一种光催化材料及其制备方法

By combining hollow cadmium sulfide microspheres with silver sulfide and metallic gold to form a heterostructure, the problems of limited light absorption range and severe carrier recombination in the treatment of complex industrial waste gases by photocatalytic materials are solved, achieving efficient synergistic degradation of multi-component waste gases with good visible light response and stability.

CN123148968APending Publication Date: 2026-11-24CHINA TOBACCO FUJIAN IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611398467.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing photocatalytic materials suffer from limited light absorption range, severe recombination of photogenerated electron-hole pairs, and low carrier separation efficiency when treating complex industrial waste gases. This results in low degradation efficiency of competitive reactions of multiple pollutants, making it difficult to achieve efficient and simultaneous degradation of multi-component waste gases.

Method used

Hollow cadmium sulfide microspheres are combined with silver sulfide and metallic gold to form a heterostructure. Through photogenerated carrier separation and the generation of various active oxygen species, the synergistic and efficient degradation of multi-component industrial waste gases is achieved.

Benefits of technology

It enhances visible light response, improves carrier separation efficiency, and provides multi-site synergistic catalytic capability, achieving efficient oxidative degradation of volatile organic compounds such as phenol, formaldehyde, and toluene, as well as odorous gases such as ammonia and hydrogen sulfide, and exhibits good continuous operation stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148968A_ABST
    Figure CN123148968A_ABST
Patent Text Reader

Abstract

This invention provides a photocatalytic material and its preparation method. The photocatalytic material comprises: hollow cadmium sulfide microspheres; and silver sulfide and metallic gold loaded on the surface of the hollow cadmium sulfide microspheres. The preparation method of the photocatalytic material includes the following steps: providing hollow cadmium sulfide microspheres; dispersing the hollow cadmium sulfide microspheres in a solution containing silver sulfide precursor and gold precursor to obtain a precursor mixture; reducing the precursor mixture to generate silver sulfide and metallic gold on the surface of the hollow cadmium sulfide microspheres, thereby obtaining the photocatalytic material. This photocatalytic material enhances visible light absorption and shortens carrier migration paths through its hollow structure, while the silver sulfide and gold dual co-catalysts promote the directional separation of photogenerated electrons and the generation of various active species, thereby achieving efficient and synergistic degradation of multi-component industrial waste gases containing volatile organic compounds and nitrogen- and sulfur-containing odorous gases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalytic materials technology, specifically to a photocatalytic material and its preparation method. Background Technology

[0002] The tobacco industry emits large amounts of complex industrial waste gases during production, mainly including volatile organic compounds (VOCs) such as formaldehyde, toluene, and phenol, as well as typical odorous gases such as ammonia (NH3) and hydrogen sulfide (H2S). These waste gases are characterized by complex composition, large concentration fluctuations, high toxicity, and difficulty in degradation, posing a serious threat to the environment and human health.

[0003] Traditional treatment technologies for the aforementioned waste gases include activated carbon adsorption, combustion, and biological treatment. However, activated carbon adsorption suffers from drawbacks such as rapid saturation and the need for frequent replacement or regeneration; combustion is energy-intensive and may generate secondary pollutants; and biological treatment has high operating costs, and its treatment efficiency and stability are insufficient to meet the requirements of continuous industrial operation. Therefore, these methods are difficult to simultaneously meet the demands for efficient, stable, and environmentally friendly treatment in practical applications.

[0004] In recent years, photocatalytic oxidation technology has been considered a promising green waste gas treatment technology due to its ability to drive pollutant mineralization using light energy under mild conditions. However, existing photocatalytic materials generally suffer from the following bottlenecks: first, limited light absorption range and low utilization rate of visible light; second, severe recombination of photogenerated electron-hole pairs, resulting in low quantum efficiency; and third, single active sites on the catalyst surface. Especially when treating multi-component mixed waste gases, there is significant competitive adsorption and reaction between different pollutants, leading to a significant reduction in overall degradation efficiency. Furthermore, traditional photocatalysts lack effective structural design to achieve synergistic regulation of different reaction pathways, making it difficult to achieve simultaneous and efficient removal of multiple pollutants.

[0005] Therefore, there is an urgent need to develop a photocatalytic material with high light absorption capacity, excellent carrier separation performance and multi-site synergistic catalytic ability to meet the needs of efficient treatment of complex industrial waste gas. Summary of the Invention

[0006] To address the problems of severe recombination of photogenerated carriers and low degradation efficiency due to competitive reactions of multiple pollutants in existing photocatalytic materials, this invention provides a photocatalytic material and its preparation method. Hollow cadmium sulfide microspheres are combined with silver sulfide and gold as dual co-catalysts to form a heterostructure, thereby efficiently separating photogenerated carriers and generating various reactive oxygen species under visible light, achieving synergistic and efficient degradation of multi-component industrial waste gases.

[0007] The first aspect of this application provides a photocatalytic material comprising: hollow cadmium sulfide microspheres; and silver sulfide and metallic gold loaded on the surface of the hollow cadmium sulfide microspheres.

[0008] The applicant discovered that, in the aforementioned photocatalytic materials, hollow cadmium sulfide microspheres can enhance visible light absorption and shorten carrier migration paths, while providing a large specific surface area and abundant surface active sites, which is beneficial for the adsorption of pollutant molecules and interfacial reactions, effectively reducing the probability of electron-hole recombination. Silver sulfide, as an electron capture and surface reaction regulation center, helps to regulate the local charge distribution and promote the activation process of surface adsorbed molecules, thereby improving the oxidation conversion efficiency of nitrogen- and sulfur-containing gases. Gold, mainly as an electron enrichment and transport center, is beneficial to promoting the activation of oxygen molecules to generate reactive oxygen species such as superoxide radicals, thereby enhancing the ability to oxidize and decompose volatile organic pollutants. Silver sulfide and gold synergistically promote the directional separation and rapid migration of photogenerated electrons from cadmium sulfide to the cocatalyst sites. Thus, electrons migrating to the cocatalyst react with adsorbed oxygen to generate superoxide radicals, which are further converted into hydroxyl radicals, while holes directly oxidize organic pollutants or water molecules adsorbed on the cadmium sulfide surface to generate hydroxyl radicals. The synergistic effect of the aforementioned multiple reactive oxygen species enables the material to possess the potential for oxidative degradation of volatile organic compounds such as phenol, formaldehyde, and toluene, as well as malodorous gases such as ammonia and hydrogen sulfide. It exhibits characteristics such as strong visible light response, high carrier separation efficiency, and good stability during continuous operation.

[0009] In any embodiment of the first aspect, the average particle size of silver sulfide is 5 nm-10 nm, and / or the average particle size of metallic gold is 5 nm-10 nm.

[0010] In any embodiment of the first aspect, the total loading of silver sulfide and metallic gold is 1 wt% to 5 wt% of the mass of the photocatalytic material.

[0011] In any embodiment of the first aspect, the mass ratio of silver sulfide to metallic gold is 1:5 to 5:1. Optionally, the mass ratio of silver sulfide to metallic gold is 1:2 to 2:1.

[0012] In any embodiment of the first aspect, the loading of silver sulfide is 0.5wt%-3wt% of the mass of the photocatalytic material.

[0013] In any embodiment of the first aspect, the loading of metallic gold is 0.5wt%-3wt% of the mass of the photocatalytic material.

[0014] In any embodiment of the first aspect, the average particle size of the hollow cadmium sulfide microspheres is 100 nm to 800 nm, and / or the shell thickness of the hollow cadmium sulfide microspheres is 5 nm to 20 nm.

[0015] In any embodiment of the first aspect, the shell of the hollow cadmium sulfide microspheres comprises a porous structure. Optionally, the hollow cadmium sulfide microspheres satisfy at least one of the following: (1) the average pore size of the hollow cadmium sulfide microspheres is 9 nm-14 nm, and (2) the BET specific surface area of ​​the hollow cadmium sulfide microspheres is 50 m². 2 g -1 -80m 2 g -1 .

[0016] The second aspect of this application provides a method for preparing a photocatalytic material, comprising the following steps: providing hollow cadmium sulfide microspheres; dispersing the hollow cadmium sulfide microspheres in a solution containing a silver sulfide precursor and a gold precursor to obtain a precursor mixture; and reducing the precursor mixture to generate silver sulfide and metallic gold on the surface of the hollow cadmium sulfide microspheres to obtain the photocatalytic material.

[0017] The above preparation method employs a stepwise strategy of first preparing hollow cadmium sulfide microspheres and then loading them with dual co-catalysts. This allows for independent control of the hollow structure construction and co-catalyst deposition, facilitating uniform loading of the co-catalysts on the pre-formed hollow structure surface. Pre-dispersing and mixing the hollow cadmium sulfide microspheres with silver sulfide and gold precursors before reduction treatment ensures uniform adsorption of the two co-catalyst precursors on the cadmium sulfide surface. This promotes the formation of highly dispersed silver sulfide and gold dual co-catalyst sites on the cadmium sulfide surface after reduction, and the resulting co-catalysts exhibit tight interfacial bonding with the cadmium sulfide substrate, facilitating rapid interfacial migration of photogenerated electrons. This method offers strong process controllability; the co-catalyst loading and dispersion state can be precisely controlled by adjusting the precursor concentration and reduction conditions, demonstrating good industrial feasibility and process stability.

[0018] In any embodiment of the second aspect, the ratio of the sum of the molar amounts of the silver sulfide precursor and the gold precursor to the molar amount of the hollow cadmium sulfide microspheres is 0.95%-3.8%, the molar amount of the hollow cadmium sulfide microspheres is calculated as CdS, the molar amount of the silver sulfide precursor is calculated as silver element, and the molar amount of the gold precursor is calculated as gold element.

[0019] In any embodiment of the second aspect, the molar ratio of the silver sulfide precursor to the gold precursor is 0.3:1 to 8:1.

[0020] In any embodiment of the second aspect, the molar ratio of silver sulfide precursor to gold precursor in the precursor mixture is 0.8:1 to 3.2:1.

[0021] In any embodiment of the second aspect, the molar concentration of the silver sulfide precursor in the precursor mixture is 0.05 mmol / L to 0.5 mmol / L.

[0022] In any embodiment of the second aspect, the molar concentration of the gold precursor in the precursor mixture is 0.02 mmol / L to 0.3 mmol / L.

[0023] In any embodiment of the second aspect, the silver sulfide precursor includes at least one of silver nitrate, sodium sulfide, and thioacetamide, and the gold precursor includes at least one of chloroauric acid and sodium borohydride.

[0024] In any implementation of the second aspect, the reduction process is a photoreduction process.

[0025] In any embodiment of the second aspect, the illumination conditions for the light reduction process satisfy one or more of the following: 1) the light source for the light reduction process is a xenon lamp or an LED light source; 2) the light intensity for the light reduction process is 800 mW / cm². 2 -1000mW / cm 2 3) The photoreduction treatment time is 2-4 hours.

[0026] In any embodiment of the second aspect, the step of providing hollow cadmium sulfide microspheres includes: using silica nanospheres as templates, forming a cadmium sulfide shell on the surface of silica nanospheres to obtain a silica / cadmium sulfide core-shell structure; and removing the silica nanospheres to obtain hollow cadmium sulfide microspheres.

[0027] In any embodiment of the second aspect, the average particle size of the silica nanospheres is 350 nm to 400 nm. Attached Figure Description

[0028] The accompanying drawings are provided to further illustrate the invention and form part of this invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation thereof. In the drawings:

[0029] Figure 1 The XRD patterns of SiO2, SiO2@CdS, and hollow cadmium sulfide microspheres prepared in Example 1 are shown.

[0030] Figure 2 The XRD patterns of the photocatalytic materials modified with different Ag2S and Au loadings (XAg2S-YAu) prepared in Examples 1-6 and Comparative Examples 1-3 are shown.

[0031] Figure 3 SEM (ac) and TEM (df) images of the hollow cadmium sulfide microspheres prepared in Example 1.

[0032] Figure 4SEM (a), TEM (b), HRTEM (c) and EDS energy spectrum (d) of 3Au / CdSH prepared for Comparative Example 1, and SEM (e), TEM (f), HRTEM (g) and EDS energy spectrum (h) of 3Ag2S / CdSH prepared for Comparative Example 2.

[0033] Figure 5 SEM (a), TEM (b, c), HRTEM (d), and EDS energy spectrum (e) of 1.5Ag2S-1.5Au / CdSH prepared in Example 1.

[0034] Figure 6 The formaldehyde photocatalytic degradation performance of hollow CdS and catalysts with different Ag2S and Au loadings prepared for Examples 1 and Comparative Examples 3-5 is shown in the figure.

[0035] Figure 7 The graph shows the photocatalytic degradation performance of ammonia by hollow CdS and catalysts with different Ag2S and Au loadings prepared for Examples 1 and Comparative Examples 3-5.

[0036] Figure 8 Comparison of formaldehyde photocatalytic degradation kinetics for hollow CdS and catalysts with different Ag2S and Au loadings prepared in Examples 1 and Comparative Examples 3-5.

[0037] Figure 9 Cyclic stability tests of formaldehyde photocatalytic degradation using hollow CdS and catalysts with different Ag2S and Au loadings prepared for Examples 1 and Comparative Examples 3-5. Detailed Implementation

[0038] The embodiments of the present invention will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are for illustrative purposes only and should not be considered as limiting the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0039] To address the problems of severe photogenerated carrier recombination and low degradation efficiency due to competitive reactions among multiple pollutants in existing photocatalytic materials, this application conducted in-depth research and found that traditional photocatalysts have single active sites, are prone to photogenerated electron-hole recombination, and the oxidation and reduction processes occur disorderly in the same surface region. This leads to different pollutants in multi-component waste gases competing for the same active sites, making it difficult to achieve simultaneous and efficient degradation. This application proposes to construct a heterogeneous structure system composed of hollow cadmium sulfide microspheres and silver sulfide and gold dual co-catalysts. Superoxide radicals and hydroxyl radicals are generated at the electron and hole ends, respectively, providing differentiated reaction pathways for different pollutants. Based on this idea, this application proposes a photocatalytic material and its preparation method.

[0040] The first embodiment of this application provides a photocatalytic material, comprising: hollow cadmium sulfide microspheres; and silver sulfide and metallic gold loaded on the surface of the hollow cadmium sulfide microspheres.

[0041] The applicant discovered that, in the aforementioned photocatalytic materials, hollow cadmium sulfide microspheres can enhance visible light absorption and shorten carrier migration paths, while providing a large specific surface area and abundant surface active sites, which is beneficial for the adsorption of pollutant molecules and interfacial reactions, effectively reducing the probability of electron-hole recombination. Silver sulfide, as an electron capture and surface reaction regulation center, helps to regulate the local charge distribution and promote the activation process of surface adsorbed molecules, thereby improving the oxidation conversion efficiency of nitrogen- and sulfur-containing gases. Gold, mainly as an electron enrichment and transport center, is beneficial to promoting the activation of oxygen molecules to generate reactive oxygen species such as superoxide radicals, thereby enhancing the ability to oxidize and decompose volatile organic pollutants. Silver sulfide and gold synergistically promote the directional separation and rapid migration of photogenerated electrons from cadmium sulfide to the cocatalyst sites. Thus, electrons migrating to the cocatalyst react with adsorbed oxygen to generate superoxide radicals, which are further converted into hydroxyl radicals, while holes directly oxidize organic pollutants or water molecules adsorbed on the cadmium sulfide surface to generate hydroxyl radicals. The synergistic effect of the aforementioned multiple reactive oxygen species enables the material to possess the potential for oxidative degradation of volatile organic compounds such as phenol, formaldehyde, and toluene, as well as malodorous gases such as ammonia and hydrogen sulfide. It exhibits characteristics such as strong visible light response, high carrier separation efficiency, and good stability during continuous operation.

[0042] In some embodiments, the average particle size of silver sulfide is 5 nm to 10 nm. For example, the average particle size of silver sulfide can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or within any two of the above values. The above average particle size is beneficial for the dispersion of silver sulfide nanoparticles on the surface of hollow cadmium sulfide microspheres, resulting in a more uniform distribution of electron trapping sites and reducing carrier recombination caused by local charge accumulation.

[0043] In some embodiments, the average particle size of metallic gold is 5 nm to 10 nm. For example, the average particle size of metallic gold can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or within any two of the above values. This average particle size allows gold nanoparticles to expose more active crystal faces, enhancing their adsorption and activation capacity for oxygen molecules, thereby promoting the generation efficiency of superoxide radicals.

[0044] In some embodiments, the total loading of silver sulfide and metallic gold is 1wt%-5wt% of the mass of the photocatalytic material. For example, the total loading of silver sulfide and metallic gold can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt% of the mass of the photocatalytic material, or within any two of the above values. Controlling the total loading within the above range is beneficial to achieve sufficient active sites while reducing the masking effect of excessive loading on the light absorption of the hollow cadmium sulfide microspheres, thus maintaining the generation and separation efficiency of photogenerated carriers.

[0045] In some embodiments, the mass ratio of silver sulfide to metallic gold is 1:5 to 5:1. For example, the mass ratio of silver sulfide to metallic gold can be 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, or within any two of the above ratios. By adjusting the ratio of the two, the oxidative conversion function for nitrogen- and sulfur-containing gases and the oxidative decomposition function for volatile organic compounds can be adjusted, enabling the catalyst to play a synergistic degradation role in waste gas systems with different pollutant compositions.

[0046] In some embodiments, the mass ratio of silver sulfide to metallic gold is 1:2 to 2:1, within which the functional synergy between the two is more prominent.

[0047] In some embodiments, the loading of silver sulfide is 0.5 wt%-3 wt% of the photocatalytic material. For example, the loading of silver sulfide can be 0.5 wt%, 1 wt%, 2 wt%, 3 wt% of the photocatalytic material, or within any two of the above values. This loading of silver sulfide facilitates the formation of electron trapping and surface reaction regulation sites of suitable density on the surface of hollow cadmium sulfide microspheres, promoting the activation and conversion of nitrogen- and sulfur-containing gases.

[0048] In some embodiments, the loading of metallic gold is 0.5 wt%-3 wt% of the mass of the photocatalytic material. For example, the loading of metallic gold can be 0.5 wt%, 1 wt%, 2 wt%, 3 wt% of the mass of the photocatalytic material, or within any two of the above values. The above-mentioned loading of metallic gold is beneficial for forming sufficient electron enrichment and transport centers, enabling photogenerated electrons to rapidly migrate to the gold surface to participate in the reduction and activation reaction of oxygen molecules.

[0049] In some embodiments, the average particle size of the hollow cadmium sulfide microspheres is 100 nm to 800 nm. For example, the average particle size of the hollow cadmium sulfide microspheres can be 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or within any two of the above values. Controlling the average particle size of the hollow cadmium sulfide microspheres within the above range is beneficial for balancing the light scattering enhancement effect of the hollow structure with the path length of charge carrier migration to the surface, thus maintaining both light energy utilization and charge separation at a relatively optimal level.

[0050] In some embodiments, the shell thickness of the hollow cadmium sulfide microspheres is 5 nm-20 nm. For example, the shell thickness of the hollow cadmium sulfide microspheres can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, or within any two of the above values. A shell thickness within this range facilitates the rapid migration of photogenerated carriers to the shell surface to participate in the reaction, reducing recombination losses of carriers during bulk migration.

[0051] In some embodiments, the shell of the hollow cadmium sulfide microspheres includes a porous structure, which is beneficial for increasing the specific surface area and exposing more reactive sites, while providing channels for pollutant molecules to diffuse into the interior of the shell, thereby enhancing the contact efficiency between pollutants and reactive sites.

[0052] In some embodiments, the average pore size of the hollow cadmium sulfide microspheres is 9 nm to 14 nm. For example, the average pore size of the hollow cadmium sulfide microspheres can be 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, or within any two of the above values. This pore size is advantageous in maintaining a high specific surface area of ​​the shell and providing sufficient active sites for the catalytic reaction, while allowing pollutants of various molecular sizes to effectively enter the pores and participate in the reaction, thus improving the catalyst's adaptability to multi-component mixed waste gases.

[0053] In some embodiments, the BET specific surface area of ​​the hollow cadmium sulfide microspheres is 50 m². 2 g -1 -80m 2 g -1 For example, 50m 2 g -1 60m 2 g -1 70m 2 g -1 80m 2 g -1Or within the range of any two of the above values. This specific surface area is beneficial for providing sufficient adhesion area for the co-catalyst loading, while enhancing the adsorption and enrichment capacity for gaseous pollutants and improving the photocatalytic reaction rate.

[0054] The second embodiment of this application provides a method for preparing a photocatalytic material, comprising the following steps: providing hollow cadmium sulfide microspheres; dispersing the hollow cadmium sulfide microspheres in a solution containing a silver sulfide precursor and a gold precursor to obtain a precursor mixture; and reducing the precursor mixture to generate silver sulfide and metallic gold on the surface of the hollow cadmium sulfide microspheres to obtain the photocatalytic material.

[0055] The above preparation method employs a stepwise strategy of first preparing hollow cadmium sulfide microspheres and then loading them with dual co-catalysts. This allows for independent control of the hollow structure construction and co-catalyst deposition, facilitating uniform loading of the co-catalysts on the pre-formed hollow structure surface. Pre-dispersing and mixing the hollow cadmium sulfide microspheres with silver sulfide and gold precursors before reduction treatment ensures uniform adsorption of the two co-catalyst precursors on the cadmium sulfide surface. This promotes the formation of highly dispersed silver sulfide and gold dual co-catalyst sites on the cadmium sulfide surface after reduction, and the resulting co-catalysts exhibit tight interfacial bonding with the cadmium sulfide substrate, facilitating rapid interfacial migration of photogenerated electrons. This method offers strong process controllability; the co-catalyst loading and dispersion state can be precisely controlled by adjusting the precursor concentration and reduction conditions, demonstrating good industrial feasibility and process stability.

[0056] In some embodiments, the ratio of the sum of the molar amounts of the silver sulfide precursor and the gold precursor to the molar amount of the hollow cadmium sulfide microspheres in the precursor mixture is 0.95%-3.8%, where the molar amount of the hollow cadmium sulfide microspheres is calculated as CdS, the molar amount of the silver sulfide precursor is calculated as silver element, and the molar amount of the gold precursor is calculated as gold element. For example, the ratio of the sum of the molar amounts of the silver sulfide precursor and the gold precursor to the molar amount of the hollow cadmium sulfide microspheres in the precursor mixture can be 0.95%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8%, or within any two of the above values. Controlling the ratio within the above range is beneficial for regulating the loading of the co-catalyst on the surface of hollow cadmium sulfide microspheres, so that silver sulfide and gold can provide sufficient active sites, but are not prone to agglomeration or covering of the light-absorbing surface of cadmium sulfide due to excessive loading.

[0057] In some embodiments, the molar ratio of silver sulfide precursor to gold precursor in the precursor mixture is 0.3:1 to 8:1. For example, the molar ratio of silver sulfide precursor to gold precursor in the precursor mixture can be 0.3:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, or within any two of the above ratios. By adjusting the feeding ratio of the two precursors, it is beneficial to flexibly adjust the relative content of silver sulfide and gold in the final product, thereby specifically optimizing the synergistic degradation performance of the catalyst on nitrogen- and sulfur-containing gases and volatile organic compounds.

[0058] In some embodiments, the molar ratio of silver sulfide precursor to gold precursor in the precursor mixture is 0.8:1 to 3.2:1.

[0059] In some embodiments, the molar concentration of silver sulfide precursor in the precursor mixture is 0.05 mmol / L to 0.5 mmol / L. For example, the molar concentration of silver sulfide precursor in the precursor mixture can be 0.05 mmol / L, 0.06 mmol / L, 0.07 mmol / L, 0.08 mmol / L, 0.09 mmol / L, 0.1 mmol / L, 0.2 mmol / L, 0.3 mmol / L, 0.4 mmol / L, 0.5 mmol / L, or within any two of the above values. Controlling the mass percentage of silver sulfide precursor within this range is beneficial for forming a suitable number of silver sulfide deposition sites during the subsequent reduction process, thereby enhancing the catalyst's ability to oxidize and convert nitrogen- and sulfur-containing gases.

[0060] In some embodiments, the molar concentration of the gold precursor in the precursor mixture is 0.02 mmol / L-0.3 mmol / L. For example, the molar concentration of the gold precursor in the precursor mixture can be 0.02 mmol / L, 0.03 mmol / L, 0.04 mmol / L, 0.05 mmol / L, 0.06 mmol / L, 0.07 mmol / L, 0.08 mmol / L, 0.09 mmol / L, 0.1 mmol / L, 0.2 mmol / L, 0.3 mmol / L, or within any two of the above values. Controlling the mass percentage of the gold precursor within this range is beneficial for forming a uniformly distributed gold layer on the cadmium sulfide surface, which serves as an electron enrichment and transport center, thereby enhancing the interfacial migration rate of photogenerated electrons.

[0061] In some embodiments, the silver sulfide precursor includes at least one of silver nitrate, sodium sulfide, and thioacetamide.

[0062] In some embodiments, the gold precursor includes at least one of chloroauric acid and sodium borohydride.

[0063] In some embodiments, the reduction process is a photoreduction process, which can directly reduce precursor ions into a cocatalyst by using electrons generated by cadmium sulfide itself under light. This facilitates the formation of a tight interfacial contact between the cocatalyst and cadmium sulfide, reduces the hindrance of charge migration by interfacial defects, and eliminates the need for external reducing agents, making the process green and simple.

[0064] In some embodiments, the light source for the photoreduction process is a xenon lamp or an LED light source, which can provide illumination that matches the light absorption range of cadmium sulfide, thus facilitating the efficient excitation of cadmium sulfide to generate photogenerated electrons to drive the reduction reaction.

[0065] In some embodiments, the light intensity of the light reduction process is 800 mW / cm². 2 -1000mW / cm 2 For example, the light intensity of the light reduction process can be 800 mW / cm². 2 900mW / cm 2 1000mW / cm 2 Or within the range of any two of the above values. Controlling the light intensity within the above range helps to balance the reaction rate and the uniformity of catalyst nucleation, reducing particle agglomeration caused by excessively rapid reaction.

[0066] In some embodiments, the photoreduction treatment time is 2-4 hours, for example, the photoreduction treatment time can be 2 hours, 3 hours, 4 hours or within any two of the above values. The above treatment time is conducive to the full reduction and deposition of precursor ions on the cadmium sulfide surface, while completing the loading process in a shorter time and reducing photocorrosion that may be caused by prolonged light exposure.

[0067] In some embodiments, the step of providing hollow cadmium sulfide microspheres includes: using silica nanospheres as templates, forming a cadmium sulfide shell on the surface of the silica nanospheres to obtain a silica / cadmium sulfide core-shell structure; and removing the silica nanospheres to obtain hollow cadmium sulfide microspheres. Using the above-described hard template method to construct hollow structures allows for independent control of the particle size and shell thickness of the hollow microspheres through template size and shell deposition conditions, resulting in hollow structures with regular morphology and good size uniformity.

[0068] In some embodiments, the average particle size of the silica nanospheres is 350 nm to 400 nm. By selecting silica nanospheres within the above particle size range as templates, it is beneficial to prepare hollow cadmium sulfide microspheres with the target cavity size, thereby achieving both enhanced light scattering effect and control of carrier migration distance.

[0069] [Example]

[0070] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0071] Example 1

[0072] This embodiment provides a photocatalytic material, comprising hollow cadmium sulfide microspheres and silver sulfide and metallic gold loaded on the surface of the hollow cadmium sulfide microspheres. The specific preparation method is as follows:

[0073] 1) Provide hollow cadmium sulfide microspheres:

[0074] a) Synthesis of SiO2 template: 20 mL of anhydrous ethanol, 6 mL of concentrated ammonia (28% by mass), and 20 mL of deionized water were mixed and magnetically stirred at 800 rpm at room temperature to ensure complete homogenization. Then, 3 mL of tetraethyl orthosilicate (TEOS) was pre-dissolved in 15 mL of ethanol to form a precursor solution, which was slowly added dropwise (over 10-15 minutes) to the mixture. After the addition was complete, the reaction was stirred for approximately 3 hours to allow TEOS to fully hydrolyze and condense under alkaline conditions to form SiO2 nanoparticles. After the reaction, the precipitate was separated by centrifugation and washed repeatedly with deionized water and ethanol alternately. Finally, it was vacuum dried at 50 °C for 12 hours to obtain spherical SiO2 template particles with a relatively uniform particle size distribution and an average particle size of approximately 350 nm-400 nm.

[0075] b) Construction of the SiO2@CdS core-shell structure: 100 mg of the SiO2 template prepared above was dispersed in 80 mL of a 1:1 water / ethanol mixture and sonicated for 30 minutes to obtain a stable and homogeneous suspension. Then, 1 mL of 0.5 mol·L⁻¹ mol·L⁻¹ mol·L⁻¹ was added to the system. -1 A sodium citrate solution was used as a surface coordination modifier. Then, an aqueous solution containing 0.5 mmol of CdCl2 was slowly added under continuous stirring to allow the CdCl2 to react with the surrounding material. 2+ The CdS core-shell structure was uniformly distributed on the SiO2 surface. Then, 1 mmol of thioacetamide (TAA) was added as a sulfur source, and the reaction was carried out at 70°C for 4 hours to allow CdS to grow in situ on the SiO2 surface, forming a shell. After the reaction was complete, the product was centrifuged, washed, and dried to obtain the SiO2@CdS core-shell structure.

[0076] c) Construction of porous hollow cadmium sulfide microspheres: The above SiO2@CdS sample was dispersed in 0.5 mol·L⁻¹ -1In a sodium carbonate (Na₂CO₃) solution, the mixture was heated and stirred at 80°C for approximately 4 hours to remove the SiO₂ template while retaining the outer CdS shell. The CdS shell formed a hollow structure while simultaneously creating a porous structure. After the reaction, the mixture was centrifuged and washed until neutral, then dried at 60°C to obtain porous hollow cadmium sulfide microspheres (CdSH, or CdShollow) with a shell thickness of approximately 5-15 nm. The average pore size of these hollow cadmium sulfide microspheres was measured to be 10 nm, and the BET specific surface area was 63.7 m². 2 g -1 .

[0077] 2) Hollow cadmium sulfide microspheres were dispersed in an ethanol / water mixed solution, and silver sulfide precursor and gold precursor were added to obtain a precursor mixture:

[0078] 50 mg of the above hollow cadmium sulfide microspheres were dispersed in 40 mL of a 2:1 volume ratio ethanol / water mixture. After sonication for 20 minutes, 0.00605 mmol AgNO3 and 0.00381 mmol HAuCl4 solution were added under light-protected conditions, and the mixture was stirred continuously for one hour until homogeneous to obtain the precursor mixture.

[0079] 3) The precursor mixture was reduced to generate silver sulfide and metallic gold on the surface of hollow cadmium sulfide microspheres, thus obtaining the photocatalytic material:

[0080] Slowly add 0.02 mmol of Na₂S solution dropwise to the above precursor mixture, allowing the adsorbed Ag to... + In-situ conversion into silver sulfide nanoparticles was achieved over a period of 2 hours. Subsequently, the reaction was carried out for another 2 hours under visible light LED illumination (420 nm wavelength), resulting in photoreduction deposition of Au at the interface region, forming a tightly coupled silver sulfide-gold interface structure. After the reaction, the material was washed and dried to obtain the photocatalytic material, denoted as 1.5Ag₂S-1.5Au / CdSH, where the mass ratio of Ag₂S to Au was approximately 1:1.

[0081] The measurements showed that in the final 1.5Ag2S-1.5Au / CdSH, the average particle size of silver sulfide was about 5 nm, the average particle size of metallic gold was about 5 nm, the average particle size of hollow cadmium sulfide microspheres was about 420 nm, and the shell thickness of the hollow cadmium sulfide microspheres was about 10 nm.

[0082] Comparative Example 1

[0083] The difference from Example 1 is that silver sulfide is not loaded, that is, in step 2), only 0.00762 mmol of HAuCl4 solution is added instead of AgNO3, and in step 3), Na2S solution is not added dropwise. Only photoreduction deposition of metallic gold is performed. The remaining steps are the same as in Example 1, and 3Au / CdSH material is obtained.

[0084] Comparative Example 2

[0085] The difference from Example 1 is that no metallic gold is loaded, that is, in step 2), only 0.0121 mmol of AgNO3 solution is added instead of HAuCl4 solution, and in step 3), no photoreduction treatment is performed after adding Na2S solution. The remaining steps are the same as in Example 1, and 3Ag2S / CdSH material is obtained.

[0086] Comparative Example 3

[0087] The difference from Example 1 is that silver sulfide and metallic gold are not loaded, that is, AgNO3 and HAuCl4 solution are not added in step 2), and reduction treatment is not performed in step 3), only step 1) is completed to obtain hollow cadmium sulfide microspheres (CdSH).

[0088] Examples 2-5

[0089] The difference between this series of examples and Example 1 is that photocatalytic materials with different mass ratios of silver sulfide to gold are prepared by adjusting the amount of AgNO3 and HAuCl4 solutions added. The remaining steps are the same as in Example 1. Specifically, in Examples 2-5, the mass ratios of Ag2S to Au are 2:1, 1:2, 0.5:2.5 and 2.5:0.5, respectively.

[0090] The following describes the structural characterization and performance evaluation of the photocatalytic materials prepared in the above examples and comparative examples.

[0091] Structural characterization

[0092] The photocatalytic materials in Examples 1-5 and Comparative Examples 1-3 were systematically characterized and analyzed, and the results are as follows: Figure 1-5 As shown in the image.

[0093] like Figure 1 and 2X-ray powder diffraction (XRD) results showed that the hollow cadmium sulfide microspheres and Ag2S-Au / CdSH composite photocatalyst materials prepared in Examples 1-5 all exhibited characteristic diffraction peaks consistent with hexagonal CdS, indicating that the CdS crystal structure was successfully formed. Furthermore, comparison of the XRD diffraction patterns revealed that the positions of the main diffraction peaks did not change significantly after loading silver sulfide and gold, indicating that the introduction of the co-catalyst did not disrupt the CdS crystal structure. Simultaneously, due to the low loading and high dispersion of silver sulfide and gold, their characteristic peaks did not show significant enhancement, indirectly indicating that the co-catalyst existed in a highly dispersed form on the surface of the hollow cadmium sulfide microspheres.

[0094] Figure 3 The scanning electron microscope (SEM) test results showed that the hollow cadmium sulfide microspheres prepared in Example 1 exhibited a uniformly distributed spherical structure with an average particle size concentrated in the range of 200-350 nm and good dispersibility. Figure 3 The results of high-resolution transmission electron microscopy (HRTEM) in the middle (df) showed that the hollow cadmium sulfide microspheres prepared in Example 1 had obvious hollow structure characteristics, uniform shell thickness, and clearly visible internal cavities.

[0095] Figure 4 (a)-(d) show the relevant spectra of 3Au / CdSH prepared in Comparative Example 1. Figure 4 (e)-(h) show the relevant spectra of 3Ag2S / CdSH prepared in Comparative Example 2. It can be seen that they all have spherical hollow structures, and the surface elements have also been confirmed.

[0096] Figure 5 The scanning electron microscope (SEM) test results in (a) show that after loading silver sulfide and metallic gold in Example 1, the sample still maintains the original spherical structure, and no obvious structural collapse or particle agglomeration was observed, indicating that the loading method used in this application has a good retention effect on the main structure.

[0097] Figure 5 High-resolution transmission electron microscopy (HRTEM) results from (bc) indicate that the prepared cadmium sulfide material exhibits a distinct hollow structure with uniform shell thickness and clearly visible internal cavities. Figure 5 In the high-magnification image (d), nanoparticles distributed on the surface of hollow cadmium sulfide microspheres can be observed, corresponding to the supported silver sulfide and gold metal co-catalysts. Figure 5 Energy dispersive X-ray spectroscopy (EDS) analysis in (e) clearly detected the signals of Cd, S, Ag and Au elements, and each element was uniformly distributed in the nanosphere structure, further proving that the dual co-catalyst was successfully loaded on the surface of hollow cadmium sulfide microspheres.

[0098] Formaldehyde degradation performance test

[0099] Comparative Example 4

[0100] The difference from Example 1 is that no metallic gold is loaded, that is, in step 2), only 0.00605 mmol of AgNO3 solution is added instead of HAuCl4 solution, and in step 3), no photoreduction treatment is performed after adding Na2S solution. The remaining steps are the same as in Example 1, and 1.5Ag2S / CdSH material is obtained.

[0101] Comparative Example 5

[0102] The difference from Example 1 is that silver sulfide is not loaded, that is, in step 2), only 0.00381 mmol of HAuCl4 solution is added instead of AgNO3, and in step 3), Na2S solution is not added dropwise. Only photoreduction deposition of metallic gold is performed. The remaining steps are the same as in Example 1, and 1.5Au / CdSH material is obtained.

[0103] Using formaldehyde as a typical volatile organic pollutant, the degradation performance of the photocatalytic materials prepared in Example 1 (1.5Ag₂S-1.5Au / CdS), Comparative Example 3 (CdS), Comparative Example 4 (1.5Ag₂S / CdS), and Comparative Example 5 (1.5Au / CdS) was evaluated. The results are as follows: Figure 6 As shown in the figure. The experiment was conducted in a closed photocatalytic reaction system. 0.05 g of photocatalytic material was uniformly dispersed in a quartz reactor, and formaldehyde simulated waste gas with an initial concentration of 20-100 ppm was introduced. After reaching adsorption-desorption equilibrium, a visible light source (λ≥420 nm) was turned on to carry out the photocatalytic reaction.

[0104] Experimental results showed that formaldehyde concentration decreased rapidly within the first 30 minutes of the light-induced reaction. The 1.5Ag₂S-1.5Au / CdSH (silver sulfide to gold mass ratio of 1.5:1.5) prepared in Example 1 achieved a formaldehyde removal rate of over 95% after 60 minutes of reaction, significantly higher than that of CdSH in Comparative Example 3 (approximately 40%), Au / CdSH in Comparative Example 1, and Ag₂S / CdSH in Comparative Example 2 (approximately 65%-80%). Furthermore, no significant accumulation of intermediate toxic byproducts was detected during the reaction, indicating that this catalytic system possesses excellent mineralization capabilities.

[0105] Furthermore, further comparisons show that, under the same test conditions, the formaldehyde removal rate of 1.5Ag₂S-1.5Au / CdSH prepared in Example 1 is higher than the total removal rate measured after physically mixing 1.5Ag₂S / CdSH from Comparative Example 4 and 1.5Au / CdSH from Comparative Example 5 with the same catalyst dosage. This result indicates that when silver sulfide and metallic gold are co-loaded on the surface of hollow cadmium sulfide microspheres, the degradation effect is not simply an additive result of the degradation effects of two single co-catalysts, but rather a superior photocatalytic degradation performance is achieved through the synergistic effect between the two co-catalysts.

[0106] Ammonia degradation performance test

[0107] Using ammonia as a typical nitrogen-containing odorous gas, the degradation performance of the photocatalytic materials prepared in Example 1 and Comparative Examples 3-5 was evaluated, and the results are as follows: Figure 7 As shown in the figure. The experiment was conducted in a closed photocatalytic reaction system. 0.2 g of photocatalytic material was uniformly dispersed in a quartz reactor, and ammonia gas with an initial concentration of 10-30 ppm was introduced to simulate waste gas. The humidified air flow rate was 1.0 mL / min. After adsorption-desorption equilibrium was reached, a visible light source (λ ≥ 420 nm) was turned on to carry out the photocatalytic reaction.

[0108] Experimental results show that the 1.5Ag₂S-1.5Au / CdSH (silver sulfide to gold mass ratio of 1.5:1.5) prepared in Example 1 achieved an ammonia removal rate of over 80% after 180 min of reaction, significantly higher than that of CdSH in Comparative Example 3 (approximately 10%), 1.5Ag₂S / CdS in Comparative Example 4, and 1.5Au / CdS in Comparative Example 5 (approximately 45%-65%). Furthermore, no significant accumulation of intermediate toxic byproducts was detected during the reaction process.

[0109] Furthermore, further comparisons show that, under the same test conditions, the ammonia removal rate of the 1.5 Ag₂S-1.5Au / CdSH prepared in Example 1 is higher than the total removal rate measured after physically mixing 1.5 Ag₂S / CdSH from Comparative Example 4 and 1.5Au / CdSH from Comparative Example 5 with the same catalyst dosage. This result indicates that when silver sulfide and metallic gold are co-loaded on the surface of hollow cadmium sulfide microspheres, the degradation effect is not simply a superposition of the degradation effects of two single co-catalysts, but rather a superior photocatalytic degradation performance for nitrogen-containing odorous gases is achieved through the synergistic effect between the two co-catalysts.

[0110] Photocatalytic kinetics analysis

[0111] The formaldehyde degradation process of the photocatalytic materials prepared in Example 1 and Comparative Examples 1-3 was fitted with pseudo-first-order kinetics, and the kinetic equations are as follows:

[0112] ln(q e -qt ) = lnq e - kt

[0113] Where, q e q represents the amount of formaldehyde adsorption and degradation that reaches equilibrium. t t represents the amount of formaldehyde adsorbed and degraded at reaction time t, and k is the apparent rate constant.

[0114] The results are as follows Figure 8 As shown in the figure, the experimental results indicate that the apparent rate constant of 1.5Ag₂S-1.5Au / CdSH (silver sulfide to gold mass ratio of 1.5:1.5) in Example 1 is significantly higher than that of the control sample, with a k value of approximately 0.150 min⁻¹. -1 In contrast, the CdSH content in Comparative Example 3 was only 0.125 min. -1 The 1.5Ag₂S / CdSH ratios of Comparative Example 4 and Comparative Example 5 were 0.133 min⁻¹. -1 and 0.140min -1 .

[0115] Based on the pseudo-first-order kinetic rate constant k, the synergistic factor SI was calculated using the following formula: SI = k dual co-catalyst / (k single Ag2S + k single Au - kCdS). The calculated synergistic factor SI is approximately 1.014, which is greater than 1. This result indicates that there is a positive synergistic effect between the silver sulfide and gold dual co-catalysts, which makes a positive contribution to the photocatalytic reaction kinetic rate.

[0116] Cyclic stability test

[0117] The 1.5Ag₂S-1.5Au / CdSH (silver sulfide to gold mass ratio of 1.5:1.5) prepared in Example 1 was subjected to five consecutive cyclic degradation experiments (with formaldehyde as the target pollutant). The results are as follows: Figure 9 As shown in the figure. After each reaction, the material was centrifuged, washed, and reused. The results showed that after 5 cycles, the formaldehyde removal rate remained above 90%, and the activity decay was less than 5%, indicating that the photocatalytic material has good stability for repeated use.

[0118] The results of the above examples and comparative examples show that the hollow cadmium sulfide microspheres and silver sulfide-gold dual co-catalyst system constructed in this application have been successfully prepared and have good structural stability and dispersibility. They can exhibit excellent multi-pollutant synergistic degradation ability and continuous operation stability in the photocatalytic degradation of complex industrial waste gases containing volatile organic compounds and nitrogen- and sulfur-containing odorous gases.

[0119] Although specific embodiments of the invention have been described in detail, those skilled in the art will understand that various modifications and substitutions can be made to those details based on all the teachings disclosed, and all such changes are within the scope of protection of the invention. The full scope of the invention is given by the appended claims and any equivalents thereof.

Claims

1. A photocatalytic material, comprising: Hollow cadmium sulfide microspheres; In addition, silver sulfide and metallic gold are loaded on the surface of the hollow cadmium sulfide microspheres.

2. The photocatalytic material according to claim 1, wherein, The average particle size of the silver sulfide is 5nm-10nm, and / or the average particle size of the metallic gold is 5nm-10nm.

3. The photocatalytic material according to claim 1 or 2, wherein, The total loading of silver sulfide and metallic gold is 1wt%-5wt% of the mass of the photocatalytic material.

4. The photocatalytic material according to any one of claims 1 to 3, wherein, The mass ratio of the silver sulfide to the metallic gold is 1:5 to 5:

1. Optionally, the mass ratio of the silver sulfide to the metallic gold is 1:2 to 2:

1. Optionally, the loading of silver sulfide is 0.5wt%-3wt% of the mass of the photocatalytic material. Optionally, the loading of the metallic gold is 0.5wt%-3wt% of the mass of the photocatalytic material.

5. The photocatalytic material according to any one of claims 1 to 4, wherein, The hollow cadmium sulfide microspheres have an average particle size of 100nm-800nm, and / or the shell thickness of the hollow cadmium sulfide microspheres is 5nm-20nm.

6. The photocatalytic material according to any one of claims 1 to 5, wherein, The shell of the hollow cadmium sulfide microspheres includes a porous structure. Optionally, the hollow cadmium sulfide microspheres satisfy at least one of the following: (1) The average pore size of the hollow cadmium sulfide microspheres is 9 nm-14 nm. (2) The BET specific surface area of ​​the hollow cadmium sulfide microspheres is 50 m². 2 g -1 -80m 2 g -1 .

7. A method for preparing a photocatalytic material, comprising the following steps: Hollow cadmium sulfide microspheres are available; The hollow cadmium sulfide microspheres were dispersed in a solution containing silver sulfide precursor and gold precursor to obtain a precursor mixture. The precursor mixture was reduced to generate silver sulfide and metallic gold on the surface of the hollow cadmium sulfide microspheres, thus obtaining a photocatalytic material.

8. The preparation method according to claim 7, wherein, In the precursor mixture, the ratio of the sum of the molar amounts of the silver sulfide precursor and the gold precursor to the molar amount of the hollow cadmium sulfide microspheres is 0.95%-3.8%. The molar amount of the hollow cadmium sulfide microspheres is calculated as CdS, the molar amount of the silver sulfide precursor is calculated as silver element, and the molar amount of the gold precursor is calculated as gold element.

9. The preparation method according to claim 7 or 8, wherein, In the precursor mixture, the molar ratio of the silver sulfide precursor to the gold precursor is 0.3:1-8:

1. Optionally, in the precursor mixture, the molar ratio of the silver sulfide precursor to the gold precursor is 0.8:1-3.2:

1. Optionally, the molar concentration of the silver sulfide precursor in the precursor mixture is 0.05 mmol / L to 0.5 mmol / L. Optionally, the molar concentration of the gold precursor in the precursor mixture is 0.02 mmol / L to 0.3 mmol / L.

10. The preparation method according to any one of claims 7 to 9, wherein, The silver sulfide precursor includes at least one of silver nitrate, sodium sulfide, and thioacetamide, and the gold precursor includes at least one of chloroauric acid and sodium borohydride.

11. The preparation method according to any one of claims 7 to 10, wherein, The reduction process is a photo-reduction process. Optionally, the illumination conditions for the light reduction process satisfy any one or more of the following: 1) The light source for the light reduction process is a xenon lamp or an LED light source. 2) The light intensity of the light reduction treatment is 800 mW / cm². 2 -1000mW / cm 2 , 3) The time for the light reduction process is 2-4 hours.

12. The preparation method according to any one of claims 7 to 11, wherein, The step of providing hollow cadmium sulfide microspheres includes: Using silica nanospheres as templates, a cadmium sulfide shell is formed on the surface of the silica nanospheres to obtain a silica / cadmium sulfide core-shell structure; The silica nanospheres were removed to obtain the hollow cadmium sulfide microspheres.

13. The preparation method according to any one of claims 7 to 12, wherein, The average particle size of the silica nanospheres is 350nm-400nm.