Humic acid-based aerogel for adsorbing metal ions and method for preparing the same
By modifying the sodium alginate aerogel with epichlorohydrin through chemical crosslinking, a covalent crosslinking network is constructed, which enhances the skeletal stability of the humic acid alginate aerogel. This solves the problems of weak matrix bonding and easy swelling and collapse in the existing technology, and improves the adsorption capacity of metal ions and the recycling performance.
Patent Information
- Application Number
- CN202611472919.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-24
AI Technical Summary
The existing humic acid-sodium alginate composite aerogel matrix has weak bonding strength, is prone to swelling and collapse when exposed to water, has low metal ion adsorption capacity, and poor recycling performance.
Epichlorohydrin was used as a crosslinking agent to chemically crosslink the humic acid-sodium alginate composite system, thereby constructing a covalent crosslinking network and enhancing the stability of the aerogel matrix skeleton.
This improved the metal ion adsorption capacity and recycling stability of aerogels, solved the problems of weak matrix bonding and easy swelling and collapse, and achieved a stable material skeleton and improved adsorption performance.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aerogel preparation technology, specifically relating to a humic acid-based aerogel for adsorbing metal ions and its preparation method. Background Technology
[0002] Humic acid is widely available and inexpensive. Its molecular structure contains numerous active functional groups such as carboxyl and hydroxyl groups, giving it great potential for application in the adsorption of heavy metal ions. Combining humic acid with sodium alginate to prepare aerogel adsorbent materials leverages the advantages of both functional groups and their three-dimensional porous network structure, making them suitable for treating wastewater containing metal ions. Currently, humic acid-based composite aerogels have become a research hotspot in water treatment adsorbent materials. How to control the crosslinking modification process to improve the pore structure stability and metal ion adsorption capacity of the aerogel is a key research direction for this type of material.
[0003] Existing humic acid When sodium alginate composite aerogels are directly blended, the matrix molecules are bound together only by intermolecular forces, resulting in weak physical bonding. In environments where metal ion-containing wastewater is immersed, the matrix is prone to swelling and disintegration, and the three-dimensional porous structure easily collapses, leading to the loss of active adsorption sites. Furthermore, the simple blend products have insufficient cross-linking, limiting their adsorption capacity for metal ions in water and resulting in poor recyclability. These limitations restrict the widespread application of this type of aerogel in the treatment of wastewater containing metal ions.
[0004] While some patents related to humic acid-based aerogels for water treatment have been disclosed in the prior art, they still suffer from defects such as weak matrix bonding strength and insufficient adsorption and cycling performance. For example, CN114146528A discloses a humic acid composite sodium alginate adsorption gel, which only involves simple physical blending and cross-linking. The gel is prone to swelling and breakage when exposed to water, and its adsorption performance significantly decreases after multiple cycles. Another example is CN112755823A, which discloses a humic acid-based heavy metal adsorption aerogel. However, it has not undergone chemical cross-linking modification, resulting in poor aerogel framework stability and limiting its practical application in wastewater treatment.
[0005] In summary, existing humic acid Sodium alginate composite aerogels suffer from drawbacks such as weak matrix bonding, easy swelling and collapse upon contact with water, low metal ion adsorption capacity, and poor recyclability. The key technical problem this invention aims to solve is to provide a humic acid-based aerogel for adsorbing metal ions. Through epichlorohydrin chemical crosslinking modification, the stability of the aerogel matrix framework is enhanced, thereby improving the metal ion adsorption capacity and recyclability. Summary of the Invention
[0006] For existing humic acid Sodium alginate composite aerogels suffer from drawbacks such as weak matrix bonding, easy swelling and collapse upon contact with water, low metal ion adsorption capacity, and poor recycling performance. This invention provides a humic acid-based aerogel for adsorbing metal ions and its preparation method.
[0007] The first objective of this invention is to provide a humic acid-based aerogel for adsorbing metal ions, which is achieved by the following method: First, humic acid and sodium alginate are weighed and added to an aqueous sodium hydroxide solution, and stirred evenly to obtain a humic acid / sodium alginate mixture; second, epichlorohydrin is added dropwise to the humic acid / sodium alginate mixture; finally, the reaction solution is heated and stirred to obtain a modified humic acid hydrogel; the modified humic acid aerogel is obtained by washing with distilled water until neutral and then freeze-drying.
[0008] A second objective of this invention is to provide a method for preparing humic acid-based aerogels for adsorbing metal ions, the method comprising the following steps: (1) Weigh humic acid and sodium alginate at room temperature, add them to a 3wt% sodium hydroxide aqueous solution, stir evenly, and prepare a humic acid / sodium alginate mixture.
[0009] Preferably, the ratio of the amount of humic acid, sodium alginate, and sodium hydroxide aqueous solution is 1g:(0.2-0.3)g:(25-30)mL.
[0010] (2) Under room temperature stirring conditions, add 5 mL of epichlorohydrin to the humic acid / sodium alginate mixture and stir for 30 min.
[0011] Preferably, the ratio of the humic acid / sodium alginate mixture to epichlorohydrin is 1 mL : (0.1-0.2) mL.
[0012] (3) Heat the reaction solution to 30°C and continue stirring for 2-4 hours to obtain modified humic acid hydrogel; wash with distilled water until neutral, and freeze dry to obtain modified humic acid aerogel.
[0013] The present invention has the following significant beneficial effects: (1) In this invention, epichlorohydrin is used as a crosslinking agent for humic acid. Humic acid-based aerogels were prepared by chemical cross-linking modification of a sodium alginate composite system. Performance test results showed that epichlorohydrin constructs a chemical cross-linking network to strengthen the aerogel matrix framework, alleviates the problem of material swelling and collapse upon contact with water, and improves the metal ion adsorption capacity and cycle stability. This solves the key technical problems of weak matrix bonding, easy swelling and collapse, and poor adsorption and cycling performance proposed in this invention.
[0014] (2) Compared with the comparative samples without epichlorohydrin and those without the heating crosslinking process, the epichlorohydrin chemical crosslinking can construct a covalent crosslinking network between humic acid and sodium alginate molecules, stabilizing the three-dimensional porous framework of the aerogel and retaining sufficient active sites for metal ion adsorption. The swelling rate, metal ion adsorption capacity, and adsorption retention rate after 5 cycles of the example sample are significantly better than the two comparative samples. The raw material compounding and the epichlorohydrin crosslinking process work synergistically, and the technical solution has outstanding inventiveness.
[0015] (3) The main raw materials of this invention are humic acid and sodium alginate. The raw materials are widely available and easy to obtain. The preparation process is mild and controllable and does not require expensive large-scale equipment. The humic acid-based aerogel can be used for the adsorption and removal of metal ion pollutants in water. The raw materials are green and environmentally friendly, and have good economic value and environmental application prospects. Detailed Implementation
[0016] The above-described solution will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application. The implementation conditions used in the embodiments may be further adjusted according to the conditions of specific manufacturers, and the implementation conditions not specified are generally those in routine experiments.
[0017] Example 1 A humic acid-based aerogel for adsorbing metal ions, the aerogel being prepared by the following method: (1) Weigh 10g of humic acid and 2g of sodium alginate at room temperature, add 250mL of 3wt% sodium hydroxide aqueous solution, stir evenly to obtain humic acid / sodium alginate mixture, and record the total volume of the mixture as V1.
[0018] (2) Under room temperature stirring conditions, epichlorohydrin was added dropwise to a volume V1 of the mixture. The amount added was 0.1 mL of epichlorohydrin per 1 mL of the mixture, and the mixture was stirred for 30 min.
[0019] (3) Heat the reaction solution to 30°C and continue stirring for 2 hours to obtain the modified hydrogel; wash with distilled water until neutral, and freeze dry to obtain humic acid-based aerogel.
[0020] Example 2 A humic acid-based aerogel for adsorbing metal ions, the aerogel being prepared by the following method: (1) Weigh 10g of humic acid and 2.5g of sodium alginate at room temperature, add 275mL of 3wt% sodium hydroxide aqueous solution, stir evenly to obtain humic acid / sodium alginate mixture, and record the total volume of the mixture as V2.
[0021] (2) Under room temperature stirring conditions, epichlorohydrin was added dropwise to a V2 volume of mixture. The amount of epichlorohydrin added was 0.15 mL per 1 mL of mixture. The mixture was stirred for 30 min.
[0022] (3) Heat the reaction solution to 30°C and continue stirring for 3 hours to obtain the modified hydrogel; wash with distilled water until neutral, and freeze dry to obtain humic acid-based aerogel b.
[0023] Example 3 A humic acid-based aerogel for adsorbing metal ions, the aerogel being prepared by the following method: (1) Weigh 10g of humic acid and 3g of sodium alginate at room temperature, add 300mL of 3wt% sodium hydroxide aqueous solution, stir evenly to obtain humic acid / sodium alginate mixture, and record the total volume of the mixture as V3.
[0024] (2) Under room temperature stirring conditions, epichlorohydrin was added dropwise to a V3 volume of mixture, with an addition amount of 0.2 mL of epichlorohydrin per 1 mL of mixture, and stirred for 30 min.
[0025] (3) Heat the reaction solution to 30°C and continue stirring for 4 hours to obtain the modified hydrogel; wash with distilled water until neutral, and freeze dry to obtain humic acid-based aerogel c.
[0026] Comparative Example 1 This comparative example is a humic acid-based aerogel without epichlorohydrin. Compared to Example 2, the step of adding epichlorohydrin was omitted, and the remaining preparation parameters and processes were completely consistent, resulting in the comparative sample d.
[0027] Comparative Example 2 This comparative example is a humic acid-based aerogel that did not use a temperature-increasing crosslinking process. Compared with Example 2, the 30°C heating and stirring step was omitted, and the mixture was stirred at room temperature for 3 hours throughout the process. All other preparation parameters and processes were completely consistent, and comparative sample e was obtained.
[0028] Performance Evaluation I. Test Sample The test sample is from Example 1 of this invention. Samples a, b, and c were prepared, as well as samples d and e prepared in Comparative Examples 1 and 2. Under standardized testing conditions, the three key indicators of each sample—aqueous phase swelling rate, copper ion adsorption capacity, and adsorption retention rate after 5 cycles—were compared.
[0029] II. Test Items and Test Methods 1. Aqueous phase swelling ratio test: Weigh the dried aerogel sample and record the weight as m0. Weigh 0.2g of the aerogel sample and immerse it in 100mL of deionized water with pH=7. Incubate at 25℃ with shaking for 24h. Remove the sample, quickly wipe off the free water on the sample surface with filter paper, and record the weight as m1. Swelling ratio = (m1...) / (m0...) m0) / m0×100%; each group was tested in parallel 5 times, and the arithmetic mean was taken. The result was rounded to two decimal places. The lower the swelling rate, the better the skeleton stability of the aerogel in the water environment.
[0030] 2. Copper ion adsorption capacity test: Prepare a 100 mg / L copper sulfate aqueous solution. Add 0.10 g of aerogel sample to 50 mL of the copper sulfate aqueous solution, and incubate at 25 °C with shaking for 120 min until adsorption equilibrium is reached. Filter to separate the solid and liquid. Measure the remaining mass concentration of copper ions in the filtrate using an atomic absorption spectrophotometer. Adsorption capacity calculation formula: In the formula This represents the initial copper ion concentration. To balance the copper ion concentration, V is the solution volume and m is the mass of aerogel added; each group was tested in parallel 5 times, and the arithmetic mean was taken, with the result rounded to two decimal places; the higher the adsorption capacity value, the stronger the material's ability to adsorb metal ions.
[0031] 3. Adsorption retention rate test after 5 cycles: Collect the sample after the adsorption experiment, wash thoroughly with distilled water, freeze dry, and complete one cycle. Repeat the above adsorption experiment a total of 5 times, and test the copper ion adsorption capacity after the 5th cycle; Cyclic adsorption retention rate = 5th adsorption capacity / initial adsorption capacity × 100%; Each group is tested in parallel 5 times, and the arithmetic mean is taken. The result is rounded to two decimal places; the higher the retention rate, the better the stability of the material in cycle use.
[0032] III. Test Results ; IV. Test Result Analysis The test data show that the aqueous phase swelling rates of samples a, b, and c in the embodiments of this invention are all below 125.00%, the copper ion adsorption capacity is above 62.00 mg / g, and the adsorption retention rate after 5 cycles is above 74.00%. Among them, sample b in Example 2 has the best overall performance. This invention utilizes epichlorohydrin to chemically crosslink humic acid and sodium alginate molecules to construct a covalent crosslinked network, which stabilizes the three-dimensional porous framework of the aerogel, inhibits the swelling and collapse of the material upon contact with water, retains a large number of carboxyl and hydroxyl adsorption active sites, improves the metal ion adsorption capacity and cycling stability, and effectively solves the key technical problems of weak matrix bonding, easy swelling and collapse, and poor adsorption and cycling performance.
[0033] Comparative Example 1, without the addition of epichlorohydrin, relied solely on intermolecular forces for recombination, lacking a covalent chemical cross-linking network. The aerogel swelled severely in water, resulting in partial disintegration of the framework, significant loss of active sites, and a marked decrease in copper ion adsorption capacity and cycle retention. Comparative Example 2, by omitting the temperature-increased cross-linking process, suffered from insufficient epichlorohydrin cross-linking, incomplete cross-linking network formation, high material swelling, and adsorption performance and cycle stability significantly inferior to the embodiments of this invention. These tests demonstrate that the combination of epichlorohydrin feeding and a 30°C temperature-increased cross-linking process is essential to obtaining a humic acid-based aerogel with a stable framework, high metal ion adsorption capacity, and excellent cycle stability.
[0034] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a humic acid-based aerogel for adsorbing metal ions, characterized in that, The preparation method includes the following steps: (1) Weigh humic acid and sodium alginate at room temperature, add them to a 3wt% sodium hydroxide aqueous solution, stir evenly, and prepare a humic acid / sodium alginate mixture. (2) Under room temperature stirring conditions, add 5 mL of epichlorohydrin to the humic acid / sodium alginate mixture and stir for 30 min; (3) Heat the reaction solution to 30°C and continue stirring for 2-4 hours to obtain modified humic acid hydrogel; wash with distilled water until neutral, and freeze dry to obtain modified humic acid aerogel.
2. The method for preparing a humic acid-based aerogel for adsorbing metal ions according to claim 1, characterized in that, The ratio of the amount of humic acid, sodium alginate and sodium hydroxide aqueous solution used in step (1) is 1g:(0.2-0.3)g:(25-30)mL.
3. The method for preparing a humic acid-based aerogel for adsorbing metal ions according to claim 1, characterized in that, In step (2), the ratio of humic acid / sodium alginate mixture to epichlorohydrin is 1 mL: (0.1-0.2) mL.
4. A humic acid-based aerogel for adsorbing metal ions, characterized in that, It is prepared by the method described in any one of claims 1 to 3.
Citation Information
Patent Citations
Micro-nano bubble generating equipment