A catalyst for preparing single-walled carbon nanotubes and a method for preparing the same and use thereof

By leveraging the synergistic effect of Cu, Fe, and noble metal catalysts, combined with microwave radiation and annealing processes, the problems of low catalyst activity and uncontrollable tube diameter in the growth of single-walled carbon nanotubes were solved, achieving high yield and narrow diameter distribution of single-walled carbon nanotubes, thus promoting their large-scale application.

CN123148967APending Publication Date: 2026-11-24JIANGSU CNANO TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611610954.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing single-walled carbon nanotube growth technologies suffer from low catalyst activity, uneven particle size distribution, uncontrollable tube diameter, and narrow production process window, which hinders large-scale applications.

Method used

A catalyst composed of Cu, Fe, and noble metals was prepared by combining the binuclear synergistic effect of Fe/Cu and the synergistic electronic effect of noble metals with microwave radiation treatment, annealing, and reduction processes to achieve precise control of single-walled carbon nanotubes.

Benefits of technology

It significantly improved the yield and diameter uniformity of single-walled carbon nanotubes, enabling the preparation of narrow diameter distributions under normal pressure conditions and promoting the large-scale application of carbon nanotubes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148967A_ABST
    Figure CN123148967A_ABST
Patent Text Reader

Abstract

This application provides a catalyst for preparing single-walled carbon nanotubes, its preparation method, and its application, belonging to the technical field of catalysts and single-walled carbon nanotube preparation. The catalyst for preparing single-walled carbon nanotubes includes a substrate and an active component supported on the substrate; the active component includes Cu, Fe, and noble metals; the molar ratio of Cu to Fe is 1:(0.1-1). This application utilizes Cu, Fe, and noble metals to support the substrate, firstly through the binuclear synergy of Fe / Cu, and then combined with the synergistic electronic effect between Fe-Cu and noble metals, effectively reducing the cracking energy barrier of the carbon source and inhibiting catalyst sintering at high temperatures. While ensuring high selectivity and high catalytic activity, this significantly improves the yield of single-walled carbon nanotubes and achieves precise control of the carbon nanotube diameter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of catalyst and single-walled carbon nanotube preparation technology, and relates to a catalyst for preparing single-walled carbon nanotubes, its preparation method and application. Background Technology

[0002] Since their discovery in the 1990s, single-walled carbon nanotubes (SWCNTs) have shown great promise for applications in various fields such as electronic devices, sensors, composite materials, and energy storage due to their excellent mechanical strength, flexibility, electrical, mechanical, and thermal properties.

[0003] However, existing SWCNT growth technologies still face many bottlenecks: First, traditional single-metal catalysts have limited activation performance and are prone to sintering and agglomeration under high-temperature conditions, leading to a wider catalyst particle size or even deactivation, resulting in low carbon source cracking efficiency and uncontrollable SWCNT tube diameter and increased structural defects; Second, the current production process window is narrow, and the overall reaction is greatly affected by parameters such as temperature and atmosphere, which significantly affects the quality of single-walled carbon nanotubes and hinders large-scale production and application.

[0004] Current research has attempted to improve catalyst performance through alloying strategies, but the proportion of alloy components, particle size control, and preparation process lack systematic optimization, making it difficult to simultaneously achieve high activity, high selectivity, and uniformity of the catalyst.

[0005] Therefore, there is a need to develop a novel catalyst system and its preparation method that combines high catalytic activity, excellent thermal stability, and precise control of SWCNT diameter. Summary of the Invention

[0006] The purpose of this application is to provide a catalyst for the preparation of single-walled carbon nanotubes, its preparation method and application, which solves the common problems in the existing single-walled carbon nanotube growth and preparation process, such as low catalyst activity, poor particle size distribution uniformity, limited yield, uncontrollable tube diameter distribution and narrow production process window.

[0007] To achieve the purpose of this application, the following technical solution is adopted: In a first aspect, this application provides a catalyst for preparing single-walled carbon nanotubes, the catalyst comprising a substrate and an active component supported on the substrate; The active components include Cu, Fe, and noble metals; The molar ratio of Cu to Fe is 1:(0.1-1), for example, it can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8 or 1:0.9, etc.

[0008] The catalyst provided in this application utilizes Cu, Fe, and noble metals to support the matrix. First, through the dual-core synergy of Fe / Cu, and then combined with the synergistic electronic effect between Fe-Cu and noble metals, the cracking energy barrier of the carbon source is effectively reduced, and the sintering of the catalyst at high temperature is suppressed. Under the premise of ensuring high selectivity and high catalytic activity of the catalyst, the yield of single-walled carbon nanotubes is significantly improved and the precise control of the carbon nanotube diameter is achieved.

[0009] The catalyst provided in this application has an active component composed of Cu, Fe and noble metals, which solves the problem that single metal nanoparticles are prone to sintering and agglomeration under high-temperature chemical vapor deposition (CVD) conditions, leading to catalytic deactivation and an increase in uncontrolled tube diameter and structural defects. At the same time, it avoids the high cost and insufficient selectivity of using noble metals alone, which easily generate multi-walled carbon nanotubes or amorphous carbon impurities.

[0010] This application ensures that copper has sufficient volatility at high temperatures by controlling the molar ratio of Cu and Fe within a specific range, and maintains catalytic activity by introducing iron to suppress excessive copper volatilization.

[0011] In some embodiments, the precious metal includes any one or a combination of at least two of Pt, Rh, Ir, Ag, or Pd.

[0012] In some embodiments, the total molar amount of Cu and Fe and the molar ratio of the noble metal are (1-4):1, for example, 1.2:1, 1.5:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.5:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.6:1 or 3.8:1, etc.

[0013] This application achieves precise control of the diameter of single-walled carbon nanotubes by controlling the range of the total molar amount of Cu and Fe and the molar ratio of noble metals, thereby precisely regulating the particle size distribution of multi-element alloy nanoparticles within a narrow range.

[0014] In some embodiments, the particle size of the active component is 1nm-2nm, for example, it can be 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, 1.6nm, 1.7nm, 1.8nm or 1.9nm, etc.

[0015] In some embodiments, the thickness of the coating containing the active component is 50nm-200nm, for example, it can be 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm or 190nm, etc.

[0016] In some embodiments, the substrate includes a silicon wafer and / or a silicon wafer with an oxide layer loaded on its surface.

[0017] In some embodiments, the thickness of the oxide layer is 200nm-400nm, for example, it can be 220nm, 240nm, 250nm, 260nm, 280nm, 300nm, 320nm, 340nm, 350nm, 360nm or 380nm, etc.

[0018] The oxide layer described in this application includes silicon dioxide.

[0019] Secondly, this application provides a method for preparing the catalyst as described in the first aspect, the method comprising: A copper salt, an iron salt, a first organic polymer, and a first organic solvent are mixed to obtain an Fe-Cu catalytic precursor; the molar ratio of the copper salt to the iron salt is 1:(0.1-1), for example, it can be 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, or 1:0.9, etc.; a noble metal salt, a second organic polymer, and the Fe-Cu catalytic precursor are mixed and subjected to microwave irradiation treatment to obtain a multi-element alloy colloid; The multi-element alloy colloid was coated onto a substrate and then subjected to annealing and reduction in sequence to obtain the catalyst.

[0020] In this application, the copper salt includes copper chloride dihydrate; the iron salt includes ferric chloride hexahydrate.

[0021] In this application, the substrate further includes a pretreatment before use, which includes ultrasonic cleaning with acetone, methanol and deionized water for 3-6 minutes each, followed by drying with nitrogen.

[0022] The preparation method provided in this application first uses an organic polymer mixed with a metal source to obtain a multi-element alloy catalytic precursor, and then uses a combination of microwave radiation treatment, annealing, and reduction to obtain a catalyst with high selectivity and high catalytic activity, and which has a suitable catalytic activity size for growing single-walled carbon nanotubes. The preparation method is simple, energy-efficient, and has significant advantages for industrial application.

[0023] This application utilizes microwave irradiation to rapidly and uniformly nucleate the precursor in an organic polymer, forming a well-dispersed ternary alloy colloid.

[0024] In some embodiments, the first organic solvent includes an alcohol solvent.

[0025] The alcohol solvents described in this application include any one or a combination of at least two of ethanol, methanol, or isopropanol.

[0026] In some embodiments, the first organic polymer and the second organic polymer each independently comprise any one or a combination of at least two of polyvinylpyrrolidone, polyvinyl alcohol, or polymethyl methacrylate.

[0027] In some embodiments, the molar ratio of the first organic polymer to the copper salt is (1-5):1, for example, it can be 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or 4.5:1, etc.

[0028] In some embodiments, the molar ratio of the total molar amount of Cu and Fe in the Fe-Cu catalytic precursor to the molar ratio of the noble metal salt is (1-4):1, for example, it can be 1.2:1, 1.5:1, 1.6:1, 1.8:1, 2:1, 2.2:1, 2.5:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.6:1 or 3.8:1, etc.

[0029] In some embodiments, the molar ratio of the second organic polymer to the noble metal salt is (1-4):1, for example, it can be 1.5:1, 2:1, 2.5:1, 3:1 or 3.5:1, etc.

[0030] In some embodiments, the noble metal salt includes any one or a combination of at least two of Pt salts, Rh salts, Ir salts, Ag salts, or Pd salts.

[0031] In some embodiments, the power of the microwave radiation treatment is 3kW-5kW, for example, it can be 3.2kW, 3.5kW, 3.6kW, 3.8kW, 4kW, 4.2kW, 4.5kW, 4.6kW or 4.8kW, etc.; the time is 1min-3min, for example, it can be 1.2min, 1.5min, 1.6min, 1.8min, 2min, 2.2min, 2.5min, 2.6min or 2.8min, etc.

[0032] In some embodiments, the microwave radiation treatment further includes: adding a second organic solvent to the microwave radiation treatment product, performing solid-liquid separation and washing in sequence, and then dispersing the precipitate in a first organic solvent.

[0033] In this application, the second organic solvent includes acetone and / or isopropanol.

[0034] In some embodiments, the coating method includes spin coating.

[0035] In some embodiments, the coating thickness is 50nm-200nm, for example, it can be 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm or 190nm, etc.

[0036] In some embodiments, the annealing is performed in an air atmosphere.

[0037] In some embodiments, the annealing temperature is 500℃-700℃, for example, it can be 520℃, 550℃, 560℃, 580℃, 600℃, 620℃, 650℃, 660℃ or 680℃, etc.

[0038] This application achieves effective control over the structure of the catalyst active center by controlling the temperature range of the annealing process to ensure the removal of organic polymers on the catalyst surface and to avoid excessive volatilization of Cu in the catalyst.

[0039] In some embodiments, the annealing time is 20-40 minutes, for example, it can be 22 minutes, 25 minutes, 26 minutes, 28 minutes, 30 minutes, 32 minutes, 35 minutes, 36 minutes or 38 minutes.

[0040] In some embodiments, both the annealing and the reduction are performed in a tube furnace.

[0041] In some embodiments, the reduction is carried out in a hydrogen-containing atmosphere.

[0042] In this application, the hydrogen-containing atmosphere includes hydrogen and an inert gas, and the volume ratio of the two can be 1:(3-5), for example, it can be 1:3.2, 1:3.5, 1:3.8, 1:4, 1:4.2, 1:4.5 or 1:4.8, etc.

[0043] In some embodiments, the reduction temperature is 910℃-1000℃, for example, it can be 920℃, 930℃, 940℃, 950℃, 960℃, 970℃, 980℃ or 990℃, etc.

[0044] In some embodiments, the reduction time is 10-30 minutes, for example, it can be 12 minutes, 15 minutes, 16 minutes, 18 minutes, 20 minutes, 22 minutes, 25 minutes, 26 minutes or 28 minutes.

[0045] Thirdly, this application provides a method for preparing single-walled carbon nanotubes with a narrow diameter distribution, the method comprising: Under the action of the catalyst as described in the first aspect, a carbon source and a carrier gas are introduced to carry out a reaction, thereby obtaining the single-walled carbon nanotubes.

[0046] The preparation method provided in this application, by using the aforementioned catalyst, enables the preparation of narrow diameter distributed SWCNTs under normal pressure without vacuum or plasma assistance, thereby breaking through the existing technical bottleneck and promoting the large-scale application of carbon nanotubes.

[0047] In some embodiments, the carbon source includes methane.

[0048] In some embodiments, the carrier gas includes hydrogen.

[0049] In some embodiments, the volumetric flow rate ratio of the carbon source to the carrier gas is 1:(1-3), for example, it can be 1:1.2, 1:1.4, 1:1.5, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.5, 1:2.6 or 1:2.8, etc.

[0050] In some embodiments, the reaction is carried out in a tube furnace.

[0051] In this application, the annealing and reduction of the catalyst are also carried out in a tube furnace. Therefore, single-walled carbon nanotubes can be grown directly after the catalyst reduction. The catalyst preparation and single-walled carbon nanotube growth steps are highly integrated, forming a complete full-chain technical solution from catalyst precursor preparation to carbon nanotube growth.

[0052] In some embodiments, the reaction temperature is 800℃-1000℃, for example, it can be 820℃, 840℃, 850℃, 860℃, 880℃, 900℃, 920℃, 940℃, 950℃, 960℃ or 980℃, etc.

[0053] In some embodiments, the reaction time is 20 min to 40 min, for example, it can be 22 min, 25 min, 26 min, 28 min, 30 min, 32 min, 35 min, 36 min or 38 min, etc.

[0054] In some embodiments, the reaction is further followed by a first cooling and a second cooling process performed in the furnace.

[0055] In some embodiments, the cooling rate of the first cooling is 8°C / min-12°C / min, for example, it can be 8.5°C / min, 9°C / min, 9.5°C / min, 10°C / min, 10.5°C / min, 11°C / min or 11.5°C / min, etc.

[0056] In some embodiments, the cooling endpoint of the first cooling is 350°C-450°C, for example, it can be 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C or 440°C, etc.

[0057] In some embodiments, the second cooling includes continuously introducing argon gas at a rate of 4 L / min to 6 L / min to cool to room temperature, for example, 4.2 L / min, 4.5 L / min, 4.6 L / min, 4.8 L / min, 5 L / min, 5.2 L / min, 5.5 L / min, 5.6 L / min or 5.8 L / min.

[0058] Fourthly, this application provides a single-walled carbon nanotube with a narrow diameter distribution, wherein the single-walled carbon nanotube is prepared by the preparation method described in the third aspect.

[0059] In some embodiments, the average diameter of the single-walled carbon nanotubes is 1.0 nm to 2.0 nm, for example, it can be 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm or 1.9 nm, etc.

[0060] In some embodiments, the proportion of the single-walled carbon nanotubes with a diameter in the range of 0.6 nm to 1.8 nm is ≥70%, for example, it can be 72%, 74%, 75%, 76%, 78%, 80%, 82%, 84%, 85%, 86%, 88%, 90%, 92%, or 95%, etc.

[0061] The single-walled carbon nanotubes obtained in this application exhibit excellent uniformity in diameter, overcoming the problems of uneven diameter and excessively wide distribution in existing methods.

[0062] The numerical range described in this application includes not only the point values ​​listed above, but also any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of brevity, this application will not exhaustively list the specific point values ​​included in the range.

[0063] Compared with the prior art, this application has the following advantages: (1) The catalyst provided in this application utilizes Cu, Fe and noble metals to load the matrix. First, through the dual-core synergy of Fe / Cu, and then combined with the synergistic electronic effect between Fe-Cu and noble metals, the cracking energy barrier of the carbon source is effectively reduced, and the sintering of the catalyst at high temperature is suppressed. Under the premise of ensuring high selectivity and high catalytic activity of the catalyst, the yield of single-walled carbon nanotubes is significantly improved and the precise control of the carbon nanotube diameter is achieved.

[0064] (2) The catalyst preparation method provided in this application first uses an organic polymer to mix with a metal source to obtain a multi-element alloy catalytic precursor, and then uses a combination of microwave radiation treatment, annealing and reduction to obtain a catalyst with high selectivity and high catalytic activity, and it has a catalytic activity size suitable for growing single-walled carbon nanotubes. The preparation method is simple and has low energy consumption, and has significant advantages for industrial application.

[0065] (3) The method for preparing single-walled carbon nanotubes provided in this application, by using the obtained catalyst, can prepare narrow diameter distribution SWCNTs under normal pressure without vacuum or plasma assistance, so as to break through the existing technical bottleneck and promote the large-scale application of carbon nanotubes.

[0066] (4) The single-walled carbon nanotubes provided in this application have an average diameter of 1.0 nm-2.0 nm, and the proportion of tube diameters within 0.6 nm-1.8 nm is ≥70%. The obtained single-walled carbon nanotubes have excellent tube diameter uniformity, overcoming the problems of uneven tube diameter and excessively wide distribution in existing methods. Attached Figure Description

[0067] Figure 1 This is a TEM image of the single-walled carbon nanotubes prepared in Example 3.

[0068] Figure 2 This is a TEM image of the single-walled carbon nanotubes prepared in Comparative Example 1. Detailed Implementation

[0069] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0070] All materials used in the specific embodiments of this invention are commercially available or prepared using conventional methods in the prior art. All methods employed are conventional techniques in the field.

[0071] In the following examples and comparative examples, the substrate further includes a pretreatment before use, which includes ultrasonic cleaning with acetone, methanol and deionized water for 5 minutes each, followed by drying with nitrogen.

[0072] Example 1 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and a method for preparing the same, wherein the catalyst includes a substrate and an active component supported on the substrate. The active component includes Cu, Fe, and a noble metal; the molar ratio of Cu to Fe is 1:1; the noble metal is Pt; the total molar amount of Cu and Fe is in a molar ratio of 1:1 to the noble metal; the particle size of the active component is 1 nm-2 nm; and the thickness of the coating layer containing the active component is 150 nm. The substrate comprises a silicon wafer with a SiO2 layer of 300 nm thickness loaded on its surface.

[0073] The preparation method of the catalyst and single-walled carbon nanotubes includes the following steps: (1) CuCl2·2H2O (17g, 0.1mol) and FeCl3·6H2O (27g, 0.1mol) were dissolved in ethanol at a molar ratio of 1:1 and mixed under ultrasonic conditions. Then, polyvinylpyrrolidone (55.5g, 0.5mol) was added and the mixture was magnetically stirred for 30 min to obtain the Fe-Cu catalytic precursor. (2) The Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are mixed according to the total molar amount of Cu and Fe in the Fe-Cu catalyst precursor and the molar ratio of the noble metal salt is 1:1. In step (1), the Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are placed in polyvinylpyrrolidone (44.4g, 0.4mol) and microwave irradiated for 2min at a power of 4kW to form a ternary alloy colloid. (3) Add 10 mL of acetone to the ternary alloy colloid, centrifuge at 8000 rpm for 10 min, collect the precipitate, wash it twice with methanol, and then redisperse the precipitate in methanol to obtain a clean ternary alloy colloid. (4) The multi-element alloy colloid was spin-coated onto the substrate at a speed of 3500 rpm for 30s, and the thickness of the spin coating was 150nm. Then it was placed in a tube furnace and annealed at 600℃ in air atmosphere for 30min to remove polyvinylpyrrolidone. Then the atmosphere was switched to Ar / H2 mixed gas (volume ratio of 4:1) and the temperature was raised to 940℃ for reduction for 20min to obtain the catalyst. (5) Keep the temperature of the tube furnace constant, switch the atmosphere to CH4 / H2 mixed gas (volume flow ratio 1:1), and react for 30 min. After the reaction is completed, reduce the temperature to 400℃ at a rate of 10℃ / min, and then continuously introduce pure argon gas at a rate of 5L / min to cool down to room temperature to obtain single-walled carbon nanotubes.

[0074] Example 2 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the molar ratio of Cu to Fe is 1:0.7, and the amount of CuCl2·2H2O is 20g (0.118mol) and FeCl3·6H2O is 22.1g (0.082mol).

[0075] Example 3 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the molar ratio of Cu to Fe is 1:0.4, and the amount of CuCl2·2H2O is 24.3g (0.143mol) and FeCl3·6H2O is 15.4g (0.057mol).

[0076] Figure 1 This is a TEM image of the single-walled carbon nanotubes prepared in this embodiment. Figure 1 It can be seen that single-walled carbon nanotube products have been successfully produced.

[0077] Example 4 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the molar ratio of Cu to Fe is 1:0.1, and the amount of CuCl2·2H2O is 30.9g (0.182mol) and FeCl3·6H2O is 4.86g (0.018mol).

[0078] Example 5 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the total molar ratio of Cu and Fe to the noble metal salt in the Fe-Cu catalyst precursor is 0.2:1, and the amounts of CuCl2·2H2O are 3.4g and 0.02mol, FeCl3·6H2O are 5.4g and 0.02mol, and H2PtCl6·6H2O1 are kept at 104g and 0.2mol.

[0079] Example 6 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the total molar ratio of Cu and Fe to the noble metal salt in the Fe-Cu catalytic precursor is 2:1, and the amounts of CuCl2·2H2O (34g, 0.2mol), FeCl3·6H2O (54g, 0.2mol), and H2PtCl6·6H2O (104g, 0.2mol) are maintained in the preparation method.

[0080] Example 7 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the total molar ratio of Cu and Fe to the noble metal salt in the Fe-Cu catalyst precursor is 3:1, and the amounts of CuCl2·2H2O are 51g and 0.3mol, FeCl3·6H2O is 81g and 0.3mol, and H2PtCl6·6H2O is 104g and 0.2mol respectively.

[0081] Example 8 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the total molar ratio of Cu and Fe to the noble metal salt in the Fe-Cu catalyst precursor is 4:1, and the amounts of CuCl2·2H2O are 68g and 0.4mol, FeCl3·6H2O is 108g and 0.4mol, and H2PtCl6·6H2O is 104g and 0.2mol.

[0082] Example 9 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the total molar ratio of Cu and Fe to the noble metal salt in the Fe-Cu catalyst precursor is 5:1, and the amounts of CuCl2·2H2O are 85g and 0.5mol, FeCl3·6H2O is 135g and 0.5mol, and H2PtCl6·6H2O is 104g and 0.2mol respectively.

[0083] Example 10 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. Except that the noble metal is Ir and IrCl3·3H2O (71g, 0.2mol) is used in the preparation method, all other conditions are the same as in Example 1.

[0084] Example 11 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. Except that the noble metal is Rh and RhCl3·3H2O (52g, 0.2mol) is used in the preparation method, all other conditions are the same as in Example 1.

[0085] Example 12 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and a method for preparing the same, as well as the preparation method for single-walled carbon nanotubes, which includes the following steps: (1) CuCl2·2H2O (17g, 0.1mol) and FeCl3·6H2O (27g, 0.1mol) were dissolved in ethanol at a molar ratio of 1:1 and mixed under ultrasonic conditions. Then, polyvinylpyrrolidone (11.1g, 0.1mol) was added and the mixture was magnetically stirred for 30 min to obtain the Fe-Cu catalytic precursor. (2) The Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are mixed in polyvinylpyrrolidone (22.2g, 0.2mol) according to the total molar amount of Cu and Fe in the Fe-Cu catalyst precursor and the molar ratio of noble metal salt is 1:1. In step (1), the Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are placed in polyvinylpyrrolidone (22.2g, 0.2mol) and microwave irradiated for 1min at a power of 5kW to form a ternary alloy colloid. (3) Add 10 mL of acetone to the ternary alloy colloid, centrifuge at 8000 rpm for 10 min, collect the precipitate, wash it twice with methanol, and then redisperse the precipitate in methanol to obtain a clean ternary alloy colloid. (4) The multi-element alloy colloid was spin-coated onto the substrate at a speed of 3500 rpm for 30s, and the thickness of the spin coating was 150nm. Then it was placed in a tube furnace and annealed at 700℃ in air atmosphere for 20min to remove polyvinylpyrrolidone. Then the atmosphere was switched to Ar / H2 mixed gas (volume ratio of 3:1) and the temperature was raised to 1000℃ for reduction for 10min to obtain the catalyst. (5) Keep the temperature of the tube furnace constant, switch the atmosphere to CH4 / H2 mixed gas (volume flow ratio 1:3), and react for 20 min. After the reaction is completed, reduce the temperature to 350℃ at a rate of 12℃ / min, and then continuously introduce pure argon gas at 6L / min to cool down to room temperature to obtain single-walled carbon nanotubes. All other conditions are the same as in Example 1.

[0086] Example 13 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and a method for preparing the same, as well as the preparation method for single-walled carbon nanotubes, which includes the following steps: (1) CuCl2·2H2O (17g, 0.1mol) and FeCl3·6H2O (27g, 0.1mol) were dissolved in ethanol at a molar ratio of 1:1 and mixed under ultrasonic conditions. Then, polyvinylpyrrolidone (33.3g, 0.3mol) was added and the mixture was magnetically stirred for 30 min to obtain the Fe-Cu catalytic precursor. (2) The Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are mixed according to the total molar amount of Cu and Fe in the Fe-Cu catalyst precursor and the molar ratio of the noble metal salt is 1:1. In step (1), the Fe-Cu catalyst precursor and H2PtCl6·6H2O (104g, 0.2mol) are placed in polyvinylpyrrolidone (88.8g, 0.8mol) and microwave irradiated for 3min at a power of 3kW to form a ternary alloy colloid. (3) Add 10 mL of acetone to the ternary alloy colloid, centrifuge at 8000 rpm for 10 min, collect the precipitate, wash it twice with methanol, and then redisperse the precipitate in methanol to obtain a clean ternary alloy colloid. (4) The multi-element alloy colloid was spin-coated onto the substrate at a speed of 3500 rpm for 30s, and the thickness of the spin coating was 150nm. Then it was placed in a tube furnace and annealed at 500℃ in air atmosphere for 40min to remove polyvinylpyrrolidone. Then the atmosphere was switched to Ar / H2 mixed gas (volume ratio of 5:1) and the temperature was raised to 910℃ for reduction for 30min to obtain the catalyst. (5) Keep the temperature of the tube furnace constant, switch the atmosphere to CH4 / H2 mixed gas (volume flow ratio 1:2), and react for 40 min. After the reaction is completed, the temperature is reduced to 450℃ at a rate of 8℃ / min. Then, pure argon gas is continuously introduced at a rate of 4L / min to cool down to room temperature, and single-walled carbon nanotubes are obtained. All other conditions are the same as in Example 1.

[0087] Example 14 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the annealing temperature in step (4) is 200°C.

[0088] Example 15 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the annealing temperature in step (4) is 400°C.

[0089] Example 16 This embodiment provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the annealing temperature in step (4) is 800°C.

[0090] Comparative Example 1 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. Except that the active component is only Fe and the amount of FeCl3·6H2O used in the preparation method is 54g and 0.2mol, all other conditions are the same as in Example 1.

[0091] Figure 2 This is a TEM image of the single-walled carbon nanotubes prepared for comparison. Figure 2 It can be seen that the diameter of single-walled carbon nanotubes increases, and only 53% of the single-walled carbon nanotubes have a diameter in the range of 0.6nm-1.8nm, with an average diameter of 2.48nm.

[0092] Comparative Example 2 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. Except that the active component is only Cu and the amount of CuCl2·2H2O used in the preparation method is 34g and 0.2mol, all other conditions are the same as in Example 1.

[0093] Comparative Example 3 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the active components are only Cu (CuCl2·2H2O, 17g, 0.1mol) and Fe (FeCl3·6H2O, 27g, 0.1mol) in a molar ratio of 1:1.

[0094] Comparative Example 4 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the active components are only Fe (FeCl3·6H2O, 54g, 0.2mol) and noble metal (H2PtCl6·6H2O, 104g, 0.2mol) in a molar ratio of 1:1.

[0095] Comparative Example 5 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the active components are only Cu (CuCl2·2H2O, 34g, 0.2mol) and noble metal (H2PtCl6·6H2O, 104g, 0.2mol) in a molar ratio of 1:1.

[0096] Comparative Example 6 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that the molar ratio of Cu to Fe is 1:2, and the amount of CuCl2·2H2O is 11.4g (0.067mol) and FeCl3·6H2O is 36g (0.133mol).

[0097] Comparative Example 7 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that Cu in the active component is replaced with Mn (MnCl2·4H2O, 20g, 0.1mol).

[0098] Comparative Example 8 This comparative example provides a catalyst for preparing single-walled carbon nanotubes and its preparation method. The preparation of single-walled carbon nanotubes is the same as in Example 1, except that microwave radiation treatment is not performed in step (2).

[0099] The single-walled carbon nanotube products obtained in the above embodiments and comparative examples were characterized. TEM was used to statistically analyze the average diameter and distribution of the products. Gas adsorption method was used to test the specific surface area of ​​the products after acid washing and purification. Raman spectroscopy was used to test the Ig of the products. G / I D The yield of single-walled carbon nanotube products is calculated based on hourly yield, and the corresponding yield is calculated with 1 as the standard yield.

[0100] The test results are shown in Table 1.

[0101] Table 1

[0102] As shown in Table 1: The catalysts and preparation methods for preparing single-walled carbon nanotubes (SWCNTs) provided in Examples 1-4, 6-8, and 10-13 of this application, along with the preparation methods of SWCNTs, utilize catalysts whose active components consist of Cu, Fe, and noble metals. By combining specific feed ratios and controlling the annealing temperature, the structure of the active centers of the catalyst is effectively controlled, reducing the carbon source cracking energy barrier and achieving a significant increase in SWCNT yield and precise control of SWCNT diameter. Under preferred conditions, the average diameter of the SWCNTs is 1.0 nm-2.0 nm; the proportion of SWCNTs with a diameter between 0.6 nm and 1.8 nm is ≥70%; and the yield is significantly higher than the standard yield.

[0103] A comparison of Examples 1 and 5 shows that if the proportion of the total Fe-Cu in the active component is too low, the high activity of the noble metal leads to insufficient catalyst selectivity, resulting in excessive carbon impurities as a byproduct of the grown single-walled carbon nanotubes. A comparison of Examples 1 and 9 shows that if the proportion of the total Fe-Cu in the active component is too high, the insufficient activity leads to low catalyst utilization efficiency, resulting in low yield and wide diameter range of the grown single-walled carbon nanotubes.

[0104] A comparison of Examples 1 and 14-15 shows that if the annealing temperature is low, the organic polymers on the catalyst surface cannot be effectively removed, resulting in the catalyst being unable to exert its own activity, which in turn leads to a low yield and a wide range of diameters of the grown single-walled carbon nanotubes. A comparison of Examples 1 and 16 shows that if the annealing temperature is high, the excessive volatilization of Cu in the catalyst leads to catalyst agglomeration and deactivation or excessively large particle size, which in turn leads to a low yield and a wide range of diameters of the grown single-walled carbon nanotubes.

[0105] A comparison of Example 1 and Comparative Examples 1-3 shows that if the active component is only Fe (Comparative Example 1), Cu (Comparative Example 2), or Fe-Cu (Comparative Example 3), catalyst agglomeration leads to catalyst deactivation or large particle size, resulting in low yield and wide diameter range of the grown single-walled carbon nanotubes.

[0106] A comparison of Example 1 and Comparative Example 4 shows that if Cu is lacking in the active component, the presence of only Fe prevents the formation of a binuclear synergistic precursor, leading to catalyst agglomeration and deactivation, resulting in a wider diameter distribution and lower yield of the grown single-walled carbon nanotubes. A comparison of Example 1 and Comparative Example 5 shows that if Fe is lacking in the active component, the presence of only Cu prevents the formation of a binuclear synergistic precursor, leading to rapid activity decay of the Cu active component, resulting in a lower yield and wider diameter distribution of the grown single-walled carbon nanotubes. A comparison of Example 1 and Comparative Example 6 shows that when the molar ratio of Cu to Fe is 1:2, the relatively insufficient Cu content causes Fe to lose its binuclear constraint, making it prone to agglomeration, resulting in larger catalyst particles or deactivation, leading to a lower yield and wider diameter range of the grown single-walled carbon nanotubes. A comparison of Example 1 and Comparative Example 7 shows that when Cu is replaced with Mn, the inability of Fe and Mn to form a binuclear synergistic precursor results in insufficient catalyst size constraint, leading to a wider diameter distribution of the grown single-walled carbon nanotubes.

[0107] A comparison of Example 1 and Comparative Example 8 shows that without microwave radiation treatment, the insufficient synergistic constraint of the ternary metal leads to insufficient catalyst activity or uneven size distribution, resulting in low yield and wide diameter range of the grown single-walled carbon nanotubes.

[0108] This application illustrates its detailed structural features through the above embodiments, but it is not limited to these detailed structural features, meaning that this application does not necessarily rely on them for implementation. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of selected components, additions of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this application.

Claims

1. A catalyst for preparing single-walled carbon nanotubes, characterized in that, The catalyst includes a substrate and an active component supported on the substrate; The active components include Cu, Fe, and noble metals; The molar ratio of Cu to Fe is 1:(0.1-1).

2. The catalyst according to claim 1, characterized in that, The precious metal includes any one or a combination of at least two of Pt, Rh, Ir, Ag or Pd; And / or, the total molar amount of Cu and Fe to the molar ratio of the noble metal is (1-4):1; And / or, the particle size of the active component is 1nm-2nm; The thickness of the coating containing the active components is 50nm-200nm.

3. The catalyst according to claim 1, characterized in that, The substrate includes a silicon wafer and / or a silicon wafer with an oxide layer loaded on its surface; The thickness of the oxide layer is 200nm-400nm.

4. A method for preparing the catalyst according to any one of claims 1-3, characterized in that, The preparation method includes: A copper salt, an iron salt, a first organic polymer, and a first organic solvent are mixed to obtain an Fe-Cu catalytic precursor; the molar ratio of the copper salt to the iron salt is 1:(0.1-1). A mixture of noble metal salt, second organic polymer and the Fe-Cu catalytic precursor is subjected to microwave irradiation to obtain a multi-element alloy colloid. The multi-element alloy colloid was coated onto a substrate and then subjected to annealing and reduction in sequence to obtain the catalyst.

5. The preparation method according to claim 4, characterized in that, The first organic solvent includes alcohol solvents; And / or, the first organic polymer and the second organic polymer each independently comprise any one or a combination of at least two of polyvinylpyrrolidone, polyvinyl alcohol, or polymethyl methacrylate; And / or, the molar ratio of the first organic polymer to the copper salt is (1-5):

1.

6. The preparation method according to claim 4, characterized in that, The total molar amount of Cu and Fe in the Fe-Cu catalytic precursor is in the molar ratio of the noble metal salt to (1-4):

1. And / or, the molar ratio of the second organic polymer to the noble metal salt is (1-4):1; And / or, the noble metal salt includes any one or a combination of at least two of Pt salts, Rh salts, Ir salts, Ag salts or Pd salts; And / or, the power of the microwave radiation treatment is 3kW-5kW and the time is 1min-3min; And / or, the microwave radiation treatment further includes: adding a second organic solvent to the microwave radiation treatment product, performing solid-liquid separation and washing in sequence, and then dispersing the precipitate in a first organic solvent.

7. The preparation method according to claim 4, characterized in that, The coating method includes spin coating; And / or, the coating thickness is 50nm-200nm; And / or, the annealing is performed in an air atmosphere; And / or, the annealing temperature is 500℃-700℃; And / or, the annealing time is 20 min-40 min; And / or, both the annealing and the reduction are carried out in a tube furnace; And / or, the reduction is carried out in a hydrogen-containing atmosphere; And / or, the reduction temperature is 910℃-1000℃; And / or, the reduction time is 10 min to 30 min.

8. A method for preparing single-walled carbon nanotubes with a narrow diameter distribution, characterized in that, The preparation method includes: Under the action of the catalyst as described in any one of claims 1-3, a carbon source and a carrier gas are introduced to carry out a reaction to obtain the single-walled carbon nanotubes.

9. The preparation method according to claim 8, wherein the carbon source comprises methane; And / or, the carrier gas includes hydrogen; And / or, the volumetric flow rate ratio of the carbon source to the carrier gas is 1:(1-3); And / or, the reaction is carried out in a tube furnace; And / or, the temperature of the reaction is 800℃-1000℃; And / or, the reaction time is 20 min-40 min; And / or, the reaction may further include: The first and second cooling processes carried out during the furnace; The cooling rate of the first cooling is 8℃ / min-12℃ / min; The initial cooling temperature reaches 350℃-450℃; The second cooling process includes continuously introducing argon gas at a rate of 4 L / min to 6 L / min to cool to room temperature.

10. A single-walled carbon nanotube with a narrow diameter distribution, characterized in that, The single-walled carbon nanotubes are prepared using the preparation method described in claim 8 or 9; And / or, the average diameter of the single-walled carbon nanotubes is 1.0 nm to 2.0 nm; And / or, the proportion of the single-walled carbon nanotubes with a diameter in the range of 0.6 nm to 1.8 nm is ≥70%.