Method of preparing aerogel material, aerogel material, and semiconductor device
By preparing porous aerogel materials, the problems of low efficiency and high energy consumption in existing gas filtration technologies have been solved, achieving a highly efficient gas purification effect that meets the stringent requirements of semiconductor manufacturing.
Patent Information
- Application Number
- CN202510679873.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
Existing gas filtration technologies are inefficient, energy-intensive, and prone to secondary pollution in semiconductor manufacturing, failing to meet the stringent cleanroom environment requirements.
The preparation method involves dissolving a hydroxyl-containing polymer material and an aldehyde-containing crosslinking agent in a solvent to form a wet gel. The porous aerogel material is then formed through a freeze-drying process, controlling the polymerization reaction of hydroxyl and aldehyde groups and the sublimation of the solvent during freeze-drying.
The preparation process is simple and low-cost. Aerogel materials have excellent gas adsorption properties and can effectively filter micron-sized particles, thereby improving the gas purification effect in semiconductor manufacturing.
Smart Images

Figure CN123148944A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing, and more particularly to a method for preparing an aerogel material, the aerogel material, and semiconductor equipment. Background Technology
[0002] Gas filtration technology plays a vital role in modern industrial production, with applications spanning semiconductor manufacturing, chemical production, and medical gas supply, among others. As industrial technology continues to advance, various sectors are placing higher demands on gas filtration technology, particularly in precision manufacturing, where the effectiveness of gas filtration directly impacts product quality and production efficiency.
[0003] In the semiconductor manufacturing industry, continuous advancements in integrated circuit technology have led to more stringent requirements for cleanroom environments. Particulate contamination in cleanrooms can severely impact the chip manufacturing process; even the smallest particles can disrupt electron flow, causing chip performance degradation and affecting product yield.
[0004] Therefore, efficient gas filtration systems are of great significance for increasing the output of semiconductor manufacturing facilities, reducing production costs, and minimizing equipment maintenance and downtime. Summary of the Invention
[0005] The problem solved by the embodiments of the present invention is to provide a method for preparing an aerogel material, an aerogel material, and a semiconductor device, thereby forming an aerogel material with a porous structure and excellent gas adsorption performance.
[0006] To address the aforementioned problems, this invention provides a method for preparing an aerogel material, comprising: dissolving a hydroxyl-containing polymer material in a solvent to obtain a first solution; dissolving an aldehyde-containing crosslinking agent in a solvent to obtain a second solution; mixing the first solution and the second solution to allow the hydroxyl groups in the first solution to undergo an aldol polymerization reaction with the aldehyde groups in the second solution to form a wet gel with a network structure; freezing the wet gel to form a cryogel, wherein the solvent in the cryogel is solid; and drying the cryogel to sublimate the solid solvent, thereby obtaining an aerogel material with a porous structure.
[0007] Optionally, the hydroxyl-containing polymeric material includes one or more of the following: polyvinyl alcohol, chitosan, carboxymethyl cellulose, hydroxyethyl cellulose, polyethylene glycol, and polyvinylpyrrolidone.
[0008] Optionally, in the step of dissolving the hydroxyl-containing polymer material in a solvent, the solvent may include deionized water or an organic solvent; in the step of dissolving the aldehyde-containing crosslinking agent in a solvent, the solvent may include deionized water or an organic solvent.
[0009] Optionally, the aldehyde-containing crosslinking agent includes one or more combinations of glyoxal, glutaraldehyde, paraformaldehyde, terephthalaldehyde, 2,5-furandialdehyde, isophthalaldehyde, and o-phthalaldehyde.
[0010] Optionally, in the step of mixing the first solution with the second solution, the pH value of the mixed solution is adjusted to acidic.
[0011] Optionally, in the step of adjusting the pH of the mixed solution to acidic, an acidic solution is used to adjust the pH of the mixed solution to 1.99 to 2.01.
[0012] Optionally, in the step of adjusting the pH of the mixed solution to acidic, the acidic solution is hydrochloric acid with a mass fraction of 35% to 36%.
[0013] Optionally, the step of mixing the first solution and the second solution includes: stirring the first solution and the second solution with a magnetic stirrer; and after the first solution and the second solution are mixed evenly, placing the mixed solution in a constant temperature device for cross-linking aging.
[0014] Optionally, the step of freezing the wet gel includes freezing the wet gel at a temperature below -20°C or in a liquid nitrogen environment.
[0015] Optionally, in the step of drying the cryogel, the process temperature is -70°C to -40°C, the vacuum degree is 1 Pa to 10 Pa, and the drying time is 12 hours to 96 hours.
[0016] Optionally, in the step of drying the cryogel, the porosity of the aerogel material is greater than or equal to 85% and less than 97%.
[0017] Optionally, in the step of drying the cryogel, the pore size of the aerogel material is from 0.4 μm to 1.5 μm.
[0018] Optionally, the density of the aerogel material is less than 60 kg / m³. 3 .
[0019] Optionally, when the thickness of the aerogel material is 10 mm, it can withstand a pressure of not less than 3.5 kPa without collapsing or cracking, and the filtration rate of the aerogel material for particles with a diameter greater than 0.5 μm is not less than 97%.
[0020] Optionally, in the step of mixing the first solution with the second solution, the number of hydroxyl groups in the mixed solution is greater than the number of aldehyde groups.
[0021] An aerogel material, the aerogel material comprising: a porous structure, wherein the pores in the porous structure are interconnected and form a network structure; the porosity of the aerogel material is greater than or equal to 85% and less than 97%.
[0022] Optionally, the density of the aerogel material is less than 60 kg / m³. 3 .
[0023] Optionally, the aerogel material has a pore size of 0.4 μm to 1.5 μm.
[0024] Optionally, when the thickness of the aerogel material is 10 mm, it can withstand a pressure of not less than 3.5 kPa without collapsing or cracking, and the filtration rate of the aerogel material for particles with a diameter greater than 0.5 μm is not less than 97%.
[0025] A semiconductor device for use in a cleanroom, the semiconductor device employing the aerogel material.
[0026] Compared with the prior art, the technical solution of the embodiments of the present invention has the following advantages:
[0027] In the aerogel material preparation method provided in this invention, a polymer material containing hydroxyl groups is dissolved in a solvent to obtain a first solution, and a crosslinking agent containing aldehyde groups is dissolved in a solvent to obtain a second solution. The first and second solutions are mixed to allow the hydroxyl groups in the first solution to undergo an aldol polymerization reaction with the aldehyde groups in the second solution, forming a wet gel with a network structure. The wet gel is then frozen, causing the solvent to solidify and forming a cryogel. The solidified solvent is then dried to sublimate, thereby obtaining an aerogel material with a porous structure. Therefore, the aerogel material preparation process is simple and low-cost. By controlling the polymerization reaction of hydroxyl and aldehyde groups, and combining the freezing of the solvent during freezing with the sublimation of the solidified solvent during drying, an aerogel material with a porous structure is formed, exhibiting excellent gas adsorption performance. Attached Figure Description
[0028] Figure 1 This is a flowchart of the aerogel material preparation method of the present invention;
[0029] Figure 2 This is the stress-strain curve of the aerogel material of the present invention under compression test;
[0030] Figure 3 This is an electron microscope image of the aerogel material obtained in the first embodiment of the aerogel material preparation method of the present invention;
[0031] Figure 4 This is an electron microscope image of the aerogel material obtained in the second embodiment of the aerogel material preparation method of the present invention;
[0032] Figure 5 This is an electron microscope image of the aerogel material obtained in the third embodiment of the aerogel material preparation method of the present invention;
[0033] Figure 6 This is an electron microscope image of the aerogel material obtained in the fourth embodiment of the aerogel material preparation method of the present invention;
[0034] Figure 7 This is an electron microscope image of the aerogel material obtained in the fifth embodiment of the aerogel material preparation method of the present invention;
[0035] Figure 8 The density and porosity of the aerogel materials in various embodiments of the present invention are illustrated. Detailed Implementation
[0036] As the background technology indicates, efficient gas filtration systems are crucial for increasing the output of semiconductor manufacturing facilities, reducing production costs, and minimizing equipment maintenance and downtime. Currently, traditional gas filtration methods mainly include cryogenic distillation, adsorption, and membrane separation. These methods generally suffer from high energy consumption, low efficiency, and the potential for secondary pollution. Although porous aerogel materials exhibit good particulate matter adsorption performance due to their high porosity and low density, current technologies have not yet enabled their efficient application in the field of gas filtration. Therefore, there is an urgent need to develop a novel, highly efficient aerogel material and its preparation method to meet the stringent gas purification requirements of the semiconductor manufacturing industry.
[0037] To address the aforementioned technical problems, the aerogel material preparation method provided in this invention involves dissolving a hydroxyl-containing polymer in a solvent to obtain a first solution, dissolving an aldehyde-containing crosslinking agent in a solvent to obtain a second solution, and mixing the first and second solutions to allow the hydroxyl groups in the first solution to undergo an aldol polymerization reaction with the aldehyde groups in the second solution to form a wet gel with a network structure. The wet gel is then frozen, causing the solvent to solidify and forming a cryogel. The solidified solvent is then dried to sublimate, thereby obtaining an aerogel material with a porous structure. Therefore, the aerogel material preparation process is simple and cost-effective. By controlling the polymerization reaction of hydroxyl and aldehyde groups, and combining the freezing of the solvent during freezing with the sublimation of the solidified solvent during drying, an aerogel material with a porous structure is formed, exhibiting excellent gas adsorption performance.
[0038] To make the above-mentioned objects, features and advantages of the embodiments of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0039] Accordingly, the present invention provides a method for preparing aerogel materials. For example... Figure 1 This is a flowchart of the preparation method of the aerogel material according to an embodiment of the present invention.
[0040] refer to Figure 1 Step S1: Dissolve the polymer material containing hydroxyl groups in a solvent to obtain a first solution.
[0041] A first solution is prepared by dissolving a hydroxyl-containing polymer material in a solvent, forming a homogeneous solution with polymers, which provides suitable reactants for the subsequent reaction with the second solution.
[0042] Specifically, the hydroxyl-containing polymeric materials include one or more of polyvinyl alcohol, chitosan, carboxymethyl cellulose, hydroxyethyl cellulose, polyethylene glycol, and polyvinylpyrrolidone. In this embodiment, using polyvinyl alcohol as the hydroxyl-containing polymeric material has the following advantages: First, polyvinyl alcohol has good water solubility, which makes it easy to prepare the first solution; second, the hydroxyl groups in polyvinyl alcohol have high activity, enabling subsequent reactions such as acetalization, which ensures effective reaction with the aldehyde crosslinking agent; third, polyvinyl alcohol has excellent physical and mechanical properties (such as high strength, high wear resistance, high elasticity, and good fatigue resistance), which helps to form a stable aerogel structure; in addition, polyvinyl alcohol has good chemical resistance and can resist the effects of weak acids and weak bases, which is important when adjusting the pH of the mixture of the first and second solutions; finally, the first solution has good stability at room temperature, which is beneficial for precise process control.
[0043] In this embodiment, the molecular weight of the polyvinyl alcohol is between 1,000 and 10,000. By setting the molecular weight of the polyvinyl alcohol to between 1,000 and 10,000, the polyvinyl alcohol maintains appropriate solubility and reactivity, which is beneficial for the subsequent formation of a gel with a porous network structure.
[0044] In this embodiment, the mass percentage of polyvinyl alcohol in the first solution is 1% to 10%. By maintaining the mass percentage of polyvinyl alcohol in the first solution at 1% to 10%, the first solution can undergo sufficient aldol polymerization with the aldehyde groups of the crosslinking agent in subsequent processes. This directly affects the porosity and density of the aerogel material, ultimately influencing its filtration performance.
[0045] In this embodiment, the step of dissolving the hydroxyl-containing polymer material in a solvent includes deionized water. Deionized water does not contain soluble salts and has very few impurity ions, exhibiting good stability in chemical reactions. In other embodiments, the step of dissolving the hydroxyl-containing polymer material in a solvent includes an organic solvent, such as ethanol.
[0046] In this embodiment, in the step of dissolving the hydroxyl-containing polymer material in the solvent, polyvinyl alcohol is swollen in deionized water, and the heating temperature is controlled within the range of 70°C to 150°C, with the dissolution time controlled within 0.5 hours to 6 hours. The dissolution process promotes the full dissolution of polyvinyl alcohol in the solvent by first swelling and then heating, thereby ensuring that the polymer chains are fully extended and uniformly dispersed in the first solution, thus preparing for the subsequent crosslinking reaction with the second solution.
[0047] It should be noted that in the step of dissolving hydroxyl-containing polymers in a solvent, it is necessary to ensure that the first solution is uniform and transparent, without any insoluble matter.
[0048] refer to Figure 1 In step S2, the crosslinking agent containing aldehyde groups is dissolved in a solvent to obtain a second solution.
[0049] A second solution is obtained by dissolving an aldehyde-containing crosslinking agent in a solvent, which provides reactants for the subsequent aldol polymerization reaction of the first and second solutions.
[0050] In this embodiment, the crosslinking agent containing aldehyde groups includes one or more combinations of glyoxal, glutaraldehyde, paraformaldehyde, terephthalaldehyde, 2,5-furandialdehyde, isophthalaldehyde, and o-phthalaldehyde.
[0051] In this embodiment, the step of dissolving the aldehyde-containing crosslinking agent in a solvent includes deionized water. Deionized water does not contain soluble salts and has very few impurity ions, exhibiting good stability in chemical reactions. In other embodiments, the step of dissolving the aldehyde-containing crosslinking agent in a solvent includes an organic solvent.
[0052] refer to Figure 1 In step S3, the first solution and the second solution are mixed to allow the hydroxyl groups in the first solution to undergo an aldol polymerization reaction with the aldehyde groups in the second solution, forming a wet gel with a network structure.
[0053] The first solution contains hydroxyl groups, and the second solution contains aldehyde groups. During the mixing of the first and second solutions, the hydroxyl groups in the first solution and the aldehyde groups in the second solution undergo an aldol polymerization reaction to form a wet gel with a network structure. This prepares the wet gel with the network structure for subsequent freezing and freezing, thereby forming a porous aerogel material with high porosity and excellent gas adsorption performance. This allows the aerogel material to achieve gas filtration through active adsorption.
[0054] In this embodiment, during the step of mixing the first solution and the second solution, the pH value of the mixed solution is adjusted to acidic.
[0055] Adjusting the pH of the mixed solution to acidic conditions creates an acidic environment that promotes the full aldol polymerization reaction of hydroxyl and aldehyde groups in the mixed solution, thereby improving the formation quality of the aerogel network structure.
[0056] In this embodiment, the step of adjusting the pH of the mixed solution to acidic is carried out using an acidic solution to adjust the pH to 1.99 to 2.01. If the pH of the mixed solution is too low, although it may accelerate the aldol polymerization reaction, it can lead to excessively rapid cross-linking in certain areas of the mixed solution, forming an uneven gel network and creating structural defects, such as uneven pore size distribution or locally dense regions. This uneven structure is prone to stress during the drying process, leading to cracks or structural collapse and reducing porosity. If the pH of the mixed solution is too high, it may cause a decrease in the reaction rate or even incomplete reaction. Incomplete reaction may result in insufficient molecular weight of the prepolymer, leading to insufficient structural strength of the wet gel, making it prone to collapse and affecting the formation of aerogel during the subsequent drying process.
[0057] In this embodiment, the step of adjusting the pH of the mixed solution to acidic is carried out using hydrochloric acid with a mass fraction of 35% to 36%. If the mass fraction of the acidic solution is too high, the hydrochloric acid will evaporate too quickly, leading to large pH fluctuations during the aldol polymerization reaction and causing the porous structure of the aerogel material to easily collapse. If the mass fraction of the acidic solution is too low, more hydrochloric acid will be needed to achieve a suitable pH value, increasing costs and making it easier to introduce impurities, resulting in insufficient porosity of the aerogel, decreased mechanical strength, and impaired filtration performance.
[0058] In this embodiment, the step of mixing the first solution and the second solution includes: stirring the first solution and the second solution with a magnetic stirrer; after the first solution and the second solution are mixed evenly, placing the mixed solution in a constant temperature device for cross-linking aging.
[0059] The first and second solutions were stirred using a magnetic stirrer to allow the hydroxyl groups in the polyvinyl alcohol solution to come into full contact with the aldehyde groups in the crosslinking agent solution and undergo an aldol polymerization reaction, thereby promoting the formation of wet gel. This prepares the material for subsequent freeze-drying to prepare porous aerogel materials and helps improve the quality of porous aerogel materials.
[0060] The cross-linking and aging of hydroxyl and aldehyde groups under isothermal conditions ensures the full progress of the aldol polymerization reaction and achieves precise control of the reaction process, thereby forming a wet gel with a network structure. This prepares the material for the subsequent preparation of aerogel materials with a porous structure, which is beneficial for obtaining aerogel materials with excellent filtration and mechanical properties.
[0061] In this embodiment, the temperature control device includes a water bath. The water bath is equipped with a temperature control system, which can precisely control the temperature of the mixed solution during the crosslinking and aging process. Furthermore, the water bath uses water as the heating medium, which can evenly distribute heat, ensuring uniform heating of the mixed solution. This is crucial for the stable temperature and uniform heating conditions required in the crosslinking and aging reaction.
[0062] Specifically, the aging temperature is 25°C to 70°C, and the aging time is preferably 1 hour (h) to 24 hours (h).
[0063] In the step of mixing the first solution with the second solution, the number of hydroxyl groups in the mixed solution is much greater than the number of aldehyde groups, and the hydroxyl functional groups in the mixed solution are in a state of significant excess.
[0064] The number of hydroxyl groups in the mixed solution is much greater than the number of aldehyde groups. By controlling the ratio of hydroxyl to aldehyde groups, polyvinyl alcohol becomes the main skeleton, thereby forming a wet gel with a network structure during the aldol polymerization reaction. Then, through the subsequent freeze-drying process, a porous structure with high porosity is formed. Therefore, the aerogel material has both excellent gas adsorption performance and good mechanical properties, so that the final aerogel material can meet the application requirements of gas filtration in semiconductor cleanrooms.
[0065] refer to Figure 1 Step S4: Freeze the wet gel to form a cryogel, wherein the solvent in the cryogel is solid.
[0066] Freezing wet gels to form cryogels transforms the solvent into a solid state, thereby creating a stable ice crystal structure. This provides the necessary preconditions for the subsequent sublimation process, thus maintaining the porous network structure of the material during sublimation. The resulting aerogel material has ideal porosity and density, improving filtration performance and facilitating efficient filtration of micron-sized particles.
[0067] In this embodiment, the step of freezing the wet gel includes freezing the wet gel at a temperature below -20°C or in a liquid nitrogen environment.
[0068] The wet gel is frozen at a temperature below -20°C or in a liquid nitrogen environment, so that the solvent in the wet gel can be completely converted into a solid state. This prepares the material for subsequent drying of the frozen gel, which sublimates the solid solvent to obtain an aerogel material with a micro-nano porous structure.
[0069] It should be noted that freezing at temperatures below -20°C requires a longer freezing time, such as 48 hours; however, liquid nitrogen can achieve rapid freezing. During the freezing process, the completion of the freezing process can be determined by observing the gel change from a soft state to a hard state.
[0070] It should also be noted that during the freezing process of the wet gel, the solvent (deionized water) in the wet gel turns into ice crystals. The size and distribution of these ice crystals directly affect the final pore size and distribution. In the subsequent drying stage, the ice crystals are directly sublimated, leaving the desired pore structure.
[0071] refer to Figure 1 Step S5: Dry the cryogel to sublimate the solid solvent and obtain an aerogel material with a porous structure.
[0072] By sublimating a solid solvent to form a porous structure, the final aerogel material achieves high porosity and low density, enabling efficient adsorption and removal of microparticles and other impurities in gases. This allows the aerogel material to meet the stringent requirements of gas filtration in semiconductor cleanrooms, thus improving gas purification efficiency in semiconductor manufacturing. Therefore, the aerogel material preparation process is simple and cost-effective. By controlling the polymerization reaction of hydroxyl and aldehyde groups, combined with the freezing of the solvent during the freezing process and the sublimation during the drying process, aerogel materials with micro / nanoporous structures can be formed, exhibiting excellent gas adsorption performance.
[0073] In this embodiment, the drying process of the cryogel involves a process temperature of -70°C to -40°C, a vacuum degree of 1 Pa to 10 Pa, and a drying time of 12 hours to 96 hours.
[0074] In the preparation of aerogel materials, the process parameters of the drying step are crucial for obtaining high-performance aerogel materials. By controlling the process temperature within the range of -70℃ to -40℃ and performing drying treatment for 12 to 96 hours under a high vacuum environment of 1 Pa to 10 Pa, the solid solvent is ensured to fully sublimate, thereby forming an aerogel material with a micro-nano porous structure. This enables efficient adsorption and filtration of microparticles in the gas, providing a reliable gas purification solution for semiconductor manufacturing processes.
[0075] refer to Figure 2 , Figure 2 This is the stress-strain curve of the aerogel material of the present invention under compression test. When the thickness of the aerogel material is 10 mm, it can withstand a pressure of not less than 3.5 kPa without collapsing or cracking.
[0076] In this embodiment, during the drying step of the cryogel, the porosity of the aerogel material is greater than or equal to 85% and less than 97%, achieving a good balance between mechanical properties and filtration efficiency. If the porosity of the aerogel material is too high, the three-dimensional network structure of the aerogel material becomes too loose, leading to a significant decrease in mechanical properties. During actual use, it cannot withstand the impact of gas and is prone to structural defects such as collapse and cracks. Simultaneously, while excessively high porosity provides more adsorption sites, it can negatively impact the overall stability and service life of the aerogel material, reducing the filtration effect. If the porosity of the aerogel material is too low, the density of the aerogel material is likely to be too high, resulting in a reduced number of sites for adsorbing gaseous impurities and poor filtration performance.
[0077] In this embodiment, during the drying step of the cryogel, the density of the aerogel material is less than 60 kg / m³. 3 The density of aerogel materials is less than 60 kg / m³. 3 This gives aerogel materials a large specific surface area and high porosity, enabling them to effectively adsorb particulate matter in the air, such as PM2.5 and dust, thereby improving the efficiency of gas filtration.
[0078] In this embodiment, during the drying step of the cryogel, the pore size of the aerogel material is between 0.4 μm and 1.5 μm. If the pore size of the aerogel material is too large, the three-dimensional network structure of the aerogel material will become too loose, leading to a significant decrease in mechanical properties and making it prone to structural defects such as collapse and cracks during actual use. Simultaneously, while excessively high porosity provides more adsorption sites, it can negatively impact the overall stability and lifespan of the aerogel material, reducing the filtration efficiency. If the pore size of the aerogel material is too small, the density of the aerogel material will be too high, resulting in a reduced number of sites for adsorbing gaseous impurities and poor filtration performance.
[0079] It should be noted that, in the step of drying the cryogel, the porosity of the aerogel material is greater than or equal to 85% and less than 97%, the pore size of the aerogel material is 0.4 μm to 1.5 μm, and the density of the aerogel material is less than 60 kg / m³. 3 When the thickness of the aerogel material is 10 mm, the aerogel material has a filtration efficiency of not less than 97% for particles with a diameter greater than 0.5 μm, and can withstand a pressure of not less than 3.5 kPa without collapsing or cracking. When two 10 mm thick aerogel materials are stacked, the filtration efficiency for particles with a diameter greater than 0.5 μm is 99%.
[0080] It should be noted that the density and porosity of aerogel can be controlled by adjusting the ratio of crosslinking agent and the concentration of polyvinyl alcohol.
[0081] It should also be noted that during the drying process of the cryogel, the ice crystals in the cryogel are directly sublimated through sublimation, leaving the desired pore structure.
[0082] The first embodiment of the method for preparing aerogel materials proposed in this invention is as follows:
[0083] Step one involves dissolving the hydroxyl-containing polymer material in a solvent to obtain a first solution. Specifically, polyvinyl alcohol is dissolved in deionized water to obtain a 10% (w / w) polyvinyl alcohol aqueous solution.
[0084] Step two involves dissolving the aldehyde-containing crosslinking agent in a solvent to obtain a second solution. Specifically, a standard solution of the crosslinking agent is prepared by dissolving 0.67 g of terephthalaldehyde and 0.29 g of glyoxal in 100 g of deionized water. This step provides a suitable concentration of aldehyde groups for the subsequent aldol polymerization reaction by precisely controlling the amount and concentration of the crosslinking agent. Preparing a standard solution facilitates accurate control of the amount of crosslinking agent added later.
[0085] Step three involves mixing the first solution with the second solution. Specifically, 30g of a 10% (w / w) polyvinyl alcohol aqueous solution and 8.52g of the crosslinking agent standard solution prepared in step two are mixed in a specific ratio, and 52.96g of deionized water is added to adjust the final mixed solution to a polyvinyl alcohol content of 3%. This step controls the concentration of polyvinyl alcohol to ensure the formation of the network structure subsequently. It should be noted that polyvinyl alcohol, as the main backbone structure, needs to be maintained in excess to ensure that the abundant hydroxyl groups on its molecular chain can fully participate in the subsequent crosslinking reaction.
[0086] The pH of the mixed solution is precisely adjusted to 1.99 to 2.01 using 35% to 36% hydrochloric acid. This step aims to create the most suitable acidic environment for the aldol polymerization reaction, ensuring that polyvinyl alcohol and the crosslinking agent can react fully. Precise pH control has a significant impact on the extent of the reaction.
[0087] The mixed solution was subjected to cross-linking aging in a 50°C water bath for 2 hours. This step, by controlling the temperature and time parameters, promoted the full cross-linking reaction between hydroxyl and aldehyde groups, forming a wet gel with a network structure. Temperature control has a significant impact on the completeness of the reaction.
[0088] Step four involves freezing the prepared wet gel at below -20°C for 48 hours to allow the water molecules to form ice crystals. This step, by controlling the freezing temperature and time, ensures the orderly crystallization of water molecules, laying the foundation for the subsequent formation of micro / nano porous structures. The freezing process must ensure that the water is completely converted to a solid state.
[0089] Step five involves drying the prepared cryogel at -50°C and a vacuum of 1 Pa for 48 hours, allowing the solvent to sublimate and form a micro / nano porous structure. This step ensures complete sublimation of water molecules by strictly controlling the temperature, vacuum, and time parameters, thereby forming the desired porous structure within the material. High vacuum conditions are essential for achieving water molecule sublimation.
[0090] The first embodiment of the aerogel material preparation method yields an aerogel material with an interpenetrating network three-dimensional structure, a density of 40.91 kg / m³, and a porosity as high as 96.93%. This structural feature gives the material excellent gas filtration performance. The prepared aerogel material has a pore size distribution in the range of 0.4 μm to 1.5 μm, and can effectively filter particles with a particle size greater than 0.5 μm.
[0091] refer to Figure 3 This is a cross-sectional scanning electron microscope image of a porous aerogel material obtained according to the first embodiment of the aerogel material preparation method.
[0092] The present invention also proposes a second embodiment of the method for preparing aerogel materials. The similarities between the second embodiment and the first embodiment are not repeated here; the differences are as follows:
[0093] In step three, take 40g of the 10% polyvinyl alcohol aqueous solution prepared in step one of the first embodiment, take 37.28g of the prepared deionized water, and take 11.36g of the terephthalaldehyde standard solution and glyoxal standard solution prepared in step two of the first embodiment, and mix the three together.
[0094] The second embodiment of the aerogel material preparation method yields an aerogel material with an interpenetrating network three-dimensional structure and a density of 63.51 kg / m³. 3 The porosity is as high as 91.25%. This structural feature gives the material excellent gas filtration performance. The prepared aerogel material has a pore size distribution in the range of 0.4 μm-1.5 μm, and can effectively filter particles with a particle size greater than 0.5 μm.
[0095] refer to Figure 4 This is a cross-sectional scanning electron microscope image of a porous aerogel material obtained according to the second embodiment of the aerogel material preparation method.
[0096] This invention also proposes a third embodiment of the method for preparing aerogel materials. The similarities between the third embodiment and the first embodiment are not repeated here; the differences are as follows:
[0097] In step three, take 50g of the 10% polyvinyl alcohol aqueous solution from step one of the first embodiment, take 21.6g of deionized water, and take 14.2g of the terephthalaldehyde standard solution and glyoxal standard solution from step two of the first embodiment, and mix the three together.
[0098] The aerogel material prepared in the third embodiment of the preparation method has an interpenetrating network three-dimensional structure and a density of 70.52 kg / m³. 3 The porosity is as high as 88.31%. This structural feature gives the material excellent gas filtration performance. The prepared aerogel material has a pore size distribution in the range of 0.4 μm-1.5 μm, and can effectively filter particles with a particle size greater than 0.5 μm.
[0099] refer to Figure 5 This is a cross-sectional scanning electron microscope image of a porous aerogel material obtained according to the third embodiment of the aerogel material preparation method.
[0100] This invention also proposes a fourth embodiment of the method for preparing aerogel materials. The similarities between the fourth embodiment and the first embodiment are not repeated here; the differences are as follows:
[0101] Step 2: Dissolve 0.62g of 2,5-furandicarboxaldehyde in 100g of deionized water to prepare a crosslinking agent standard solution.
[0102] Step 3: Take 30g of the 10% polyvinyl alcohol aqueous solution prepared in Step 1 of the first embodiment, take 52.95g of the prepared deionized water, and take 17.05g of the standard solution from Step 2 of this embodiment, and mix the three together.
[0103] The fourth embodiment of the preparation method for the aerogel material yields an aerogel material with an interpenetrating network three-dimensional structure and a density of 50.72 kg / m³. 3 The porosity is as high as 94.87%. This structural feature gives the material excellent gas filtration performance. The prepared aerogel material has a pore size distribution in the range of 0.4 μm-1.5 μm, and can effectively filter particles with a particle size greater than 0.5 μm.
[0104] refer to Figure 6 This is a cross-sectional scanning electron microscope image of a porous aerogel material obtained according to the fourth embodiment of the aerogel material preparation method.
[0105] This invention also proposes a fifth embodiment of the method for preparing aerogel materials. The similarities between the fifth embodiment and the first embodiment will not be repeated here; the differences are as follows:
[0106] Step 2: Dissolve 0.62g of 2,5-furandicarboxaldehyde in 100g of deionized water to prepare a crosslinking agent standard solution.
[0107] Step 3: Take 30g of the 10% polyvinyl alcohol aqueous solution from Step 1 in the first embodiment, 42.8g of deionized water, and 34.10g of the standard solution from Step 2 in this embodiment, and mix the three together.
[0108] The fifth embodiment of the preparation method for the aerogel material yields an aerogel material with an interpenetrating network three-dimensional structure and a density of 74.09 kg / m³. 3 The porosity is as high as 85.38%. This structural feature gives the material excellent gas filtration performance. The prepared aerogel material has a pore size distribution in the range of 0.4 μm-1.5 μm, and can effectively filter particles with a particle size greater than 0.5 μm.
[0109] refer to Figure 7 This is a cross-sectional scanning electron microscope image of a porous aerogel material obtained according to the fifth embodiment of the aerogel material preparation method.
[0110] refer to Figures 3 to 5 Furthermore, based on the first, second, and third embodiments of the aerogel material preparation method, it can be seen that micro-nano-scale porous aerogel structures can be obtained. Moreover, within a reasonable range, the porosity of the aerogel material decreases as the concentration of polyvinyl alcohol in the first solution increases.
[0111] refer to Figures 6 to 7 Furthermore, in conjunction with the fourth and fifth embodiments of the preparation method of aerogel materials, it can be seen that micro-nano-scale porous aerogel structures can be obtained. Moreover, within a reasonable range, as the concentration of crosslinking agent increases, the porosity of the aerogel decreases and the pore size distribution becomes more uniform.
[0112] refer to Figure 8 , Figure 8 The relationship between the density and porosity of aerogel materials is illustrated. Five embodiments of aerogel material preparation methods demonstrate that by adjusting the concentration of polyvinyl alcohol in the first solution and the type and proportion of the crosslinking agent, porous aerogel structures with different densities and porosities can be obtained. Therefore, this invention demonstrates that, through proper design, high-porosity porous aerogel structures can be prepared.
[0113] This invention also provides an aerogel material. The aerogel material comprises a porous structure, wherein the pores in the porous structure are interconnected and form a network structure; the porosity of the aerogel material is greater than or equal to 85% and less than 97%.
[0114] The aerogel material provided in this embodiment of the invention is formed using the aforementioned aerogel material preparation method. Therefore, the aerogel material preparation process is simple and the preparation cost is low. By controlling the polymerization reaction of hydroxyl and aldehyde groups, combined with the freezing of the solvent during the freezing process and the sublimation during the drying process, an aerogel material with a porous structure can be formed, which has excellent gas adsorption performance.
[0115] In this embodiment, when the thickness of the aerogel material is 10 mm, it can withstand a pressure of not less than 3.5 kPa without collapsing or cracking.
[0116] In this embodiment, the porosity of the aerogel material is greater than or equal to 85% and less than 97%, achieving a good balance between mechanical properties and filtration efficiency. If the porosity of the aerogel material is too high, the three-dimensional network structure of the aerogel material will become too loose, leading to a significant decrease in mechanical properties and making it prone to structural defects such as collapse and cracks during actual use. Simultaneously, while excessively high porosity provides more adsorption sites, it can negatively impact the overall stability and lifespan of the aerogel material, reducing the filtration effect. If the porosity of the aerogel material is too low, the density of the aerogel material will be too high, resulting in a reduced number of sites for adsorbing gaseous impurities and poor filtration performance.
[0117] In this embodiment, the density of the aerogel material is less than 60 kg / m³. 3 The density of aerogel materials is less than 60 kg / m³. 3 This gives aerogel materials a large specific surface area and high porosity, enabling them to effectively adsorb particulate matter in the air, such as PM2.5 and dust, thereby improving the efficiency of gas filtration.
[0118] In this embodiment, the pore size of the aerogel material is between 0.4 μm and 1.5 μm. If the pore size of the aerogel material is too large, the three-dimensional network structure of the aerogel material will become too loose, resulting in a significant decrease in mechanical properties and making it prone to structural defects such as collapse and cracks during actual use. Simultaneously, while excessively high porosity provides more adsorption sites, it can negatively impact the overall stability and lifespan of the aerogel material, reducing its filtration efficiency. If the pore size of the aerogel material is too small, the density of the aerogel material will be too high, leading to a reduction in the number of sites available for adsorbing gaseous impurities and poor filtration performance.
[0119] It should be noted that the porosity of the aerogel material is greater than or equal to 85% and less than 97%, the pore size of the aerogel material is 0.4 μm to 1.5 μm, and the density of the aerogel material is less than 60 kg / m³. 3Furthermore, when the thickness of the aerogel material is 10 mm, the filtration rate of the aerogel material for particles with a diameter greater than 0.5 μm is not less than 97%, and it can withstand a pressure of not less than 3.5 kPa without collapsing or cracking. When two 10 mm thick aerogel materials are stacked, the filtration rate for particles with a diameter greater than 0.5 μm is not less than 99%.
[0120] This invention also provides a semiconductor device for use in a cleanroom, wherein the semiconductor device employs the aforementioned aerogel material.
[0121] By employing the aforementioned aerogel material in semiconductor equipment, the problem of particulate contamination in cleanrooms can be effectively solved. Due to its high porosity and excellent gas adsorption properties, this aerogel material can achieve highly efficient filtration of particles larger than 0.5 μm, thereby preventing tiny particles from disrupting electron flow and causing chip performance issues. This significantly improves product yield, makes the production process more reliable and stable, and helps reduce production costs and equipment maintenance time.
[0122] Furthermore, because the porosity of aerogel materials is greater than or equal to 85% and less than 97%, the density of aerogel materials is less than 60 kg / m³. 3 This allows the aerogel material, with a thickness of 10 mm, to withstand a pressure of no less than 3.5 kPa without collapsing or cracking. This gives the aerogel material excellent mechanical properties and ensures that the material structure remains stable during gas impact, thereby maintaining the continuous filtration effect of semiconductor devices.
[0123] The aerogel material described in this embodiment can be formed using the formation method described in the foregoing embodiments, or it can be formed using other formation methods. For a detailed description of the aerogel material described in this embodiment, please refer to the corresponding descriptions in the foregoing embodiments; these descriptions will not be repeated here.
[0124] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method of making an aerogel material, characterized by, The application relates to a preparation method of a hydrogel and an aerogel material. The method comprises the following steps: dissolving a high-molecular material containing hydroxyl groups in a solvent to obtain a first solution; dissolving a crosslinking agent containing aldehyde groups in a solvent to obtain a second solution; mixing the first solution and the second solution, so that the hydroxyl groups in the first solution and the aldehyde groups in the second solution undergo an aldol polymerization reaction to form a wet gel with a network structure; freezing the wet gel to form a frozen gel, wherein the solvent in the frozen gel is in a solid state; and drying the frozen gel to sublimate the solvent in a solid state, so that an aerogel material with a porous structure is obtained. The high-molecular material containing hydroxyl groups comprises one or more of polyvinyl alcohol, chitosan, carboxymethyl cellulose, hydroxyethyl cellulose, polyethylene glycol and polyvinylpyrrolidone. In the step of dissolving the high-molecular material containing hydroxyl groups in a solvent, the solvent comprises deionized water or an organic solvent. In the step of dissolving the crosslinking agent containing aldehyde groups in a solvent, the solvent comprises deionized water or an organic solvent. The crosslinking agent containing aldehyde groups comprises a combination of one or more of glyoxal, glutaraldehyde, paraformaldehyde, p-phenylenedimethylaldehyde, 2,5-furandimethylaldehyde, m-phenylenedimethylaldehyde and o-phenylenedimethylaldehyde.
2. The production method according to claim 1, wherein In the step of mixing the first solution and the second solution, the pH value of the mixed solution is adjusted to be acidic.
3. The production method according to claim 1, wherein In the step of adjusting the pH value of the mixed solution to be acidic, an acidic solution is used to adjust the pH value of the mixed solution to 1.99-2.
01. In the step of adjusting the pH value of the mixed solution to be acidic, the acidic solution is hydrochloric acid with a mass fraction of 35%-36%.
4. The production method according to claim 1, wherein The step of mixing the first solution and the second solution comprises the following steps:
5. The production method according to claim 1, wherein The first solution and the second solution are stirred by using a magnetic stirrer.
6. The production method according to claim 5, wherein After the first solution and the second solution are uniformly mixed, the mixed solution is placed in a constant-temperature device for crosslinking aging.
7. The production method according to claim 6, wherein In the step of freezing the wet gel, the wet gel is frozen at a temperature lower than-20 DEG C or in a liquid nitrogen environment.
8. The production method according to claim 1, wherein In the step of drying the frozen gel, the process temperature is-70 DEG C to-40 DEG C, the vacuum degree is 1 Pa to 10 Pa, and the drying time is 12 hours to 96 hours. In the step of drying the frozen gel, the porosity of the aerogel material is greater than or equal to 85% and less than 97%. In the step of drying the frozen gel, the pore size of the aerogel material is 0.4 mu m to 1.5 mu m.
9. The production method according to claim 1, wherein When the thickness of the aerogel material is 10 mm, the aerogel material can withstand a pressure of not less than 3.5 kPa without collapsing and cracking, and the filtration rate of the aerogel material to particles with a particle size greater than 0.5 mu m is not less than 97%.
10. The production method according to claim 1, wherein In the step of mixing the first solution and the second solution, the number of hydroxyl groups in the mixed solution is greater than the number of aldehyde groups.
11. The production method according to claim 1, wherein The aerogel material comprises a porous structure, and the pores in the porous structure are mutually penetrated and communicated, forming a network structure.
12. The production method according to claim 1, wherein The porosity of the aerogel material is greater than or equal to 85% and less 97%.
13. The production method according to claim 1, wherein The density of the aerogel material is less than 60 kg / m 3 .
14. The production method according to claim 1, wherein The pore size of the aerogel material is 0.4 mu m to 1. 5 mu m.
15. The production method according to claim 1, wherein 16. An aerogel material characterized in that, 17. The aerogel material of claim 16, wherein, The aerogel material has a density of less than 60 kg / m 3 .
18. The aerogel material of claim 16, wherein, 19. The aerogel material of claim 16, wherein, The aerogel material can withstand a pressure of not less than 3.5 kPa without collapsing and cracking when the thickness of the aerogel material is 10 mm, and the filtration rate of the aerogel material for particles with a particle size greater than 0.5 μm is not less than 97%.
20. A semiconductor device, comprising: The aerogel material according to any one of claims 16 to 19 is used in a clean room for purifying.