A noble metal adsorbent and a method for preparing the same

By constructing a silica protective layer and a nitrogen-sulfur grafted functional layer on a carbon matrix, and combining it with a zirconium-phytic acid network for protection, the problems of easy oxidation of carbon-based precious metal adsorbents in strongly acidic wastewater and the instability of the functional layer are solved, achieving efficient and stable precious metal adsorption and multiple recycling.

CN123148940APending Publication Date: 2026-11-24JIANGXI PUHE SHENGYE ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611578201.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing carbon-based precious metal adsorbents are easily oxidized and corroded in strongly acidic refining wastewater, and have poor functional layer stability, leading to pore collapse and rapid decay of adsorption capacity, making it difficult to achieve efficient and repeated use.

Method used

A silica protective layer is constructed on a carbon matrix and grafted with nitrogen and sulfur functional layers, combined with zirconium-phytic acid network protection, to form an acid-resistant adsorbent rich in nitrogen and sulfur active sites.

Benefits of technology

It improves the structural stability and precious metal adsorption capacity of the adsorbent in strong acid wastewater, extends the cycle life, and maintains high selectivity and rapid adsorption capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148940A_ABST
    Figure CN123148940A_ABST
Patent Text Reader

Abstract

The application discloses a kind of noble metal adsorbents and preparation method thereof, it is related to carbon material adsorbent technical field.The method includes first dispersing carbon matrix after oxidation pretreatment in solvent, by hydrolysis-polycondensation of ethyl silicate in-situ generating silica protective layer on carbon pore wall surface, obtain acid-resistant protective carbon matrix;React with amino-containing silane coupling agent to obtain aminated acid-resistant protective carbon matrix;Under acidic, heating condition, it is added to aqueous solution containing thiourea and formaldehyde in-situ polycondensation, make the surface of protective layer grafting thiourea-formaldehyde chelation functional layer rich in nitrogen and sulfur;Finally, immerse in phytic acid solution impregnation, add zirconium oxychloride solution reaction, in-situ crosslinking is formed zirconium-phytic acid coordination network outside functional layer, namely obtained.The application constructs multistage functional layer on the surface of carbon matrix, and the obtained adsorbent has high selectivity, high adsorption capacity and excellent acid resistance stability to noble metal ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon material adsorbent technology, specifically to a noble metal adsorbent and its preparation method. Background Technology

[0002] The refining process of precious metals (gold, platinum, palladium, etc.) generates a large amount of refining wastewater. A prominent characteristic of this wastewater is its high acidity and high chloride ion concentration (primarily hydrochloric acid, with a pH typically below 1). Precious metals in this wastewater mainly exist as [AuCl4]. - [PtCl6] 2- [PdCl4] 2- Precious metals exist in the form of anionic chloride complexes, with low concentrations but high value. Failure to recover them results in both the loss of precious metals and heavy metal pollution. Adsorption methods are widely used for precious metal recovery due to their simplicity, adjustable selectivity, and ease of enrichment. Among these, carbon-based adsorbent materials (activated carbon, biomass porous carbon, etc.) show the greatest industrial potential due to their large specific surface area, low cost, and wide availability. To improve their ability to capture precious metals, existing technologies often employ the introduction of nitrogen- and sulfur-containing functional groups, such as in-situ co-doping of nitrogen and sulfur during the pyrolysis and carbonization of carbon materials, to prepare nitrogen- and sulfur-doped porous carbon adsorbents. While these materials do exhibit good affinity for precious metals, they still suffer from two drawbacks: First, the nitrogen- and sulfur-containing sites introduced through doping or functionalization are mostly organic groups. In highly acidic, chlorine-containing, and often oxidizing refining wastewater, the edges and defects of the carbon skeleton are easily eroded by the oxidizing medium, leading to pore collapse and a decrease in specific surface area. Second, the active functional groups and their polymeric structures introduced to enhance adsorption have limited stability in strong acids, easily undergoing acid-catalyzed hydrolysis, chain breakage, or shedding. This causes the material's adsorption capacity to rapidly decline with repeated use, resulting in poor reusability. In other words, improving the adsorption performance of precious metals and maintaining structural and functional stability in highly acidic wastewater are often mutually restrictive. Therefore, developing a carbon-based adsorbent that is both resistant to strong acids and has a high adsorption capacity for precious metals, and can be recycled multiple times, has significant industrial implications. Summary of the Invention

[0003] The purpose of this invention is to provide a noble metal adsorbent and its preparation method to solve the technical problems mentioned in the background.

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A method for preparing a noble metal adsorbent includes the following steps:

[0006] (1) Disperse the carbon matrix that has undergone oxidation pretreatment in a solvent, and allow tetraethyl orthosilicate to hydrolyze and condense in situ on the surface of the carbon pore wall to generate a silica protective layer, thereby obtaining an acid-resistant protective carbon matrix;

[0007] (2) React the acid-resistant protective carbon matrix with an amino-containing silane coupling agent to obtain an amino-modified acid-resistant protective carbon matrix;

[0008] (3) The aminated acid-resistant protective carbon matrix is ​​added to an aqueous solution containing thiourea and formaldehyde, and polycondensed in situ under acidic and heated conditions to graft a nitrogen- and sulfur-rich thiourea-formaldehyde chelate functional layer onto the surface of the protective layer to obtain a functionalized adsorption material.

[0009] (4) The functionalized adsorbent material is immersed in phytic acid solution for impregnation, and then zirconium oxychloride solution is added to react, so that phytic acid and zirconium ions are cross-linked in situ on the outside of the functional layer to form a zirconium-phytic acid coordination network, thus obtaining the noble metal adsorbent.

[0010] Preferably, the carbon-based material in step (1) is one or more of activated carbon, coconut shell carbon, or biomass porous carbon.

[0011] Preferably, the oxidation pretreatment in step (1) specifically involves first oxidizing the carbon-based material with dilute nitric acid or ammonium persulfate aqueous solution, then washing it with water until neutral and drying it to obtain a carbon matrix with oxygen-containing functional groups on its surface.

[0012] Preferably, the solvent in step (1) is a mixture of ethanol and water;

[0013] The ratio of tetraethyl orthosilicate to carbon matrix is ​​0.5–1.5 mL: 1 g;

[0014] The hydrolysis-condensation reaction was carried out at 30-50°C for 4-8 hours under conditions of pH 2-3.

[0015] Preferably, the silica protective layer is a thin layer continuously coated on the surface of the carbon pore walls, and the specific surface area retention rate of the carbon matrix after coating is not less than 85%.

[0016] Preferably, the amino-containing silane coupling agent in step (2) is γ-aminopropyltriethoxysilane;

[0017] The reaction conditions are 50–60°C in an aqueous ethanol solution for 2–6 hours.

[0018] Preferably, the mass ratio of thiourea to formaldehyde in step (3) is 1:(0.5-1.5);

[0019] The polycondensation was carried out at a pH of 3-4 and a temperature of 70-75°C for 4-6 hours.

[0020] Preferably, the phytic acid solution in step (4) has a mass fraction of 3-8% and an immersion time of 1-3 hours.

[0021] Preferably, the concentration of the zirconium oxychloride solution in step (4) is 0.1-0.3 mol / L, and the solution is added dropwise and reacted at room temperature for 3-5 hours.

[0022] A noble metal adsorbent is prepared by the method described above.

[0023] Compared with the prior art, the beneficial effects of the present invention are:

[0024] 1. The silica protective layer isolates and protects the carbon skeleton, providing a strong and uniform anchoring foundation for the functional layers without sacrificing mass transfer. The edges and defects of the carbon skeleton are most susceptible to erosion by oxidizing media. The thin and dense inorganic silica shell constructed on the pore walls exhibits almost no chemical reaction with strong inorganic acids, creating a barrier between the vulnerable active sites and the medium, mitigating the damage to the carbon skeleton caused by oxidizing wastewater (activated carbon is already relatively stable in non-oxidizing strong acids such as pure hydrochloric acid and sulfuric acid; therefore, the corrosion resistance of this layer is primarily aimed at oxidizing media). Simultaneously, the surface of this layer is rich in silanol groups, providing a uniform and anchorable deposition surface for the subsequent nitrogen and sulfur functional layers. Furthermore, the covalent introduction of -NH2 through a silane coupling agent upgrades the functional layer from simple hydrogen bonding / etherification adhesion to partial covalent bonding, resulting in stronger bonds and fewer byproducts, reducing the risk of the functional layer peeling off entirely in strong acids from the source. The protective layer itself is thin and remains hydrophilic, allowing water and dissolved metal ions to freely enter and exit the pores with minimal loss of mass transfer performance.

[0025] 2. High-density nitrogen and sulfur active sites, primarily through soft coordination and secondarily through electrostatic attraction, endow the material with high capacity, high selectivity, and rapid adsorption. Noble metals such as gold and palladium are typical soft metal centers, naturally inclined to bind with sulfur and nitrogen soft donors. The densely distributed nitrogen- and sulfur-containing sites on the material surface can firmly fix them through soft coordination, which is the main source of the material's high adsorption capacity. In strong acid chloride wastewater, noble metals exist as negatively charged chloride anions. After protonation, the positively charged nitrogen-containing sites can be drawn closer to the coordination sites through electrostatic attraction, serving as channels to accelerate adsorption and assist in enrichment. The synergy of coordination and electrostatic attraction, coupled with the distribution of sites within well-developed and accessible pores, gives the material the characteristics of high capacity, good selectivity, and rapid adsorption.

[0026] 3. The zirconium-phytic acid synergistic protection network inhibits the hydrolysis and shedding of the functional layer through physical encapsulation and chemical constraint, significantly improving the stability of the material in strong acids. The real reason for the material's cyclic degradation is that the polymeric structure of the nitrogen-rich and sulfur-rich functional layer is slowly hydrolyzed, broken, and detached in strong acids. To address this, phytic acid and zirconium salt are introduced on the outside of the functional layer: one end of the phytic acid phosphate group is attached to the functional layer, and the other end is coordinated with zirconium ions. The zirconium ions crosslink the phytic acid into a three-dimensional, insoluble, and strong acid-resistant network shell. This network cannot be formed by phytic acid alone (which is easily soluble and washed away) or by zirconium salt alone (which is difficult to form a film in an aqueous phase at room temperature); both coordination and crosslinking are indispensable. It firmly binds the inner functional layer, significantly inhibiting the dissolution of hydrolysis products, while its own rich hydrated ion channels do not hinder the diffusion of noble metal chloride anions to the inner layer for capture. Thus, while maintaining the basic adsorption capacity (phytic acid only occupies some of the outer electrostatic auxiliary sites, and the main capture is still at the inner soft coordination sites, with only a slight decrease in capacity), the durability and cycle life of the material in strong acid wastewater are substantially improved. Attached Figure Description

[0027] Figure 1 This is a SEM image of the noble metal adsorbent prepared in Example 1 of the present invention. Detailed Implementation

[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0029] Example 1

[0030] A method for preparing a noble metal adsorbent includes the following steps:

[0031] (1) Take 10.0g of coconut shell activated carbon (particle size 200-300 mesh, dried at 105℃ for 12h before use), add 150mL of 1mol / L nitric acid solution, mechanically stir and oxidize in a 60℃ water bath for 4h, filter and wash repeatedly with deionized water until the filtrate is neutral, dry at 105℃ for 12h to obtain a carbon matrix with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface; take 8.0g of the carbon matrix and disperse it in 120mL of anhydrous ethanol and 40mL of deionized water. In a mixed solvent, the mixture was ultrasonically dispersed for 30 min. Hydrochloric acid was added to adjust the pH of the system to 2.5. 10 mL of tetraethyl orthosilicate was slowly added dropwise under mechanical stirring at 40 °C. The reaction was continued for 7 h to allow the tetraethyl orthosilicate to hydrolyze and condense in situ on the carbon pore wall surface to form a thin and continuous silica protective layer. The mixture was filtered, washed with ethanol and deionized water, and dried at 80 °C for 10 h to obtain an acid-resistant protective carbon matrix (the specific surface area retention rate of the carbon matrix after oxidation pretreatment is >85%).

[0032] (2) Take 6.0 g of acid-resistant protective carbon matrix and disperse it in a mixed solvent of 114 mL anhydrous ethanol and 6 mL deionized water. Add 5.0 mL of γ-aminopropyltriethoxysilane and reflux the mixture at 55 °C for 3 h with mechanical stirring. After filtration, wash with anhydrous ethanol to remove unreacted coupling agent and self-condensing oligomers. Dry under vacuum at 60 °C for 10 h to obtain an amino-rich amino-resistant protective carbon matrix.

[0033] (3) Take 5.0g of amino acid-resistant protective carbon matrix and add it to 150mL of aqueous solution containing 8.0g of thiourea and formaldehyde (containing 10g of formaldehyde). Adjust the pH of the system to 3.5 with 1mol / L hydrochloric acid, and mechanically stir and reflux at 73℃ for 5h. After filtration, wash with deionized water until neutral, and vacuum dry at 60℃ for 12h to obtain functionalized adsorption material.

[0034] (4) Take 4.0g of functionalized adsorbent material and add it to 100mL of 7% phytic acid aqueous solution. Soak at room temperature for 2h to allow phytic acid to be fully adsorbed and anchored on the surface of the functional layer. Then, under stirring, slowly add 50mL of 0.25mol / L zirconium oxychloride aqueous solution at a rate of about 1mL / min. After the addition is complete, continue the reaction at room temperature for 4h. After filtration, wash with deionized water until there are no free chloride ions in the filtrate (AgNO3 test). Dry under vacuum at 60℃ for 12h to obtain the noble metal adsorbent.

[0035] Example 2

[0036] A method for preparing a noble metal adsorbent includes the following steps:

[0037] (1) Take 10.0g of coconut shell activated carbon (particle size 200-300 mesh, dried at 105℃ for 12h before use), add 150mL of 1mol / L nitric acid solution, mechanically stir and oxidize in a 60℃ water bath for 4h, filter and wash repeatedly with deionized water until the filtrate is neutral, dry at 105℃ for 12h to obtain a carbon matrix with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface; take 8.0g of the carbon matrix and disperse it in 120mL of anhydrous ethanol and 40mL of deionized water. In a mixed solvent, the mixture was ultrasonically dispersed for 30 min. Hydrochloric acid was added to adjust the pH of the system to 2.5. 6 mL of tetraethyl orthosilicate was slowly added dropwise under mechanical stirring at 40 °C. The reaction was continued for 5 h to allow the tetraethyl orthosilicate to hydrolyze and condense in situ on the carbon pore wall surface to form a thin and continuous silica protective layer. The mixture was filtered, washed with ethanol and deionized water, and dried at 80 °C for 10 h to obtain an acid-resistant protective carbon matrix (the specific surface area retention rate of the carbon matrix after oxidation pretreatment is >85%).

[0038] (2) Take 6.0 g of acid-resistant protective carbon matrix and disperse it in a mixed solvent of 114 mL anhydrous ethanol and 6 mL deionized water. Add 5.0 mL of γ-aminopropyltriethoxysilane and reflux the mixture at 55 °C for 3 h with mechanical stirring. After filtration, wash with anhydrous ethanol to remove unreacted coupling agent and self-condensing oligomers. Dry under vacuum at 60 °C for 10 h to obtain an amino-rich amino-resistant protective carbon matrix.

[0039] (3) Take 5.0g of amino acid-resistant protective carbon matrix and add it to 150mL of aqueous solution containing 8.0g of thiourea and formaldehyde (containing 6g of formaldehyde). Adjust the pH of the system to 3.5 with 1mol / L hydrochloric acid, and mechanically stir and reflux at 73℃ for 5h. After filtration, wash with deionized water until neutral, and vacuum dry at 60℃ for 12h to obtain functionalized adsorbent material.

[0040] (4) Take 4.0g of functionalized adsorbent material and add it to 100mL of 4% phytic acid aqueous solution. Soak at room temperature for 2h to allow phytic acid to be fully adsorbed and anchored on the surface of the functional layer. Then, under stirring, slowly add 50mL of 0.15mol / L zirconium oxychloride aqueous solution at a rate of about 1mL / min. After the addition is complete, continue the reaction at room temperature for 4h. After filtration, wash with deionized water until there are no free chloride ions in the filtrate (AgNO3 test). Dry under vacuum at 60℃ for 12h to obtain the noble metal adsorbent.

[0041] Example 3

[0042] A method for preparing a noble metal adsorbent includes the following steps:

[0043] (1) Take 10.0g of coconut shell activated carbon (particle size 200-300 mesh, dried at 105℃ for 12h before use), add 150mL of 1mol / L nitric acid solution, mechanically stir and oxidize in a 60℃ water bath for 4h, filter and wash repeatedly with deionized water until the filtrate is neutral, dry at 105℃ for 12h to obtain a carbon matrix with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface; take 8.0g of the carbon matrix and disperse it in 120mL of anhydrous ethanol and 40mL of deionized water. In a mixed solvent, the mixture was ultrasonically dispersed for 30 min. Hydrochloric acid was added to adjust the pH of the system to 2.5. 8 mL of tetraethyl orthosilicate was slowly added dropwise under mechanical stirring at 40 °C. The reaction was continued for 6 h to allow the tetraethyl orthosilicate to hydrolyze and condense in situ on the carbon pore wall surface to form a thin and continuous silica protective layer. The mixture was filtered, washed with ethanol and deionized water, and dried at 80 °C for 10 h to obtain an acid-resistant protective carbon matrix (the specific surface area retention rate of the carbon matrix after oxidation pretreatment is >85%).

[0044] (2) Take 6.0 g of acid-resistant protective carbon matrix and disperse it in a mixed solvent of 114 mL anhydrous ethanol and 6 mL deionized water. Add 5.0 mL of γ-aminopropyltriethoxysilane and reflux at 55 °C for 4 h with mechanical stirring. After filtration, wash with anhydrous ethanol to remove unreacted coupling agent and self-condensing oligomers. Dry under vacuum at 60 °C for 10 h to obtain an amino-rich amino-resistant protective carbon matrix.

[0045] (3) Take 5.0g of amino acid-resistant protective carbon matrix and add it to 150mL of aqueous solution containing 8.0g of thiourea and formaldehyde (containing 8g of formaldehyde). Adjust the pH of the system to 3.5 with 1mol / L hydrochloric acid, and mechanically stir and reflux at 73℃ for 5h. After filtration, wash with deionized water until neutral, and vacuum dry at 60℃ for 12h to obtain functionalized adsorption material.

[0046] (4) Take 4.0g of functionalized adsorbent material and add it to 100mL of 5% phytic acid aqueous solution. Soak at room temperature for 2h to allow phytic acid to be fully adsorbed and anchored on the surface of the functional layer. Then, under stirring, slowly add 50mL of 0.2mol / L zirconium oxychloride aqueous solution at a rate of about 1mL / min. After the addition is complete, continue the reaction at room temperature for 4h. After filtration, wash with deionized water until there are no free chloride ions in the filtrate (AgNO3 test). Dry under vacuum at 60℃ for 12h to obtain the noble metal adsorbent.

[0047] Example 4

[0048] A method for preparing a noble metal adsorbent includes the following steps:

[0049] (1) Take 10.0g of coconut shell activated carbon (particle size 200-300 mesh, dried at 105℃ for 12h before use), add 150mL of 1mol / L nitric acid solution, mechanically stir and oxidize in a 60℃ water bath for 4h, filter and wash repeatedly with deionized water until the filtrate is neutral, dry at 105℃ for 12h to obtain a carbon matrix with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface; take 8.0g of the carbon matrix and disperse it in 120mL of anhydrous ethanol and 40mL of deionized water. In a mixed solvent, the mixture was ultrasonically dispersed for 30 min, and hydrochloric acid was added to adjust the pH of the system to 3. 12 mL of tetraethyl orthosilicate was slowly added dropwise under mechanical stirring at 50 °C, and the reaction was continued for 8 h. This allowed the tetraethyl orthosilicate to hydrolyze and condense in situ on the carbon pore wall surface to form a thin and continuous silica protective layer. The mixture was then filtered, washed with ethanol and deionized water, and dried at 80 °C for 10 h to obtain an acid-resistant protective carbon matrix (the specific surface area retention rate of the carbon matrix after oxidation pretreatment is >85%).

[0050] (2) Take 6.0 g of acid-resistant protective carbon matrix and disperse it in a mixed solvent of 114 mL anhydrous ethanol and 6 mL deionized water. Add 5.0 mL of γ-aminopropyltriethoxysilane and reflux at 60 °C for 6 h with mechanical stirring. After filtration, wash with anhydrous ethanol to remove unreacted coupling agent and self-condensing oligomers. Dry under vacuum at 60 °C for 10 h to obtain an amino-rich amino-resistant protective carbon matrix.

[0051] (3) Take 5.0g of amino acid-resistant protective carbon matrix and add it to 150mL of aqueous solution containing 8.0g of thiourea and formaldehyde (containing 12g of formaldehyde). Adjust the pH of the system to 4 with 1mol / L hydrochloric acid, and mechanically stir and reflux at 75℃ for 6h. After filtration, wash with deionized water until neutral, and vacuum dry at 60℃ for 12h to obtain functionalized adsorbent material.

[0052] (4) Take 4.0g of functionalized adsorbent material and add it to 100mL of 8% phytic acid aqueous solution. Soak at room temperature for 3h to allow phytic acid to be fully adsorbed and anchored on the surface of the functional layer. Then, under stirring, slowly add 50mL of 0.3mol / L zirconium oxychloride aqueous solution at a rate of about 1mL / min. After the addition is complete, continue the reaction at room temperature for 5h. After filtration, wash with deionized water until there are no free chloride ions in the filtrate (AgNO3 test). Dry under vacuum at 60℃ for 12h to obtain the noble metal adsorbent.

[0053] Example 5

[0054] A method for preparing a noble metal adsorbent includes the following steps:

[0055] (1) Take 10.0g of coconut shell activated carbon (particle size 200-300 mesh, dried at 105℃ for 12h before use), add 150mL of 1mol / L nitric acid solution, mechanically stir and oxidize in a 60℃ water bath for 4h, filter and wash repeatedly with deionized water until the filtrate is neutral, dry at 105℃ for 12h to obtain a carbon matrix with oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface; take 8.0g of the carbon matrix and disperse it in 120mL of anhydrous ethanol and 40mL of deionized water. In a mixed solvent, the mixture was ultrasonically dispersed for 30 min, and hydrochloric acid was added to adjust the pH of the system to 2. 4 mL of tetraethyl orthosilicate was slowly added dropwise under mechanical stirring at 30 °C, and the reaction was continued for 4 h. This allowed the tetraethyl orthosilicate to hydrolyze and condense in situ on the carbon pore wall surface to form a thin and continuous silica protective layer. The mixture was then filtered, washed successively with ethanol and deionized water, and dried at 80 °C for 10 h to obtain an acid-resistant protective carbon matrix (the specific surface area retention rate of the carbon matrix after oxidation pretreatment was >85%).

[0056] (2) Take 6.0 g of acid-resistant protective carbon matrix and disperse it in a mixed solvent of 114 mL anhydrous ethanol and 6 mL deionized water. Add 5.0 mL of γ-aminopropyltriethoxysilane and reflux at 50 °C for 2 h with mechanical stirring. After filtration, wash with anhydrous ethanol to remove unreacted coupling agent and self-condensing oligomers. Dry under vacuum at 60 °C for 10 h to obtain an amino-rich amino-resistant protective carbon matrix.

[0057] (3) Take 5.0g of amino acid-resistant protective carbon matrix and add it to 150mL of aqueous solution containing 8.0g of thiourea and formaldehyde (containing 4g of formaldehyde). Adjust the pH of the system to 3 with 1mol / L hydrochloric acid, and mechanically stir and reflux at 70℃ for 4h. After filtration, wash with deionized water until neutral, and vacuum dry at 60℃ for 12h to obtain functionalized adsorption material.

[0058] (4) Take 4.0g of functionalized adsorbent material and add it to 100mL of 3% phytic acid aqueous solution. Soak at room temperature for 1h to allow phytic acid to be fully adsorbed and anchored on the surface of the functional layer. Then, under stirring, slowly add 50mL of 0.1mol / L zirconium oxychloride aqueous solution at a rate of about 1mL / min. After the addition is complete, continue the reaction at room temperature for 3h. After filtration, wash with deionized water until there are no free chloride ions in the filtrate (AgNO3 test). Dry under vacuum at 60℃ for 12h to obtain the noble metal adsorbent.

[0059] Comparative Example 1: Compared with Example 4, step (1) was omitted, and the silica protective layer was not constructed. That is, the carbon matrix after oxidation pretreatment was directly subjected to step (2) amination and subsequent treatment, and all other conditions were the same.

[0060] Comparative Example 2: Compared with Example 4, step (2) aminosilane coupling agent modification was omitted, that is, the acid-resistant protective carbon matrix was directly subjected to step (3) thiourea-formaldehyde polycondensation and subsequent treatment without amination, and all other conditions were the same.

[0061] Comparative Example 3: Compared with Example 4, step (3) was omitted, and the thiourea-formaldehyde nitrogen-sulfur chelate functional layer was not grafted. Instead, the aminated acid-resistant protective carbon matrix was directly subjected to step (4) zirconium-phytic acid network treatment. All other conditions were the same.

[0062] Comparative Example 4: Compared with Example 4, step (4) is omitted, and the zirconium-phytic acid synergistic protection network is not introduced. That is, the functionalized adsorbent material obtained in step (3) is used directly as the finished product, and all other conditions are the same.

[0063] Comparative Example 5: Compared with Example 4, in step (4), only 8% phytic acid aqueous solution was immersed without adding zirconium oxychloride solution (i.e., zirconium crosslinking was not performed), and all other conditions were the same.

[0064] Comparative Example 6: Compared with Example 4, in step (4), the functionalized adsorbent material was treated with 0.3 mol / L zirconium oxychloride aqueous solution instead of impregnating with phytic acid, and all other conditions were the same.

[0065] Performance testing

[0066] 1. Pore Structure (Specific Surface Area) Measurement: Appropriate amounts of adsorbent samples from each example and comparative example were degassed under vacuum at 80℃ for 6 hours (due to the presence of a thiourea-formaldehyde functional layer and a zirconium-phytic acid organic network on the outer layer of the sample, the degassed temperature should not be too high to avoid thermal decomposition of the functional components). Using a fully automated specific surface area and pore size analyzer, with high-purity nitrogen as the adsorbate, the nitrogen adsorption-desorption isotherm was measured at 77K. Data within the relative pressure P / P0 range of 0.05–0.30 were used to calculate the specific surface area using the BET equation (multi-point method), and the t-plot method was used to assist in determining whether the micropores were blocked by the coating layer. This index is used to characterize the effect of layer-by-layer modification and zirconium-phytic acid network coating on the pore structure and mass transfer channels of the material. A high specific surface area indicates that the modified layer is thin and does not block the pores.

[0067] 2. Determination of the saturated adsorption capacity of precious metals: Simulated refining wastewater containing single metals Au(III), Pd(II), and Pt(IV) was prepared (hydrochloric acid system, pH≈0.5, Cl...). - (Concentration 2 mol / L). To obtain the saturated adsorption capacity, a series of single-metal solutions with different initial concentrations (50, 100, 150, 200, 300, 400 mg / L) were prepared. 50 mL of each solution was mixed with 20.0 mg of dried adsorbent and incubated at 25℃ and 180 r / min for 24 h until adsorption equilibrium was reached. The supernatant was centrifuged, and the equilibrium concentration was determined using inductively coupled plasma optical emission spectrometry (ICP-OES). The equilibrium adsorption capacity at each initial concentration was calculated using the difference method combined with the dosage and liquid volume. Adsorption isotherms were plotted and fitted using the Langmuir equation to obtain the saturated adsorption capacity qmax (mg / g). Note: The difference method obtained at a single initial concentration represents the equilibrium adsorption capacity under that condition and is not equivalent to the Langmuir saturated capacity; the table below lists the fitted isotherm values.

[0068] 3. Determination of adsorption equilibrium time (adsorption rate): The amount of adsorbent added and the initial concentration were fixed in the Au(III) adsorption system. Samples were taken at 5, 10, 20, 30, 45, 60, 90, 120, 150 and 180 min respectively. The concentration of the remaining Au(III) was determined by ICP-OES. The change curve of adsorption capacity over time was plotted. The time corresponding to the adsorption capacity reaching 95% of the equilibrium adsorption capacity was recorded as the adsorption equilibrium time (min), which was used to characterize the adsorption rate.

[0069] 4. Non-oxidizing strong acid (hydrolysis) stability determination: The dried adsorbent before adsorption was placed in 3 mol / L hydrochloric acid (non-oxidizing) and soaked at 25℃ for 24 h. After removal, it was washed with deionized water until neutral, dried under vacuum at 60℃, and then its saturated adsorption capacity for Au(III) was determined according to Test 2. The capacity retention rate was expressed as the ratio (%) of the capacity after soaking to that before soaking. This item mainly examines the degree of functional layer hydrolysis and loss by acid catalysis, and is used to characterize the binding effect of the zirconium-phytic acid synergistic protection network on the functional layer.

[0070] 5. Cyclic performance determination: Using a mixed solution of 0.7 mol / L thiourea + 0.1 mol / L hydrochloric acid as the eluent, the saturated sample was eluted and regenerated (shaking at 25℃ for 4 h). After washing and drying, it was reused for Au(III) adsorption. Ten adsorption-elution cycles were performed. The adsorption capacity after the 10th cycle was measured. The percentage decrease in the adsorption capacity relative to the initial adsorption capacity was used to represent the cycle capacity loss, which was used to characterize the repeated service life.

[0071] Table 1:

[0072] sample Specific surface area (m² / g) Au(III) (mg / g) Pd(II) (mg / g) Pt(IV) (mg / g) Adsorption equilibrium time (min) Volume retention rate (%) after immersion in non-oxidizing strong acid Capacity loss after 10 cycles (%) Example 1 762 465 214 167 150 92.3 10.4 Example 2 798 412 198 157 135 88.7 15.2 Example 3 781 446 196 156 140 90.8 12.3 Example 4 738 457 206 151 165 93.6 8.6 Example 5 819 389 167 156 130 86.2 18.5 Comparative Example 1 858 468 220 192 155 72.0 34.8 Comparative Example 2 741 362 159 130 145 79.8 25.6 Comparative Example 3 842 88 28 19 90 90.5 12.0 Comparative Example 4 792 474 218 180 120 67.8 39.5 Comparative Example 5 786 469 211 174 122 71.9 34.6 Comparative Example 6 779 471 221 184 125 74.6 31.2

[0073] 6. Determination of Stability to Oxidizing Strong Acids: The dried adsorbent before adsorption was placed in a medium simulating the oxidizing properties of actual wastewater (3 mol / L hydrochloric acid with 0.3 mol / L nitric acid added to introduce oxidizing properties), soaked at 25℃ for 24 h, washed, and dried before determining: ① Specific surface area retention rate (relative to before soaking), used to characterize the carbon skeleton's resistance to oxidative erosion and the pores' resistance to collapse; ② Au(III) capacity retention rate. Samples with and without a silica protective layer were compared to verify the antioxidant protection effect of the silica layer on the carbon skeleton. It should be noted that the oxidizing medium will simultaneously oxidize and damage the thiourea-formaldehyde functional layer; therefore, the capacity retention rate in this item reflects the combined result of carbon skeleton oxidation and functional layer oxidation / hydrolysis, while the specific surface area retention rate specifically reflects the antioxidant protection of the carbon skeleton.

[0074] Table 2:

[0075] sample Specific surface area retention rate (%) Au(III) Capacity retention rate (%) Example 1 92.5 84.1 Example 2 90.1 80.3 Example 3 91.6 82.4 Example 4 93.8 86.2 Example 5 88.7 77.9 Comparative Example 1 65.4 54.8 Comparative Example 2 90.8 73.6 Comparative Example 3 92.0 89.5 Comparative Example 4 90.3 61.5 Comparative Example 5 89.9 64.7 Comparative Example 6 90.0 66.8

[0076] In non-oxidizing pure hydrochloric acid (Table 1), the activated carbon framework itself is relatively stable, and the effect of the silica layer on capacity and capacity retention is not significant. Comparative Example 1 even has a slightly higher initial capacity (468 mg / g) due to its more open pores. The main reason for the decrease in stability of Comparative Example 1 (72.0% retention) is that the loss of silica surface leads to the inability of aminosilanes to anchor and the functional layer to adhere poorly and fall off, rather than the destruction of the carbon framework. The true value of the silica layer is fully demonstrated in oxidizing media: as shown in Table 2, the specific surface area retention of each sample containing the silica protective layer is still as high as 88.7% to 93.8% after immersion in strong oxidizing acid, indicating that the edges and defect sites of its carbon framework are effectively shielded by the inorganic shell, resisting oxidation and erosion, and the pores are not easily collapsed. However, the specific surface area retention of Comparative Example 1, which omits the protective layer, drops sharply to 65.4%, and the Au capacity retention is only 54.8%, indicating that its carbon framework is significantly oxidized and eroded in strong oxidizing acid, the pores collapse, and the functional sites are lost. The comparison directly proves that the silica protective layer, by isolating oxidizing media and protecting the carbon skeleton, is a key barrier for maintaining the structural stability of materials in oxidizing refining wastewater.

[0077] The initial capacities of Comparative Examples 5 (phytic acid only) and 6 (zirconium salt only) were similar to those of Example 4, but their retention rates in non-oxidizing strong acids (71.9%, 74.6%), cycle losses (34.6%, 31.2%), and Au capacity retention rates in oxidizing strong acids (64.7%, 66.8%) were significantly worse than those of Example 4, only slightly better than Comparative Example 4 which completely omitted the protective network. This indicates that neither phytic acid alone (easily soluble in strong acids and washed away) nor zirconium salt alone (difficult to form a film in aqueous phase at room temperature) can form an effective protective shell. Only when the two are coordinated and crosslinked into a three-dimensional insoluble network can the functional layer be physically encapsulated and chemically confined. It is worth noting that although Comparative Examples 4 / 5 / 6 contained a silica protective layer and still had a high specific surface area retention rate (approximately 90%) in oxidizing media, their Au capacity retention rates were significantly lower. This further illustrates that the silica layer protects the carbon skeleton, while the zirconium-phytic acid network protects the nitrogen and sulfur functional layers. The two act on different targets and cannot be substituted for each other.

[0078] 7. Selective Adsorption Test: Prepare a competitive mixed solution containing multiple metal ions, including Au. 3+ Cu 2+ Ni 2+ Zn 2+ Fe 3+ Pb 2+ The initial concentration of each ion was 100 mg / L. 10 mg of adsorbent was weighed and added to 20 mL of the above mixed solution, and the mixture was shaken for 2 h for adsorption. The concentration changes of each ion in the solution before and after adsorption were measured by ICP-OES, and the selectivity coefficient (Au / Cu) was calculated to evaluate the specific recognition and capture ability of the adsorbent in a complex ionic environment.

[0079] After testing, the selectivity coefficients (Au / Cu) of Examples 1-5 were in the range of 782-938, while the selectivity coefficient α (Au / Cu) of Comparative Example 2 was 208, and that of Comparative Example 3 was 36. Comparative Example 3, which omitted the nitrogen-sulfur functional layer, lost its soft coordination sites, resulting in a sharp drop in selectivity coefficient α (Au / Cu) to 36, essentially losing its selectivity. Comparative Example 2, lacking amino covalent anchoring and with insufficient functional layer grafting, also showed a significantly lower selectivity coefficient α (Au / Cu) than the other examples. These comparisons demonstrate that the nitrogen-rich and sulfur-rich chelating functional layer is fundamental to achieving high selectivity in the material.

[0080] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for producing a noble metal adsorbent, characterized by, Includes the following steps: (1) Disperse the carbon matrix that has undergone oxidation pretreatment in a solvent, and allow tetraethyl orthosilicate to hydrolyze and condense in situ on the surface of the carbon pore wall to generate a silica protective layer, thereby obtaining an acid-resistant protective carbon matrix; (2) React the acid-resistant protective carbon matrix with an amino-containing silane coupling agent to obtain an amino-modified acid-resistant protective carbon matrix; (3) The aminated acid-resistant protective carbon matrix is ​​added to an aqueous solution containing thiourea and formaldehyde, and polycondensed in situ under acidic and heated conditions to graft a nitrogen- and sulfur-rich thiourea-formaldehyde chelate functional layer onto the surface of the protective layer to obtain a functionalized adsorption material. (4) The functionalized adsorbent material is immersed in phytic acid solution for impregnation, and then zirconium oxychloride solution is added to react, so that phytic acid and zirconium ions are cross-linked in situ on the outside of the functional layer to form a zirconium-phytic acid coordination network, thus obtaining the noble metal adsorbent.

2. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: The carbon-based material mentioned in step (1) is one or more of activated carbon, coconut shell carbon, or biomass porous carbon. ​ 3. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: The oxidation pretreatment in step (1) specifically involves first oxidizing the carbon-based material with dilute nitric acid or ammonium persulfate aqueous solution, then washing it with water until neutral and drying it to obtain a carbon matrix with oxygen-containing functional groups on its surface. ​ 4. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: In step (1), the solvent is a mixture of ethanol and water; ​ The ratio of tetraethyl orthosilicate to carbon matrix is ​​0.5–1.5 mL: 1 g; The hydrolysis-condensation reaction was carried out at 30-50°C for 4-8 hours under conditions of pH 2-3.

5. The method of claim 4, wherein the noble metal adsorbent is prepared by the steps of: The silica protective layer is a thin layer continuously coated on the surface of the carbon pore walls, and the specific surface area retention rate of the carbon matrix after coating is not less than 85%.

6. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: The amino-containing silane coupling agent mentioned in step (2) is γ-aminopropyltriethoxysilane; The reaction conditions are 50–60°C in an aqueous ethanol solution for 2–6 hours.

7. The method for preparing a noble metal adsorbent according to claim 1, characterized in that, The mass ratio of thiourea to formaldehyde in step (3) is 1:(0.5-1.5); The polycondensation was carried out at a pH of 3-4 and a temperature of 70-75°C for 4-6 hours.

8. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: In step (4), the phytic acid solution has a mass fraction of 3-8% and the soaking time is 1-3 hours. ​ 9. The method of claim 1, wherein the noble metal adsorbent is prepared by the steps of: In step (4), the concentration of the zirconium oxychloride solution is 0.1-0.3 mol / L, and the reaction is carried out at room temperature for 3-5 hours after the addition. ​ 10. A noble metal adsorbent, characterized by, It is prepared by the method described in any one of claims 1 to 9.