A composite magnetic material for activating persulfate to degrade benzene series wastewater and a preparation method thereof
By optimizing the preparation method, Fe₃O₄ and molybdenum disulfide are uniformly distributed in the biochar framework, forming a tight interfacial heterojunction. This solves the problem of insufficient active sites in the catalyst, achieving efficient degradation and stable catalysis of benzene series wastewater, which is suitable for industrial application.
Patent Information
- Application Number
- CN202611422220.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing magnetic biochar catalysts have insufficient catalytic active sites when treating benzene series wastewater, low efficiency in generating free radicals through PMS activation, poor degradation effect, poor catalyst cycle stability, and weak water quality adaptability.
By ball milling a mixture of potassium ferrate, molybdenum source, and thiourea with biochar, followed by hydrothermal reaction with sodium sulfide solution and calcination under an inert atmosphere, a composite magnetic material in which Fe₃O₄ and molybdenum disulfide are uniformly distributed in the biochar framework is prepared, forming a tight interfacial heterojunction, which improves the exposure of catalytic active sites and cycle stability.
The catalyst's catalytic performance was significantly improved, enabling efficient degradation of benzene series wastewater. The material exhibits stable catalysis over a wide pH range, good magnetic properties, and recyclability, meeting the requirements of green chemistry.
Smart Images

Figure CN123148972A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, and in particular relates to a composite magnetic material for activating persulfate to degrade benzene series wastewater and its preparation method. Background Technology
[0002] The petrochemical and aromatic hydrocarbon processing industries continuously discharge wastewater containing xylene. Xylene is a toxic pollutant belonging to the benzene family. Its stable benzene ring chemical structure results in high resistance to biodegradation and strong microbial inhibitory toxicity. Direct entry into the biological treatment system would disrupt the activity of sludge bacteria, significantly reducing the efficiency of biological treatment. Existing conventional water treatment processes have drawbacks in xylene removal: coagulation sedimentation and simple flotation can only remove suspended xylene, with a removal rate of less than 40% for dissolved xylene. Traditional aerobic and anaerobic biological treatment processes have low tolerance to xylene concentrations. High-concentration xylene wastewater must undergo oxidation pretreatment to reduce pollutant toxicity and improve biodegradability before entering the biological treatment unit. The sulfate radical oxidation process based on persulfate (PMS) has the advantages of high oxidation potential and wide pH applicability, making it a major technology for the pretreatment of recalcitrant organic wastewater. However, this process relies on a highly efficient and stable solid catalyst to activate PMS and generate active free radicals to achieve ring-opening degradation of organic pollutants. Magnetic biochar, with its advantages of low raw material cost and easy recovery, has become a research hotspot for PMS activation catalysts.
[0003] In recent years, some progress has been made in the modification research of biochar-based catalysts. Chinese invention patent application CN118458920A discloses a method for activating persulfate (PMS) to degrade macrolide antibiotic wastewater using a biochar composite catalyst. This catalyst uses sawdust biochar as a carrier, and is prepared by impregnation with potassium ferrate, high-temperature pyrolysis, and subsequent loading with polyethyleneimine to obtain a PBC@PEI composite catalyst. This method can effectively activate PMS to generate sulfate and hydroxyl radicals, showing good degradation effects on macrolide antibiotics such as tylosin, and the catalyst has a certain degree of recyclability. However, the catalyst in the above technical solution relies on a single iron-based component to activate PMS, resulting in a limited number of catalytic active sites. Furthermore, PEI only plays a stabilizing and dispersing role, leaving room for improvement in PMS activation efficiency. Additionally, the above technical solution mainly targets the treatment of antibiotic wastewater and does not address the treatment of benzene series pollutants. Chinese invention patent application CN118437277A discloses a molybdenum disulfide-supported magnetic potato residue biochar, its preparation method, and its application. This composite material uses potato residue biochar as a carrier, and magnetic Fe3O4 is loaded via co-precipitation followed by MoS2 loading via hydrothermal method to prepare a MoS2@MBC ternary composite material. This material is mainly used as an adsorbent for removing the heavy metal Pb from wastewater. 2+The above-mentioned composite materials are mainly used for the adsorption and removal of pollutants, and do not involve the oxidation process of activated persulfate. The preparation process adopts a stepwise synthesis route, and the interface between the two active components, MoS2 and Fe3O4, is loose, resulting in a decrease in catalytic efficiency.
[0004] In summary, magnetic biochar still has the following problems in the treatment of benzene series wastewater: insufficient number of catalyst active sites, low efficiency of PMS activation to generate free radicals, and poor degradation effect of benzene series wastewater; poor catalyst cycle stability, with metal leaching and agglomeration; and weak water quality adaptability.
[0005] Therefore, there is an urgent need for a modified magnetic biochar catalytic material that is wide pH tolerant, magnetically recoverable, and cycle-stable, for use in the treatment of xylene-containing wastewater. Summary of the Invention
[0006] The purpose of this invention is to provide a composite magnetic material for activating persulfate to degrade benzene series wastewater and its preparation method, so as to solve the problem that existing magnetic biochar as a catalyst has insufficient catalytic active sites and poor degradation effect in the treatment of benzene series wastewater.
[0007] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a composite magnetic material, comprising the following steps: (1) Potassium ferrate, biochar, molybdenum source and thiourea were mixed and then ball-milled to obtain a mixed powder; (2) Mix the powder and sodium sulfide solution, sonicate and let stand, then place in a reaction vessel for hydrothermal reaction to obtain the precursor; (3) The precursor is calcined in an inert atmosphere to obtain a composite magnetic material.
[0008] This invention addresses the problem of poor catalytic performance caused by the limited number of catalytic sites in existing magnetic biochar catalysts. It optimizes the composition and preparation steps of the catalyst material. The catalyst comprises Fe3O4, molybdenum disulfide, and biochar, with improved catalytic performance achieved through the synergistic effect of Fe3O4 and molybdenum disulfide. In the preparation method, step (1) involves uniformly dispersing potassium ferrate, molybdenum source, and thiourea at the micro-nano scale using ball milling. The shearing and impact effects of ball milling further allow these materials to adhere and embed into the porous structure of the biochar, providing a basis for the simultaneous in-situ growth of Fe3O4 and molybdenum disulfide on the biochar framework during subsequent heat treatment. This method of mixing all precursors at once in step (1) differs from traditional stepwise synthesis. In stepwise methods, the later-loaded components can only cover the outer surface of the earlier-loaded components, failing to achieve a uniform and dense distribution of Fe3O4 and molybdenum disulfide throughout the entire biochar framework. Step (2) involves adding a sodium sulfide solution after solid-phase premixing. Sodium sulfide dissolves in water and releases sulfide ions, which then contact the molybdenum source, potassium ferrate, and biochar in the liquid phase. The sulfide ions form Mo-S chemical bonds with the molybdenum in the molybdenum source, ensuring uniform nucleation and growth of molybdenum disulfide at the appropriate locations during subsequent calcination, reducing agglomeration. The sulfur in sodium sulfide also has reducing properties, while the iron in potassium ferrate has strong oxidizing properties. These two components can undergo a redox reaction, reducing the high-valence iron to a mixed valence state of divalent and trivalent iron. Furthermore, the sulfur in sodium sulfide can react with the oxygen-containing functional groups on the surface of biochar, forming CS covalent bonds at the edge of the carbon skeleton of the biochar, achieving in-situ doping of sulfur. This effect of sodium sulfide in various raw materials forms a certain inorganic isolation layer, inhibiting agglomeration during subsequent calcination and thus exposing more catalytically active sites. Step (3) involves the final calcination process, during which the originally disordered biochar carbon layers undergo structural rearrangement, transforming from amorphous carbon to a graphene-like ordered carbon structure. Potassium ferrate undergoes thermal decomposition and phase transformation at high temperatures, generating Fe3O4 in situ, thus achieving embedded distribution of active sites within the carbon framework. The active sulfur species generated by the decomposition of thiourea at high temperatures react with the uniformly distributed molybdenum source, generating MoS2 nanosheets in situ. MoS2 grows outward with the molybdenum source as the nucleation center, forming a thin-layered structure that exposes abundant edge active sites. Because potassium ferrate and the molybdenum source are uniformly distributed in the biochar beforehand, Fe3O4 and molybdenum disulfide are generated in situ during calcination, forming a tighter bond between them. This close contact allows the electron-rich properties of MoS2 to directly act on adjacent Fe3O4, efficiently promoting the cyclic conversion of ferric and ferrous iron. The above preparation process can significantly affect the distribution of the two active components in the biochar, increasing and fully exposing catalytic active sites, thereby improving the catalytic performance of the catalyst.
[0009] Preferably, the biochar includes, but is not limited to, coconut shell biochar powder.
[0010] Preferably, the mass ratio of potassium ferrate, biochar, molybdenum source and thiourea is 0.8~1.0:1.0~1.5:0.5~0.8:1.0~2.0.
[0011] Preferably, the ball milling speed is 300~500 r / min and the ball milling time is 2~6 h.
[0012] Preferably, the ratio of the mixed powder to the sodium sulfide solution is 0.1~0.3g:10~30mL.
[0013] Preferably, the concentration of the sodium sulfide solution is 1-3%.
[0014] To fully utilize the role of sodium sulfide solution, this invention limits the concentration of the sodium sulfide solution. Within this concentration range, it can provide an appropriate amount of sulfide ions to the reaction system, moderately reduce high-valent iron, form suitable Mo-S chemical bonds with the molybdenum source, and also dope and modify the carbon skeleton of biochar. If the sodium sulfide concentration is too low, the above effects are difficult to achieve, and the interaction between sulfide ions and high-valent iron, molybdenum source, and biochar cannot be balanced. If the sodium sulfide concentration is too high, excess sulfide ions will react with high-valent iron and molybdenum source, possibly generating some elemental iron and excessive accumulation of molybdenum disulfide crystals, which will affect the full exposure of catalytic active sites and lead to a decrease in the catalytic performance of the catalyst.
[0015] Preferably, the hydrothermal reaction temperature is 160~200℃ and the hydrothermal reaction time is 1~5h.
[0016] Preferably, the calcination temperature is 550~650℃, the calcination time is 1~3h, and the heating rate is 3~6℃ / min.
[0017] A second aspect of the present invention provides a composite magnetic material prepared by the above-described preparation method.
[0018] Preferably, the composite magnetic material includes biochar, magnetic Fe3O4 supported on biochar, and MoS2 supported on biochar. Fe3O4 and MoS2 can coexist in situ within the pores and on the surface of biochar, forming a Fe3O4-MoS2 heterogeneous interface.
[0019] This invention employs a one-step mixing method for the main raw materials. Potassium ferrate and molybdenum source have already entered the micropores or mesopores of biochar during the ball milling stage. During the high-temperature calcination stage, Fe3O4 and molybdenum disulfide are generated simultaneously in situ. Therefore, in the structure of the composite magnetic material, the active components (Fe3O4 particles and MoS2 sheets) are uniformly distributed on the surface and in the internal pores of the biochar, rather than just accumulating on the outer surface. This distribution significantly increases the exposure of active sites.
[0020] The third aspect of this invention provides an application of a composite magnetic material in activated persulfate-degraded benzene series wastewater.
[0021] The catalytic degradation of benzene series compounds in benzene series wastewater in this invention differs from the degradation of general organic pollutants. General organic pollutants, such as antibiotics and dyes, although structurally complex, contain functional groups such as double bonds, amino groups, and azo groups, which serve as targets for free radical attack, making them relatively easy to degrade. In contrast, benzene series compounds have a benzene ring as their core and possess a highly stable conjugated system. This invention obtains a catalyst with multiple catalytic sites and superior catalytic performance through a specific preparation method, achieving rapid and effective degradation of benzene series compounds.
[0022] In the process of activating PMS to degrade benzene compounds using the composite magnetic material of this invention, superoxide radicals (O2•-) are the dominant active species, supplemented by sulfate radicals (SO4•-) and hydroxyl radicals (•OH). In addition, carbon defects and oxygen-containing functional groups on the material surface can promote PMS activation through non-radical pathways of electron transfer. The synergistic effect of the two pathways ensures efficient degradation under complex water quality conditions.
[0023] Preferably, the benzene derivative is xylene.
[0024] The present invention, by adopting the above-described technical solution, has at least the following beneficial effects compared with the prior art: (1) The present invention can obtain the target product by mixing all solid raw materials at one time, treating with sodium sulfide solution and calcining at high temperature. This eliminates the cumbersome process of multiple solid-liquid separation, washing and drying in the stepwise synthesis method, significantly shortens the production cycle, reduces waste liquid generation, and has mild process conditions and low cost, making it suitable for industrial scale-up production.
[0025] (2) The biochar raw material used in this invention comes from agricultural waste, realizing the high-value utilization of waste resources. The catalyst preparation process does not use toxic and harmful reagents, has good environmental compatibility, and the material itself has good magnetic properties, which can be quickly recovered through magnetic separation, avoiding secondary pollution of water bodies by powdered catalysts, and meeting the requirements of green chemistry and sustainable development.
[0026] (3) The composite magnetic material prepared by this invention can form a tight interfacial heterojunction, and the electron-rich properties of MoS2 promote the formation of Fe in magnetic biochar. 3+ / Fe 2+ The efficient circulation enhances the activation efficiency of PMS, enabling efficient degradation of benzene series wastewater.
[0027] (4) The composite magnetic material prepared by the present invention can be used as a catalyst to stably catalyze degradation in a wide pH range and under complex water quality conditions. It has a long service life and a wide range of applications. Attached Figure Description
[0028] Figure 1 The images are SEM images of the composite magnetic material in Example 1 under different magnifications, where (a) is the SEM image of the composite magnetic material at 5 μm and (b) is the SEM image of the composite magnetic material at 1 μm. Figure 2 The graph shows the xylene wastewater degradation effect of the composite magnetic material in Example 1. Figure 3 The graph shows the degradation effect of the composite magnetic material in Example 1 at different pH values. Figure 4 This is a diagram illustrating the recycling effect of the composite magnetic material in Example 1. Detailed Implementation
[0029] Example 1 A method for preparing a composite magnetic material for activating persulfate-degraded benzene series wastewater includes the following steps: (1) Take 0.86g K2FeO4 powder, 1.20g coconut shell biochar powder, 0.6g ammonium heptamolybdate tetrahydrate and 1.5g thiourea and put them into a ball mill jar. Add 5 zirconium beads with a diameter of 6mm and 10 zirconium beads with a diameter of 3mm. After sealing, set the speed to 400r / min and continuously ball mill for 4h. Collect the ball milled material, wash it with anhydrous ethanol, and dry it to obtain a mixed powder.
[0030] (2) Take 0.2g of the mixed powder obtained in step (1) and place it in a 50mL beaker. Add 20mL of 2% Na2S solution and ultrasonically disperse for 30min. Let it stand for 12h. Place the mixture after standing in a reaction vessel and place it in an oven with nitrogen gas to carry out hydrothermal reaction. The reaction temperature is 180℃ and the reaction time is 2h. After it has completely cooled down, filter, wash and dry to obtain the precursor.
[0031] (3) Transfer the precursor obtained in step (2) into a tube furnace, introduce nitrogen gas, heat the precursor powder to 600℃ and hold for 2 hours, with a heating rate of 5℃ / min. After cooling, take out the product, wash it with deionized water several times and dry it to obtain the composite magnetic material.
[0032] Example 2 A method for preparing a composite magnetic material for activating persulfate-degraded benzene series wastewater includes the following steps: (1) Take 0.92g K2FeO4 powder, 1.30g coconut shell biochar powder, 0.75g ammonium heptamolybdate tetrahydrate and 1.64g thiourea and place them in a ball mill jar. Add 5 zirconium beads with a diameter of 6mm and 10 zirconium beads with a diameter of 3mm. After sealing, set the rotation speed to 450r / min and continuously ball mill for 3h. Collect the ball-milled material, wash it with anhydrous ethanol, and dry it to obtain a mixed powder.
[0033] (2) Take 0.3g of the mixed powder obtained in step (1) and place it in a 50mL beaker. Add 30mL of 2.5% Na2S solution and ultrasonically disperse for 30min. Let it stand for 12h. Place the mixture after standing in a reaction vessel and place it in an oven with nitrogen gas to carry out hydrothermal reaction. The reaction temperature is 190℃ and the reaction time is 1.5h. After it has completely cooled down, filter, wash and dry to obtain the precursor.
[0034] (3) Transfer the precursor obtained in step (2) into a tube furnace, introduce nitrogen gas, heat the precursor powder to 620°C and hold for 1.5 h, with a heating rate of 5°C / min. After cooling, take out the product, wash it several times with deionized water and dry it to obtain the composite magnetic material.
[0035] Comparative Example 1 The difference between this comparative example and Example 1 is that the sodium sulfide solution was added in a different way; no sodium sulfide solution was added in this comparative example.
[0036] This comparative example provides a method for preparing a composite magnetic material, including the following steps: (1) Take 0.86g K2FeO4 powder, 1.20g coconut shell biochar powder, 0.6g ammonium heptamolybdate tetrahydrate and 1.5g thiourea and put them into a ball mill jar. Add 5 zirconium beads with a diameter of 6mm and 10 zirconium beads with a diameter of 3mm. After sealing, set the speed to 400r / min and continuously ball mill for 4h. Collect the ball milled material, wash it with anhydrous ethanol, and dry it to obtain a mixed powder.
[0037] (2) Take 0.2g of the mixed powder obtained in step (1) and place it in a 50mL beaker. Add 20mL of water, sonicate for 30min and let stand for 12h. Place the mixture after standing in a reaction vessel and place it in an oven with nitrogen gas to carry out hydrothermal reaction. The reaction temperature is 180℃ and the reaction time is 2h. After it has completely cooled down, filter, wash and dry to obtain the precursor.
[0038] (3) Transfer the precursor obtained in step (2) into a tube furnace, introduce nitrogen gas, heat the precursor powder to 600℃ and hold for 2 hours, with a heating rate of 5℃ / min. After cooling, take out the product, wash it with deionized water several times and dry it to obtain the composite magnetic material.
[0039] Comparative Example 2 The difference between this comparative example and Example 1 is that the concentration of the sodium sulfide solution is different; the concentration of the sodium sulfide solution added in this comparative example is 6%.
[0040] Comparative Example 3 The difference between this comparative example and Example 1 is that the preparation steps are different. This comparative example uses a conventional stepwise method, first preparing Fe3O4 and then preparing molybdenum disulfide.
[0041] This comparative example provides a method for preparing a composite magnetic material, including the following steps: (1) Dissolve 0.86g of K2FeO4 powder in deionized water, disperse 1.20g of coconut shell biochar powder in the solution, stir continuously for 8 hours, filter and dry to obtain mixed powder.
[0042] (2) Place the mixed powder in a tube furnace, introduce N2, heat to 600℃ and hold for 2 hours (heating rate is 5℃ / min) to obtain magnetic biochar.
[0043] (3) Take 0.2g of magnetic biochar, 0.6g of ammonium heptamolybdate tetrahydrate and 1.5g of thiourea and place them in a ball mill jar. Add 5 zirconium beads with a diameter of 6mm and 10 zirconium beads with a diameter of 3mm. After sealing, set the rotation speed to 400r / min and continuously ball mill for 4h.
[0044] (4) Place the ball-milled product in a tube furnace, introduce N2, heat to 600℃ and hold for 2 hours (heating rate is 5℃ / min), wash and dry to obtain composite magnetic material.
[0045] Test case (1) Characterization of surface morphology of composite magnetic materials The microstructure of the samples was characterized using scanning electron microscopy (SEM). The sample preparation process was as follows: conductive adhesive was uniformly coated on a copper sample substrate, the composite magnetic material of Example 1 was precisely loaded using a micromanipulation tip, unattached particles were removed by air pump purging, a conductive layer was deposited by ion sputtering, and finally, observation was completed at an accelerating voltage of 5 kV.
[0046] from Figure 1 As can be seen in (a), since all raw materials (K2FeO4, ammonium molybdate, thiourea) are pre-embedded in the micropores / mesopores of biochar during the ball milling stage in step (1), Fe3O4 and MoS2 grow synchronously in situ within the carbon skeleton pores during high-temperature calcination. Therefore, the active components (Fe3O4 particles and MoS2 sheets) are uniformly distributed in the internal pores of the biochar, rather than all accumulating on the outer surface. This distribution can significantly increase the exposure of active sites. Figure 1 As can be seen in (b), Fe3O4 is granular and MoS2 is lamellar, and the two are stacked together.
[0047] (2) Pollutant degradation performance test A 100 mg / L xylene wastewater sample (pH 6.5, water temperature 22℃) was prepared. 500 mL of the xylene wastewater was placed in a reactor, and the composite magnetic materials prepared in Examples 1-2 and Comparative Examples 1-3 were added at a dosage of 0.10 g / L. Subsequently, sodium persulfate (PMS) was added to the system in a single addition at a concentration of 15 mg / L. The moment of PMS addition was recorded as the zero point, and the reaction was continuously stirred for 20 min. During the reaction, samples were taken at 2, 4, 6, 8, 10, 15, and 20 min. Immediately after sampling, the samples were injected into headspace vials containing saturated sodium thiosulfate solution to quench residual free radicals and terminate the reaction. After filtration through a 0.22 μm filter membrane, the residual concentration of xylene in the liquid phase was determined by gas chromatography-FID (GC-FID).
[0048] Degradation efficiency = (1-C) t / C0)×100%, Among them, C t C0 represents the xylene content in the wastewater after reaction t min, and C0 represents the initial xylene content in the wastewater.
[0049] Table 1. Degradation effects of composite magnetic materials in the examples and comparative examples.
[0050] From Table 1 and Figure 2 As can be seen, the composite magnetic material prepared in Example 1 achieved a 99% degradation efficiency in xylene in wastewater within 20 minutes, demonstrating excellent degradation effect and a short degradation time. Meanwhile, Example 2 showed a degradation efficiency of 95%, indicating that the composite magnetic material of the present invention has excellent degradation effect on xylene in wastewater. In Comparative Example 1, the step of adding sodium sulfide solution was omitted; instead, the mixed powder was added to water. The degradation efficiency decreased because the lack of sodium sulfide solution treatment reduced the reduction of high-valent iron in potassium ferrate, leading to a decrease in Fe... 2+ / Fe 3+Insufficient active sites in the redox cycle lead to poor catalytic degradation. Furthermore, MoS2 relies solely on thiourea for sulfidation, causing nanosheets to easily aggregate, reducing active sites and ultimately decreasing degradation efficiency. In Comparative Example 2, increasing the sodium sulfide solution concentration to 6% resulted in a decrease in degradation efficiency. This indicates that excessive sulfur ions have overly strong reducing power, leading to excessive reduction of high-valence iron and deactivation of active sites. Additionally, excess sulfur ions react with ammonium molybdate to form molybdenum sulfide precursors, which undergo abnormal crystallization after high-temperature calcination, significantly weakening the catalytic function and reducing both pollutant adsorption and enrichment capacity and active sites. In Comparative Example 3, the stepwise composite of Fe3O4 and molybdenum disulfide on biochar also resulted in a decrease in degradation efficiency. This is because the formed Fe3O4 particles preferentially occupy the outer surface of the biochar and block the pore inlets, preventing the subsequent MoS2 precursor from effectively penetrating the internal pores of the carbon framework. The physical stacking of Fe3O4 and MoS2 results in a loose contact, and this non-in-situ symbiotic chemical bonding interface may affect electron transfer during degradation, leading to poor degradation efficiency.
[0051] (3) Effect of pH on pollutant degradation performance Prepare 100 mg / L xylene wastewater samples (water temperature 22℃), and adjust the pH value to 2.5, 7.0 and 9.5 respectively. Then, conduct degradation performance tests at different pH values according to the above pollutant degradation performance experiments.
[0052] from Figure 3 As can be seen, when the pH of the wastewater is adjusted to 2.5 and 7.0, the degradation efficiency is 99%, and the degradation effect of xylene remains basically unchanged. When the pH of the wastewater is adjusted to 9.5, the degradation efficiency drops to 87%, but it is still maintained above 85%. This shows that the composite magnetic material of the present invention has a good degradation effect in neutral, acidic and alkaline environments and has a wider range of applications.
[0053] (4) Stability assessment of composite magnetic materials The above pollutant degradation performance experiment was conducted. After the first round of reaction, the liquid after the reaction was filtered, washed and dried, and the reaction material was collected. The reaction material was then subjected to the above degradation process again, and the process was repeated four times.
[0054] from Figure 4 As can be seen from the results, the composite magnetic material of Example 1 can still maintain a degradation efficiency of over 90% after four rounds of degradation experiments, which indicates that the composite magnetic material of the present invention has good stability and reusability.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A method for preparing a composite magnetic material, characterized in that, Includes the following steps: (1) Potassium ferrate, biochar, molybdenum source and thiourea were mixed and then ball-milled to obtain a mixed powder; (2) Mix the powder and sodium sulfide solution, sonicate and let stand, then place in a reaction vessel for hydrothermal reaction to obtain the precursor; (3) The precursor is calcined in an inert atmosphere to obtain a composite magnetic material.
2. The method for preparing a composite magnetic material according to claim 1, characterized in that, The mass ratio of potassium ferrate, biochar, molybdenum source and thiourea is 0.8~1.0:1.0~1.5:0.5~0.8:1.0~2.
0.
3. The method for preparing a composite magnetic material according to claim 1, characterized in that, The ball milling speed is 300~500 r / min, and the ball milling time is 2~6 h.
4. The method for preparing a composite magnetic material according to claim 1, characterized in that, The ratio of mixed powder to sodium sulfide solution is 0.1~0.3g:10~30mL.
5. The method for preparing a composite magnetic material according to claim 1, characterized in that, The concentration of the sodium sulfide solution is 1-3%.
6. The method for preparing a composite magnetic material according to claim 1, characterized in that, The hydrothermal reaction temperature is 160~200℃, and the hydrothermal reaction time is 1~5h.
7. The method for preparing a composite magnetic material according to claim 1, characterized in that, The calcination temperature is 550~650℃, the calcination time is 1~3h, and the heating rate is 3~6℃ / min.
8. A composite magnetic material, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 7.
9. The application of the composite magnetic material as described in claim 8 in activated persulfate degradation of benzene series wastewater.
10. The application of the composite magnetic material according to claim 9, characterized in that, The benzene series compound is xylene.
Citation Information
Patent Citations
Molybdenum disulfide loaded magnetic potato residue biochar as well as preparation method and application thereof
CN118437277A
Method for degrading macrolide antibiotic wastewater by activating persulfate with biochar composite catalyst
CN118458920A