liquor produced after solid-liquid separation contains more than 30% caustic soda and 5% silica. In order to prevent the mother liquor falling into the mother liquor tank from crystallizing due to the low temperature, a heating coil needs to be installed in the mother liquor tank to heat the mother liquor with steam. S18. There are two ways to use the mother liquor. One is to use it as a raw material for sodium metasilicate pentahydrate and then use it for secondary batching. However, due to its low concentration, the cost of subsequent concentration is high. The other is to use it for the production of wet water glass. It is mixed with 50% caustic soda and quartz sand in a certain proportion and then sent to the reactor to produce 50Be water glass.
[0027] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A production apparatus for sodium metasilicate pentahydrate, characterized in that: It includes a water glass storage tank, a caustic soda storage tank, a metering tank, a crystallization tank, an automatic centrifuge, and a steam tank. A connecting pipe 1 is provided between the water glass storage tank and the metering tank, and a connecting pipe 2 is provided between the caustic soda storage tank and the metering tank. The first connecting pipe is equipped with a valve and a mud pump. The second connecting pipe is equipped with a valve and a mud pump. The top of the water glass storage tank is equipped with a detachable cover plate. The top of the caustic soda storage tank is equipped with a detachable cover plate. The side walls of both the water glass storage tank and the caustic soda storage tank are equipped with detachable auxiliary feed pipes. The interiors of the water glass storage tank and the caustic soda storage tank are respectively equipped with detachable mesh plates. The bottoms of both mud pumps are equipped with detachable movable support plates. The metering tank includes a movable support metering plate. The top of the movable metering plate is equipped with a metering tank. The metering tank and the crystallization tank are connected by a third connecting pipe.
2. The production equipment for sodium metasilicate pentahydrate according to claim 1, characterized in that: The connecting pipe 3 is equipped with valve 3 and mud pump 3. The crystallization tank and the automatic centrifuge are connected by a connecting pipe 4, and valve 8 is provided on the connecting pipe 4. The automatic centrifuge and the steam tank are connected by a connecting pipe 5, and valve 12 is provided on the connecting pipe 5. The upper part of the crystallization tank is equipped with pipe 1 and pipe 2.
3. The production equipment for sodium metasilicate pentahydrate according to claim 2, characterized in that: The lower part of the crystallization tank is provided with pipes three and four. Pipe one is provided with valve four, pipe two is provided with valve five, pipe three is provided with valve six, and pipe four is provided with valve seven. The steam tank is provided with a mother liquor tank, and the side wall of the steam tank is provided with discharge pipe one. The discharge pipe one is provided with valve nine and a sludge pump, and the other side of the sludge pump is provided with discharge branch pipe one and discharge branch pipe two.
4. The production equipment for sodium metasilicate pentahydrate according to claim 3, characterized in that: The discharge branch pipe 1 and discharge branch pipe 2 are respectively equipped with valve 10 and valve 11. The bottom of the steam tank is equipped with a heating pipe, and the top of the steam tank is equipped with a steam inlet and a steam outlet. The interior of the crystallization tank is equipped with a heat exchange coil. The heat exchange coil includes an annular plate. The side wall of the annular plate is equipped with several through-hole threads, and the through-hole threads are equipped with a detachable annular placement plate.
5. The production equipment for sodium metasilicate pentahydrate according to claim 4, characterized in that: The crystallization tank is equipped with a motor on its top. The output shaft of the motor has a first part, a second part, a third part, a fourth part, a fifth part, and a sixth part. The length of the fifth part is greater than the lengths of the first, second, third, fourth, and fifth parts. The sixth part is detachably connected to the fifth part. The crystallization tank consists of a straight cylindrical section and a head. The height of the heat exchange coil is 20 mm lower than the height of the straight cylindrical section, and the diameter is 30 mm smaller than the diameter of the straight cylindrical section. The coil must be reliably fixed to the tank wall. The distance between the two outer sides of the heat exchange coil and the inner side of the tank wall must be the same. The distance between the bottom and top of the coil and the head and the tank opening must be the same.
6. The production equipment for sodium metasilicate pentahydrate according to claim 5, characterized in that: The upper end of the heat exchange coil is welded to the upper end of the straight section of the tank body and passes through the tank body, where a flange is installed. The lower end is welded to the lower end of the straight section of the tank body and passes through the tank body, where a flange is installed. A tee is connected at the upper flange, one end connecting to the steam pipe (pipe one) and the other end connecting to the cooling water outlet pipe (pipe two). A tee is connected at the lower flange, one end being the steam outlet pipe (pipe three) and the other end being the cooling water inlet pipe (pipe four). A water glass injection pipe and a liquid alkali injection pipe, along with corresponding valves, are installed on the crystallization tank. When 50% sodium hydroxide and 50%... Be water glass is fed into the crystallization tank in a certain proportion. After the motor is started and the mixture is evenly mixed, a sample is taken for testing. If the solid content does not meet the requirements, the cooling water inlet valve is closed, the condensate valve is opened, and then the steam inlet valve is opened. Steam enters the heat exchange coil to concentrate the slurry. After reaching the specified value, the steam inlet valve is closed, the cooling water inlet valve is opened, and the slurry is cooled down. The cooling is carried out according to the cooling curve to ensure that the quality of the crystals meets the requirements. The cooling water after heat exchange enters the circulation tank, is cooled by the cooling tower, and is reused.
7. The production equipment for sodium metasilicate pentahydrate according to claim 6, characterized in that: The output shaft of the motor is provided with a stirring frame, which includes a horizontal stirring frame one and a horizontal stirring frame two. The horizontal stirring frame one and the horizontal stirring frame two are staggered. The horizontal stirring frame one and the horizontal stirring frame two each include a horizontal stirring plate and a vertical stirring plate. The horizontal stirring plate and the vertical stirring plate are connected by bolts. The horizontal stirring plate and the vertical stirring plate are provided with a fixed through hole thread two.
8. The preparation process using the production equipment for sodium metasilicate pentahydrate as described in claim 7, characterized in that; Includes the following steps: S11. 50Be water glass and 50% caustic soda that have passed the test shall be sent to the storage tank for storage. S12. Based on the production of 8 tons of sodium metasilicate pentahydrate per batch, 8 tons of 50Be water glass and 8 tons of 50% caustic soda are required. The operation method is as follows: Open valve one and start mud pump one to first draw the required water glass into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve one and mud pump one, open valve three and start mud pump three to transfer the water glass in the metering tank to the crystallization tank. Open valve two and start mud pump two to draw the required caustic soda into the metering tank. The quantity is controlled by a 20-ton electronic scale. After reaching the specified value, close valve two and mud pump two, open valve three and start mud pump three to transfer the 50% caustic soda in the metering tank to the crystallization tank. S13. Start motor one on the crystallizer and stir continuously for 30 minutes. After the slurry is evenly mixed, take a sample for testing. The required Beaufort concentration is 51±1Be and the modulus M=0.58-0.
6. If the above requirements are not met, fine-tuning is required. The method is as follows: S131, (1) Modulus adjustment: The content of SiO2 and Na2O in the slurry is detected. Based on the content and the weight of the slurry, the amount of water glass or caustic soda required is calculated. The addition method in the second part of the working principle is used. After the addition is completed, the mixture is stirred continuously for 30 minutes and then a sample is taken for testing. If the sample fails to meet the requirements, the process is repeated until the modulus is qualified. S132, (2) Concentration Adjustment Before adjustment, ensure that the modulus of the slurry meets the requirements. If the concentration is lower than the Poisson concentration of 51±1Be, close valves five and seven, and open valves four and six. Steam enters the heat exchange coil through valve four to heat and concentrate the slurry. Take multiple samples to test the concentration during the process. Once the concentration meets the requirements, close valve four. The remaining steam is discharged into the recovery water system through valve six. If the concentration is higher than the Poisson concentration of 51±1Be, water needs to be added to reduce the concentration in order to ensure smooth discharge. The amount added is controlled by a quantitative water meter and is calculated based on the initial concentration. S14. After the slurry concentration and modulus meet the requirements, the cooling crystallization stage begins. The specific operating method is as follows: Open valves seven and five, and cool water should be introduced from high temperature to low temperature to cool the material in the crystallizer through the heat exchange coil. To ensure the quality of the crystallized particles, the cooling gradient needs to be controlled. Depending on the ambient temperature, the cooling should continue for 1-2 hours, and the slurry temperature should be 60℃-70℃. To induce crystallization, seed crystals (sodium metasilicate pentahydrate) should be added at a ratio of 0.15%. The time for the temperature to drop to around 50℃ should be controlled at 7-8 hours, and uniform cooling is required. After the requirement is met, add sodium dodecylbenzene sulfonate P70 at a ratio of 0.075%, stir evenly, and then cool to 46℃-47℃ before discharging for solid-liquid separation. S15. When the slurry temperature reaches 46℃-47℃, start the automatic centrifuge and open valve eight. The mixture of sodium metasilicate pentahydrate and mother liquor in the crystallization tank enters the automatic centrifuge. The feeding speed should be determined according to the discharge of sodium metasilicate pentahydrate. If the feeding speed is too fast, the solid-liquid separation will be incomplete, and more mother liquor will be adsorbed on the surface of the sodium metasilicate pentahydrate particles, making the product prone to agglomeration. If the feeding speed is too low, it will affect the output. S16. The granular sodium metasilicate pentahydrate from the centrifuge falls into the screw conveyor, where it is manually bagged, weighed, and sewn at the discharge end of the screw conveyor. S17. The mother liquor produced after solid-liquid separation contains more than 30% caustic soda and 5% silica. In order to prevent the mother liquor falling into the mother liquor tank from crystallizing due to the low temperature, a heating coil needs to be installed in the mother liquor tank to heat the mother liquor with steam. S18. There are two ways to use the mother liquor. One is to use it as a raw material for sodium metasilicate pentahydrate and then use it for secondary batching. However, due to its low concentration, the cost of subsequent concentration is high. The other is to use it for the production of wet water glass. It is mixed with 50% caustic soda and quartz sand in a certain proportion and then sent to the reactor to produce 50Be water glass.
Citation Information
Patent Citations
Continuous production process and device of sodium metasilicate pentahydrate
CN113955764A