A sulfur-selenium bifunctional adsorbent, a preparation method and application thereof
By loading a sulfur-selenium bifunctional adsorbent onto a carrier, the synergistic effect of sulfur and selenium is utilized to solve the problem of low mercury removal efficiency of activated carbon adsorbents over a wide temperature range, achieving a highly efficient and economical mercury removal effect.
Patent Information
- Application Number
- CN202611095242.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
Smart Images

Figure CN123148933A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of adsorbent technology, specifically to a sulfur-selenium bifunctional adsorbent, its preparation method, and its application. Background Technology
[0002] Currently, mercury removal technologies mainly include adsorbent adsorption and catalytic oxidation. Among these, activated carbon injection technology is the most mature and developed flue gas mercury emission control technology, widely used due to its lack of additional facilities and high cost-effectiveness. However, its application is limited by the following factors: high operating costs due to limited adsorption capacity, secondary release of mercury during activated carbon treatment, strong inhibitory effect of SO2 on mercury removal, the potential impact of activated carbon on the reuse of fly ash in the cement industry, and the complex and costly process of activated carbon recovery and regeneration. These shortcomings limit the widespread application of existing technologies in the field of mercury removal, especially in the efficient removal of mercury over a wide temperature range.
[0003] Therefore, there is an urgent need to develop an adsorbent to achieve efficient removal of mercury over a wide temperature range. Summary of the Invention
[0004] The purpose of this invention is to provide a sulfur-selenium bifunctional adsorbent, its preparation method, and its application. This adsorbent has high adsorption efficiency and can efficiently remove mercury over a wide temperature range.
[0005] To achieve the above objectives, the first aspect of the present invention provides a sulfur-selenium bifunctional adsorbent, which includes a carrier and an active component loaded on the carrier; the carrier is one or more selected from silica, alumina, activated carbon, copper foam, zeolite and carbon nanotubes, and the active component is selenium and sulfur; based on the weight of the adsorbent, the content of the carrier is 60-90% by weight, and the content of selenium and sulfur is 10-40% by weight.
[0006] Optionally, based on the weight of the adsorbent, the content of the carrier is 60-70% by weight, and the content of selenium and sulfur is 30-40% by weight.
[0007] A second aspect of this invention provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: A selenium-containing compound solution is mixed with a carrier and subjected to ultrasonic treatment to obtain a carrier loaded with selenium-containing compounds; the mass ratio of the selenium-containing compound in the selenium-containing compound solution to the carrier is 1:(0.5-4). At a certain activation temperature, the support loaded with selenium-containing compounds is purged with hydrogen sulfide gas.
[0008] Optionally, the mass ratio of the selenium-containing compound in the selenium-containing compound solution to the carrier is 1:(1-3).
[0009] Optionally, the mass concentration of the selenium-containing compound in the selenium-containing compound solution is 10-40%.
[0010] Optionally, the selenium-containing compound solution is one or more of selenic acid solution, selenite solution, selenate solution, selenite solution, and selenium dioxide solution.
[0011] Optionally, the conditions for the ultrasonic treatment include: a temperature of 25-30°C and a time of 25-40 minutes.
[0012] Optionally, the activation temperature is 60-180℃, the hydrogen sulfide gas concentration is 500-2000ppm, and the purging time is 0.5-2h.
[0013] The third aspect of this invention provides the application of the sulfur-selenium bifunctional adsorbent provided in the first aspect of this invention or the adsorbent obtained by the preparation method provided in the second aspect of this invention in the removal of mercury from flue gas or the removal of mercury from liquid phase.
[0014] Through the above technical solution, the present invention uniformly loads elemental selenium and elemental sulfur on the surface of a carrier by in-situ reduction to form a sulfur-selenium bifunctional adsorbent. The sulfur-selenium bifunctional adsorbent fixes mercury through the sulfur component at low temperature and through the selenium component at high temperature. By utilizing the synergistic effect of sulfur and selenium, the adsorption efficiency of mercury can be achieved in a wide temperature range, significantly improving the adsorption efficiency of mercury.
[0015] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0016] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof. In the drawings: Figure 1 This is a schematic diagram of the reaction process of selenite and hydrogen sulfide in an embodiment of the present invention; Figure 2 This is the flue gas mercury adsorption experimental reaction workstation in the embodiments of the present invention. Detailed Implementation
[0017] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0018] The first aspect of the present invention provides a sulfur-selenium bifunctional adsorbent, which includes a carrier and an active component loaded on the carrier; the carrier is one or more selected from silica, alumina, activated carbon, copper foam, zeolite and carbon nanotubes, and the active component is selenium and sulfur; based on the weight of the adsorbent, the content of the carrier is 60-90% by weight, and the content of selenium and sulfur is 10-40% by weight.
[0019] According to the present invention, optionally, the content of the carrier is 60-70% by weight, and the content of selenium and sulfur is 30-40% by weight, based on the weight of the adsorbent.
[0020] A second aspect of this invention provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: A selenium-containing compound solution is mixed with a carrier and subjected to ultrasonic treatment to obtain a carrier loaded with selenium-containing compounds; the mass ratio of the selenium-containing compound in the selenium-containing compound solution to the carrier is 1:(0.5-4). At a certain activation temperature, the support loaded with selenium-containing compounds is purged with hydrogen sulfide gas.
[0021] According to the present invention, optionally, the mass ratio of the selenium-containing compound in the selenium-containing compound solution to the support is 1:(1-3). Through the above embodiments, selenium can be uniformly loaded onto the support, fully exposing the selenium active sites and improving the adsorption efficiency of mercury.
[0022] According to the present invention, optionally, the mass concentration of the selenium-containing compound in the selenium-containing compound solution is 10-40%.
[0023] According to the present invention, optionally, the selenium-containing compound solution is one or more selected from selenic acid solution, selenite solution, selenate solution, selenite solution, and selenium dioxide solution.
[0024] According to the present invention, optionally, the conditions for the ultrasonic treatment include: a temperature of 25-30°C and a time of 25-40 min. By utilizing the cavitation effect of ultrasound, the dispersion and uniform loading of substances in the solution can be promoted, ensuring that the selenium compound is uniformly loaded on the carrier surface.
[0025] According to the present invention, optionally, the activation temperature is 60-180°C, the hydrogen sulfide gas concentration is 500-2000 ppm, and the purging time is 0.5-2 h. The present invention utilizes hydrogen sulfide gas to directly reduce the selenium-containing compound surface, simultaneously generating elemental selenium and elemental sulfur; and at the aforementioned activation temperature, the surface reactivity of the material can be activated.
[0026] The third aspect of this invention provides the application of the sulfur-selenium bifunctional adsorbent provided in the first aspect of this invention or the adsorbent obtained by the preparation method provided in the second aspect of this invention in the removal of mercury from flue gas or the removal of mercury from liquid phase.
[0027] Through the above technical solution, this invention uniformly loads elemental selenium and elemental sulfur onto the surface of a carrier via in-situ reduction, forming a sulfur-selenium bifunctional adsorbent. This adsorbent immobilizes mercury through the sulfur component at low temperatures and through the selenium component at high temperatures. Utilizing the synergistic effect of sulfur and selenium, it achieves highly efficient mercury removal over a wide temperature range, significantly improving mercury adsorption efficiency. Furthermore, the preparation method of this invention is simple, the operating conditions are mild, and it can be prepared in batches. The selected carrier material is readily available, reducing preparation costs. Simultaneously, it can reduce secondary mercury release and environmental pollution. It is suitable for various scenarios, such as waste gas treatment and liquid-phase mercury removal.
[0028] The present invention will be further illustrated by the following examples, but the present invention is not limited thereto.
[0029] Example 1 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 1g of selenite in 9mL of deionized water to form a selenite solution with a mass concentration of 10%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 100℃, the support loaded with selenium compounds was purged with 500 ppm hydrogen sulfide gas for 2 hours.
[0030] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 60% by weight, and the selenium and sulfur content is 40% by weight.
[0031] Example 2 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution was mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier was 1:2; the temperature was 25℃ and the time was 25min. S3. At an activation temperature of 100℃, the support loaded with selenium compounds is purged with 500ppm hydrogen sulfide gas for 2 hours.
[0032] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 70% by weight, and the selenium and sulfur content is 30% by weight.
[0033] Example 3 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 3g of selenite in 7mL of deionized water to form a selenite solution with a mass concentration of 30%. S2. The selenite solution was mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier was 1:3; the temperature was 25℃ and the time was 25min. S3. At an activation temperature of 100℃, the support loaded with selenium compounds was purged with 500 ppm hydrogen sulfide gas for 2 h.
[0034] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 80% by weight, and the selenium and sulfur content is 20% by weight.
[0035] Example 4 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 100℃, the support loaded with selenium compounds was purged with 1000 ppm hydrogen sulfide gas for 2 h.
[0036] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 60% by weight, and the selenium and sulfur content is 40% by weight.
[0037] Example 5 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 150°C, the support loaded with selenium compounds was purged with 1000 ppm hydrogen sulfide gas for 2 hours.
[0038] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 60% by weight, and the selenium and sulfur content is 40% by weight.
[0039] Example 6 This embodiment provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 200℃, the support loaded with selenium-containing compounds was purged with 2000 ppm hydrogen sulfide gas for 2 hours.
[0040] In the sulfur-selenium bifunctional adsorbent obtained in this embodiment, the carrier content is 60% by weight, and the selenium and sulfur content is 40% by weight.
[0041] Comparative Example 1 This comparative example provides a method for preparing a sulfur-selenium bifunctional adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 100℃, the support loaded with selenium-containing compounds was purged with 2000ppm sulfur dioxide gas for 2 hours.
[0042] In the sulfur-selenium bifunctional adsorbent obtained in this comparative example, the content of the carrier is 60% by weight, and the content of selenium and sulfur is 40% by weight.
[0043] Comparative Example 2 This comparative example provides a method for preparing a selenium-based adsorbent, the method comprising: S1. Dissolve 2g of selenite in 8mL of deionized water to form a selenite solution with a mass concentration of 20%. S2. The selenite solution is mixed with the carrier silica and subjected to ultrasonic treatment to obtain the carrier loaded with selenite; wherein the mass ratio of selenite to carrier is 1:1; the temperature is 25℃ and the time is 25min. S3. At an activation temperature of 100℃, the support loaded with selenium compounds is purged with 50ppm hydrogen for 2 hours.
[0044] In the selenium-based adsorbent obtained in this comparative example, the carrier content is 80% by weight and the selenium content is 20% by weight.
[0045] Test case The adsorbents prepared in the examples and comparative examples were used to remove mercury from flue gas, and the specific process is as follows: Figure 2 As shown.
[0046] The mercury removal efficiencies of Examples 1-6 were 90%, 85%, 82%, 95%, 92%, and 80%, respectively, while the mercury removal efficiencies of Comparative Examples 1-2 were 68% and 72%, respectively. Therefore, the adsorbents of Examples 1-5 have better adsorption efficiency for mercury, while the adsorbents of Examples 6 and Comparative Examples 1-2 have lower adsorption efficiency for mercury.
[0047] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0048] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0049] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A sulfur-selenium bifunctional adsorbent, characterized in that, The sulfur-selenium bifunctional adsorbent includes a carrier and an active component loaded on the carrier; the carrier is one or more of silica, alumina, activated carbon, copper foam, zeolite and carbon nanotubes, and the active component is selenium and sulfur; Based on the weight of the adsorbent, the content of the carrier is 60-90% by weight, and the content of selenium and sulfur is 10-40% by weight.
2. The sulfur-selenium bifunctional adsorbent according to claim 1, wherein, Based on the weight of the adsorbent, the content of the carrier is 60-70% by weight, and the content of selenium and sulfur is 30-40% by weight.
3. A method for preparing a sulfur-selenium bifunctional adsorbent, characterized in that, The preparation method includes: A selenium-containing compound solution is mixed with a carrier and subjected to ultrasonic treatment to obtain a carrier loaded with selenium-containing compounds; the mass ratio of the selenium-containing compound in the selenium-containing compound solution to the carrier is 1:(0.5-4). At a certain activation temperature, the support loaded with selenium-containing compounds is purged with hydrogen sulfide gas.
4. The preparation method according to claim 3, wherein, The mass ratio of the selenium-containing compound in the selenium-containing compound solution to the carrier is 1:(1-3).
5. The preparation method according to claim 3, wherein, The mass concentration of the selenium-containing compound in the selenium-containing compound solution is 10-40%.
6. The preparation method according to claim 3, wherein, The selenium-containing compound solution is one or more of the following: selenic acid solution, selenite solution, selenate solution, selenite solution, and selenium dioxide solution.
7. The preparation method according to claim 3, wherein, The conditions for ultrasonic treatment include: a temperature of 25-30℃ and a time of 25-40 minutes.
8. The preparation method according to claim 3, wherein, The activation temperature is 60-180℃.
9. The preparation method according to claim 3, wherein, The concentration of hydrogen sulfide gas is 500-2000 ppm, and the purging time is 0.5-2 hours.
10. The application of the sulfur-selenium bifunctional adsorbent according to claim 1 or 2, or the adsorbent obtained by the preparation method according to any one of claims 3-9, in the removal of mercury from flue gas or the removal of mercury from liquid phase.