Method for synthesizing different morphology Ce-Ti materials in a rotary oven and application thereof

By controlling the morphology of Ce–Ti materials using a rotating oven method, the problems of complex processes and poor morphology controllability in existing technologies have been solved, achieving high oxygen vacancy concentration and excellent catalytic activity, which is suitable for VOCs catalytic oxidation and exhaust gas purification.

CN123148951APending Publication Date: 2026-11-24JIANGSU FUCHENG ENVIRONMENTAL PROTECTION NEW MATERIAL RES CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611273985.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing methods for synthesizing Ce–Ti materials suffer from complex processes, difficulties in scaling up, and poor morphological controllability, making it difficult to meet the needs of practical industrial applications.

Method used

Ce–Ti materials with different morphologies, including nanorods and cubic structures, were synthesized by using a rotary oven method and by controlling the rotation speed, temperature, and atmosphere. The materials showed significantly better performance than ordinary Ce–Ti in terms of high oxygen vacancy concentration and catalytic activity.

Benefits of technology

It achieves high oxygen vacancy concentration and excellent catalytic activity in Ce–Ti materials, making them suitable for VOCs catalytic oxidation and exhaust gas purification, with the advantages of simple process, inexpensive raw materials, and suitability for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148951A_ABST
    Figure CN123148951A_ABST
Patent Text Reader

Abstract

This invention relates to a method for synthesizing Ce-Ti materials with different morphologies using a rotary oven and their applications. The method includes: dissolving a cerium source and a titanium source in a water or alcohol solution, reacting them in a rotary oven under set temperature, rotation speed, and atmosphere conditions, followed by drying and calcination to obtain Ce-Ti materials with different morphologies. By adjusting the process conditions, nanorods, cubic structures, etc., can be obtained; these materials have large specific surface areas and high oxygen vacancy concentrations, exhibiting excellent catalytic activity and stability. The Ce-Ti materials can be widely used in the catalytic oxidation of volatile organic compounds and the removal of nitrogen oxides. This invention features a simple process, low cost, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of inorganic functional material preparation, and in particular to a process for synthesizing cerium-titanium composite oxides with different morphologies by controlling reaction conditions using a rotary oven, and its application in catalysis and environmental remediation. Background Technology

[0002] Cerium oxide (CeO2) is widely used in automotive exhaust purification, catalytic oxidation of volatile organic compounds (VOCs), and fuel cells due to its excellent oxygen storage / release capabilities. However, CeO2 tends to agglomerate at high temperatures, leading to a decrease in specific surface area and reduced activity. Titanium oxide (TiO2), on the other hand, is an important environmental and energy material due to its chemical stability and photocatalytic properties. Studies have shown that the composite of Ce and Ti can improve the thermal stability of CeO2, regulate oxygen vacancy concentration, and optimize the band structure, thereby enhancing its catalytic performance. Existing methods for synthesizing Ce–Ti materials mainly include sol-gel methods, hydrothermal methods, and coprecipitation methods. However, these methods suffer from complex processes, difficulties in scaling up, and poor morphology controllability, making it difficult to meet the needs of practical industrial applications. Therefore, developing a scalable and morphology-controllable Ce–Ti synthesis method has become an urgent technical problem to be solved. Summary of the Invention

[0003] The purpose of this invention is to provide a method for synthesizing Ce-Ti materials with different morphologies using a rotary oven. By controlling the rotation speed, temperature distribution, and atmospheric environment, the method enables the controllable synthesis of various morphologies such as nanorods and cubic structures. The resulting materials exhibit high oxygen vacancy concentrations, excellent catalytic activity, and stability, making them suitable for applications such as VOCs catalytic oxidation and exhaust gas purification.

[0004] To achieve the above objectives, the present invention can adopt the following technical solutions: Using cerium nitrate, cerium oxalate, or cerium acetate as the cerium source and tetrabutyl titanate, tetraisopropyl titanate, or titanium sulfate as the titanium source, the molar ratio is adjusted, and the resulting mixture is placed in a rotary oven. The rotation speed (5–100 rpm), temperature (80–200 °C), and atmosphere (air, oxygen, or nitrogen) are set, and the reaction is carried out for 12–24 h. After cooling, filtration, and drying, the mixture is calcined at 300–700 °C for 3–6 h to obtain Ce–Ti materials with different morphologies.

[0005] The beneficial effects of this invention include: (1) The process of this invention is simple, the raw materials are inexpensive, and it is suitable for large-scale production; (2) By adjusting the parameters of the rotary oven and the ratio of precursors, various morphologies of Ce–Ti can be achieved. (3) The obtained Ce–Ti material has a high oxygen vacancy concentration and its catalytic activity is significantly better than that of ordinary Ce–Ti; (4) The material exhibits excellent performance in VOCs catalytic oxidation and NOx removal. Attached Figure Description

[0006] Figure 1 SEM images of Ce–Ti: (a) R-Ce 0.8 Ti 0.2 O2、(b)C-Ce 0.8 Ti 0.2 O2、(c)R / X-Ce 0.8 Ti 0.2 O2、(d)C / X-Ce 0.8 Ti 0.2 O2); Figure 2 Conversion efficiency curves of Ce–Ti materials in the toluene oxidation reaction; Figure 3 Conversion efficiency curves of Ce–Ti materials in NOx oxidation reaction; Figure 4 Comparison of oxygen vacancy concentrations in Ce–Ti with different morphologies. Detailed Implementation

[0007] The embodiments described are provided to better illustrate the present invention, but are not intended to limit the scope of the invention to the embodiments described. Therefore, non-essential improvements and adjustments made to the embodiments by those skilled in the art based on the above description are still within the scope of protection of the present invention.

[0008] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit this disclosure. Singular expressions include plural expressions unless they have a distinct meaning in the context. As used herein, it should be understood that terms such as “comprising,” “having,” “including,” are intended to indicate the presence of features, numbers, operations, components, parts, elements, materials, or combinations thereof. The terminology of the invention is disclosed in the specification and is not intended to exclude the possibility that one or more other features, numbers, operations, components, parts, elements, materials, or combinations thereof may be present or added. As used herein, “ / ” may be interpreted as “and” or “or,” depending on the context.

[0009] This invention provides a method for synthesizing Ce-Ti materials with different morphologies using a rotary oven. The preparation method includes: using cerium nitrate, cerium oxalate, or cerium acetate as a cerium source, and tetrabutyl titanate, tetraisopropyl titanate, or titanium sulfate as a titanium source, dissolving them in water or an alcohol solvent, stirring evenly, and then placing them in a rotary oven. The reaction is carried out in a temperature range of 80 ℃-200 ℃, a rotation speed of 5-100 rpm, and an atmosphere of air, oxygen, or nitrogen. After drying and calcination at 300-700 ℃, Ce-Ti materials with different morphologies can be obtained.

[0010] It should be noted that, through extensive comparative experiments and characterization, this invention has revealed that the Ce–Ti materials synthesized by the rotary oven method exhibit significant morphology dependence in the catalytic oxidation reactions of VOCs and NOx. Specifically, the nanorod structure Ce–Ti synthesized by the rotary oven method possesses a higher specific surface area and oxygen vacancy concentration, resulting in higher exposure of reactive sites and superior catalytic performance for both VOCs and NOx.

[0011] In some specific embodiments, in the above-described method for preparing Ce–Ti materials, the cerium source is one of cerium nitrate, cerium oxalate, or cerium acetate. Cerium nitrate is preferred. The cerium source is one of tetrabutyl titanate, tetraisopropyl titanate, or titanium sulfate. Titanium sulfate is preferred.

[0012] I. Preparation of Doped Cobalt-Based Oxides

[0013] Example 1 Rod-shaped Ce-Ti was synthesized using a hydrothermal method. 38.4 g of sodium hydroxide was dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate was completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate was dissolved in 20 mL of distilled water to form solution C. Solutions B and C were added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D was added to a 200 °C reactor and reacted in a rotary oven at 100 °C and 50 rpm for 24 h to obtain the rod-shaped Ce-Ti precursor. This precursor was then calcined in a muffle furnace at 400 °C for 5 h at a heating rate of 5 °C / min to finally obtain rod-shaped Ce-Ti (R / X-Ce). 0.8 Ti 0.2 O2).

[0014] Example 2 Rod-shaped Ce-Ti was synthesized using a hydrothermal method. 38.4 g of sodium hydroxide was dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate was completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate was dissolved in 20 mL of distilled water to form solution C. Solutions B and C were added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D was added to a 200 mL reactor and reacted in a rotary oven at 180 ℃ and 50 rpm for 24 h to obtain a cubic Ce-Ti precursor. This precursor was then calcined in a muffle furnace at 400 ℃ for 5 h at a heating rate of 5 ℃ / min to finally obtain cubic Ce-Ti (C / X-Ce). 0.8 Ti 0.2 O2).

[0015] Comparative Example 1 Rod-shaped Ce-Ti was synthesized using a hydrothermal method. 38.4 g of sodium hydroxide was dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate was completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate was dissolved in 20 mL of distilled water to form solution C. Solutions B and C were added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D was added to a 200 °C reactor and reacted in a 100 °C oven for 24 h to obtain the rod-shaped Ce-Ti precursor. This precursor was then calcined in a muffle furnace at 400 °C for 5 h at a heating rate of 5 °C / min to finally obtain rod-shaped Ce-Ti (R-Ce). 0.8 Ti 0.2 O2).

[0016] Comparative Example 2 Rod-shaped Ce-Ti was synthesized using a hydrothermal method. 38.4 g of sodium hydroxide was dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate was completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate was dissolved in 20 mL of distilled water to form solution C. Solutions B and C were added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D was added to a 200 mL reactor and reacted in a conventional oven at 180 ℃ for 24 h to obtain a cubic Ce-Ti precursor. This precursor was then calcined in a muffle furnace at 400 ℃ for 5 h at a heating rate of 5 ℃ / min to finally obtain cubic Ce-Ti (C-Ce). 0.8 Ti 0.2 O2).

[0017] II. Morphology Testing of Doped Cobalt-Based Oxides

[0018] Example 3 like Figure 1 As shown, cerium titanium oxides prepared by different methods exhibit significant differences in morphology. Figure 1 (a) is a sample synthesized in a conventional oven, exhibiting an irregular rod-shaped structure with significant differences in length distribution and obvious agglomeration. Figure 1 (b) is another morphology synthesized in a conventional oven, mainly cubic in shape, with uneven particle size and disordered arrangement; Figure 1 (c) is the sample synthesized in a rotary oven. It has a uniformly distributed rod-shaped structure with a length of about 230 nm and a diameter of 10 nm. It has a regular morphology and good dispersibility. Figure 1 (d) shows a cubic sample synthesized in a rotary oven, exhibiting uniform particle morphology, clear edges and corners, and a more concentrated distribution. This demonstrates that cerium titanium oxide samples prepared in a rotary oven, whether rod-shaped or cubic, exhibit more uniform morphology and a more complete structure, while samples synthesized in a conventional oven suffer from irregular morphology and agglomeration.

[0019] III. Performance Testing of Doped Cobalt-Based Oxides

[0020] Example 4 The cerium titanium oxide (catalyst) prepared in Examples 1, 2, Comparative Example 1, and 2 was used to remove VOCs from the atmosphere. The main steps were as follows: 100 mg of the above catalysts (Examples 1, 2, Comparative Example 1, and Comparative Example 2) were weighed and placed in a quartz tube fixed-bed flow reactor (6 mm inner diameter), which was then placed in the center of a temperature-programmable tube furnace under atmospheric pressure. In the dry gas reaction, 100 mL / min of synthesis air (10 vol% O2 and N2) containing approximately 500 ppm toluene passed through the catalyst bed, and the gas hourly space velocity (GHSV) was 60,000 mL / g / h. The temperature programming was as follows: heating to each measurement temperature at a rate of 5 °C / min. The removal efficiency of the catalyst for toluene was investigated, and the results are as follows: Figure 1 As shown. The removal efficiencies of cerium titanium oxides with different morphologies for toluene, from highest to lowest (at the temperature at which removal efficiency reaches 90%), are as follows: R / X-Ce 0.8 Ti 0.2 O2>R-Ce 0.8 Ti 0.2 O2>C / X-Ce 0.8 Ti 0.2 O2>C-Ce 0.8 Ti 0.2 O2, R / X-Ce 0.8 Ti 0.2 O2-toluene T 90 It is 89.5%.

[0021] Example 5 The cerium titanium oxide (catalyst) prepared in Examples 1, 2, Comparative Example 1, and 2 was used to remove NOx from the atmosphere. The main steps are as follows: 100 mg of the above catalysts (Examples 1, 2, Comparative Example 1, and Comparative Example 2) were weighed and placed in a quartz tube fixed-bed flow reactor (6 mm inner diameter), which was then placed in the center of a temperature-programmable tube furnace under atmospheric pressure. In the dry gas reaction, 100 mL / min of synthesis air (10 vol% O2 and N2) containing approximately 500 ppm NOx passed through the catalyst bed, and the gas space-time velocity (GHSV) was 60,000 mL / g / h. The temperature programming was as follows: heating to each measurement temperature at a rate of 5 °C / min. The removal efficiency of the catalyst for toluene was investigated, and the results are as follows: Figure 1 As shown. The NOx removal efficiencies of cerium titanium oxides with different morphologies, from highest to lowest (at the temperature at which removal efficiency reaches 100%), are as follows: R / X-Ce 0.8 Ti 0.2 O2>R-Ce 0.8 Ti 0.2 O2>C / X-Ce 0.8 Ti 0.2 O2>C-Ce 0.8 Ti 0.2 O2, R / X-Ce 0.8 Ti 0.2 The removal efficiency of O2 for NOx is 100% at a temperature of 250 ℃.

[0022] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A method for synthesizing Ce-Ti materials with different morphologies using a rotary oven, characterized in that, The process includes the following steps: dissolving cerium salt and titanium salt in water or alcohol solution to obtain a precursor solution; placing the precursor in a rotary oven and reacting it under a set rotation speed, temperature, and atmosphere; and then drying and calcining it to obtain Ce-Ti materials with different morphologies. The rotary oven reaction conditions include reacting at 80-200℃ and a rotation speed of 5-100 rpm for 12-24 hours, and the calcination conditions include calcining at 300-700℃ for 3-6 hours.

2. The method according to claim 1, characterized in that, The cerium salt is selected from cerium nitrate, cerium oxalate or cerium acetate, and the titanium salt is selected from tetrabutyl titanate, tetraisopropyl titanate or titanium sulfate.

3. The Ce-Ti materials with different morphologies according to claim 2, characterized in that, The preferred cerium salt is cerium nitrate, and the preferred cerium salt is titanium sulfate.

4. The method according to claim 3, characterized in that, The rotary oven has a rotational speed of 5–80 rpm, a temperature of 80–200 ℃, and an atmosphere of air, oxygen, or nitrogen.

5. The method according to any one of claims 1–4, characterized in that, The process includes the following steps: Rod-shaped Ce-Ti is synthesized using a hydrothermal method. Sodium hydroxide is dissolved in distilled water to form solution A; cerium nitrate is completely dissolved in distilled water to form solution B; titanium sulfate is dissolved in distilled water to form solution C; solutions B and C are added to solution A and mixed thoroughly to form solution D. After stirring, solution D is added to a reaction vessel and reacted in a rotary oven at 100 °C and 50 rpm for 24 h to obtain the rod-shaped Ce-Ti precursor. This precursor is then calcined in a muffle furnace at 400 °C for 5 h at a heating rate of 5 °C / min to finally obtain rod-shaped Ce-Ti, i.e., R / X-Ce. 0.8 Ti 0.2 O2.

6. The method according to claim 5, characterized in that, The process includes the following steps: Rod-shaped Ce-Ti is synthesized using a hydrothermal method. 38.4 g of sodium hydroxide is dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate is completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate is dissolved in 20 mL of distilled water to form solution C; solutions B and C are added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D is added to a 200 °C reactor and reacted in a rotary oven at 100 °C and 50 rpm for 24 h to obtain the rod-shaped Ce-Ti precursor. This precursor is then calcined in a muffle furnace at 400 °C for 5 h at a heating rate of 5 °C / min to finally obtain rod-shaped Ce-Ti, i.e., R / X-Ce. 0.8 Ti 0.2 O2.

7. The method according to any one of claims 1–4, characterized in that, The process includes the following steps: Rod-shaped Ce-Ti is synthesized using a hydrothermal method. Sodium hydroxide is dissolved in distilled water to form solution A; cerium nitrate is completely dissolved in distilled water to form solution B; titanium sulfate is dissolved in distilled water to form solution C; solutions B and C are added to solution A and mixed thoroughly to form solution D. After stirring, solution D is added to a reaction vessel and reacted in a rotary oven at 180 °C and 50 rpm for 24 h to obtain a cubic Ce-Ti precursor. This precursor is then calcined in a muffle furnace at 400 °C for 5 h at a heating rate of 5 °C / min to finally obtain cubic Ce-Ti, i.e., C / X-Ce. 0.8 Ti 0.2 O2.

8. The method according to claim 7, characterized in that, The process includes the following steps: Rod-shaped Ce-Ti is synthesized using a hydrothermal method. 38.4 g of sodium hydroxide is dissolved in 100 mL of distilled water to form solution A; 3.47 g of cerium nitrate is completely dissolved in 20 mL of distilled water to form solution B; 0.6 g of titanium sulfate is dissolved in 20 mL of distilled water to form solution C; solutions B and C are added to solution A and mixed thoroughly to form solution D. After stirring for 30 min, solution D is added to a 200 mL reactor and reacted in a rotary oven at 180 ℃ and 50 rpm for 24 h to obtain a cubic Ce-Ti precursor. This precursor is then calcined in a muffle furnace at 400 ℃ for 5 h at a heating rate of 5 ℃ / min to finally obtain cubic Ce-Ti, i.e., C / X-Ce. 0.8 Ti 0.2 O2.

9. The Ce-Ti material prepared by the method according to any one of claims 1-8, characterized in that, Its shape is rod-shaped or cubic.

10. The application of the Ce-Ti material according to claim 9 in the catalytic oxidation of VOCs and removal of NOx.