A tin-containing spherical alumina carrier, a preparation method and application thereof

By forming a rough surface structure on the alumina support through weak acid etching and high-pressure spraying, combined with segmented calcination, the problem of tin enrichment and uniform distribution on the support surface is solved, thus achieving efficient catalyst preparation suitable for propane dehydrogenation and naphtha reforming.

CN123148952APending Publication Date: 2026-11-24SHENYANG SANJUKAITE CATALYST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611353954.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve tin enrichment, uniform loading, and excellent activity on the surface while maintaining high carrier strength, and the processes are complex and unsuitable for industrial mass production.

Method used

A weak acid etching process combined with high-pressure spraying was used to form a rough surface structure on the alumina carrier. The tin component was then uniformly attached to the carrier surface using high-pressure spraying technology. Combined with a segmented calcination process, a core-shell spherical alumina carrier was prepared.

Benefits of technology

This method achieves surface enrichment and uniform distribution of tin, improves the activity and stability of the catalyst, simplifies the process, reduces production costs, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148952A_ABST
    Figure CN123148952A_ABST
Patent Text Reader

Abstract

This invention relates to the field of catalyst support preparation technology, and discloses a tin-containing spherical alumina support, its preparation method, and its application. The preparation method of the tin-containing spherical alumina support of this invention includes the following steps: etching the alumina support and preparing a tin-containing acidic impregnation solution; high-pressure spraying the tin-containing acidic impregnation solution onto the etched alumina support; and drying and calcining the sprayed alumina support. This invention, through a combination of weak acid etching and high-pressure spraying, prepares a core-shell type spherical alumina support with a tin-enriched surface layer, which can inhibit the hydrolysis and agglomeration of tin salts, protect the internal framework of the support, and maintain the mechanical strength of the support. The process is simple and suitable for industrial production. Catalysts prepared using this support can be applied in propane dehydrogenation and naphtha reforming, exhibiting good catalytic effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst support preparation technology, specifically to a tin-containing spherical alumina support, its preparation method, and its application. Background Technology

[0002] Sn-containing spherical alumina supports (Sn / Al2O3) with a particle size of 1.6–1.8 mm are widely used as catalyst supports in moving bed reactors due to their good flowability and wear resistance, such as propane dehydrogenation catalysts and naphtha continuous reforming catalysts. Sn, as an important component, can effectively inhibit Pt particle sintering, reduce coking formation, and improve reaction selectivity. With increasingly stringent product quality requirements and continuous process improvements, higher demands are being placed on the stability and selectivity of catalysts.

[0003] Currently, the mainstream method for preparing uniformly spherical Sn / Al2O3 supports is the oil column forming method. The basic steps of this process are: reacting hydrochloric acid with aluminum powder to synthesize basic aluminum chloride sol; adding a tin source, such as SnCl2 or SnCl4, and thoroughly mixing it with a hexamethylenetetramine gelling agent solution; dripping the mixed sol into a hot oil column to form the support; and then aging, washing, drying, and calcining to finally obtain the spherical Sn / Al2O3 support. This method can achieve high dispersion of the tin source within the alumina framework and can prepare catalyst samples with excellent catalytic performance. However, this process has several inherent shortcomings that are difficult to overcome: First, the oil column forming process has stringent equipment requirements, necessitating a dedicated hot oil column spheroidizing device; the process flow is long, requiring sol preparation, drop spheroidizing, long-term aging, and multiple washing steps, resulting in a long production cycle and high overall energy consumption, which is not conducive to low-cost large-scale production. Second, tin salts are incorporated into the alumina framework in situ via the sol. During calcination, the decomposition of tin salts releases corrosive gases such as hydrogen chloride, which can erode the alumina framework and easily lead to a decrease in the mechanical strength of the support. Third, the active sites for reforming and dehydrogenation reactions are mainly concentrated on the outer surface of the catalyst particles. The oil column forming process encapsulates a large number of tin species in the core of the support particles. This internal tin is difficult to participate in the synergistic effect with platinum, resulting in a low effective utilization rate of tin additives.

[0004] Existing research indicates that if tin components can be concentrated in the surface region of spherical alumina supports, forming a core-shell distribution structure, it is beneficial to improve catalytic activity. Current technology employs an impregnation method to load Sn elements after alumina spherical formation, producing surface-enriched spherical Sn / Al2O3 supports. However, the conventional liquid-phase impregnation method, which involves immersing spherical alumina spheres in a tin-containing salt solution and relying on capillary adsorption to complete tin loading, also has significant drawbacks: tin salts are highly susceptible to hydrolysis, leading to tin species agglomeration and uneven local loading; the impregnation process is limited by pore adsorption, making it difficult to accurately achieve concentrated tin distribution on the outermost layer of the particles; and multiple impregnations are often required to achieve the target loading, resulting in poor process repeatability and low production efficiency.

[0005] Therefore, there is an urgent need to develop a method for preparing tin-loaded spherical alumina that can achieve tin enrichment on the surface, uniform loading, excellent activity, and simple process suitable for industrial mass production while maintaining the high strength of the carrier. Summary of the Invention

[0006] This invention provides a tin-supported spherical alumina, its preparation method, and its application. By combining weak acid etching with high-pressure spraying, a core-shell type spherical alumina support with tin component enriched on the surface can be prepared. This can inhibit the hydrolysis and agglomeration of tin salts, protect the internal framework of the support, and maintain the mechanical strength of the support. The process is simple and convenient for industrial production. The Pt-Sn / Al2O3 catalyst prepared with this support can be applied in the fields of propane dehydrogenation and naphtha reforming, with good catalytic effect.

[0007] In a first aspect, the present invention provides a method for preparing a tin-containing spherical alumina support, comprising the following steps: The alumina carrier was etched and a tin-containing acidic impregnation solution was prepared. A tin-containing acidic impregnation solution was high-pressure sprayed onto an etched alumina substrate; The sprayed alumina carrier is dried and calcined to obtain tin-containing spherical alumina carrier.

[0008] In one optional embodiment, the etching is performed using a weak acid treatment for 1 to 2.5 hours, wherein the weak acid is at least one of citric acid, acetic acid, and oxalic acid.

[0009] This invention uses weak acids such as citric acid, acetic acid, and oxalic acid to etch the outer surface of the alumina support, which does not erode the internal skeletal structure of the support particles, thus preserving the excellent mechanical strength of the alumina support itself. After etching, a rough surface is formed on the support, which provides physical anchoring points and chemical bonding sites. Furthermore, etching increases the number of exposed hydroxyl groups on the support surface. These hydroxyl groups on the alumina surface can coordinate with tin ions in the solution, enhancing the interfacial bonding force between tin species and the support. During subsequent drying and calcination heat treatment, this effectively inhibits the diffusion and migration of tin ions into the internal pores of the support particles, ensuring that the tin component remains stably on the support surface, achieving a core-shell distribution.

[0010] In one optional embodiment, the tin-containing acidic impregnation solution comprises a Sn source, concentrated hydrochloric acid, ethanolamine, and water; The mass ratio of Sn source, concentrated hydrochloric acid, ethanolamine and water is (5-8):(15-25):(1-2):(200-400); The Sn source is at least one of SnCl2, SnCl4 and Sn(CH3COO)2; The ethanolamine includes diethanolamine; The concentration of the tin-containing acidic impregnation solution is 0.75–1.20 wt%, based on the Sn element content.

[0011] In this invention, the concentrated hydrochloric acid in the tin-containing acidic impregnation solution formulation provides a strongly acidic environment, effectively inhibiting the hydrolysis of tin ions. Ethanolamine, as an organic amine additive, does not simply neutralize the acidity; it forms a weak coordination complex with tin ions, moderately buffering their reactivity and preventing rapid precipitation and aggregation of tin salts during spraying, thus facilitating the uniform spreading of tin species on the carrier surface. If the system lacks ethanolamine, the tin ion adsorption rate is too fast under high hydrochloric acid concentrations, easily causing localized aggregation of tin components; conversely, excessive ethanolamine addition leads to overly strong complexation, making the tin components prone to migration and aggregation after calcination.

[0012] In one optional embodiment, the pressure of the high-pressure spraying is 5 to 10 MPa.

[0013] The high-pressure spraying process used in this invention differs from traditional impregnation. In traditional impregnation, the carrier is completely immersed in the solution, and ions diffuse into the inner pores based on the concentration gradient. High-pressure spraying, on the other hand, directly sprays the atomized tin-containing acidic impregnation solution onto the outer surface of the carrier particles. The liquid mainly adheres to the surface layer of the particles, reducing the diffusion of tin ions into the interior of the carrier and facilitating the enrichment of tin elements on the surface.

[0014] In one optional embodiment, the drying temperature is 90–120°C, and the drying time is 8–12 hours. The roasting process includes roasting at 450–600℃ for 1–5 hours; The calcination is a segmented gradient calcination, which includes a first stage calcination and a second stage calcination. The calcination temperature of the first stage calcination is 250-350℃ and the calcination time is 0.5-1.5h. The calcination temperature of the second stage calcination is 450-600℃ and the calcination time is 1-5h.

[0015] This invention employs a segmented gradient calcination process. In the low-temperature range of 250–350°C, the solvent adhering to the surface of the carrier is slowly evaporated, and organic amines and residual hydrochloric acid are slowly decomposed and released, preventing the rapid boiling of the solvent from causing localized aggregation of tin salts. The temperature is then raised to a high-temperature range of 450–600°C to complete the decomposition of tin species and crystal phase regulation, inhibiting abnormal growth of tin oxide grains and ensuring high dispersion of tin species.

[0016] In one optional embodiment, the Sn loading in the tin-containing spherical alumina support is 0.25–0.60 wt%, and the Cl content is 0.15–0.30 wt%.

[0017] Secondly, the present invention also provides a tin-containing spherical alumina carrier prepared by the preparation method described in the first aspect.

[0018] Thirdly, the present invention also provides a catalyst comprising the tin-containing spherical alumina support described in the second aspect, and an active substance supported on the tin-containing spherical alumina support.

[0019] In one optional embodiment, the active material is Pt, and the loading of Pt in the tin-containing spherical alumina support is 0.30 to 0.35 wt%.

[0020] Fourthly, the present invention also provides the application of the tin-containing spherical alumina support prepared according to the preparation method described in the first aspect in the preparation of a Pt-Sn / Al2O3 catalyst, wherein the Pt-Sn / Al2O3 catalyst is used for propane dehydrogenation or alkane reforming.

[0021] The technical solution of this invention has the following advantages: 1. This invention involves surface etching of an alumina carrier to create a roughened surface structure. This rough surface provides numerous adhesion sites, enhancing the adsorption and fixation of tin components on the carrier surface and strengthening the interfacial interaction between the alumina carrier and the active tin components. In subsequent processing steps, it effectively confines tin elements, preventing their migration and diffusion, and preventing tin components from penetrating into the carrier's internal pores or detaching from the surface, thus stabilizing the core-shell distribution structure of tin enrichment on the surface. The high-pressure spraying process used in this invention differs from traditional impregnation. Traditional impregnation involves the carrier being completely immersed in a solution, with ions diffusing into the internal pores based on the concentration gradient. High-pressure spraying directly sprays the atomized tin-containing acidic impregnation solution onto the outer surface of the carrier particles. The liquid mainly adheres to the particle surface, reducing the diffusion of tin ions into the carrier's interior and facilitating tin enrichment on the surface. Simultaneously, the acidic environment created during the preparation of the tin-containing spraying solution inhibits Sn from the source. n+ Hydrolysis and precipitation ensure that the tin component can be uniformly adhered to the surface of the alumina spheres after high-pressure spraying, thereby improving the overall uniformity of the tin component distribution on the carrier.

[0022] 2. This invention modifies the surface of the alumina support by etching with weak acids such as citric acid, acetic acid, and oxalic acid. This process does not damage the intact pore and framework structure inside the support, but creates a rough surface structure on the outer surface. This rough surface provides a large number of physical anchoring points and chemical bonding sites, effectively preserving the original mechanical strength of the support while strengthening the bonding strength between the tin component and the support. On the other hand, the increased number of surface hydroxyl groups exposed by etching allows for stronger chemical bonding with the tin precursor. This dual effect significantly enhances the interfacial interaction between the alumina support and the tin active component. In subsequent post-processing steps such as drying and segmented calcination, the tin element is effectively anchored on the surface of the support, making it difficult for it to penetrate and migrate into the internal pores or detach from the surface, thus stabilizing the core-shell distribution structure enriched on the surface of the tin element. Meanwhile, since the tin component only adheres to the surface of the carrier, the corrosive gases such as HCl and Cl2 released by the decomposition of tin salt during the calcination process can escape directly from the particle surface without penetrating and corroding the internal skeleton of alumina. This can completely preserve the original mechanical strength of the carrier, effectively overcoming the defects of the hot oil method, which causes the internal tin salt to decompose and corrode the carrier, destroy the internal structure of alumina, and cause its strength to decrease, thus extending the industrial service life of the catalyst.

[0023] 3. The tin-containing acidic impregnation solution prepared in this invention utilizes high-concentration hydrochloric acid to create a strongly acidic environment, significantly improving the solubility and stability of tin salts and thermodynamically inhibiting the hydrolysis and precipitation of tin ions. The system incorporates ethanolamine as a weak complexing component, which can form appropriate coordination with tin ions, buffering their reactivity and preventing the tin precursor from agglomerating on the carrier surface due to excessively rapid precipitation during spraying. Unlike traditional equal-volume impregnation methods, this invention employs a high-pressure atomization spraying loading mode, allowing for precise control of the actual tin loading. This provides a wide process window, effectively mitigating the defects of traditional impregnation processes such as localized agglomeration, uneven loading, and large performance fluctuations between different batches of samples. It also improves the repeatability of the preparation process and facilitates stable batch preparation of the target carrier.

[0024] 4. The segmented gradient calcination process of this invention can precisely control the type of tin species crystal phase and grain size, inhibit excessive growth of tin grains, improve their dispersibility, and give full play to the role of tin element in inhibiting Pt sintering and reducing carbon deposition.

[0025] 5. The overall process of this invention is simple, eliminating the need for complex steps such as sol preparation, hot oil droplet forming, long-term aging, and multiple washing required by the oil column forming method. It only requires sequential weak acid surface etching, high-pressure spraying of loaded tin, drying, and segmented calcination to obtain the target core-shell type tin-containing spherical alumina support. The process is short and easy to operate, which helps reduce production energy consumption and manufacturing costs. The Pt-Sn / Al2O3 catalyst prepared using the tin-supported material of this invention achieves catalytic performance comparable to that of traditional processes; under optimized process conditions, key indicators such as feed conversion rate and aromatic selectivity can be further improved. This invention balances process simplification and product performance, avoiding many structural defects associated with traditional oil column forming processes while overcoming the difficulty in controlling tin distribution in ordinary impregnation methods. It has promising industrial application prospects in the fields of propane dehydrogenation and moving bed catalyst supports for continuous naphtha reforming.

[0026] 6. The tin element on the surface of the spherical alumina prepared by this invention exhibits a core-shell distribution, with the tin element concentrated on the surface layer of the support and a low tin content inside the particles. The tin element can fully synergize with the subsequently loaded platinum active components. The support completely retains the original alumina's pore structure and excellent mechanical strength, avoiding the erosion and damage of the internal pore skeleton by corrosive gases. The particles have strong friction resistance and anti-breakage ability. The prepared Pt-Sn / Al2O3 catalyst can be applied in chemical catalysis fields such as propane dehydrogenation and naphtha reforming, with good catalytic effect. Attached Figure Description

[0027] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0028] Figure 1 This is a SEM image of the spherical alumina product prepared in Example 1 of this invention; Figure 2 This is a Sn element distribution diagram of the spherical alumina product prepared in Example 1 of the present invention; Figure 3 This is a physical image of the spherical alumina catalyst loaded with Sn prepared in Example 1 of this invention. Detailed Implementation

[0029] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.

[0030] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0031] Example 1 This embodiment uses a high-pressure spraying method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support S1: Place the spherical Al2O3 in a 0.15 mol / L oxalic acid solution and etch for 2 h until a rough surface is formed.

[0032] S2: Weigh 6g of SnCl2 and place it in a dry beaker. Add 20g of concentrated hydrochloric acid until the SnCl2 is completely dissolved. Continue to add 1.5g of diethanolamine, cool and stir thoroughly. Add 390g of deionized water and continue stirring until the solution is white and uniform to obtain the spraying liquid.

[0033] S3: The spraying liquid in S2 is uniformly sprayed onto the surface of the spherical Al2O3 carrier treated in S1 using a high-pressure spray gun at a pressure of 5 MPa.

[0034] S4: The support obtained in S3 was dried at 120℃ for 8 hours, then placed in a muffle furnace and heated to 300℃ at 2℃ / min for 1 hour, then heated to 500℃ at 3℃ / min for 3 hours. After cooling, Sn / Al2O3 support was obtained, with Sn content of 0.35% by mass and Cl content of 0.24% by mass.

[0035] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, then evaporate to dryness under reduced pressure at 90°C to obtain the following... Figure 3 The Pt-Sn / Al2O3 catalyst shown is illustrated in the scanning electron microscope (SEM) results. Figure 1 As shown. EDS (Energy Dispersive X-ray Spectroscopy) line scan analysis reveals the Sn elemental distribution as follows. Figure 2 As shown in Table 2, the Pt and Sn contents in the catalyst were calculated.

[0036] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0037] Example 2 This embodiment uses a high-pressure spraying method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support S1: Place the spherical Al2O3 in a 0.25 mol / L citric acid solution and etch for 1.5 h until a rough surface is formed.

[0038] S2: Weigh 6g of SnCl4 and place it in a dry beaker. Add 20g of concentrated hydrochloric acid until the SnCl4 is completely dissolved. Continue to add 1.5g of diethanolamine, cool and stir thoroughly. Add 300g of deionized water and continue stirring until the solution is white and uniform to obtain the spraying liquid.

[0039] S3: The spraying liquid in S2 is uniformly sprayed onto the surface of the spherical Al2O3 carrier treated in S1 using a high-pressure spray gun at a pressure of 10 MPa.

[0040] S4: The support obtained in S3 was dried at 90℃ for 12h, then placed in a muffle furnace and calcined at 600℃ for 4h before being taken out and cooled to obtain the Sn / Al2O3 support, which has a Sn content of 0.35% by mass and a Cl content of 0.24% by mass.

[0041] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0042] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0043] Example 3 This embodiment uses a high-pressure spraying method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support S1: Place the spherical Al2O3 in a 0.4 mol / L acetic acid solution and etch for 1.0 h until a rough surface is formed.

[0044] S2: Weigh 5g of Sn(CH3COO)2 and place it in a dry beaker. Add 15g of concentrated hydrochloric acid until Sn(CH3COO)2 is completely dissolved. Continue to add 1g of diethanolamine, cool and stir thoroughly. Add 200g of deionized water and continue stirring until the solution is white and uniform to obtain the spraying liquid.

[0045] S3: The spraying liquid in S2 is uniformly sprayed onto the surface of the spherical Al2O3 carrier treated in S1 using a high-pressure spray gun at a pressure of 7.5 MPa.

[0046] S4: The support obtained in S3 was dried at 105℃ for 10h, and then placed in a muffle furnace. The temperature was increased to 300℃ at 2℃ / min and held for 1h, and then increased to 500℃ at 3℃ / min and held for 3h. After cooling, the Sn / Al2O3 support was obtained. The Sn content in the support was 0.35% by mass and the Cl content was 0.24% by mass.

[0047] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0048] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0049] Example 4 This embodiment uses a high-pressure spraying method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support S1: Place the spherical Al2O3 in a 0.15 mol / L oxalic acid solution and etch for 2.5 h until a rough surface is formed.

[0050] S2: Weigh 8g of SnCl2 and place it in a dry beaker. Add 25g of concentrated hydrochloric acid until the SnCl2 is completely dissolved. Continue to add 2g of diethanolamine, cool and stir thoroughly. Add 400g of deionized water and continue stirring until the solution is white and uniform to obtain the spraying liquid.

[0051] S3: The spraying liquid in S2 is uniformly sprayed onto the surface of the spherical Al2O3 carrier treated in S1 using a high-pressure spray gun at a pressure of 5 MPa.

[0052] S4: The support obtained in S3 was dried at 90℃ for 12h, then placed in a muffle furnace and calcined at 600℃ for 4h before being taken out and cooled to obtain the Sn / Al2O3 support, which has a Sn content of 0.35% by mass and a Cl content of 0.24% by mass.

[0053] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0054] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0055] Example 5 This embodiment uses a high-pressure spraying method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support S1: Place the spherical Al2O3 in a 0.25 mol / L citric acid solution and etch for 2 h until a rough surface is formed.

[0056] S2: Weigh 7g of SnCl2 and place it in a dry beaker. Add 22g of concentrated hydrochloric acid until the SnCl2 is completely dissolved. Continue to add 1.8g of diethanolamine, cool and stir thoroughly. Add 350g of deionized water and continue stirring until the solution is white and uniform to obtain the spraying liquid.

[0057] S3: The spraying liquid in S2 is uniformly sprayed onto the surface of the spherical Al2O3 carrier treated in S1 using a high-pressure spray gun at a pressure of 5 MPa.

[0058] S4: The support obtained in S3 was dried at 90℃ for 12h, then placed in a muffle furnace and heated to 300℃ at 2℃ / min and held for 1h, then heated to 550℃ at 3℃ / min and held for 3h, and then taken out and cooled to obtain Sn / Al2O3 support with Sn content of 0.35% by mass and Cl content of 0.24% by mass.

[0059] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0060] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0061] Comparative Example 1 This comparative example uses a conventional equal-volume vacuum impregnation method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, while simultaneously evaluating the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support A spherical Al2O3 support was placed in a vacuum impregnation machine, and an aqueous SnCl2 solution was prepared with a Sn loading of 0.35% by mass. Concentrated hydrochloric acid was added to adjust the pH to 1.5. The support was impregnated at 25°C for 2 hours, then dried at 110°C for 12 hours, and calcined at 550°C for 4 hours to obtain the Sn / Al2O3 support.

[0062] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0063] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0064] Comparative Example 2 This comparative example uses the oil column molding method to prepare spherical alumina supports and Pt-Sn / Al2O3 catalysts, and simultaneously evaluates the reforming reaction. The specific steps are as follows: (1) Preparation of Sn / Al2O3 support Basic aluminum chloride sol was prepared by reacting aluminum powder with hydrochloric acid. SnCl2 solution was added, and the Sn content was controlled at 0.35% by mass. 30% by mass of hexamethylenetetramine was added. The mixed sol was dropped into a hot oil column at 95°C to form a spherical Sn / Al2O3 support. After aging, washing, and drying, it was calcined at 550°C for 4 hours to obtain a spherical Sn / Al2O3 support.

[0065] (2) Preparation of Pt-Sn / Al2O3 catalyst Take 0.56 g of chloroplatinic acid, add 2.45 ml of 37% hydrochloric acid and 147.2 mL of deionized water to prepare an impregnation solution. Vacuum impregnate the tin-containing Al2O3 microspheres obtained in step (1) at a liquid-to-solid ratio of 1.8 ml / g, and then evaporate them under reduced pressure at 90 °C to obtain the Pt-Sn / Al2O3 catalyst.

[0066] (3) Evaluation of reforming reaction The catalytic reforming reaction of the prepared catalyst was evaluated using n-heptane as a feedstock in a micro fixed-bed reactor. The evaluation conditions were: reaction temperature 500℃, reaction pressure 0.7 MPa, hydrogen-to-hydrogen volume ratio 800:1, and volume hourly space velocity 2 h⁻¹. -1 The catalyst loading was 2 mL, and the reaction results are shown in Table 3.

[0067] The process parameters for each embodiment are shown in Table 1.

[0068] Table 1

[0069] Table 2

[0070] Table 3

[0071] As shown in Table 3, the catalytic performance of some embodiments of the present invention is comparable to that of Comparative Example 2, which represents the mainstream oil column forming process in the industry. This process requires multiple steps, including the reaction of aluminum powder with hydrochloric acid to synthesize a sol, the introduction of a tin source and a gelling agent, hot oil column droplet forming, aging, washing, drying, and calcination. It is highly dependent on specialized equipment, has a lengthy production process, a long cycle, and high energy consumption. In contrast, the present invention uses a simplified process route of alumina through surface etching, high-pressure spraying, and drying and calcination. It eliminates the need for complex steps such as hot oil column forming and long-term aging and washing. Under the premise of significantly simplifying the preparation process and reducing production requirements, the catalyst prepared by the present invention can achieve catalytic effects comparable to or even better than those of the traditional oil column forming process.

[0072] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a tin-containing spherical alumina carrier, characterized in that, Includes the following steps: The alumina carrier was etched and a tin-containing acidic impregnation solution was prepared. A tin-containing acidic impregnation solution was high-pressure sprayed onto an etched alumina substrate; The sprayed alumina carrier is dried and calcined to obtain tin-containing spherical alumina carrier.

2. The method for preparing the tin-containing spherical alumina carrier according to claim 1, characterized in that, The etching is performed using a weak acid treatment for 1 to 2.5 hours, wherein the weak acid is at least one of citric acid, acetic acid, and oxalic acid.

3. The method for preparing the tin-containing spherical alumina carrier according to claim 1, characterized in that, The tin-containing acidic impregnation solution includes a Sn source, concentrated hydrochloric acid, ethanolamine, and water; The mass ratio of Sn source, concentrated hydrochloric acid, ethanolamine and water is (5-8):(15-25):(1-2):(200-400); The Sn source is at least one of SnCl2, SnCl4 and Sn(CH3COO)2; The concentration of the tin-containing acidic impregnation solution is 0.75–1.20 wt%, based on the Sn element content.

4. The method for preparing the tin-containing spherical alumina carrier according to claim 1, characterized in that, The pressure of the high-pressure spraying is 5. 10MPa.

5. The method for preparing the tin-containing spherical alumina carrier according to claim 1, characterized in that, The drying temperature is 90–120°C, and the drying time is 8–12 hours. The roasting process includes roasting at 450–600℃ for 1–5 hours; The calcination is a segmented gradient calcination, which includes a first stage calcination and a second stage calcination. The calcination temperature of the first stage calcination is 250-350℃ and the calcination time is 0.5-1.5h. The calcination temperature of the second stage calcination is 450-600℃ and the calcination time is 1-5h.

6. The method for preparing the tin-containing spherical alumina carrier according to claim 1, characterized in that, The tin-containing spherical alumina support has a Sn loading of 0.25–0.60 wt% and a Cl content of 0.15–0.30 wt%.

7. A tin-containing spherical alumina carrier, characterized in that, It is prepared by the preparation method described in any one of claims 1 to 6.

8. A catalyst, characterized in that, It includes the tin-containing spherical alumina support as described in claim 7, and the active material loaded on the tin-containing spherical alumina support.

9. The catalyst according to claim 8, characterized in that, The active material is Pt, and the loading of Pt in the tin-containing spherical alumina support is 0.30 to 0.35 wt%.

10. The application of a tin-containing spherical alumina support prepared by any one of claims 1 to 6 in the preparation of a Pt-Sn / Al2O3 catalyst, wherein the Pt-Sn / Al2O3 catalyst is used for propane dehydrogenation or alkane reforming.