A hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst and a preparation method and application thereof
By preparing a hydrothermal carbon/high-entropy sulfide nanocomposite photocatalyst, the shortcomings of high-entropy sulfides in the photocatalytic carbon dioxide reduction coupled with 5-hydroxymethylfurfural conversion were solved, achieving high catalytic activity and stability, and possessing industrial application potential.
Patent Information
- Application Number
- CN202611429399.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, high-entropy sulfides have not been used for photocatalytic carbon dioxide reduction coupled with 5-hydroxymethylfurfural conversion, and the efficiency and stability of photocatalysts limit large-scale application.
A one-step microwave hydrothermal method was used to synthesize hydrothermal carbon/high-entropy sulfide nanocomposite photocatalysts. Two-dimensional S-shaped heterojunction nanocomposite materials were prepared by combining polymetallic salts with thioacetamide and waste biomass powder, which improved the separation efficiency and catalytic activity of photogenerated carriers.
It achieves selective conversion of CO₂ and HMF, improves the activity and stability of photocatalysts, simplifies the preparation process, and has good prospects for industrial application.
Smart Images

Figure CN123148971A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photocatalytic materials and biomass conversion technology, specifically relating to a hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst and its preparation method, as well as the application of the catalyst in photocatalytic carbon dioxide reduction coupled with 5-hydroxymethylfurfural (HMF) conversion. Background Technology
[0002] Using atmospheric CO2 as an abundant carbon source for solar catalytic conversion into low-carbon fuels offers an alternative solution to the potential shortage crisis resulting from the current heavy reliance on fossil fuels. Photocatalytic solar CO2 reduction (CO2-PR), inspired by natural photosynthesis, has attracted considerable attention due to its eco-friendly nature. However, despite efforts over the past few decades, the development of practical systems for large-scale applications has been limited by the efficiency and stability of the CO2-PR reaction. The selective oxidation of the biomass platform compound 5-hydroxymethylfurfural (HMF) to 2,5-dicarboxyfuran (DFF) is widely used in the chemical and medical fields due to its furanyl molecular ring.
[0003] The most common advantages of photocatalysts include their light-harvesting ability, extended charge carriers, abundant surface area, and active sites that promote intermediate transformations. Sulfur atoms possess a narrow band gap across the entire spectrum for photoactivation due to the more negative valence band generated by their 3p orbitals. Furthermore, the low electronegativity of sulfide atoms makes metal sulfides among the most conductive photocatalysts. On the other hand, compared to other nonmetallic materials, metallic elements in metallic materials contain empty d orbitals, which can acquire much more negative conduction band energies favorable for the CO2-PR reaction.
[0004] High-entropy materials, due to their increased structural entropy, lower the Gibbs free energy of the system and have been explored for CO2-PR and biomass conversion. High-entropy materials possess heterogeneous valence electron distribution and atomic disorder, and defects / strain can be generated in their structure, increasing active sites and facilitating CO2 adsorption and conversion. Furthermore, synergistic multi-metal interactions induce specific configurational and functional effects, the so-called "cocktail effect," thereby enhancing the system's CO2-PR capability. Recently, Akrami et al. synthesized TiZrNbHfTaO via impact wafer oxidation. 11The study evaluated the CO2-PR performance of high-entropy oxides, confirming their potential as novel CO2-PR materials. On the other hand, some previous researchers explored the application of high-entropy materials in biomass; for example, Xu et al. reported the biomass photoconversion potential of high-entropy materials. Currently, most research focuses on high-entropy alloys (HEM), high-entropy nitrides (HEN), and high-entropy oxides (HEO); there are no reports on the application of high-entropy sulfides (HES) in photocatalytic CO2 reduction coupled with biomass value-added utilization.
[0005] Currently, there is no evidence of high-entropy sulfides (HES) being used as catalysts in the photocatalytic carbon dioxide reduction coupled with 5-hydroxymethylfurfural (HMF) conversion. Summary of the Invention
[0006] To address the problems in the background technology, this invention provides a hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst and its preparation method. This invention uses a multi-metal salt (Co, Fe, Ni, Cu, Mn) precursor as an intermediate template, thioacetamide (C2H5NS) as the sulfur source for HES synthesis, and hydrothermal carbon (HTCC) prepared from waste biomass pomegranate peel powder. A two-dimensional nanocomposite material HTCC / (FeCuNiCoMn)S is synthesized via a one-step microwave hydrothermal method. x The two components form a strong interfacial interaction, resulting in an S-shaped heterostructure. This improves the separation efficiency of photogenerated carriers and also increases the reduction capacity of photogenerated electrons and the oxidation capacity of holes. By adjusting the loading of HTCC, the photocatalytic selective conversion of CO2 and HMF was achieved.
[0007] To achieve the above objectives, the present invention provides the following technical solution:
[0008] A hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst, wherein the composite photocatalyst is composed of high-entropy sulfide (HES) and hydrothermal carbon (HTCC) supported thereon; the high-entropy sulfide is (NiFeMnCoCu)S containing five metal elements. x A two-dimensional S-shaped heterojunction structure is formed between the two.
[0009] This invention also provides a method for preparing a hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst, specifically including the following steps:
[0010] (1) Add soluble copper salt, iron salt, manganese salt, cobalt salt and nickel salt to deionized water in an equimolar ratio and stir until completely dissolved to obtain a precursor solution;
[0011] (2) Add thioacetamide to the precursor solution and stir to dissolve it completely to obtain a mixture; wherein the molar ratio of the total molar amount of the five metal elements to the molar ratio of sulfur in the thioacetamide is controlled at 1:5 to 1:50.
[0012] (3) Add biomass powder to the mixture in step (2), stir evenly, transfer the mixture to a microwave hydrothermal reactor, and carry out microwave hydrothermal reaction at 140 ℃~200 ℃ for 60 min~120 min; after the reaction is completed, wash and dry the product to obtain hydrothermal carbon / high entropy sulfide nanocomposite photocatalyst.
[0013] Further, in step (1), the soluble copper salt, iron salt, manganese salt, cobalt salt and nickel salt are specifically copper acetate monohydrate, ferric nitrate nonahydrate, manganese acetate tetrahydrate, cobalt nitrate hexahydrate and nickel acetate tetrahydrate.
[0014] Furthermore, in step (2), the molar ratio of the total molar amount of the five metal elements in the precursor solution to the molar ratio of sulfur in the thioacetamide is preferably 1:20 to 1:40, and most preferably 1:30.
[0015] Furthermore, in step (3), the biomass powder is waste pomegranate peel powder, orange peel, chestnut shell or walnut shell;
[0016] Furthermore, the mass of biomass powder fed accounts for a certain percentage of the high-entropy sulfide [(Ni 0.2 Fe 0.2 Mn 0.2 Co 0.2 Cu 0.2 )S2】10 wt% ~ 50 wt% of the theoretically generated mass.
[0017] Furthermore, the feed mass of biomass powder is preferably 20 wt% to 40 wt% of the theoretical mass of the high-entropy sulfide, and most preferably 30 wt%.
[0018] Furthermore, in step (3), the temperature of the microwave hydrothermal reaction is preferably 160 ℃ ~ 180 ℃, and the time is preferably 80 min ~ 100 min.
[0019] Microwave hydrothermal technology can promote the simultaneous carbonization of biomass and its close in-situ recombination with high-entropy sulfides to form a two-dimensional S-shaped heterojunction structure.
[0020] Application of a hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst prepared by the above method in photocatalytic carbon dioxide reduction coupled with HMF conversion.
[0021] Specifically, in a photochemical reactor, the composite photocatalyst is used as the catalyst, an aqueous solution containing HMF is used as the reaction medium, CO2 gas is introduced, and under visible light irradiation, the reactions of CO2 reduction to CO and HMF selective oxidation to DFF are carried out simultaneously.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) This invention combines hydrothermal carbon (HTCC) with high-entropy sulfide (HES), forming a tight contact at the interface and generating a built-in electric field, resulting in an S-shaped heterojunction structure. Under photoexcitation, it not only effectively suppresses the recombination of photogenerated electrons and holes, but also retains electrons with strong reducing ability in the conduction band of high-entropy sulfide and holes with strong oxidizing ability in the valence band of hydrothermal carbon, thereby enhancing the photocatalytic activity of the material.
[0024] (2) The (NiFeMnCoCu)S used in this invention x High-entropy sulfides exhibit significant lattice expansion and structural defects due to the presence of multiple metal atoms. The synergistic effect among these metals exposes a large number of unsaturated catalytic active centers, lowering the reaction energy barrier for CO2 adsorption and activation. Meanwhile, hydrothermal carbon possesses a large specific surface area, abundant pore structure, and oxygen-containing functional groups on its surface, providing excellent electrical conductivity and substrate mass transfer channels for the reaction, thus promoting the catalytic reaction.
[0025] (3) The photocatalyst of this invention couples the reduction of CO2 with the oxidation of 5-hydroxymethylfurfural (HMF). During the photocatalytic process, the generated electrons are used to reduce CO2 to produce carbon monoxide (CO) fuel, and the holes are used to selectively oxidize HMF to 2,5-diformylfuran (DFF). Furthermore, the photocatalyst of this invention is prepared by a one-step microwave hydrothermal method, which completes the carbonization of hydrothermal carbon and the crystallization of high-entropy sulfides in a short time. It is time-saving, energy-efficient, and directly utilizes waste agricultural and forestry products as precursors. This process is simple to operate and has good prospects for industrial scale-up and economic benefits. Attached Figure Description
[0026] Figure 1 This is a schematic diagram of the preparation process of the HTCC / HES composite material in an embodiment of the present invention.
[0027] Figure 2 The images show the XRD patterns of composite materials prepared in the embodiments of the present invention with different molar ratios and mass fractions of (FeCuNiCoMn) and sulfur source. (a) shows the XRD patterns of (FeCuNiCoMn) with different molar ratios of sulfur source; (b) shows the XRD patterns of HTCC and 10-50 wt% HTCC / HES samples.
[0028] Figure 3 The images show the TEM and EDS elemental mappings of the 30 wt% HTCC / HES sample in this embodiment of the invention. (a) is the TEM image of the 30 wt% HTCC / HES sample; (b)-(c) are magnified views of the 30 wt% HTCC / HES sample at 50 nm and 10 nm; (d) is the HRTEM image of the 30 wt% HTCC / HES sample; and (e)-(n) are the EDS energy maps of the 30 wt% HTCC / HES sample regarding the distribution of each element (Co, Fe, Ni, Mn, Cu, S, C, and O).
[0029] Figure 4 The graph shows the photocatalytic CO2 reduction coupled HMF conversion performance and cycle stability test results of the composite photocatalyst in the embodiments of the present invention. Detailed Implementation
[0030] Source of pomegranate peel powder: Commercially available pomegranate peel powder is ground and sieved through a 100-mesh sieve;
[0031] Example 1:
[0032] First, synthesize the high-entropy sulfide (NiFeMnCoCu)S x :
[0033] (1) Add equimolar amounts (0.3 mmol) of 0.0599 g copper acetate monohydrate, 0.1212 g ferric nitrate nonahydrate, 0.0735 g manganese acetate tetrahydrate, 0.0873 g cobalt nitrate hexahydrate and 0.0747 g nickel acetate tetrahydrate to 200 mL of deionized water and stir until the metal salt solution is completely dissolved to obtain the precursor solution.
[0034] (2) Thioacetamide was added to the precursor solution to control the total molar ratio of each metal element (NiFeMnCoCu) in the precursor solution and the molar ratio of sulfur in the thioacetamide, i.e., the molar ratio of (NiFeMnCoCu):S was controlled to be 1:5, 1:10, 1:20, 1:30, 1:40 and 1:50. The calculated amount of thioacetamide relative to the sulfur source was added to the above solution, and the amounts of thioacetamide were 0.56 g, 1.13 g, 2.25 g, 3.38 g, 4.51 g and 5.64 g, respectively. The solution was then subjected to microwave hydrothermal treatment at 180 °C for 90 min with a microwave power of 1800 W. After the reaction was completed, the product was washed and dried to obtain the high-entropy sulfide (NiFeMnCoCu)S. x .
[0035] like Figure 2 As shown. Among them Figure 2(a) The relationship between (FeCuNiCoMn) and different molar ratios of sulfur source was studied. As the added sulfur source increased, the sulfur content of (FeCuNiCoMn)S... x The peak intensity of (HES) gradually increased to 29.3°, 31.5°, and 38.2°, corresponding to crystal planes (111), (200), and (220), respectively. These observations are consistent with PDF#73-1703. Furthermore, as the sulfur source ratio increased, impurity peaks unrelated to the target sample began to decrease. When the molar ratio (FeCuNiCoMn):S reached 1:30, the impurity characteristic peaks were the fewest, and the target characteristic peak intensity was the largest, indicating that at this ratio, sulfur and polymetallic elements formed a single, homogeneous pyrite-like crystal structure. When the molar ratio was increased to 1:40 and 1:50, oxide impurities began to appear at 36.1°.
[0036] Therefore, a molar ratio (NiFeMnCoCu):S of 1:30 was chosen for subsequent experiments.
[0037] Example 2:
[0038] (1) Add equimolar amounts (0.3 mmol) of 0.0599 g copper acetate monohydrate, 0.1212 g ferric nitrate nonahydrate, 0.0735 g manganese acetate tetrahydrate, 0.0873 g cobalt nitrate hexahydrate and 0.0747 g nickel acetate tetrahydrate to 200 mL of deionized water and stir until the metal salt solution is completely dissolved to obtain the precursor solution;
[0039] (2) Add 3.38 g of thioacetamide to the precursor solution, i.e., the molar ratio of (NiFeMnCoCu):S is 1:30, stir to dissolve it completely, and obtain a mixture;
[0040] (3) Add 0.0184 g of pomegranate peel powder to the mixture in step (2), that is, add pomegranate peel powder at 10 wt% relative to the mass fraction of HES according to the theoretical mass of HES (0.184 g). After stirring thoroughly, transfer the mixed solution to a microwave hydrothermal reactor and perform microwave hydrothermal reaction at 180 ℃ for 90 min. After the reaction is completed, the product is washed and vacuum dried at 60 ℃ to obtain the target catalyst, which is calculated as 10% HES / HTCC.
[0041] Example 3:
[0042] The only difference between Example 3 and Example 2 is that the amount of pomegranate peel powder added in step (3) is 0.0368g, which is the mass corresponding to 20 wt%. The other operations are the same as in Example 2, and the catalyst 20%HES / HTCC is prepared.
[0043] Example 4
[0044] The only difference between Example 4 and Example 2 is that the amount of pomegranate peel powder added in step (3) is 0.0552g, which corresponds to 30 wt% of the mass. The other operations are the same as in Example 2, and the catalyst 30%HES / HTCC is prepared.
[0045] Figure 3 (a)-(d) are transmission electron microscopy (TEM) images of the sample at 30 wt% HTCC / HES. Figure 3 (a) It can be seen that the target sample exhibits a typical sheet-like two-dimensional nanostructure, which means that the target sample has a large specific surface area and more exposed catalytic active sites that can be used for catalytic reactions. No thick stacking of the sample was found, and the material edges are smooth. Figure 3 In (d), (FeCuNiCoMn)S x The principal lattice edge spacings are 0.32 nm and 0.28 nm, respectively, corresponding to the lattice fringe spacings of the (111) and (200) planes. Elemental mapping results obtained using high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) revealed that, as... Figure 3 As shown in (e)-(n), the elements Co, Fe, Ni, Mn, Cu, S, C and O contained in hydrothermal carbon and high-entropy sulfides are uniformly distributed in the 30 wt% HTCC / HES sample, confirming that the two materials achieve uniform composite at the nanoscale with good interfacial bonding at this ratio.
[0046] Example 5
[0047] The only difference between Example 5 and Example 2 is that the amount of pomegranate peel powder added in step (3) is 0.0736g, which corresponds to 40 wt% of the mass. The other operations are the same as in Example 2, and the catalyst 40%HES / HTCC is prepared.
[0048] Example 6
[0049] The only difference between Example 5 and Example 2 is that the amount of pomegranate peel powder added in step (3) is 0.092g, which corresponds to 50 wt% of the mass. The other operations are the same as in Example 2, and the catalyst 50%HES / HTCC is prepared.
[0050] Figure 2(b) are the XRD patterns of the high-entropy sulfide (HES) and hydrothermal carbon (HTCC) materials prepared in Examples 3-6 with different mass fractions of 10 wt%-50 wt%. All of these different mass fractions contain the (111), (200), and (220) crystal planes, and the peak intensity increases with the addition of HTCC, indicating that the addition of HTCC did not destroy the original crystal structure of HES, and that the two were not simply physically mixed, but rather formed a tightly bonded composite material.
[0051] Application example:
[0052] Photocatalytic CO2 reduction coupled with biomass conversion was conducted in a 100 mL photochemical reactor. First, 0.05 g of catalyst and 0.1 mmol of HMF were added to 50 mL of water and stirred thoroughly. CO2 gas was continuously injected into the reactor, and the reactor gas was vented until the pressure inside the reactor was equal to atmospheric pressure at room temperature (0.2 MPa). This process was repeated three times. A 300 W xenon lamp with a 420 nm filter was used to vertically irradiate the reactor through a transparent window (30-40 mm in diameter) at the top for 4 h. The reaction products were analyzed by gas chromatography (GC-7860 Plus) and liquid chromatography (Thermo (Dionex) UltiMate3000 UHPLC).
[0053] Table 1: Photocatalytic reduction performance of different catalysts for CO2 in pure water system; and CO yield and selectivity in photocatalytic CO2 reduction coupled with HMF oxidation under visible light irradiation.
[0054]
[0055] Figure 4 (a) The photocatalytic carbon dioxide reduction performance of HES, HTCC, and 10%–50% HTCC / HES in pure water under simulated visible light irradiation was studied. As shown in the figure, with the gradual increase of HTCC loading, the CO production reached its highest value of 113.59 μmol·g when the loading reached 30 wt% HTCC / HES. -1 ·h -1 .
[0056] The yield and selectivity of CO produced by photocatalytic CO2 reduction coupled with HMF oxidation under visible light were studied for HES, HTCC, and 10-50 wt% HTCC / HES samples. Figure 4 (b). In a 30 wt% HTCC / HES sample, CO reached 350 μmol·g. -1 ·h -1Alongside high yield, selectivity also reached 93.4%. Figure 4 Figure (c) shows the DFF selectivity and HMF conversion under visible light catalysis. The figure indicates that the sample exhibits the highest catalytic conversion performance at a mass fraction of 30 wt%. However, when the mass fraction of the loading is further increased to 40 wt% or 50 wt%, both the DFF selectivity and HMF conversion decrease, indicating the formation of more byproducts. Figure 4 (d) Catalytic cycling test: Four repeated experiments were conducted to evaluate the cycling performance of the 30 wt% HTCC / HES sample. The catalyst maintained high CO yield and HMF conversion after four cycles, indicating good reusability.
[0057] Comparative Example 1:
[0058] The only difference between Comparative Example 1 and Example 4 is that the conventional hydrothermal reaction method was used instead of the microwave hydrothermal method, and the composite material was prepared by conventional hydrothermal reaction at 180°C for 12 hours. All other operations were the same as in Example 4.
[0059] The application method is the same as in Example 4. Test results show that the CO yield is 37.5 μmol·g. -1 ·h -1 The HMF conversion rate was 76.0%.
[0060] Comparative Example 2:
[0061] The only difference between Comparative Example 2 and Example 4 is that an equal amount of cellulose was used instead of pomegranate peel powder in the microwave hydrothermal reaction to prepare the composite material. All other operations were the same as in Example 4.
[0062] The application method is the same as in Example 4. Test results show that the CO yield is 43.2 μmol·g. -1 ·h -1 The HMF conversion rate was 78.0%.
[0063] Comparative Example 3:
[0064] Compared with Example 4, Comparative Example 3 differs only in that an equimolar amount of a single metal is used instead of the pentagonal high-entropy metal, specifically: (1) 1.5 mmol of nickel acetate tetrahydrate (0.373 g) is added to 200 mL of deionized water and stirred until completely dissolved;
[0065] (2) Add thioacetamide (3.38 g, metal to sulfur molar ratio of 1:30) and stir until fully dissolved;
[0066] (3) Add 0.0408 g of pomegranate peel powder, stir thoroughly, transfer the mixed solution to a microwave hydrothermal reactor, and perform microwave hydrothermal treatment at 180°C for 90 min. After washing and drying, a single metal sulfide composite material is obtained: 30wt%NiS / HTCC.
[0067] The application method is the same as in Example 4. Test results show that the CO yield is 49.8 μmol·g. -1 ·h -1 The HMF conversion rate was 75.2%.
[0068] Comparative Example 4:
[0069] The only difference between Comparative Example 4 and Example 4 is that an equimolar amount of bimetallic salt is used instead of the pentagonal high-entropy metal salt, specifically: (1) 0.75 mmol of ferric nitrate nonahydrate (0.303 g) and 0.75 mmol of nickel acetate tetrahydrate (0.187 g) are added to 200 mL of deionized water and stirred until completely dissolved;
[0070] (2) Add 3.38 g of thioacetamide, with a metal to sulfur molar ratio of 1:30, and stir to dissolve it completely;
[0071] (3) Add 0.0402 g of pomegranate peel powder, stir thoroughly, transfer the mixed solution to a microwave hydrothermal reactor, and perform microwave hydrothermal treatment at 180 °C for 90 min. After washing and drying, a single metal sulfide composite material is obtained: 30wt%FeNiS / HTCC.
[0072] The application method is the same as in Example 4, and the test results show that the CO yield is 105.6 μmol·g. -1 ·h -1 The HMF conversion rate was 79.3%.
[0073] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst, characterized in that, The composite photocatalyst is composed of a high-entropy sulfide and hydrothermal carbon; the high-entropy sulfide is (NiFeMnCoCu)Sx; a two-dimensional S-shaped heterojunction structure is formed between the high-entropy sulfide and the hydrothermal carbon.
2. A method for preparing the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst as described in claim 1, characterized in that, Specifically, the following steps are included: (1) Add soluble copper salt, iron salt, manganese salt, cobalt salt and nickel salt to deionized water in an equimolar ratio and stir until completely dissolved to obtain a polymetallic salt precursor solution; (2) Add thioacetamide as a sulfur source to the polymetallic salt precursor solution and stir to dissolve it completely to obtain a mixed solution; wherein, the total molar ratio of the five metal elements in the precursor solution to the sulfur element in the thioacetamide is 1:5 ~ 1:
50. (3) Add biomass powder to the mixture in step (2), stir evenly, transfer it to a microwave hydrothermal reactor, and carry out microwave hydrothermal reaction at 140 ℃ ~ 200 ℃ for 60 min ~ 120 min. After the reaction is completed, wash and dry the product to obtain the hydrothermal carbon / high entropy sulfide nanocomposite photocatalyst. Among them, the feed mass of biomass powder accounts for 10 wt% to 50 wt% of the theoretical mass of high-entropy sulfides.
3. The preparation method of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 2, characterized in that, The feed mass of biomass powder accounts for 20 wt% to 40 wt% of the theoretically generated mass of the high-entropy sulfide.
4. The preparation method of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 2, characterized in that, In step (1), the soluble copper salt, iron salt, manganese salt, cobalt salt and nickel salt are copper acetate monohydrate, ferric nitrate nonahydrate, manganese acetate tetrahydrate, cobalt nitrate hexahydrate and nickel acetate tetrahydrate, respectively.
5. The preparation method of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 2, characterized in that, In step (2), the total molar ratio of the five metal elements to the sulfur element in the thioacetamide is 1:20 to 1:
40.
6. The preparation method of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 2, characterized in that, In step (3), the biomass powder is pomegranate peel powder, orange peel, chestnut shell or walnut shell.
7. The preparation method of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 2, characterized in that, In step (3), the temperature of the microwave hydrothermal reaction is 160 ℃ ~ 180 ℃ and the time is 80 min ~ 100 min.
8. An application of the hydrothermal carbon / high-entropy sulfide nanocomposite photocatalyst according to claim 1, characterized in that: Application of nanocomposite photocatalysts in photocatalytic carbon dioxide reduction coupled with HMF conversion.
9. The application according to claim 8, characterized in that, The specific application process is as follows: In a photochemical reactor, a nanocomposite photocatalyst is used as the catalyst, and an aqueous solution containing 5-hydroxymethylfurfural is used as the reaction medium. Carbon dioxide gas is introduced into the reaction system. Under visible light irradiation, carbon dioxide is simultaneously reduced to carbon monoxide, and 5-hydroxymethylfurfural is selectively oxidized to 2,5-dicarboxyfuran.