Straw-based iron-manganese oxide composite thallium removal material and in-situ loading preparation method thereof
By in-situ growing iron-manganese oxides in straw-based materials, constructing Fe-O-Mn heterostructures and microgalvanic cell networks, the problem of low thallium removal efficiency in traditional composite materials was solved, achieving efficient and stable thallium oxidation and adsorption.
Patent Information
- Application Number
- CN202611421661.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies are ineffective at removing low concentrations of thallium ions, and traditional precipitation methods suffer from problems such as oxide agglomeration, low electron transfer efficiency, and low utilization of active sites in composite materials.
By using straw-based iron-manganese oxide composite materials, iron-manganese oxides are grown in situ within the natural vascular bundles of straw to construct Fe-O-Mn heterostructures and micro-galvanic cell networks, forming a gradient functional structure to achieve efficient oxidation and fixation of thallium.
It significantly improves the adsorption capacity and oxidation activity of thallium, maintains high efficiency over a wide pH range, has long-lasting self-healing ability, and exhibits excellent cycle stability.
Smart Images

Figure CN123148931A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of environmental functional materials technology, specifically to a straw-based iron-manganese oxide composite thallium removal material and its in-situ loading preparation method. Background Technology
[0002] Thallium (Tl) is a highly toxic heavy metal, far exceeding the toxicity of elements such as Hg, Cd, and Pb, and is listed in my country's priority pollutant control list. Thallium-containing wastewater mainly originates from industrial processes such as lead-zinc smelting, desulfurization in coal-fired power plants, and sulfuric acid production. Its Tl(I) exhibits high solubility, high mobility, and bioaccumulation, making it difficult to effectively remove using conventional precipitation methods. Actual thallium concentrations in wastewater are typically in the range of μg / L to mg / L; at extremely low concentrations, traditional precipitation methods cannot meet emission limits. Furthermore, the water contains a large number of coexisting ions (such as K+). + Ca 2+ Na + (etc.) and Tl + Competing for adsorption sites severely interferes with removal efficiency.
[0003] Currently, thallium-containing wastewater treatment technologies mainly include chemical precipitation, ion exchange, solvent extraction, membrane separation, and adsorption. Among these, adsorption has become a research hotspot due to its advantages such as simple operation, low cost, fast removal rate, and scalability. In recent years, the use of biochar-supported iron-manganese oxides as thallium removal adsorbents has attracted much attention. The principle is to utilize the adsorption and enrichment effect of biochar combined with the oxidative precipitation effect of iron-manganese oxides to synergistically remove Tl(I).
[0004] Previous studies have attempted to load iron and manganese oxides onto biochar such as rice husk charcoal and corn cob charcoal (e.g., Zhang et al., 2019; Li et al., 2021), but most of these studies use the impregnation-calcination method, which results in severe agglomeration of oxides on the charcoal surface, with particle sizes reaching hundreds of nanometers and low utilization of active sites. Furthermore, the iron and manganese are only physically mixed, lacking a heterogeneous interface with chemical bonding, which hinders electron transfer, resulting in insufficient oxidation conversion efficiency of Tl(I) to Tl(III), generally lower than 100 mg / g, and poor cycle stability.
[0005] To address the aforementioned problems, this invention proposes the following scientific hypothesis: If iron-manganese precursors can be pre-loaded into biomass rich in natural vascular structures, and then iron-manganese oxides can be grown in situ within the nanoscale space of the vascular wall through confined pyrolysis, it is expected that the spatial confinement effect of the vascular wall can be used to suppress the agglomeration and growth of oxide particles. Simultaneously, by utilizing the interfacial solid-state reaction between the carbon substrate and the oxide precursor during pyrolysis, a Fe-O-Mn heterostructure with lattice matching can be constructed in situ. This heterostructure can serve as a channel for directional electron migration. Combined with the spontaneous micro-galvanic cell effect formed between the carbon skeleton and the iron-manganese oxide due to the difference in electrode potential, electrons can be continuously supplied to the heterostructure, enabling Tl(I) to be efficiently oxidized to Tl(III) at the interface. This three-in-one design concept of 'confined growth-heterostructure-micro-galvanic cell' is expected to fundamentally solve the key problems of easy agglomeration of active components and low electron transfer efficiency in traditional composite materials, significantly improving the thallium removal capacity and oxidation activity of the material. Summary of the Invention
[0006] The purpose of this invention is to provide a straw-based iron-manganese oxide composite thallium removal material and its in-situ loading preparation method, so as to solve the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] In a first aspect, this application provides a straw-based iron-manganese oxide composite thallium removal material, comprising a straw-based porous carbon skeleton and an iron-manganese oxide composite loaded on the carbon skeleton;
[0009] The iron-manganese oxide composite contains α-MnO2 and γ-FeOOH crystal phases, and has Fe-O-Mn heterostructure and oxygen vacancies;
[0010] The material has a gradient functional structure consisting of an outer oxide layer, a middle complex layer, and an inner fixing layer, from the outside to the inside.
[0011] Secondly, this application provides an in-situ loading preparation method for a straw-based iron-manganese oxide composite thallium removal material, comprising:
[0012] Pretreated straw is provided, wherein the pretreated straw is impregnated with an iron-manganese precursor solution to obtain impregnated straw loaded with iron-manganese precursors;
[0013] The impregnated straw is used for confined pyrolysis crystallization treatment in an oxygen-containing atmosphere, so that the iron-manganese precursor grows in situ in the natural vascular bundles of the straw into Fe-Mn oxide heterojunctions with oxygen vacancies, thus obtaining the primary composite material.
[0014] The nascent composite material is used for gradient activation treatment in an oxygen-containing atmosphere to form a gradient functional structure of an outer oxide layer, a middle complex layer, and an inner fixing layer on the surface of the nascent composite material, thereby obtaining an activated composite material.
[0015] The activated composite material is used for in-situ mineralization and stabilization treatment in an oxygen-containing atmosphere, so that the Fe-Mn oxide in the activated composite material is further crystallized and oxygen vacancies are stabilized to obtain the thallium removal material.
[0016] Furthermore, the pretreated straw is obtained in the following way:
[0017] After washing and drying, the straw is crushed to 20-100 mesh and then placed in an alkaline solution with a mass fraction of 1%-10% at 60-90°C for 1-4 hours. After washing and drying, the pretreated straw is obtained.
[0018] The straw is selected from at least one of corn straw, rice straw, and wheat straw.
[0019] Furthermore, the iron-manganese precursor solution is prepared by dissolving iron salt, manganese salt and chelating agent in deionized water, wherein the molar ratio of iron salt to manganese salt is 1:0.5 to 1:3, and the ratio of chelating agent to total molar number of metal ions is 0.5:1 to 2:1.
[0020] The iron salt is selected from at least one of Fe(NO3)3·9H2O, FeCl3·6H2O, and Fe2(SO4)3; the manganese salt is selected from at least one of KMnO4, MnSO4·H2O, and Mn(NO3)2; and the chelating agent is selected from at least one of citric acid, ethylenediaminetetraacetic acid, and oxalic acid.
[0021] The impregnation process is as follows: pretreated straw is mixed with iron-manganese precursor solution at a mass ratio of 1:5 to 1:20, stirred and impregnated at 25 to 60°C for 4 to 12 hours, and then dried at 40 to 80°C for 6 to 24 hours to obtain the impregnated straw.
[0022] Furthermore, the confined pyrolysis crystallization treatment is as follows:
[0023] The impregnated straw is placed in a tube furnace and heated to 400-700°C at a heating rate of 1-10°C / min. It is then kept at this temperature for 1-4 hours in an oxygen-containing atmosphere, so that the iron-manganese precursor crystallizes in situ into an α-MnO2 / γ-FeOOH composite crystal phase within the confined space of the straw's natural vascular bundle wall, and simultaneously forms a micro galvanic cell network supported by a carbon skeleton, thus obtaining the nascent composite material.
[0024] The oxygen-containing atmosphere is air or a nitrogen-oxygen mixture with an oxygen volume fraction of 5% to 21%.
[0025] Furthermore, in the confined pyrolysis crystallization treatment, the mass ratio of α-MnO2 to γ-FeOOH crystal phases is controlled to be 1:2 to 3:1 by controlling the heating rate and holding temperature, and the oxygen vacancy concentration is controlled by controlling the oxygen partial pressure in the oxygen-containing atmosphere, so that the relative content of oxygen vacancy in the nascent composite material is 15% to 35%.
[0026] Further, the gradient activation process is as follows:
[0027] The nascent composite material is placed in an oxygen-containing atmosphere and kept at 200–400°C for 0.5–2 hours to form a gradient functional structure on the surface of the nascent composite material, with Mn(IV) / Fe(III) oxide as the outer oxide layer, Fe-O-Mn heterostructure as the middle complex layer, and Fe(O) / Mn(II) supported by a carbon skeleton as the inner immobilization layer, thus obtaining the activated composite material.
[0028] Furthermore, in the gradient activation process, the thickness of the outer oxide layer is 50–200 nm, the Fe-O-Mn heterostructure of the middle complex layer is characterized by the XPS binding energy shift difference between Fe2p3 / 2 and Mn2p3 / 2 being 0.8–1.5 eV, and the inner immobilization layer provides a continuous electron supply through the in-situ reduction of Fe(O) and Mn(II) in the carbon skeleton, maintaining the redox cycle of the micro galvanic cell network.
[0029] Further, the in-situ mineralization stabilization treatment is as follows: the activated composite material is kept at 150-300℃ for 0.5-2h in an oxygen-containing atmosphere to stabilize the valence cycle between Mn(IV) / Mn(III) and Fe(III) / Fe(II) in the Fe-Mn oxide, while increasing the oxygen vacancy concentration to 20%-40%, to obtain the thallium removal material.
[0030] Furthermore, in the iron-manganese oxide composite, the total mass of iron-manganese oxide accounts for 30% to 70% of the total mass of the material, the mass ratio of α-MnO2 to γ-FeOOH is 1:2 to 3:1, the relative content of oxygen vacancies is 15% to 40%, and the specific surface area of the material is 200 to 600 m². 2 / g, with an average pore size of 2–10 nm.
[0031] Compared with existing technologies, this invention provides a straw-based iron-manganese oxide composite thallium removal material and its in-situ loading preparation method. Utilizing the natural vascular bundles of straw as a confined reaction space, the iron-manganese precursor is grown in situ into nanoscale iron-manganese oxide with a Fe-O-Mn heterostructure during pyrolysis, while simultaneously constructing a micro-galvanic cell network during the carbon skeleton formation. In this micro-galvanic cell network, the carbon skeleton serves as the cathode and the iron-manganese oxide as the anode. A potential difference is spontaneously generated through the standard electrode potential difference between Fe(O) / Fe(III) and Mn(II) / Mn(IV), driving electrons to migrate directionally from the carbon skeleton to the iron-manganese oxide. This continuously supplies electrons to the Fe-O-Mn heterostructure interface, enabling the efficient oxidation of Tl(I) to Tl(III) at this interface. This interfacial electron transfer mechanism operates continuously without external energy input, overcoming the technical bottleneck of traditional adsorption materials that rely on surface physicochemical adsorption and have insufficient oxidation capacity.
[0032] This invention constructs a gradient functional structure within the material through gradient activation treatment, consisting of an outer oxide layer, a middle complex layer, and an inner fixation layer. This allows Tl(I) to undergo three stages of fixation during its migration path: oxidation, complexation, and mineralization. Tl(I) is first oxidized to Tl(III) by the outer Mn(IV) / Fe(III) oxide, then complexed and anchored at the middle Fe-O-Mn heterostructure interface, and finally mineralized in the inner layer to form a stable mineral phase of Tl2O3 or TlFeO2.
[0033] Meanwhile, the reduced Mn(II) / Fe(II) can be re-oxidized to a higher valence state under oxygen-containing conditions, realizing the cyclic regeneration of oxidation activity and enabling the material to have long-term self-repair capability, effectively avoiding the problem of rapid deactivation caused by the irreversible consumption of active sites in traditional modified biochar. Attached Figure Description
[0034] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this invention. For those skilled in the art, other drawings can be obtained based on these drawings.
[0035] Figure 1 A flowchart illustrating an in-situ loading preparation method for a straw-based iron-manganese oxide composite thallium removal material provided in this embodiment of the invention. Detailed Implementation
[0036] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.
[0037] As attached Figure 1 As shown:
[0038] Example 1:
[0039] This embodiment provides a straw-based iron-manganese oxide composite thallium removal material and its preparation method.
[0040] 1. Material Composition
[0041] The straw-based iron-manganese oxide composite thallium removal material of this embodiment includes a straw-based porous carbon skeleton and an iron-manganese oxide composite loaded on the carbon skeleton.
[0042] The iron-manganese oxide composite contains α-MnO2 and γ-FeOOH crystal phases, and has Fe-O-Mn heterostructure and oxygen vacancies;
[0043] α-MnO2 has a unique [2×2] tunnel structure (pore size of about 0.46 nm), which is well matched with the diameter of the hydrated ions of Tl(I) (about 0.33 nm), which is conducive to Tl(I) entering the tunnel and making full contact with the active sites.
[0044] Meanwhile, the mixed valence state of Mn(III) / Mn(IV) in the α-MnO2 structure gives it a high intrinsic oxygen vacancy concentration and excellent redox activity, exhibiting higher catalytic efficiency than other crystal forms (such as the [1×1] tunnel of β-MnO2 and the layered structure of δ-MnO2) in the oxidation transformation of Tl(I)→Tl(III).
[0045] The present invention preferentially guides the formation of α-MnO2 crystal phase under confined pyrolysis conditions, mainly due to the coordination anchoring effect of oxygen-containing functional groups (-COOH, -OH, etc.) on Mn precursors on the inner wall of straw ducts and the mass transfer constraint in the confined space, which together promote the kinetic preferential precipitation of thermodynamically metastable α-MnO2.
[0046] This invention precisely controls confined pyrolysis conditions to form only two crystal phases, α-MnO2 and γ-FeOOH, avoiding the formation of β-MnO2 or δ-MnO2 with lower electrochemical activity, thus ensuring the optimal oxidation-complexation synergistic effect.
[0047] The material has a gradient functional structure consisting of an outer oxide layer, a middle complex layer, and an inner fixing layer, from the outside to the inside.
[0048] Of the materials, iron and manganese oxides account for 50% of the total mass, the mass ratio of α-MnO2 to γ-FeOOH is 1:1, the relative content of oxygen vacancies is 25%, and the specific surface area of the materials is 380 m². 2 / g, with an average pore size of 6 nm.
[0049] 2. Preparation method
[0050] (1) Preparation of pretreated straw: After washing and drying the corn straw, crush it to 60 mesh, place it in a 5% NaOH alkaline solution and treat it at 80℃ for 2 h. After washing with deionized water until neutral and drying at 105℃ for 12 h, the pretreated straw is obtained.
[0051] (2) Impregnation treatment: Fe(NO3)3·9H2O and KMnO4 were dissolved in deionized water at a Fe:Mn molar ratio of 1:1. Citric acid was added as a chelating agent (the ratio of citric acid to the total molar of metal ions was 1:1) to prepare an iron-manganese precursor solution. The pretreated straw was mixed with the iron-manganese precursor solution at a mass ratio of 1:10, stirred and impregnated at 40℃ for 8 h, and then dried at 60℃ for 12 h to obtain impregnated straw loaded with iron-manganese precursor.
[0052] (3) Confined pyrolysis crystallization treatment: The impregnated straw is placed in a tube furnace and heated to 550°C at a heating rate of 5°C / min. It is kept at the temperature for 2 h in an air atmosphere so that the iron-manganese precursor crystallizes in situ into α-MnO2 / γ-FeOOH composite crystal phase in the confined space of the straw natural vascular wall, and simultaneously forms a micro galvanic cell network supported by a carbon skeleton to obtain the primary composite material.
[0053] X-ray diffraction (XRD) characterization confirmed the presence of characteristic diffraction peaks for both α-MnO2 (JCPDS No. 44-0141) and γ-FeOOH (JCPDS No. 44-1415). The mass ratio of α-MnO2 to γ-FeOOH was adjusted to 1:1 by controlling the heating rate and holding temperature, and the oxygen vacancy concentration was adjusted by controlling the oxygen partial pressure (21% O2) in the air atmosphere, so that the relative content of oxygen vacancies in the nascent composite material was 25%.
[0054] The relative content of oxygen vacancies was calculated by peak fitting of the O 1s spectrum in X-ray photoelectron spectroscopy (XPS), and determined by the ratio of the peak areas of lattice oxygen (approximately 529.5 eV) to oxygen vacancies (approximately 531.5 eV).
[0055] Scanning electron microscopy (SEM) observation showed that iron-manganese oxides were uniformly distributed as nanoparticles on the inner wall of straw ducts, with a particle size of approximately 50–100 nm.
[0056] (4) Gradient activation treatment: The nascent composite material is placed in an air atmosphere and kept at 300℃ for 1 h to form a gradient functional structure on the surface of the nascent composite material, with Mn(IV) / Fe(Ⅲ) oxide as the outer oxide layer, Fe-O-Mn heterostructure as the middle complex layer, and Fe(O) / Mn(II) supported by carbon skeleton as the inner fixation layer, thus obtaining the activated composite material.
[0057] Transmission electron microscopy (TEM) revealed that the outer oxide layer was approximately 120 nm thick.
[0058] XPS analysis showed that the binding energy shift difference between Fe 2p3 / 2 and Mn 2p3 / 2 was 1.2 eV, confirming the formation of the Fe-O-Mn heterointerface.
[0059] Fe(0) and Mn(II) in the inner fixed layer are formed by in-situ reduction in the carbon framework, providing a continuous electron supply for the micro galvanic cell network.
[0060] (5) In-situ mineralization and stabilization treatment: The activated composite material is kept at 200°C for 1 h in an air atmosphere to stabilize the valence cycle between Mn(IV) / Mn(III) and Fe(III) / Fe(II) in Fe-Mn oxide, while increasing the oxygen vacancy concentration to 28% to obtain the thallium removal material.
[0061] 3. Thallium removal performance test
[0062] Take 0.5 g of the above-mentioned thallium removal material and add it to 1 L of simulated wastewater containing 10 mg / L Tl(I) (pH=7.0, prepared with thallium standard solution). Stir and react at 25℃ for 2 h. The concentration of Tl(I) in the solution before and after the reaction is determined by inductively coupled plasma mass spectrometry (ICP-MS).
[0063] Based on the Langmuir isotherm adsorption model, the maximum adsorption capacity of the thallium removal material in this embodiment for Tl(I) is 215 mg / g. The Tl(I) removal rate remains above 92% across a wide pH range of 3–11.
[0064] The reacted material was regenerated using a 0.02 M EDTA-2Na (disodium ethylenediaminetetraacetate) and 0.5 M sodium hydroxide composite desorption solution. The desorption mechanism is as follows: EDTA provides a strong coordinating group, forming a stable [Tl(EDTA)] with Tl(III). - The complex competitively disrupts the Fe–O–Tl and Mn–O–Tl chemical bonds, while higher concentrations of OH... - It helps disperse solid particles and restore the charge state of the material surface, and the two work together to achieve deep desorption.
[0065] After being regenerated by the composite desorption solution, the material can be recycled 5 times, and the removal rate of Tl(I) still maintains 85% of the initial removal rate, demonstrating excellent cycle life.
[0066] Meanwhile, the dissolution rate of Fe / Mn active components during the regeneration process was less than 1.5% (ICP-OES detection), and XRD and XPS characterization confirmed that the α-MnO2 / γ-FeOOH crystal phase and Fe–O–Mn heterostructure remained intact after multiple regenerations, and the oxygen vacancy concentration did not decrease significantly, proving that the gradient structure of the present invention has extremely strong chemical resistance and structural stability.
[0067] Compared with existing iron-manganese modified biochar materials, the material in this embodiment achieves highly efficient selective oxidation fixation of Tl(I) through an innovative four-in-one design of "confined in-situ growth of straw natural vascular bundles + Fe-O-Mn heterogeneous interface + oxygen vacancy regulation + gradient functional structure". The adsorption capacity is significantly improved (approximately 182% higher than the 76.34 mg / g of single iron modified biochar), and the pH adaptation range is wider and the cycling stability is better.
[0068] Example 2:
[0069] This embodiment provides another straw-based iron-manganese oxide composite thallium removal material and its preparation method.
[0070] 1. Material Composition
[0071] The straw-based iron-manganese oxide composite thallium removal material of this embodiment includes a straw-based porous carbon skeleton and an iron-manganese oxide composite loaded on the carbon skeleton.
[0072] The iron-manganese oxide composite contains α-MnO2 and γ-FeOOH crystal phases, and has Fe-O-Mn heterostructure and oxygen vacancies;
[0073] The material has a gradient functional structure consisting of an outer oxide layer, a middle complex layer, and an inner fixing layer, from the outside to the inside.
[0074] Of the materials, iron and manganese oxides account for 40% of the total mass, the mass ratio of α-MnO2 to γ-FeOOH is 2:1, the relative content of oxygen vacancies is 32%, and the specific surface area of the materials is 450 m². 2 / g, with an average pore size of 5 nm.
[0075] 2. Preparation method
[0076] (1) Preparation of pretreated straw: Rice straw was washed, dried and crushed to 40 mesh, placed in 3% KOH alkaline solution and treated at 70℃ for 3 h, washed with deionized water until neutral and dried at 105℃ for 12 h to obtain pretreated straw.
[0077] (2) Impregnation treatment: FeCl3·6H2O and MnSO4·H2O were dissolved in deionized water at a Fe:Mn molar ratio of 2:1, and ethylenediaminetetraacetic acid (EDTA) was added as a chelating agent (the ratio of EDTA to the total number of metal ions was 0.8:1) to prepare an iron-manganese precursor solution.
[0078] Pretreated straw was mixed with an iron-manganese precursor solution at a mass ratio of 1:15, stirred and impregnated at 30°C for 10 h, and then dried at 50°C for 18 h to obtain impregnated straw loaded with iron-manganese precursor.
[0079] (3) Confined pyrolysis crystallization treatment: The impregnated straw is placed in a tube furnace and heated to 600℃ at a heating rate of 3℃ / min. It is kept at the temperature for 3 h in a nitrogen-oxygen mixed atmosphere with an oxygen volume fraction of 10%, so that the iron-manganese precursor crystallizes in situ into α-MnO2 / γ-FeOOH composite crystal phase in the confined space of the straw natural vascular wall, and simultaneously forms a micro galvanic cell network supported by a carbon skeleton, thus obtaining the primary composite material.
[0080] XRD characterization confirmed that the mass ratio of α-MnO2 to γ-FeOOH was 2:1; by controlling a low oxygen partial pressure (10% O2), the relative content of oxygen vacancies in the nascent composite material reached 32%.
[0081] The relative content of oxygen vacancies was calculated by peak fitting of the O 1s spectrum in XPS. SEM observation showed that iron and manganese oxides were uniformly distributed as nanoparticles on the inner wall of the straw ducts, with a particle size of approximately 40–80 nm.
[0082] (4) Gradient activation treatment: The nascent composite material is placed in a nitrogen-oxygen mixed atmosphere with an oxygen volume fraction of 10% and kept at 250℃ for 1.5 h to form a gradient functional structure on the surface of the nascent composite material, with Mn(IV) / Fe(Ⅲ) oxide as the outer oxide layer, Fe-O-Mn heterostructure as the middle complex layer, and Fe(O) / Mn(II) supported by carbon skeleton as the inner fixed layer, thus obtaining the activated composite material.
[0083] TEM observations showed that the outer oxide layer was approximately 80 nm thick.
[0084] XPS analysis showed that the binding energy shift difference between Fe 2p3 / 2 and Mn 2p3 / 2 was 1.4 eV, confirming the formation of the Fe-O-Mn heterointerface.
[0085] (5) In-situ mineralization and stabilization treatment: The activated composite material is kept at 180°C for 1.5 h in a nitrogen-oxygen mixed atmosphere with an oxygen volume fraction of 10% to stabilize the valence cycle between Mn(IV) / Mn(III) and Fe(III) / Fe(II) in Fe-Mn oxide, while increasing the oxygen vacancy concentration to 35% to obtain the thallium removal material.
[0086] 3. Thallium removal performance test
[0087] Take 0.4 g of the above-mentioned thallium removal material and add it to 1 L of simulated wastewater containing 20 mg / L Tl(I) (pH=6.0, prepared with thallium standard solution (Tl2SO4)). Stir and react at 30℃ for 2 h. The concentration of Tl(I) in the solution before and after the reaction is determined by ICP-MS.
[0088] According to the Langmuir isotherm adsorption model, the maximum adsorption capacity of the thallium removal material for Tl(I) in this embodiment is 238 mg / g.
[0089] The removal rate of Tl(I) remained above 90% over a wide pH range of 3 to 11.
[0090] After the reacted material was desorbed and regenerated by a composite desorption solution containing 0.02 M EDTA-2Na and 0.5 M NaOH, it was recycled 5 times. The Tl(I) removal rate still maintained 82% of the initial removal rate, demonstrating excellent cycle life.
[0091] Compared with existing iron-manganese oxide composite thallium removal materials, this embodiment further enhances the oxidation activity and adsorption capacity of the material through a higher oxygen vacancy concentration (35%) and an optimized α-MnO2 / γ-FeOOH crystal phase ratio (2:1).
[0092] Example 3:
[0093] In one embodiment, this application provides a straw-based iron-manganese oxide composite thallium removal material and its preparation method.
[0094] 1. Material Composition
[0095] The straw-based iron-manganese oxide composite thallium removal material of this embodiment comprises a straw-based porous carbon skeleton and an iron-manganese oxide composite loaded on the carbon skeleton; the iron-manganese oxide composite contains α-MnO2 and γ-FeOOH crystal phases, and has Fe-O-Mn heterostructure and oxygen vacancies;
[0096] The material has a gradient functional structure consisting of an outer oxide layer, a middle complex layer, and an inner fixing layer, from the outside to the inside.
[0097] Of the materials, iron and manganese oxides account for 60% of the total mass, the mass ratio of α-MnO2 to γ-FeOOH is 1:2, the relative content of oxygen vacancies is 20%, and the specific surface area of the materials is 320 m². 2 / g, with an average pore size of 8nm.
[0098] 2. Preparation method
[0099] (1) Preparation of pretreated straw: Wheat straw was washed, dried and crushed to 80 mesh, placed in 8% NaOH alkaline solution and treated at 90℃ for 1.5 h, washed with deionized water until neutral and dried at 105℃ for 12 h to obtain pretreated straw.
[0100] (2) Impregnation treatment: Fe2(SO4)3 and Mn(NO3)2 are dissolved in deionized water at a Fe:Mn molar ratio of 1:2, and oxalic acid is added as a chelating agent (the ratio of oxalic acid to the total molar number of metal ions is 1.5:1) to prepare an iron-manganese precursor solution.
[0101] Pretreated straw was mixed with an iron-manganese precursor solution at a mass ratio of 1:8, stirred and impregnated at 50°C for 6 h, and then dried at 70°C for 10 h to obtain impregnated straw loaded with iron-manganese precursor.
[0102] (3) Confined pyrolysis crystallization treatment: The impregnated straw was placed in a tube furnace and heated to 450℃ at a heating rate of 8℃ / min. It was then held at this temperature for 4 h in an air atmosphere to allow the iron-manganese precursor to crystallize in situ into an α-MnO2 / γ-FeOOH composite crystal phase within the confined space of the straw's natural vascular bundle wall. Simultaneously, a micro galvanic cell network supported by a carbon skeleton was formed, resulting in a nascent composite material. XRD characterization confirmed that the mass ratio of α-MnO2 to γ-FeOOH was 1:2. By controlling the oxygen partial pressure (21% O2) in the air atmosphere, the relative content of oxygen vacancies in the nascent composite material was made to be 20%.
[0103] The relative content of oxygen vacancies was calculated by peak fitting of the O 1s spectrum in XPS.
[0104] SEM observation showed that iron-manganese oxides were uniformly distributed as nanoparticles on the inner wall of the straw conduit, with a particle size of approximately 60–120 nm.
[0105] (4) Gradient activation treatment: The nascent composite material is placed in an air atmosphere and kept at 350℃ for 0.5 h to form a gradient functional structure on the surface of the nascent composite material, with Mn(IV) / Fe(Ⅲ) oxide as the outer oxide layer, Fe-O-Mn heterostructure as the middle complex layer, and Fe(O) / Mn(II) supported by carbon skeleton as the inner fixation layer, thus obtaining the activated composite material.
[0106] TEM observations showed that the outer oxide layer was approximately 160 nm thick.
[0107] XPS analysis showed that the binding energy shift difference between Fe 2p3 / 2 and Mn 2p3 / 2 was 0.9 eV, confirming the formation of the Fe-O-Mn heterointerface.
[0108] (5) In-situ mineralization stabilization treatment: The activated composite material is kept at 250°C for 0.5 h in an air atmosphere to stabilize the valence cycle between Mn(IV) / Mn(III) and Fe(III) / Fe(II) in Fe-Mn oxide, while increasing the oxygen vacancy concentration to 22% to obtain the thallium removal material.
[0109] 3. Thallium removal performance test
[0110] Take 0.6 g of the above-mentioned thallium removal material and add it to 1 L of simulated wastewater containing 5 mg / L Tl(I) (pH=8.0, prepared with thallium standard solution). Stir and react at 20℃ for 2 h. The Tl(I) concentration in the solution before and after the reaction is determined by ICP-MS.
[0111] According to the Langmuir isotherm adsorption model, the maximum adsorption capacity of the thallium removal material for Tl(I) in this embodiment is 185 mg / g.
[0112] The removal rate of Tl(I) remained above 88% over a wide pH range of 3 to 11.
[0113] After the reaction, the material was desorbed and regenerated by a composite desorption solution containing 0.02 M EDTA-2Na and 0.5 M NaOH. After being recycled 5 times, the Tl(I) removal rate still maintained 80% of the initial removal rate, showing good cycle life.
[0114] Compared with existing iron-manganese oxide composite thallium removal materials, this embodiment further reduces the energy consumption of material preparation by using a higher γ-FeOOH ratio (α-MnO2:γ-FeOOH=1:2) and a moderate pyrolysis temperature (450℃), while ensuring a high adsorption capacity.
[0115] Comparative example:
[0116] This comparative example provides a straw-based iron-manganese oxide composite thallium removal material and its preparation method, which differs from Example 1 in that:
[0117] Instead of confined pyrolysis crystallization treatment, a conventional impregnation-high temperature calcination method is used, in which the iron-manganese precursor is directly loaded on the surface of the straw and then calcined at high temperature, rather than growing in situ within the natural vascular bundles of the straw; no gradient activation treatment is performed, that is, no gradient activation step is performed after direct calcination; the remaining steps are the same as in Example 1.
[0118] 1. Material Composition
[0119] The straw-based iron-manganese oxide composite thallium removal material of this comparative example comprises a straw-based porous carbon skeleton and an iron-manganese oxide composite loaded on the carbon skeleton.
[0120] The total mass of iron-manganese oxides accounts for 48% of the total mass of the material, and the specific surface area of the material is 195 m². 2 / g, with an average pore size of 12 nm.
[0121] XRD characterization showed that α-MnO2 and γ-FeOOH crystals coexisted in the iron-manganese oxide, but the crystallinity was significantly lower than that in Example 1, and the Fe-O-Mn heterostructure could not be formed (XPS binding energy shift difference was only 0.3 eV); O 1s XPS peak fitting showed that the relative content of oxygen vacancies was only 8%.
[0122] 2. Preparation method
[0123] (1) Preparation of pretreated straw: Same as step (1) in Example 1.
[0124] (2) Impregnation treatment: Same as step (2) in Example 1, to obtain impregnated straw loaded with iron-manganese precursor.
[0125] (3) Conventional high-temperature calcination treatment: The impregnated straw is placed in a tube furnace and heated to 550°C at a heating rate of 5°C / min. It is kept at the temperature for 2 h in an air atmosphere (the same temperature and time as in Example 1) to decompose the iron-manganese precursor and form iron-manganese oxide on the surface of the straw, thus obtaining the calcined composite material.
[0126] XRD characterization confirmed the coexistence of α-MnO2 and γ-FeOOH crystalline phases, but the diffraction peaks were significantly broadened, indicating low crystallinity.
[0127] SEM observation showed that iron and manganese oxides mainly agglomerated on the outer surface of straw, in an irregular blocky distribution, with a particle size of about 200-500 nm. There was almost no oxide load inside the straw vascular bundles.
[0128] (4) The gradient activation process is omitted.
[0129] (5) The in-situ mineralization and stabilization treatment steps are omitted (the calcined composite material is used directly as the final material).
[0130] 3. Thallium removal performance test
[0131] Take 0.5 g of the above comparative material and add it to 1 L of simulated wastewater containing 10 mg / L Tl(I) (pH=7.0, prepared with thallium standard solution). Stir and react at 25℃ for 2 h. The concentration of Tl(I) in the solution before and after the reaction is determined by ICP-MS.
[0132] According to the Langmuir isotherm adsorption model, the maximum adsorption capacity of this comparative material for Tl(I) is only 86.4 mg / g. Under the same test conditions, the removal rate of Tl(I) of the comparative material is 72.3% at pH=7.0, drops sharply to 38.6% when the pH drops to 4.0, and drops to 51.2% when the pH rises to 10.0, indicating that the applicable pH range is significantly narrower than that of Example 1.
[0133] After the reacted material was desorbed and regenerated by 0.1 M NaOH solution, the Tl(I) removal rate dropped to 62% of the initial removal rate after 3 cycles, and the cycle stability was significantly worse than that of Example 1.
[0134] 4. Performance comparison is shown in Table 1 below;
[0135] Table 1
[0136] Performance indicators Example 1 Example 2 Example 3 Comparative Example Maximum adsorption capacity (mg / g) 215 238 185 86.4 Removal rate at pH=4 93.5% 91.8% 89.2% 38.6% Removal rate at pH=10 92.1% 90.5% 88.7% 51.2% Removal rate retention rate after 5 cycles 85% 82% 80% Only 62% after 3 cycles <![CDATA[specific surface area (m 2 / g)]]> 380 450 320 195 relative oxygen vacancy content 25% 32% 20% 8% Fe-O-Mn heterostructure (Δ=1.2eV) (Δ=1.4eV) (Δ=0.9eV) None (Δ=0.3eV)
[0137] Comparative analysis of the differences in the effects of proportional techniques:
[0138] (1) Difference in adsorption capacity.
[0139] The maximum adsorption capacity of the comparative example was only 86.4 mg / g, while that of Example 1, Example 2 and Example 3 were 215 mg / g, 238 mg / g and 185 mg / g, respectively, representing an increase of 114% to 175%.
[0140] The main reason is that this invention utilizes the natural vascular bundles of straw as a confined reaction space, allowing iron-manganese oxides to grow in situ into uniform nano-sized particles, exposing more active sites; while in conventional calcination methods, iron-manganese oxides agglomerate on the outer surface of straw, resulting in a low specific surface area (195 m²). 2 / g vs 380~450 m 2 / g), insufficient exposure of active sites.
[0141] More importantly, the comparative example lacks a Fe-O-Mn heterostructure, which prevents the formation of electron transfer channels, resulting in low oxidation conversion efficiency of Tl(I) to Tl(III).
[0142] (2) Differences in pH adaptability.
[0143] The removal rate of the comparative example decreased sharply under conditions deviating from neutral pH, while Examples 1, 2, and 3 maintained a removal rate of over 88% within a pH range of 3–11. This is because the iron and manganese oxides in the comparative example were merely simple physical mixtures, exhibiting poor stability under different pH conditions and easily dissolving or undergoing phase transitions. In contrast, this invention constructs a gradient functional structure of "outer layer oxidation—middle layer complexation—inner layer fixation" through gradient activation treatment. The outer Mn(IV) / Fe(III) oxide exhibits good acid and alkali tolerance, while the inner Fe(O) / Mn(II) continuously provides electrons, enabling the material to maintain structural stability and oxidation activity over a wide pH range.
[0144] (3) Differences in cycle stability.
[0145] The removal rate of the comparative example decreased significantly after three cycles, while the removal rate of Example 1 remained above 80% of the initial removal rate after five cycles. The reason is that in the comparative example, Tl(I) was mainly removed by surface adsorption, which was difficult to regenerate after adsorption saturation; while the iron-manganese valence state cycling mechanism of the present invention (electron transfer between Mn(IV) / Mn(III) and Fe(III) / Fe(II)) achieves self-regeneration of oxidation activity: Tl(I) reduces Mn(IV) / Fe(III) to generate Mn(II) / Fe(II), and Mn(II) / Fe(II) is re-oxidized to Mn(IV) / Fe(III) under oxygen-containing conditions, thereby restoring oxidation activity.
[0146] (4) Oxygen vacancy difference.
[0147] The comparative example showed a relative oxygen vacancy content of only 8%, while Examples 1, 2, and 3 showed 20%–35%. Oxygen vacancies, as electron enrichment centers on the oxide surface, can promote O2 activation to generate reactive oxygen species (·O2). - Oxygen vacancies (such as ·OH) are key active sites for the oxidation of Tl(I) to Tl(III). In the comparative example, the oxygen vacancy concentration was low, and the oxidation activity was significantly insufficient, which directly affected the oxidation fixation efficiency of Tl(I).
[0148] As shown above, this invention utilizes the natural vascular bundles of straw as a confined reaction space, enabling the iron-manganese precursor to grow in situ into nanoscale iron-manganese oxides with a Fe-O-Mn heterostructure during pyrolysis, and constructing a micro-galvanic cell network during the simultaneous formation of the carbon skeleton. In this micro-galvanic cell network, the carbon skeleton serves as the cathode and the iron-manganese oxide as the anode. A potential difference is spontaneously generated through the standard electrode potential difference between Fe(O) / Fe(III) and Mn(II) / Mn(IV), driving electrons to migrate directionally from the carbon skeleton to the iron-manganese oxide, continuously supplying electrons to the Fe-O-Mn heterostructure interface, allowing Tl(I) to be efficiently oxidized to Tl(III) at this interface. This interfacial electron transfer mechanism can operate continuously without external energy input, overcoming the technical bottleneck of traditional adsorption materials that rely on surface physicochemical adsorption and have insufficient oxidation capacity.
[0149] This invention constructs a gradient functional structure within the material through gradient activation treatment, consisting of an outer oxide layer, a middle complex layer, and an inner fixation layer. This allows Tl(I) to undergo three stages of fixation during its migration path: oxidation, complexation, and mineralization. Tl(I) is first oxidized to Tl(III) by the outer Mn(IV) / Fe(III) oxide, then complexed and anchored at the middle Fe-O-Mn heterostructure interface, and finally mineralized in the inner layer to form a stable mineral phase of Tl2O3 or TlFeO2.
[0150] Meanwhile, the reduced Mn(II) / Fe(II) can be re-oxidized to a higher valence state under oxygen-containing conditions, realizing the cyclic regeneration of oxidation activity and enabling the material to have long-term self-repair capability, effectively avoiding the problem of rapid deactivation caused by the irreversible consumption of active sites in traditional modified biochar.
[0151] The foregoing has only described certain exemplary embodiments of the present invention by way of illustration. Undoubtedly, those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the foregoing drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. A straw-based iron-manganese oxide composite thallium removal material, characterized in that, It comprises a straw-based porous carbon framework and an iron-manganese oxide complex supported on the carbon framework; The iron-manganese oxide composite contains α-MnO2 and γ-FeOOH crystal phases, and has Fe-O-Mn heterostructure and oxygen vacancies; The material has a gradient functional structure consisting of an outer oxide layer, a middle complex layer, and an inner fixing layer, from the outside to the inside.
2. A method for in-situ loading and preparation of a straw-based iron-manganese oxide composite thallium removal material, characterized in that, include: Pretreated straw is provided, wherein the pretreated straw is impregnated with an iron-manganese precursor solution to obtain impregnated straw loaded with iron-manganese precursors; The impregnated straw is used for confined pyrolysis crystallization treatment in an oxygen-containing atmosphere, so that the iron-manganese precursor grows in situ in the natural vascular bundles of the straw into Fe-Mn oxide heterojunctions with oxygen vacancies, thus obtaining the primary composite material. The nascent composite material is used for gradient activation treatment in an oxygen-containing atmosphere to form a gradient functional structure of an outer oxide layer, a middle complex layer, and an inner fixing layer on the surface of the nascent composite material, thereby obtaining an activated composite material. The activated composite material is used for in-situ mineralization and stabilization treatment in an oxygen-containing atmosphere, so that the Fe-Mn oxide in the activated composite material is further crystallized and oxygen vacancies are stabilized to obtain the thallium removal material.
3. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The method for obtaining the pretreated straw is as follows: After washing and drying, the straw is crushed to 20-100 mesh and then placed in an alkaline solution with a mass fraction of 1%-10% at 60-90°C for 1-4 hours. After washing and drying, the pretreated straw is obtained. The straw is selected from at least one of corn straw, rice straw, and wheat straw.
4. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The iron-manganese precursor solution is prepared by dissolving iron salt, manganese salt and chelating agent in deionized water, wherein the molar ratio of iron salt to manganese salt is 1:0.5 to 1:3, and the ratio of chelating agent to total molar number of metal ions is 0.5:1 to 2:
1. The iron salt is selected from at least one of Fe(NO3)3·9H2O, FeCl3·6H2O, and Fe2(SO4)3; the manganese salt is selected from at least one of KMnO4, MnSO4·H2O, and Mn(NO3)2; and the chelating agent is selected from at least one of citric acid, ethylenediaminetetraacetic acid, and oxalic acid. The impregnation process is as follows: pretreated straw is mixed with iron-manganese precursor solution at a mass ratio of 1:5 to 1:20, stirred and impregnated at 25 to 60°C for 4 to 12 hours, and then dried at 40 to 80°C for 6 to 24 hours to obtain the impregnated straw.
5. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The confined pyrolysis crystallization treatment is as follows: The impregnated straw is placed in a tube furnace and heated to 400-700°C at a heating rate of 1-10°C / min. It is then kept at this temperature for 1-4 hours in an oxygen-containing atmosphere, so that the iron-manganese precursor crystallizes in situ into an α-MnO2 / γ-FeOOH composite crystal phase within the confined space of the straw's natural vascular bundle wall, and simultaneously forms a micro galvanic cell network supported by a carbon skeleton, thus obtaining the nascent composite material. The oxygen-containing atmosphere is air or a nitrogen-oxygen mixture with an oxygen volume fraction of 5% to 21%.
6. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 5, characterized in that, In the confined pyrolysis crystallization process, the mass ratio of α-MnO2 to γ-FeOOH crystal phases is controlled to be 1:2 to 3:1 by controlling the heating rate and holding temperature. At the same time, the oxygen vacancy concentration is controlled by controlling the oxygen partial pressure in the oxygen-containing atmosphere, so that the relative content of oxygen vacancy in the nascent composite material is 15% to 35%.
7. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The gradient activation process is as follows: The nascent composite material is placed in an oxygen-containing atmosphere and kept at 200–400°C for 0.5–2 hours to form a gradient functional structure on the surface of the nascent composite material, with Mn(IV) / Fe(III) oxide as the outer oxide layer, Fe-O-Mn heterostructure as the middle complex layer, and Fe(O) / Mn(II) supported by a carbon skeleton as the inner immobilization layer, thus obtaining the activated composite material.
8. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 7, characterized in that, In the gradient activation process, the thickness of the outer oxide layer is 50-200 nm, the Fe-O-Mn heterostructure of the middle complex layer is characterized by the XPS binding energy shift difference between Fe2p3 / 2 and Mn2p3 / 2 being 0.8-1.5 eV, and the inner fixed layer provides a continuous electron supply through the in-situ reduction of Fe(0) and Mn(II) in the carbon skeleton, maintaining the redox cycle of the micro galvanic cell network.
9. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The in-situ mineralization stabilization treatment is as follows: the activated composite material is kept at 150-300℃ for 0.5-2h in an oxygen-containing atmosphere to stabilize the valence cycle between Mn(IV) / Mn(III) and Fe(III) / Fe(II) in the Fe-Mn oxide, while increasing the oxygen vacancy concentration to 20%-40% to obtain the thallium removal material.
10. The in-situ loading preparation method of a straw-based iron-manganese oxide composite thallium removal material according to claim 2, characterized in that, The total mass of the iron-manganese oxide complex accounts for 30%-70% of the total mass of the material, the mass ratio of α-MnO2 to γ-FeOOH is 1:2-3:1, the relative content of oxygen vacancies is 15%-40%, and the specific surface area of the material is 200-600 m 2 / g, and the average pore size is 2-10 nm.