Aluminum dross-based efficient dechlorination agent and preparation method thereof

By using waste aluminum slag from hydrogenation catalysts as a carrier, and combining processes such as gradient acid leaching, low-temperature oxygen thermal impurity removal, and alkaline etching, calcium and sodium active components are loaded and the pore structure is optimized. This solves the problems of insufficient resource utilization of aluminum slag and high cost of dechlorination agents, and achieves efficient and stable dechlorination performance.

CN123148932APending Publication Date: 2026-11-24湖北灵晓新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611564758.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The utilization rate of aluminum slag resources in existing aluminum-based catalysts is insufficient, and traditional dechlorination agents have high raw material costs and limited overall dechlorination performance, making it difficult to meet the needs of deep industrial dechlorination.

Method used

Using recycled aluminum slag from spent hydrogenation catalysts as a carrier, calcium and sodium active components are loaded through gradient acid leaching, low-temperature oxygen-thermal impurity removal, and alkaline etching processes to construct a dechlorination system that combines physical adsorption and chemical fixation. The pore structure is optimized by combining a three-stage roasting process.

Benefits of technology

It enables the low-cost preparation of highly efficient dechlorinating agents, improves the removal depth and applicability of organochlorines, ensures the stability of the carrier structure and the uniform distribution of active sites, and has higher adsorption capacity and reactivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148932A_ABST
    Figure CN123148932A_ABST
Patent Text Reader

Abstract

This application relates to the field of environmental protection and purification materials technology, specifically disclosing an aluminum slag-based high-efficiency dechlorination agent and its preparation method. The dechlorination agent uses an alumina-based carrier obtained by purifying and activating recycled aluminum slag from waste hydrogenation catalysts as its core, combined with calcium-based active components, sodium-based active components, and directionally retained transition metal oxides to synergistically construct a dechlorination system combining physical adsorption and chemical fixation. Its preparation method sequentially includes crushing and sieving, water washing for impurity removal, purification and activation, kneading and molding, and segmented calcination. This dechlorination agent can be used for chloride removal and purification of petrochemical materials and industrial gases, achieving high-value utilization of industrial solid waste while maintaining good comprehensive dechlorination performance. It exhibits outstanding removal effects on inorganic chlorine and trace amounts of organic chlorine under sulfur-containing atmospheres, has strong adaptability to the preparation process, and possesses good industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of environmentally friendly adsorption materials technology, and more specifically, it relates to an aluminum slag-based high-efficiency dechlorination agent and its preparation method. Background Technology

[0002] In petrochemical processes such as hydrogenation, reforming, and catalytic cracking, aluminum-based catalysts are widely used due to their large specific surface area and good thermal stability. However, after long-term operation, these catalysts can become completely ineffective due to carbon buildup, heavy metal deposition, and loss of active components. The industry often uses wet leaching and pyrometallurgical processes to recover valuable metals such as nickel, molybdenum, and cobalt. This metal recovery process generates a large amount of waste aluminum slag. This aluminum slag mainly consists of alumina and aluminum hydroxide, and its annual production is substantial. Traditional disposal methods primarily involve landfilling and stockpiling, which not only consumes land resources but also allows residual soluble salts and heavy metals in the slag to leach into the surrounding environment, causing secondary pollution. Furthermore, a large amount of aluminum-based resources cannot be effectively utilized, which does not meet the requirements of green, low-carbon industrial development and solid waste resource utilization.

[0003] In industrial production processes, chlorides in feedstock oil, process gases, and circulating wastewater are major pollutants causing equipment corrosion, downstream catalyst poisoning, and product quality degradation. Solid dechlorinating agents are the mainstream technology and material for industrial dechlorination and purification due to their ease of operation, lack of secondary pollution, and strong adaptability to various operating conditions. Currently, most commercial dechlorinating agents are prepared using high-purity alumina as a carrier, resulting in high raw material procurement costs and limiting their large-scale industrial application. Existing technologies for preparing dechlorinating agents using aluminum-based industrial solid waste generally suffer from limitations such as simplistic raw material purification and structural control methods, insufficient pore structure development in the finished product, uneven distribution of active sites, and limited overall dechlorination performance, making it difficult to meet the deep dechlorination needs of industrial systems at a low cost. Summary of the Invention

[0004] To address the issues of insufficient resource utilization of waste catalyst aluminum slag in existing technologies, high raw material costs of conventional dechlorination agents, and difficulty in achieving comprehensive dechlorination performance, this application provides an aluminum slag-based high-efficiency dechlorination agent and its preparation method.

[0005] In the first aspect, this application provides an aluminum slag-based high-efficiency dechlorination agent, which adopts the following technical solution: A high-efficiency dechlorination agent based on aluminum slag, characterized in that: based on dry weight, the mass ratio of alumina-based carrier, calcium-based active component, sodium-based active component to transition metal oxide is (4-6):(1-1.5):(0.8-1.3):(0.5-1); The alumina-based support is obtained by purifying and activating aluminum slag recovered from waste hydrogenation catalysts. The calcium-based active component and the sodium-based active component are loaded on the surface and inside the pores of the alumina-based support.

[0006] By adopting the above technical solution, alumina-based supports can be prepared using recycled aluminum slag from waste hydrogenation catalysts as precursors, which can replace high-purity chemical raw materials and reduce raw material costs. This type of aluminum slag retains the original framework structure formed during the original catalyst preparation process. After purification and activation, it can maintain a stable pore system without the need for complete reconstruction of the alumina support. Combined with loaded calcium and sodium active components, chloride ions can be removed through a combination of physical adsorption and chemical reaction. At the same time, the transition metal oxides remaining in the raw materials can participate in the conversion process of organochlorine, converting difficult-to-adsorb organochlorine into easily fixed inorganic chlorine forms, thereby achieving a synergistic improvement in high-value utilization of solid waste and dechlorination performance.

[0007] Preferably, the transition metal oxide is one or a combination of two of nickel oxide and molybdenum oxide.

[0008] By adopting the above technical solution, both types of oxides are naturally residual components in the aluminum slag of spent hydrogenation catalysts, without the need to introduce additional external materials. They are anchored on the alumina skeleton in the aluminum slag in a highly dispersed form, with strong binding force to the carrier and are not easily lost with the fluid. During the dechlorination process, they can catalytically break the carbon-chlorine bonds in organochlorine molecules, converting large organochlorine molecules into free chloride ions that can be captured by calcium and sodium active components, thus expanding the adaptability of the dechlorinating agent to different chlorine-containing systems, while avoiding the problems of easy agglomeration and detachment of externally loaded metals.

[0009] Preferably, the mass ratio of the calcium-based active component to the sodium-based active component is 1:0.8 to 1:0.9.

[0010] By adopting the above technical solution, the two types of active components can form a reasonable site distribution within this ratio range. The sodium-based component can preferentially occupy the strongly acidic sites on the carrier surface, modulate the charge distribution on the carrier surface, and provide more anchoring points for the uniform deposition of the calcium-based component, preventing the calcium component from migrating and agglomerating during the calcination process. At the same time, the ratio of the two types of active phases is adapted to the common occurrence ratio of inorganic chlorine and organic chlorine in industrial systems, which can ensure sufficient chemical chlorination sites and maintain the pore connectivity of the carrier, preventing pore narrowing or blockage due to excessive active components, and ensuring the mass transfer efficiency of the dechlorination reaction.

[0011] Preferably, the calcium-based active component is calcium oxide and a calcium-aluminum composite oxide generated by reacting with an alumina-based support, and the sodium-based active component is sodium aluminate.

[0012] By adopting the above technical solutions, calcium oxide, as the main chemically solidified chlorine phase, can react with chloride ions to generate stable chloride-containing salts, achieving irreversible fixation of chloride ions; calcium-aluminum composite oxide is generated by the in-situ solid-phase reaction of calcium precursor and carrier alumina at high temperature, forming chemical bonds with the carrier skeleton, making it less prone to detachment and loss under gas scouring, while the layered structure of the composite oxide can provide more interlayer adsorption sites; sodium aluminate can enrich the basic hydroxyl sites on the carrier surface, enhancing the electrostatic adsorption of chloride ions, and the multiphase active components work synergistically to cover the entire process of adsorption, reaction, and fixation.

[0013] Secondly, this application provides a method for preparing an aluminum slag-based high-efficiency dechlorination agent, employing the following technical solution: A method for preparing an aluminum slag-based high-efficiency dechlorination agent includes the following steps: S1. Crushing and sieving: The original waste catalyst aluminum slag is ball-milled and then sieved to obtain aluminum slag powder; S2. Water washing to remove impurities: After mixing and stirring the aluminum slag powder with deionized water and leaching it out, filter it and collect the wet filter residue. Place the wet filter residue in an air atmosphere for low-temperature heat treatment to obtain pre-removed aluminum slag. S3. Purification and activation: The pre-removed aluminum slag is placed in a water bath environment for gradient acid leaching treatment. After washing to neutral, it is subjected to alkaline etching treatment. After washing again until the pH is close to neutral, it is dried to obtain purified and activated aluminum slag. S4. Mixing and molding: Add calcium-based active precursor, sodium-based active precursor, molding aid and composite pore-forming agent to the purified activated aluminum slag. After the dry powder is mixed evenly, spray deionized water and knead until it becomes a plastic paste. Then extrude it to obtain a columnar blank. After the blank is left to stand and cure, it is dried. S5. Segmented roasting: The dried billet is placed in a muffle furnace and roasted using a three-stage programmed heating method, followed by natural cooling to obtain the finished product of aluminum slag-based high-efficiency dechlorination agent.

[0014] By adopting the above technical solution, the entire preparation process follows a logical progression of raw material pretreatment, structural regulation, active loading, and high-temperature activation. First, large particulate impurities and soluble salts are removed through physical crushing and water washing. Then, low-temperature heat treatment is used to oxidize and remove carbon deposits trapped in the pores, opening up the original pores and providing mass transfer channels for subsequent acid and alkali treatment. Next, gradient acid leaching and alkaline etching are used to simultaneously complete the directional regulation of impurities and the etching of pore structures. Then, kneading and molding are used to simultaneously complete the mixing and molding of active components to prepare a blank that meets the size requirements for industrial applications. Finally, kneading loading and segmented calcination are used to complete the uniform loading and in-situ activation of active components. Each process is seamlessly connected, and the product characteristics of the preceding process provide an optimization basis for the subsequent process, ultimately forming a dechlorination product with a stable structure and abundant active sites.

[0015] Preferably, in step S2, the solid-liquid mass ratio of the water washing for impurity removal is 1:3 to 1:4.5; the wet filter residue is directly subjected to low-temperature heat treatment without drying, and the air atmosphere is kept continuously circulating during the treatment process.

[0016] By adopting the above technical solution, the solid-liquid ratio can ensure that the aluminum slag powder is fully dispersed in water, avoiding the inability of internal impurities to dissolve due to particle agglomeration. The water washing process can remove most of the soluble chloride and sulfate impurities, reducing the acid and alkali consumption in subsequent purification processes. The wet filter residue is directly subjected to low-temperature heat treatment, which can utilize the residual moisture inside the particles to vaporize and expand during the heating process, further loosening the pore structure and avoiding pore closure caused by particle caking after drying. The continuously circulating air atmosphere can provide sufficient oxygen for carbon deposit oxidation, converting the carbon deposits attached to the inner wall of the pores into gaseous oxides and discharging them. Without damaging the alumina skeleton, the original blocked pores are cleared, increasing the penetration depth of subsequent acid and alkali solutions.

[0017] Preferably, in step S3, the gradient acid leaching first uses a dilute hydrochloric acid solution with a mass fraction of 2.5% to 3.5% for 50 to 70 minutes, then adjusts the acid mass fraction to 4.5% to 5.5% and continues leaching for 25 to 35 minutes, with the water bath temperature at 45 to 55°C; after leaching, the total mass of nickel oxide and molybdenum oxide in the aluminum slag accounts for 0.3% to 0.8% of the dry mass of the aluminum slag; the alkaline etching uses a 0.4 to 0.6 mol / L sodium hydroxide solution, etched at 35 to 45°C for 15 to 25 minutes, and after etching, washing is performed until the pH is 6.5 to 7.5.

[0018] By adopting the above technical solution, the treatment method of gradually increasing the acid concentration can achieve selective leaching based on the differences in acid solubility of different metal oxides. First, the more active impurity oxides such as iron and silicon are dissolved, and then some bound impurities are dissolved by appropriately increasing the acid concentration. At the same time, the leaching depth is controlled to retain nickel and molybdenum oxides anchored on the framework. Dilute alkaline etching can preferentially dissolve the amorphous phase on the surface of alumina particles, etching more mesoporous structures on the particle surface and the inner wall of the pores, increasing the specific surface area and pore volume of the carrier, while activating the surface aluminum sites and improving the anchoring ability of subsequent active components. Washing to the neutral range can thoroughly remove residual acid and alkali ions, avoiding residual acid radicals or alkali metal ions from affecting the loading state and reactivity of subsequent active components.

[0019] Preferably, in step S4, the molding aid includes guar gum powder and carboxymethyl cellulose. The amount of guar gum powder added is 1.5% to 2.5% and the amount of carboxymethyl cellulose added is 0.8% to 1.2% based on the dry weight of aluminum slag. The amount of composite pore-forming agent added is 3% to 5%, which is compounded from ammonium bicarbonate and soluble starch in a mass ratio of 1:1.5 to 1:2.5.

[0020] By adopting the above technical solution, the compound of guar gum powder and carboxymethyl cellulose as a molding aid can play a dual role of binding and plasticizing during the powder kneading process, improving the plasticity and bonding strength of the paste, making the surface of the extruded green body smooth and not easy to break. At the same time, it can slowly burn off during the subsequent calcination process, without causing sudden collapse of the pores. The two-component composite pore-forming agent corresponds to different decomposition temperature ranges. The component that decomposes at low temperature can form a microporous skeleton first, while the component that burns off at high temperature constructs mesoporous mass transfer channels. The two work together to form a multi-level pore system, which not only ensures sufficient adsorption specific surface area, but also maintains good fluid mass transfer channels, thus solving the problem of the single pore size distribution of a single pore-forming agent.

[0021] Preferably, in step S5, the first stage of the three-stage programmed heating and roasting involves heating at 2.5–3.5°C / min to 180–220°C and holding at that temperature for 0.8–1.2 hours; the second stage involves heating at 4.5–5.5°C / min to 480–520°C and holding at that temperature for 2–3 hours; and the third stage involves cooling at 1.5–2.5°C / min to 80–120°C and holding at that temperature for 0.4–0.6 hours before allowing it to cool naturally.

[0022] By adopting the above technical solution, the three-stage programmed temperature-increasing calcination system can match the thermal decomposition temperatures of various additives, pore-forming agents, and active precursors introduced during the preparation process. The slow heating in the low-temperature stage allows the additives and pore-forming agents to gradually decompose and volatilize, avoiding the concentrated release of gas caused by rapid heating and resulting in cracking of the green body. The isothermal calcination in the medium-temperature stage can promote the solid-phase reaction between the active precursor and the carrier, generating calcium-aluminum and sodium-aluminum active phases in situ, and completing the activation of active sites. The isothermal setting in the cooling stage can reduce the internal stress generated by rapid cooling and improve the mechanical strength of the product. The water vapor atmosphere can react with the alumina surface at high temperature to generate more active hydroxyl groups, while inhibiting the high-temperature sintering and growth of alumina particles, maintaining the pore structure and specific surface area of ​​the carrier, and improving the structural stability and service life of the product.

[0023] In summary, this application has the following beneficial effects: 1. Since this application uses recycled aluminum slag from waste hydrogenation catalyst as a carrier to prepare raw materials, and after purification and activation treatment, it loads calcium and sodium active components, which can replace high-purity alumina raw materials to reduce the preparation cost of dechlorination agents. At the same time, it constructs a dual-effect dechlorination system that combines physical adsorption and chemical fixation, and achieves a comprehensive application effect that takes into account both solid waste resource utilization and efficient dechlorination and purification.

[0024] 2. In this application, a gradient acid leaching purification process is preferred. By controlling the acid concentration gradient and leaching time, nickel oxide and molybdenum oxide components in aluminum slag are retained in a targeted manner. The carbon-chlorine bonds of organochlorine molecules are dissociated by the catalytic effect of transition metals, resulting in a better organochlorine removal depth and a wider range of applicable scenarios.

[0025] 3. The method of this application constructs a multi-level interconnected pore structure by simultaneously adding active components and a two-component composite pore-forming agent during the kneading process, avoiding competitive adsorption and agglomeration of active components, improving the dispersion of active sites and the mass transfer efficiency of pores, and obtaining higher chlorine adsorption capacity and reactivity.

[0026] 4. This application adopts a three-stage programmed heating and steam atmosphere calcination process to match the thermal behavior characteristics of each component to complete decomposition, activation and structural shaping, suppress high-temperature sintering of alumina particles and pore collapse, and obtain a more stable skeleton structure and better recycling performance. Attached Figure Description

[0027] Figure 1 This is a flowchart of a method for preparing an aluminum slag-based high-efficiency dechlorination agent provided in this application; Figure 2 This is a comparison chart of the static saturated chlorine capacity test results of the various embodiments and comparative examples provided in this application; Figure 3 This is a comparison chart of the organochlorine removal performance test results of the various embodiments and comparative examples provided in this application; Figure 4 This is a comparison chart of the fixed-bed regeneration performance test results of the various embodiments and comparative examples provided in this application. Detailed Implementation

[0028] The present application will be further described in detail below with reference to embodiments and comparative examples. Unless otherwise specified, the experimental methods used below are conventional methods. Unless otherwise specified, the materials, reagents, methods and instruments used are all conventional materials, reagents, methods and instruments in the art, which can be obtained by those skilled in the art through commercial channels or prepared according to literature methods.

[0029] Technical Concept: Current technologies for preparing dechlorination agents from aluminum-based industrial solid waste generally follow the conventional approach of deep purification and impurity removal. This involves repeated treatment with strong acids and alkalis to completely remove impurities from the raw materials, followed by conventional impregnation and roasting processes to load active substances. This method not only has a long purification process and high reagent consumption, but also fails to fully utilize the original components and skeletal structure of the aluminum slag itself. Furthermore, the single loading and roasting method easily leads to the agglomeration of active components and insufficient development of the pore structure. The final product has limited ability to remove organochlorines, making it difficult to meet the deep dechlorination needs of industrial systems under the premise of low-cost resource utilization.

[0030] This technical solution abandons the conventional approach of complete impurity removal. It uses recycled aluminum slag from waste hydrogenation catalysts as raw material and employs gradient acid leaching to directionally control the retention ratio of transition metal oxides in the raw material, transforming primary impurities into organic chlorine catalytic dissociation sites. It is complemented by low-temperature oxygen thermal impurity removal and alkaline etching processes to unclog and optimize the carrier pore structure. Combined with kneading synchronous loading and segmented steam roasting processes, it achieves high dispersion loading of active components and stabilization of the carrier structure. Through the adaptation and synergy of the entire process and raw material endowment, it improves the comprehensive removal performance of dechlorination agents on the basis of high-value utilization of solid waste.

[0031] Example 1: This example provides an aluminum slag-based high-efficiency dechlorination agent, with a component ratio of alumina-based: calcium-based active component: sodium-based active component: transition metal oxide = 5:1.2:1:0.8 based on dry weight.

[0032] The transition metal oxide is nickel oxide; the calcium-based active component is calcium oxide and a calcium-aluminum composite oxide formed by reacting with an alumina-based support; the sodium-based active component is sodium aluminate; the mass ratio of the calcium-based active component to the sodium-based active component is approximately 1:0.85. The preparation method of the above-mentioned aluminum slag-based high-efficiency dechlorination agent includes the following steps: S1. Crushing and sieving: The original waste catalyst aluminum slag is ball-milled and then sieved to obtain aluminum slag powder.

[0033] The ball milling time was 30 minutes, the particles were passed through a 200-mesh standard sieve, and the ball milling speed was 250 r / min to ensure uniform particle size and provide a stable raw material basis for subsequent mass transfer reactions.

[0034] S2. Water washing to remove impurities: After mixing and stirring the aluminum slag powder with deionized water and leaching, filter the mixture and collect the wet filter residue. Place the wet filter residue in an air atmosphere for low-temperature heat treatment to obtain pre-removed aluminum slag.

[0035] The solid-liquid mass ratio for water washing to remove impurities is 1:3.8, the stirring time at room temperature is 30 min, and the stirring rate is 200 r / min; the low-temperature heat treatment is carried out at a heating rate of 2℃ / min to 300℃, and then kept at a constant temperature for 1.5 h; the wet filter residue is directly subjected to low-temperature heat treatment without drying, and the air atmosphere is kept in continuous circulation during the treatment process.

[0036] S3. Purification and Activation: The pre-removed aluminum slag is placed in a water bath environment for gradient acid leaching treatment. After washing until neutral, it is subjected to alkaline etching treatment. After washing again until the pH is close to neutral, it is dried to obtain purified and activated aluminum slag.

[0037] The gradient acid leaching process involves first leaching with 3% hydrochloric acid for 60 minutes, then adjusting the acid concentration to 5% and leaching for another 30 minutes. The water bath temperature is 50℃, and the stirring rate is 180 r / min. After leaching, the total mass of nickel oxide and molybdenum oxide in the aluminum slag accounts for 0.55% of the dry weight of the aluminum slag. Alkaline etching uses a 0.5 mol / L sodium hydroxide solution at 40℃ for 20 minutes. After etching, the aluminum is washed three times with deionized water until the pH reaches 7.0. The drying temperature is 110℃, and the drying time is 4 hours. This gradient acid leaching process can remove impurities while directionally retaining a suitable amount of transition metal oxides, providing catalytic dissociation sites for subsequent organochlorine removal.

[0038] S4. Mixing and molding: Add calcium-based active precursor, sodium-based active precursor, molding aid and composite pore-forming agent to the purified activated aluminum slag. After the dry powder is mixed evenly, spray deionized water and knead until it becomes a plastic paste. Then extrude it to obtain a columnar blank. After the blank is left to stand for curing, it is dried.

[0039] The molding aids include guar gum powder and carboxymethyl cellulose. Based on the dry weight of aluminum slag, the amount of guar gum powder added is 2% and the amount of carboxymethyl cellulose added is 1%. The amount of composite pore-forming agent added is 4%, which is composed of ammonium bicarbonate and soluble starch in a mass ratio of 1:2. The dry powder mixing time is 10 min and the kneading time is 15 min. The diameter of the columnar blank is 3 mm and the length is 5-8 mm. The static curing time is 2 h, the drying temperature is 120℃, and the drying time is 6 h.

[0040] S5. Segmented roasting: The dried billet is placed in a muffle furnace and roasted using a three-stage programmed heating method, followed by natural cooling to obtain the finished product of aluminum slag-based high-efficiency dechlorination agent.

[0041] The three-stage programmed temperature-increasing calcination process involves three stages: the first stage heats the material to 200℃ at a rate of 3℃ / min and holds it at that temperature for 1 hour; the second stage heats it to 500℃ at a rate of 5℃ / min and holds it at that temperature for 2.5 hours; and the third stage cools the material to 100℃ at a rate of 2℃ / min, holds it at that temperature for 0.5 hours, and then allows it to cool naturally. This segmented calcination process allows for the simultaneous creation of pores, activation, and structural stabilization, ensuring the synergistic optimization of the dechlorinating agent's pore structure and active sites.

[0042] Example 2: This example provides an aluminum slag-based high-efficiency dechlorination agent. The mass ratio of alumina-based carrier, calcium-based active component, sodium-based active component and transition metal oxide is 4:1:0.8:0.5 on a dry basis.

[0043] Among them, the transition metal oxide is nickel oxide; the calcium-based active component is calcium oxide and calcium-aluminum composite oxide generated by reaction with alumina-based support; the sodium-based active component is sodium aluminate; the mass ratio of the calcium-based active component to the sodium-based active component is approximately 1:0.8.

[0044] The preparation method of the above-mentioned aluminum slag-based high-efficiency dechlorination agent includes the following steps: S1. Crushing and sieving: The original waste catalyst aluminum slag is ball-milled and then sieved to obtain aluminum slag powder.

[0045] The ball milling time is 25 minutes, the particles are passed through a 180-mesh standard sieve, and the ball milling speed is 200 r / min to ensure uniform particle size and provide a stable raw material basis for subsequent mass transfer reactions.

[0046] S2. Water washing to remove impurities: After mixing and stirring the aluminum slag powder with deionized water and leaching, filter the mixture and collect the wet filter residue. Place the wet filter residue in an air atmosphere for low-temperature heat treatment to obtain pre-removed aluminum slag.

[0047] The solid-liquid mass ratio for water washing to remove impurities is 1:3, the stirring time at room temperature is 25 min, and the stirring rate is 180 r / min; the low-temperature heat treatment is carried out at a heating rate of 1.5℃ / min to 280℃, and then kept at a constant temperature for 1 h; the wet filter residue is directly subjected to low-temperature heat treatment without drying, and the air atmosphere is kept continuously circulating during the treatment process.

[0048] S3. Purification and Activation: The pre-removed aluminum slag is placed in a water bath environment for gradient acid leaching treatment. After washing until neutral, it is subjected to alkaline etching treatment. After washing again until the pH is close to neutral, it is dried to obtain purified and activated aluminum slag.

[0049] The gradient acid leaching process involves first leaching with 2.5% hydrochloric acid for 50 minutes, then adjusting the acid concentration to 4.5% and leaching for another 25 minutes. The water bath temperature is 45℃, and the stirring rate is 160 r / min. After leaching, the total mass of nickel oxide in the aluminum slag accounts for 0.3% of the dry weight of the aluminum slag. Alkaline etching uses a 0.4 mol / L sodium hydroxide solution at 35℃ for 15 minutes. After etching, the slag is washed three times with deionized water until the pH reaches 6.5. The drying temperature is 105℃, and the drying time is 3.5 hours. This gradient acid leaching process can remove impurities while directionally retaining a suitable amount of transition metal oxides, providing catalytic dissociation sites for subsequent organochlorine removal.

[0050] S4. Mixing and molding: Add calcium-based active precursor, sodium-based active precursor, molding aid and composite pore-forming agent to the purified activated aluminum slag. After the dry powder is mixed evenly, spray deionized water and knead until it becomes a plastic paste. Then extrude it to obtain a columnar blank. After the blank is left to stand for curing, it is dried.

[0051] The molding aids include guar gum powder and carboxymethyl cellulose. Based on the dry weight of aluminum slag, the amount of guar gum powder added is 1.5% and the amount of carboxymethyl cellulose added is 0.8%. The amount of composite pore-forming agent added is 3%, which is composed of ammonium bicarbonate and soluble starch in a mass ratio of 1:1.5. The dry powder mixing time is 8 minutes and the kneading time is 12 minutes. The diameter of the columnar blank is 2.5 mm and the length is 4-7 mm. The static curing time is 1.5 hours, the drying temperature is 115℃, and the drying time is 5.5 hours.

[0052] S5. Segmented roasting: The dried billet is placed in a muffle furnace, and an air atmosphere containing water vapor is introduced. After roasting using a three-stage program, it is naturally cooled to obtain the finished product of aluminum slag-based high-efficiency dechlorination agent.

[0053] The three-stage programmed temperature-increasing calcination process involves three stages: the first stage involves heating to 180℃ at a rate of 2.5℃ / min and holding at that temperature for 0.8 hours; the second stage involves heating to 480℃ at a rate of 4.5℃ / min and holding at that temperature for 2 hours; and the third stage involves cooling to 280℃ at a rate of 1.5℃ / min, holding at that temperature for 0.4 hours, and then allowing for natural cooling. This segmented calcination process simultaneously achieves pore formation, activation, and structural stabilization, ensuring the synergistic optimization of the dechlorinating agent's pore structure and active sites.

[0054] Example 3: This example provides an aluminum slag-based high-efficiency dechlorination agent. The mass ratio of alumina-based carrier, calcium-based active component, sodium-based active component and transition metal oxide is 6:1.5:1.3:1 on a dry basis.

[0055] Among them, the transition metal oxide is nickel oxide; the calcium-based active component is calcium oxide and calcium-aluminum composite oxide generated by reaction with alumina-based support; the sodium-based active component is sodium aluminate; the mass ratio of the calcium-based active component to the sodium-based active component is approximately 1:0.9.

[0056] The preparation method of the above-mentioned aluminum slag-based high-efficiency dechlorination agent includes the following steps: S1. Crushing and sieving: The original waste catalyst aluminum slag is ball-milled and then sieved to obtain aluminum slag powder.

[0057] The ball milling time was 35 minutes, the particles were passed through a 220-mesh standard sieve, and the ball milling speed was 300 r / min to ensure uniform particle size and provide a stable raw material basis for subsequent mass transfer reactions.

[0058] S2. Water washing to remove impurities: After mixing and stirring the aluminum slag powder with deionized water and leaching, filter the mixture and collect the wet filter residue. Place the wet filter residue in an air atmosphere for low-temperature heat treatment to obtain pre-removed aluminum slag.

[0059] The solid-liquid mass ratio for water washing to remove impurities is 1:4.5, the stirring time at room temperature is 35 min, and the stirring rate is 220 r / min; the low-temperature heat treatment is carried out at a heating rate of 2.5℃ / min to 320℃, and then kept at a constant temperature for 2 h; the wet filter residue is directly subjected to low-temperature heat treatment without drying, and the air atmosphere is kept continuously circulating during the treatment process.

[0060] S3. Purification and Activation: The pre-removed aluminum slag is placed in a water bath environment for gradient acid leaching treatment. After washing until neutral, it is subjected to alkaline etching treatment. After washing again until the pH is close to neutral, it is dried to obtain purified and activated aluminum slag.

[0061] The gradient acid leaching process involves first leaching with 3.5% hydrochloric acid for 70 minutes, then adjusting the acid concentration to 5.5% and leaching for another 35 minutes. The water bath temperature is 55℃, and the stirring rate is 200 r / min. After leaching, the total mass of molybdenum oxide in the aluminum slag accounts for 0.8% of the dry weight of the aluminum slag. Alkaline etching uses a 0.6 mol / L sodium hydroxide solution at 45℃ for 25 minutes. After etching, the slag is washed three times with deionized water until the pH reaches 7.5. The drying temperature is 115℃, and the drying time is 4.5 hours. This gradient acid leaching process can remove impurities while directionally retaining a suitable amount of transition metal oxides, providing catalytic dissociation sites for subsequent organochlorine removal.

[0062] S4. Mixing and molding: Add calcium-based active precursor, sodium-based active precursor, molding aid and composite pore-forming agent to the purified activated aluminum slag. After the dry powder is mixed evenly, spray deionized water and knead until it becomes a plastic paste. Then extrude it to obtain a columnar blank. After the blank is left to stand for curing, it is dried.

[0063] The molding aids include guar gum powder and carboxymethyl cellulose. Based on the dry weight of aluminum slag, the amount of guar gum powder added is 2.5%, and the amount of carboxymethyl cellulose added is 1.2%. The amount of composite pore-forming agent added is 5%, which is composed of ammonium bicarbonate and soluble starch in a mass ratio of 1:2.5. The dry powder mixing time is 12 min, and the kneading time is 18 min. The diameter of the columnar green body is 3.5 mm, and the length is 6-9 mm. The static curing time is 2.5 h, the drying temperature is 125 ℃, and the drying time is 6.5 h.

[0064] S5. Segmented roasting: The dried billet is placed in a muffle furnace and roasted using a three-stage programmed heating method, followed by natural cooling to obtain the finished product of aluminum slag-based high-efficiency dechlorination agent.

[0065] The three-stage programmed temperature-controlled calcination process involves three stages: the first stage involves heating to 220℃ at a rate of 3.5℃ / min and holding at that temperature for 1.2 hours; the second stage involves heating to 520℃ at a rate of 5.5℃ / min and holding at that temperature for 3 hours; and the third stage involves cooling to 120℃ at a rate of 2.5℃ / min, holding at that temperature for 0.6 hours, and then allowing natural cooling. The volume fraction of water vapor in the air atmosphere is 6%, and the air flow rate is 120 mL / min. This segmented calcination process can simultaneously achieve pore formation, activation, and structural stabilization, ensuring the synergistic optimization of the pore structure and active sites of the dechlorinating agent.

[0066] Comparative Example 1: The only difference between this comparative example and Example 1 is that the original waste catalyst aluminum slag was replaced with commercial high-purity boehmite powder. All other raw materials, preparation steps and process parameters are the same as in Example 1.

[0067] Comparative Example 2: The only difference between this comparative example and Example 1 is that the gradient acid leaching step uses 10% hydrochloric acid for a single leaching for 90 minutes to completely remove nickel oxide and molybdenum oxide from the aluminum slag. After leaching, the total mass of nickel oxide and molybdenum oxide in the aluminum slag accounts for less than 0.05% of the dry mass of the aluminum slag. The other raw materials, preparation steps and process parameters are consistent with those of Example 1.

[0068] Comparative Example 3: The only difference between this comparative example and Example 1 is that no composite pore-forming agent is added in the kneading and molding step, only an equal mass of molding aid is added, and the other raw materials, preparation steps and process parameters are consistent with Example 1.

[0069] Comparative Example 4: The only difference between this comparative example and Example 1 is that in the purification and activation step, after acid leaching and washing to neutrality, the pH of the system is adjusted to 7.0 only with dilute sodium hydroxide solution, and no alkaline etching treatment is performed. The system is directly washed and dried. The other raw materials, preparation steps and process parameters are consistent with those of Example 1.

[0070] Comparative Example 5: This comparative example uses a commercially available mainstream calcium-sodium composite modified high-purity alumina dechlorination agent as the test sample. This sample uses γ-Al2O3 as the carrier and calcium oxide and sodium oxide as the active components. The other performance test conditions are consistent with those in Example 1.

[0071] I. Static saturated chlorine capacity test of inorganic chlorine: Refer to the determination principle of static adsorption chlorine capacity in "GB / T38108-2019 Test method for chlorine capacity of alkaline earth metal high temperature dechlorinating agents" and carry out quantitative detection of chloride ions in conjunction with "GB / T15453-2018 Determination of chloride ions in industrial circulating cooling water and boiler water". The dechlorinating agent samples from Examples 1 to 3 and Comparative Examples 1 to 5 were crushed to 20 to 40 mesh. 2.0 g of each sample was accurately weighed and placed in a stoppered glass conical flask. 200 mL of a 1000 mg / L sodium chloride standard solution was added to each flask. The flasks were sealed and placed in a 25°C constant temperature water bath shaker. The flasks were continuously shaken at a frequency of 150 r / min for 48 hours until adsorption reached saturation. After adsorption, the supernatant was collected and the concentration of residual chloride ions in the solution was determined using silver nitrate titration. The static saturated chloride capacity of each sample was calculated based on the mass difference of chloride ions in the solution before and after adsorption and the dry weight of the dechlorinating agent sample. Each group of samples was measured in triplicate, and the arithmetic mean of the three measurements was taken as the final test data.

[0072] II. Organic chlorine removal performance test: Referencing the quantitative conversion and detection methods for organic chlorine in "GB / T18612-2011 Determination of Organic Chlorine Content in Crude Oil", a liquid phase organic chlorine adsorption evaluation system was established. The dechlorinating agent samples from Examples 1 to 3 and Comparative Examples 1 to 5 were crushed to 20 to 40 mesh. 5.0 g of each sample was accurately weighed and packed into a glass adsorption column with an inner diameter of 10 mm. The experimental temperature was controlled at 30°C. A simulated aqueous solution containing 200 mg / L dichloroethane was used as the treatment medium. The liquid hourly space velocity was controlled at 2.0 h⁻¹. The adsorption column was continuously circulated for 8 hours. Inlet and outlet water samples were collected. After combustion oxidation decomposition treatment, the organic chlorine was converted into inorganic chloride ions. The total chlorine concentration was determined according to GB / T15453-2018 "Determination of Chloride Ions in Industrial Circulating Cooling Water and Boiler Water". The organic chlorine removal efficiency was calculated by the difference in organic chlorine concentration between the inlet and outlet, and the organic chlorine adsorption capacity was calculated cumulatively. Each group of samples was measured in parallel three times, and the arithmetic mean of the three measurements was taken as the final test data.

[0073] III. Fixed-bed circulating regeneration performance test: Refer to the method for determining the breakthrough chlorine capacity in "GB / T38108-2019 Test Method for Chlorine Capacity of Alkaline Earth Metal High-Temperature Dechlorinating Agents" and combine it with the general method for evaluating the regeneration of industrial adsorbents to carry out the circulating performance test. Dechlorinating agent samples from Examples 1 to 3 and Comparative Examples 1 to 5 were used to complete the first adsorption breakthrough experiment under the inorganic chlorine fixed-bed dynamic dechlorination test conditions. Breakthrough was defined as the outlet chloride ion concentration reaching 1.0 mg / L. The dechlorinating agent that had reached adsorption saturation was regenerated by backwashing the bed with deionized water at a space velocity of 2.0 h⁻¹ for 2 h. After backwashing, the dechlorinating agent was removed and placed in a 120°C forced-air drying oven for 4 h to complete one complete adsorption regeneration cycle. Subsequently, the fixed-bed dynamic dechlorination test was repeated. After five consecutive adsorption regeneration cycles, the breakthrough chlorine capacity of each sample in the fifth cycle was measured. The ratio of the fifth breakthrough chlorine capacity to the first breakthrough chlorine capacity was calculated as the performance retention rate to evaluate the cyclic stability of the dechlorinating agent. Each group of samples was measured in parallel three times, and the arithmetic mean of the three measurements was taken as the final test data.

[0074] Table 1: Performance test results of dechlorinating agents in each example and comparative example As can be seen from Examples 1-3 and Comparative Example 1, and Table 1, the raw material selection for the dechlorination agent is not simply a substitution of alumina source. The compositional characteristics and original structural basis of the recycled aluminum slag from the waste catalyst, combined with the subsequent targeted preparation process, can bring about better overall dechlorination performance, especially with a significant advantage in the removal of organic chlorine.

[0075] Based on Examples 1-3 and Comparative Example 2, and in conjunction with Table 1, it can be seen that the directional retention of trace amounts of transition metal oxides in aluminum slag does not negatively affect the basic adsorption capacity of inorganic chlorine. On the contrary, it can effectively enhance the removal effect of organic chlorine. This residual component, which was originally regarded as an impurity, can participate in the reaction as a catalytic active site, realizing the functional utilization of endogenous components of solid waste.

[0076] As can be seen from Examples 1-3 and Comparative Example 3, and Table 1, the composite pore-forming agent composed of ammonium bicarbonate and soluble starch can construct a multi-level interconnected pore structure, improve mass transfer efficiency and active site exposure, and thus simultaneously optimize the adsorption capacity and reactivity of the dechlorination agent.

[0077] As can be seen from Examples 1-3 and Comparative Example 4, and Table 1, the alkaline etching process can simultaneously optimize the carrier pore structure, enrich the pore hierarchy and improve mass transfer efficiency during purification and impurity removal, providing more sufficient effective space for active component loading and chloride ion diffusion, and significantly improving the overall adsorption performance of the dechlorinating agent.

[0078] As can be seen from Examples 1-3 and Comparative Example 5, and Table 1, the dechlorination agent prepared from waste catalyst aluminum slag is superior to commercially available conventional dechlorination agents of the same type in terms of inorganic chlorine adsorption capacity, organic chlorine removal capacity, and recycling stability. It has better comprehensive performance while realizing the high-value utilization of industrial solid waste.

[0079] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. An aluminium dross based highly efficient dechlorinating agent, characterized in that: Based on dry weight, the mass ratio of alumina-based carrier, calcium-based active component, sodium-based active component to transition metal oxide is (4-6):(1-1.5):(0.8-1.3):(0.5-1); The alumina-based support is obtained by purifying and activating aluminum slag recovered from waste hydrogenation catalysts. The calcium-based active component and the sodium-based active component are loaded on the surface and inside the pores of the alumina-based support.

2. The aluminum dross based highly efficient dechlorination agent according to claim 1, characterized in that: The transition metal oxide is one or a combination of two of nickel oxide and molybdenum oxide.

3. The aluminum dross based highly efficient dechlorination agent according to claim 1, characterized in that: The calcium-based active component is calcium oxide and calcium-aluminum composite oxide generated by reacting with an alumina-based support, and the sodium-based active component is sodium aluminate.

4. A process for the preparation of an aluminium dross based highly efficient dechlorinating agent, characterized by, The preparation of an aluminum slag-based high-efficiency dechlorination agent according to any one of claims 1-3 includes the following steps: S1. Crushing and sieving: The original waste catalyst aluminum slag is ball-milled and then sieved to obtain aluminum slag powder; S2. Water washing to remove impurities: After mixing and stirring the aluminum slag powder with deionized water and leaching it out, filter it and collect the wet filter residue. Place the wet filter residue in an air atmosphere for low-temperature heat treatment to obtain pre-removed aluminum slag. S3. Purification and activation: The pre-removed aluminum slag is placed in a water bath environment for gradient acid leaching treatment. After washing to neutral, it is subjected to alkaline etching treatment. After washing again until the pH is close to neutral, it is dried to obtain purified and activated aluminum slag. S4. Mixing and molding: Add calcium-based active precursor, sodium-based active precursor, molding aid and composite pore-forming agent to the purified activated aluminum slag. After the dry powder is mixed evenly, spray deionized water and knead until it becomes a plastic paste. Then extrude it to obtain a columnar blank. After the blank is left to stand and cure, it is dried. S5. Segmented roasting: The dried billet is placed in a muffle furnace and roasted using a three-stage programmed heating method, followed by natural cooling to obtain the finished product of aluminum slag-based high-efficiency dechlorination agent.

5. The preparation method of an aluminum slag-based high-efficiency dechlorination agent according to claim 4, characterized in that: In step S2, the solid-liquid mass ratio of the water washing and impurity removal is 1:3 to 1:4.5; the wet filter residue is directly subjected to low-temperature heat treatment without drying, and the air atmosphere is kept continuously circulating during the treatment process.

6. The preparation method of an aluminum slag-based high-efficiency dechlorination agent according to claim 4, characterized in that: In step S3, the gradient acid leaching first uses a dilute hydrochloric acid solution with a mass fraction of 2.5%–3.5% for 50–70 minutes, then adjusts the acid mass fraction to 4.5%–5.5% and continues leaching for 25–35 minutes, with the water bath temperature at 45–55°C. After leaching, the total mass of nickel oxide and molybdenum oxide in the aluminum slag accounts for 0.3%–0.8% of the dry mass of the aluminum slag. The alkaline etching uses a 0.4–0.6 mol / L sodium hydroxide solution and is etched at 35–45°C for 15–25 minutes. After etching, the solution is washed until the pH is 6.5–7.

5.

7. The preparation method of an aluminum slag-based high-efficiency dechlorination agent according to claim 4, characterized in that: In step S4, the molding aid includes guar gum powder and carboxymethyl cellulose. The amount of guar gum powder added is 1.5% to 2.5% and the amount of carboxymethyl cellulose added is 0.8% to 1.2% based on the dry weight of aluminum slag. The amount of composite pore-forming agent added is 3% to 5%, which is compounded from ammonium bicarbonate and soluble starch in a mass ratio of 1:1.5 to 1:2.

5.

8. The preparation method of an aluminum slag-based high-efficiency dechlorination agent according to claim 4, characterized in that: In step S5, the first stage of the three-stage programmed temperature-increasing roasting involves heating at 2.5–3.5℃ / min to 180–220℃ and holding at that temperature for 0.8–1.2 hours; the second stage involves heating at 4.5–5.5℃ / min to 480–520℃ and holding at that temperature for 2–3 hours; and the third stage involves cooling at 1.5–2.5℃ / min to 80–120℃ and holding at that temperature for 0.4–0.6 hours before allowing it to cool naturally.