A chromium-free environment-friendly catalyst and a preparation method thereof

By using a ZrO₂-AlF₃ composite support and a chromium-free catalyst composed of Ce, Pr, and Nd rare earth elements, the environmental protection and stability issues of existing chromium-based catalysts have been solved, achieving high selectivity and long lifespan catalytic performance, suitable for the industrial preparation of trans-1-chloro-3,3,3-trifluoropropylene.

CN123148973APending Publication Date: 2026-11-24SHANDONG HUAAN NEW MATERIAL
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611425717.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing chromium-based catalysts have problems such as poor environmental performance, insufficient thermal stability, short catalyst life, many side reactions, and high cost of product separation and purification when preparing trans-1-chloro-3,3,3-trifluoropropylene. Furthermore, chromium-free catalysts are difficult to balance fluorination activity, selectivity, and long service life.

Method used

A chromium-free environmentally friendly catalyst composed of a ZrO₂-AlF₃ two-phase composite support and rare earth elements Ce, Pr, and Nd is used. ZrO₂ provides a rigid framework and AlF₃ provides Lewis acid sites. The rare earth components regulate the surface electronic state, avoiding the hazardous waste of hexavalent chromium and inhibiting the formation of carbon deposits and the loss of active components.

Benefits of technology

It achieves high yield and long lifespan catalyst performance, with a target product selectivity of 99.7%, reduces separation and purification costs, and extends the catalyst stable operation cycle to 1100 hours, making it suitable for industrial continuous gas-phase fluorination production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A chromium-free, environmentally friendly catalyst and its preparation method belong to the field of fluorochemical catalysis technology. The catalyst uses a ZrO2-AlF3 composite support, with any two or more rare earth elements selected from Ce, Pr, and Nd as active components. ZrO2 enhances the structural stability of the support, while AlF3 provides the Lewis acidic sites required for the fluorination reaction; the rare earth components can regulate the surface structure, construct oxygen vacancies, and suppress carbon deposition and side reactions. This invention abandons the traditional chromium-based formulation, is green and pollution-free, and can efficiently catalyze a one-step fluorination reaction. It exhibits high selectivity for the target product, good catalyst thermal stability, and long service life, making it suitable for continuous industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a chromium-free environmentally friendly catalyst and its preparation method, belonging to the field of fluorochemical catalysis technology. Background Technology

[0002] Trans-1-chloro-3,3,3-trifluoropropylene (HFO-1233zd(E)) is a new generation of low-ODP, low-GWP environmentally friendly fluoroolefin with excellent environmental friendliness and thermodynamic stability. It has irreplaceable application value in fields such as novel environmentally friendly refrigerants, foaming agents, cleaning agents, and fine fluorochemical intermediates. It is currently a core raw material for the fluorochemical industry to replace high-GWP fluorinated products, with urgent market demand and industry substitution needs. The mainstream industrial preparation route uses 1,1,1,3,3-pentachloropropane and anhydrous HF as raw materials, undergoing a one-step gas-phase catalytic fluorination reaction. This reaction path is complex and involves numerous side reactions; the catalyst is the core key to controlling reaction selectivity and improving production efficiency.

[0003] Existing gas-phase fluorination catalytic systems are dominated by chromium-based catalysts. Patent CN106748626A discloses a chromium-based composite catalyst for the synthesis of HFO-1233zd(E). This catalyst uses chromium trioxide as the main active component, supplemented with metal oxides and modified activated carbon. Although the selectivity is acceptable, it has significant shortcomings. The core active component is still a chromium-based material, which easily generates highly toxic hexavalent chromium waste. Furthermore, there is no rigid support to constrain the particles, and the combined activated carbon is prone to high-temperature ablation and carbon deposition, leading to catalyst sintering deactivation and short service life. This catalyst relies solely on metal oxides to adjust surface acidity, failing to construct stable Lewis acidic sites for fluorides. This not only results in a cumbersome and energy-intensive HF pre-activation process but also makes it difficult to precisely control the reaction acidity, easily generating large amounts of cis isomers and polyfluorinated byproducts, significantly increasing the cost of subsequent product separation and purification.

[0004] In addition, other publicly available fluorination catalysts in the industry also have significant shortcomings: pure aluminum fluoride catalysts are too acidic, leading to rapid carbon deposition and deactivation; single zirconium oxide supports have insufficient fluorination activation capacity and low feed conversion rates; conventional supported chromium-aluminum catalysts still cannot escape the problem of heavy metal pollution, and rare earth modified single-support systems suffer from problems such as easy agglomeration of active components and poor resistance to poisoning. In summary, existing chromium-based catalysts have poor environmental performance, insufficient thermal stability and structural stability, and chromium-free single-support catalysts cannot simultaneously achieve fluorination activity, product selectivity, and long service life. There is an urgent need to develop a novel rare earth composite fluorination catalyst that is chromium-free, environmentally friendly, structurally stable, and possesses both high activity and high selectivity. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a chromium-free environmentally friendly catalyst with high yield, long catalyst life, good stability and environmental friendliness for the gas-phase fluorination of 1,1,1,3,3-pentachloropropane to prepare trans-1-chloro-3,3,3-trifluoropropene, as well as the preparation method thereof.

[0006] The technical solution adopted by the present invention to solve its technical problem is: a chromium-free environmentally friendly catalyst, wherein the catalyst is composed of a two-phase composite support consisting of ZrO2 crystal phase and AlF3 crystal phase and two or more of the three rare earth elements Ce, Pr and Nd loaded on the surface of the support.

[0007] This technical solution employs a ZrO2-AlF3 two-phase composite support combined with two or more rare earth active components, completely eliminating chromium-based active components, avoiding the generation of hexavalent chromium hazardous waste, and reducing the cost of waste treatment. The ZrO2 crystalline phase provides a rigid framework to inhibit high-temperature sintering of the support, while AlF3 provides the Lewis acidic sites necessary for the fluorination reaction. The compounded rare earth components can regulate the electronic state of the support surface, inhibit carbon deposition, and suppress the formation of polyfluorinated byproducts. The synergistic effect of the two-phase support-rare earth interface balances raw material conversion rate, target product selectivity, and long-term catalyst stability, making it suitable for industrial continuous gas-phase fluorination production. As a preferred option, a Ce-Pr-Nd ternary composite rare earth is selected, which, compared to a binary composite, can further reduce the rare earth loss rate and extend the stable operating time.

[0008] Specifically, in the chromium-free environmentally friendly catalyst, the molar ratio of Zr to Al in the composite support is 1:2 to 1:10. Controlling the Zr / Al molar ratio within the range of 1:2 to 10 balances the support framework strength and the number of fluorination acidic sites. If the Al proportion is too high, the excessive AlF3 phase will result in excessive acidity, exacerbating cracking, carbon deposition, and side reactions; if the Zr proportion is too high, there will be insufficient AlF3 acidic sites, leading to decreased fluorination reactivity and reduced feed conversion rate. Within this ratio range, ZrO2 can form a continuous framework to constrain AlF3 grain growth while ensuring sufficient Lewis acid sites. Preferably, the Zr to Al molar ratio is 1:4 to 7. Within this preferred range, the specific surface area of ​​the support remains at a high level, the amount of catalyst carbon deposition is significantly reduced, and the overall catalytic performance is optimal.

[0009] Specifically, the described chromium-free environmentally friendly catalyst has a Ce:Pr:Nd molar ratio of (0~1):(0~1):(0~1) among the three rare earth elements, with at least two of Ce, Pr, and Nd not being zero simultaneously, and a total rare earth loading of 2wt%~12wt% of the total catalyst mass. Ce focuses on improving the conversion capacity of the feedstock HCC-240fa, while Pr and Nd focus on improving the selectivity of HFO-1233zd(E) and the stability of the support structure. If the total loading is below 2wt%, the number of active sites is insufficient, resulting in limited improvement in catalytic performance; if the loading is above 12wt%, rare earth components agglomerate, clogging the support pores and reducing activity, while also increasing the risk of rare earth loss. The molar ratio is flexible and adjustable to adapt to different production conditions. The preferred Ce:Pr:Nd molar ratio is 3:1:1, with a total rare earth loading of 5%-8wt%. Under these conditions, rare earth dispersion is high, side reactions are significantly suppressed, and the selectivity of the target product can reach over 99%.

[0010] Specifically, the chromium-free environmentally friendly catalyst is characterized in that the composite support is prepared by in-situ fluorination of zirconium-aluminum composite oxide with ammonium fluoride, where ZrO2 is the continuous framework phase and AlF3 is the surface dispersed phase. The in-situ fluorination of the zirconium-aluminum composite oxide with ammonium fluoride, unlike direct mixing of ZrO2 and AlF3 powders, enables high dispersion of AlF3 on the ZrO2 framework surface, preventing AlF3 grain agglomeration. ZrO2, as the continuous framework phase, provides physical support and inhibits AlF3 phase transformation sintering under high-temperature reaction conditions; AlF3, as the surface dispersed phase, uniformly constructs Lewis acidic sites on the support surface, eliminating the need for a complex HF pre-activation process and simplifying the production process. The in-situ fluorination process ensures tight bonding between the two phases, which is beneficial for anchoring rare earth active components and reducing the probability of active component loss.

[0011] Specifically, the preparation method of the chromium-free environmentally friendly catalyst includes the following steps: (1) preparing ZrO2-Al2O3 composite precursor by co-precipitation: dissolving zirconium salt and aluminum salt in deionized water to prepare a mixed metal salt solution, co-precipitating by adding ammonia water dropwise in parallel flow, controlling the pH of the system to be 8.0~9.0, aging, filtering, washing, drying, and then pre-calcining at 450℃~550℃ to obtain zirconium-aluminum composite oxide powder; (2) preparing ZrO2-AlF3 two-phase composite support by fluorination modification: the obtained zirconium-aluminum composite oxide powder is subjected to fluorination modification by adding ammonia water dropwise in parallel flow. The ZrO2-AlF3 composite support with two phases coexisting was prepared by impregnation with ammonium fluoride solution of equal volume for 2-6 hours at room temperature, followed by drying and fluorination calcination. (3) Loading rare earth active components: Ce, Pr and Nd nitrates were prepared into a uniform impregnation solution according to a preset ratio, and loaded onto the surface of the ZrO2-AlF3 composite support by equal volume impregnation method. The impregnation was carried out at room temperature for 4-9 hours, followed by static curing for 8-16 hours. After drying, the solution was calcined at 400℃-700℃ for 2-6 hours to obtain rare earth modified ZrO2-AlF3 fluorination catalyst. The zirconium aluminum composite oxide precursor was prepared by co-precipitation. The metal components were mixed uniformly to avoid local component segregation. The pH was controlled at 8.0-9.0 to ensure that the particle size of the precipitate was moderate and a high specific surface area precursor was obtained. The ammonium fluoride solution impregnation of equal volume achieved mild in-situ fluorination. Compared with gas phase HF fluorination, the process operation was safe and simple, and the equipment requirements were low. Equal-volume impregnation of loaded rare earth elements, combined with static curing, promotes the interaction between rare earth ions and the fluorine-oxygen interface of the carrier, enhancing the anchoring effect of the active components. The entire preparation process is mild, the raw materials are readily available, and it is easy to scale up, making it suitable for industrial-scale batch preparation. The preferred steps are: (1) pH control at 8.3-8.7; (2) impregnation at room temperature for 3-5 hours; and (3) static curing for 10-14 hours, which further improves the rare earth dispersion effect.

[0012] Specifically, in the preparation method of the chromium-free environmentally friendly catalyst, the precipitation aging temperature in step (1) is 30℃~100℃, the aging time is 1h~5h, and the pre-calcination heating rate is 1℃ / min~7℃ / min. The aging temperature and time control the growth of precipitated grains. Insufficient aging results in small grains, which are prone to sintering during subsequent calcination; excessive aging leads to excessive particle growth and a decrease in specific surface area. Slow heating at 1℃ / min-7℃ / min prevents the precursor particles from thermally stress cracking and pore structure collapse caused by excessive heating, thus ensuring the porous structure of the zirconium-aluminum composite oxide. The preferred aging temperature is 50℃~70℃, the aging time is 2h~4h, and the pre-calcination heating rate is 2℃ / min~5℃ / min. The resulting precursor has a well-developed pore structure, providing sufficient channels for subsequent fluorination and rare earth loading.

[0013] Specifically, in the preparation method of the chromium-free environmentally friendly catalyst, step (2) involves a fluorination calcination temperature of 350℃~450℃ and a calcination time of 1h~3h. If the fluorination calcination temperature is below 350℃, the ammonium fluoride decomposes incompletely, the aluminum phase fluorination conversion is insufficient, the AlF3 formation is low, and the acidic sites are insufficient. Temperatures above 450℃ will cause support sintering and a significant decrease in specific surface area. If the calcination time is too short, the fluorination reaction is incomplete; if the time is too long, grain agglomeration occurs. The preferred fluorination calcination temperature is 380℃-420℃, and the calcination time is 1.5h-2.5h, resulting in a high aluminum phase fluorination conversion rate, maintaining a high specific surface area on the support, and controllable two-phase structure.

[0014] Specifically, this describes the application of a chromium-free, environmentally friendly catalyst in the one-step gas-phase fluorination of 1,1,1,3,3-pentachloropropane to prepare trans-1-chloro-3,3,3-trifluoropropene. This chromium-free catalyst, applied to the one-step gas-phase fluorination reaction of 1,1,1,3,3-pentachloropropane, achieves near-complete conversion of the feedstock under normal pressure conditions. It exhibits high selectivity for HFO-1233zd(E), with fewer cis isomers and polyfluorinated byproducts, reducing the cost of subsequent product separation and purification. The catalyst has a low carbon deposition rate, minimal rare earth element loss, and a long stable operating cycle, eliminating the need for frequent catalyst regeneration and replacement. This improves the continuous operation efficiency of the unit, reduces production and maintenance costs, and makes it suitable for industrial continuous gas-phase fluorination production units. The preferred reaction temperature is 260℃-300℃, the HF to feedstock molar ratio is 10-15:1, and the contact time is 8s-12s, balancing conversion rate, selectivity, and energy consumption.

[0015] Compared with existing technologies, this invention has the following advantages: The catalyst of this invention is environmentally friendly, highly stable, and has excellent process adaptability. It abandons the traditional chromium-based system, using a ZrO2-AlF3 composite support with cerium, praseodymium, and neodymium rare earth active components, completely eliminating the highly toxic hexavalent chromium waste and reducing the cost of waste disposal. Under the condition of complete conversion of 1,1,1,3,3-pentachloropropane, the selectivity of the target product HFO-1233zd(E) reaches up to 99.7%, reducing cis isomers and polyfluorinated byproducts, and lowering separation and purification costs. ZrO2, as a rigid continuous framework, inhibits the high-temperature sintering phase transformation of AlF3, while the rare earth components construct oxygen vacancies and regulate surface Lewis acidity, effectively inhibiting carbon deposition and loss of active components. Stable operation can reach 1100 hours, extending the service life and reducing replacement frequency. In addition, the composite carrier is prepared by in-situ fluorination of ammonium fluoride, which eliminates the cumbersome process of high-temperature pre-activation of HF. The whole process is simple to operate, has mild conditions, and the raw materials are readily available. It can be directly adapted to continuous industrial gas phase fluorination equipment and has good prospects for industrial application. Detailed Implementation

[0016] The present invention will now be described in detail through examples. Unless otherwise stated, all raw materials used are commercially available.

[0017] Example 1

[0018] A composite carrier with a Zr:Al molar ratio of 1:6 and a Ce:Pr molar ratio of 3:1 was selected, with a total rare earth loading of 6 wt%. Zirconium oxynitrate and aluminum nitrate nonahydrate were weighed to prepare a mixed salt solution with a total metal ion concentration of 1.0 mol / L. 25 wt% ammonia water was added in parallel flow for co-precipitation over 70 min, controlling the pH of the system to 8.5. The solution was aged in a water bath at 65℃ for 3 h, filtered, washed with water until the filtrate was neutral, rinsed with anhydrous ethanol, dried at 110℃ for 12 h, passed through a 40-mesh sieve, and pre-calcined at 500℃ for 3 h at a rate of 4℃ / min to obtain zirconium-aluminum composite oxide powder. An ammonium fluoride impregnation solution was prepared with an F / (Zr+Al) molar ratio of 1.0, and the powder was impregnated with an equal volume for 4 h, followed by vacuum drying at 80℃ for 8 h. ZrO2-AlF3 composite support was prepared by fluorination and calcination at 400℃ for 2 hours with a heating rate of 3℃ / min. The support was impregnated with an equal volume of cerium nitrate hexahydrate and praseodymium nitrate hexahydrate impregnation solution, stirred at room temperature for 6 hours, sealed and allowed to stand for 12 hours to cure, dried at 120℃ for 10 hours, and calcined at 550℃ for 4 hours with a heating rate of 5℃ / min. The catalyst was then sieved to obtain a 20-40 mesh. The catalyst was evaluated under the following conditions: atmospheric pressure, 280℃, HF to HCC-240fa molar ratio of 12:1, and contact time of 10 seconds. The HCC-240fa conversion rate was 100%, the HFO-1233zd(E) selectivity was 94.5%, the stable operating time was 950 hours, the carbon deposition was 0.95 wt%, and the rare earth loss rate was 0.11 wt%.

[0019] Example 2

[0020] A composite carrier was used with a Zr to Al molar ratio of 1:2 (as claimed in the end value), and a Ce:Nd molar ratio of 3:1 was selected as a binary rare earth compound with a total rare earth loading of 6 wt%. Zirconium oxynitrate and aluminum nitrate nonahydrate were prepared into a mixed salt solution with a total metal ion concentration of 1.0 mol / L. This solution was co-precipitated with 25 wt% ammonia water under concurrent flow, with pH controlled at 8.0. The aging temperature was 30℃ for 5 hours, and the solution was pre-calcined at 450℃ for 3 hours at a rate of 1℃ / min to obtain a zirconium-aluminum composite oxide. Fluorination was then performed. A composite support was prepared by impregnating with ammonium impregnation solution at room temperature for 2 hours, drying, and then fluorinating and calcining at 350℃ for 3 hours. The catalyst was obtained by impregnating with cerium nitrate hexahydrate and neodymium nitrate hexahydrate at room temperature for 4 hours, allowing it to stand and solidify for 8 hours, and then calcining at 400℃ for 6 hours. Under the same evaluation conditions, the conversion rate of HCC-240fa was 100%, the selectivity of HFO-1233zd(E) was 95.8%, the stable operating time was 990 hours, the carbon deposition was 1.08 wt%, and the rare earth loss rate was 0.09 wt%.

[0021] Example 3

[0022] The composite support was selected with a Zr to Al molar ratio of 1:10 (as claimed in the end value), and a Pr:Nd molar ratio of 1:1 (a binary rare earth compound). The total rare earth loading was 6 wt%. A mixed salt solution of zirconium and aluminum salts was prepared, and precipitation was carried out with 25 wt% ammonia water in a co-current flow. The pH was controlled at 9.0, the aging temperature was 100℃, the aging time was 1 h, and the temperature was increased to 550℃ at a rate of 7℃ / min for 3 h to obtain a composite oxide. The composite support was prepared by impregnation with ammonium fluoride for 6 h, drying, and fluorination calcination at 450℃ for 1 h. The impregnation solution was prepared with praseodymium nitrate hexahydrate and neodymium nitrate hexahydrate, impregnated at room temperature for 9 h, allowed to stand for 16 h, and calcined at 700℃ for 2 h to obtain a catalyst. Under the same evaluation conditions, the conversion rate of HCC-240fa was 100%, the selectivity of HFO-1233zd(E) was 97.1%, the stable operating time was 1050 h, the carbon deposition was 1.26 wt%, and the rare earth loss rate was 0.07 wt%.

[0023] Example 4

[0024] The composite support was selected with a Zr to Al molar ratio of 1:6 and a Ce:Pr:Nd molar ratio of 3:1:1 ternary rare earth compound, with the total rare earth loading set at the lower limit of 2wt%. The preparation processes of the zirconium aluminum precursor and the composite support were the same as in Example 1. The three rare earth nitrates were prepared into an impregnation solution and impregnated in equal volumes. The mixture was stirred at room temperature for 6 hours, allowed to stand and solidify for 12 hours, calcined at 550℃ for 4 hours, and sieved to obtain the target catalyst. Under unified evaluation conditions, the HCC-240fa conversion rate was 100%, the HFO-1233zd(E) selectivity was 95.3%, the stable operating time was 890 hours, the carbon deposition amount was 1.41wt%, and the rare earth loss rate was 0.10wt%.

[0025] Example 5

[0026] The composite support was selected with a Zr:Al molar ratio of 1:6 and a Ce:Pr:Nd molar ratio of 4:1:1, with a total rare earth loading of 12wt%. The preparation steps of the zirconium-aluminum composite precursor and the ZrO2-AlF3 composite support were as described in Example 1. The three rare earth nitrates were weighed according to the ratio to prepare the impregnation solution, and the support was impregnated with an equal volume. The solution was stirred at room temperature for 6 hours, allowed to stand and solidify for 12 hours, and then calcined at 550℃ for 4 hours before sieving to obtain the catalyst. Under the same catalytic evaluation conditions, the HCC-240fa conversion rate was 100%, the HFO-1233zd(E) selectivity was 96.2%, the stable operating time was 930 hours, the carbon deposition amount was 0.90wt%, and the rare earth loss rate was 0.13wt%.

[0027] Example 6

[0028] A ternary composite support was selected, with a Zr:Al molar ratio of 1:6 and a Ce:Pr:Nd molar ratio of 3:1:1, and a total rare earth loading of 6 wt%. A zirconium-aluminum salt mixed solution was prepared, and co-precipitated with ammonia water at pH=8.5. After aging at 65℃ for 3 h, it was pre-calcined at 500℃ to obtain zirconium-aluminum composite oxide. Ammonium fluoride impregnation and fluorination were used to obtain a two-phase composite support. The support was impregnated with an equal volume of rare earth impregnation solution, stirred at room temperature for 6 h, allowed to stand for 12 h for solidification, and calcined at 550℃ for 4 h to prepare the catalyst. Under the unified evaluation conditions, the conversion rate of HCC-240fa was 100%, the selectivity of HFO-1233zd(E) was 99.7%, the stable operating time was 1100 h, the carbon deposition was 0.62 wt%, and the rare earth loss rate was 0.06 wt%.

[0029] Example 7

[0030] The composite carrier was selected with a Zr to Al molar ratio of 1:5, and a Ce:Pr molar ratio of 2:1 was used for binary rare earth compounding. The total rare earth loading was selected within the preferred range of 5 wt%. Zirconium oxynitrate and aluminum nitrate nonahydrate were weighed to prepare a mixed salt solution with a total metal ion concentration of 1.0 mol / L. 25 wt% ammonia water was added in parallel to co-precipitate for 70 min. The pH of the system was controlled at 8.4. The solution was aged in a water bath at 55℃ for 2.5 h, filtered and washed with water until the filtrate was neutral. It was then rinsed with anhydrous ethanol, dried at 110℃ for 12 h and passed through a 40-mesh sieve. The solution was pre-calcined at 500℃ for 3 h at a rate of 3℃ / min to obtain zirconium aluminum composite oxide powder. An ammonium fluoride impregnation solution was prepared with an F / (Zr+Al) molar ratio of 1.0. The solution was impregnated with an equal volume for 3.5 h, vacuum dried at 80℃ for 8 h, and fluorinated and calcined at 400℃ for 2 h at a rate of 3℃ / min to obtain ZrO2-AlF 3. Composite carrier: Equal volumes of cerium nitrate hexahydrate and praseodymium nitrate hexahydrate were impregnated in the carrier. The mixture was stirred at room temperature for 6 hours, sealed and allowed to stand for 11 hours to cure, dried at 120℃ for 10 hours, and calcined at 550℃ for 4 hours by heating at 5℃ / min. The catalyst was obtained by sieving and obtained as a 20-40 mesh. Under unified evaluation conditions, the conversion rate of HCC-240fa was 100%, the selectivity of HFO-1233zd(E) was 96.4%, the stable operating time was 1010 hours, the carbon deposition was 0.78 wt%, and the rare earth loss rate was 0.08 wt%.

[0031] Example 8

[0032] The composite carrier was selected with a Zr:Al molar ratio of 1:7 (optimal), a Ce:Nd molar ratio of 2:1 (binary rare earth element), and a total rare earth loading of 8 wt%. A mixed salt solution with a total metal ion concentration of 1.0 mol / L was prepared using zirconium oxynitrate and aluminum nitrate nonahydrate. The solution was co-precipitated with 25 wt% ammonia solution under concurrent flow, with pH controlled at 8.6. The solution was aged in a 60℃ water bath for 3 hours, filtered, washed with water until the filtrate was neutral, rinsed with anhydrous ethanol, dried at 110℃ for 12 hours, passed through a 40-mesh sieve, and pre-calcined at 500℃ for 3 hours at a 4℃ / min rate to obtain the zirconium-aluminum composite. Composite supports were prepared by impregnating with ammonium fluoride impregnation solution at room temperature for 4 h, drying, and then fluorinating and calcining at 390℃ for 2 h; impregnation solutions were prepared using cerium nitrate hexahydrate and neodymium nitrate hexahydrate, impregnated at room temperature for 6 h, allowed to stand and solidify for 13 h, dried at 120℃ for 10 h, and calcined at 550℃ for 4 h to obtain catalysts. Under the same evaluation conditions, HCC-240fa had a conversion rate of 100%, HFO-1233zd(E) had a selectivity of 97.2%, a stable operating time of 1040 h, a carbon deposition rate of 0.71 wt%, and a rare earth loss rate of 0.07 wt%.

[0033] Comparative Example 1

[0034] Commercial aluminum fluoride was used directly as the catalyst support without loading any rare earth active components. Commercial aluminum fluoride particles of 20-40 mesh were directly packed into the reactor for catalytic evaluation. All other evaluation conditions remained consistent with the example. The test results showed a HCC-240fa conversion rate of 97.3%, an HFO-1233zd(E) selectivity of 86.5%, a stable operating time of 620 h, and a carbon deposition of 3.75 wt%. Since there were no rare earth components, there was no data on rare earth loss. This comparative example demonstrates that the pure aluminum fluoride support is too acidic, resulting in severe carbon deposition and poor selectivity for the target product and catalyst lifetime.

[0035] Comparative Example 2

[0036] The ZrO2-AlF3 two-phase composite support was prepared according to Example 1, omitting the rare earth impregnation and loading process. The prepared 20-40 mesh ZrO2AlF3 composite support was directly used as a catalyst for evaluation. Ce, Pr, and Nd rare earth active components were not introduced. Under uniform conditions, the test results showed that the HCC-240fa conversion rate was 98.1%, the HFO-1233zd(E) selectivity was 88.2%, the stable operating time was 780 h, the carbon deposition amount was 3.12 wt%, and there was no data on rare earth loss. This comparative example proves that the ZrO2-AlF3 two-phase support itself has certain fluorination activity, but it lacks the ability of rare earth components to regulate surface acidity, construct oxygen vacancies, and suppress carbon deposition and side reactions. Its catalytic performance is significantly lower than that of the rare earth modified catalyst.

[0037] The performance of each embodiment and comparative example is summarized in Table 1.

[0038] Table 1 Performance summary of the examples and comparative examples

[0039] serial number HCC-240fa conversion rate (%) HFO-1233zd(E) Selectivity (%) Stable runtime (h) Carbon deposition amount (wt%) Rare earth loss rate (wt%) Example 1 100 94.5 950 0.95 0.11 Example 2 100 95.8 990 1.08 0.09 Example 3 100 97.1 1050 1.26 0.07 Example 4 100 95.3 890 1.41 0.10 Example 5 100 96.2 930 0.90 0.13 Example 6 100 99.7 1100 0.62 0.06 Example 7 100 96.4 1010 0.78 0.08 Example 8 100 97.2 1040 0.71 0.07 Comparative Example 1 97.3 86.5 620 3.75 - Comparative Example 2 98.1 88.2 780 3.12 -

Claims

1. A chromium-free, environmentally friendly catalyst for the gas-phase fluorination of 1,1,1,3,3-pentachloropropane to prepare trans-1-chloro-3,3,3-trifluoropropene, characterized in that: The catalyst is composed of a two-phase composite support consisting of ZrO2 and AlF3 crystal phases and two or more of the rare earth elements Ce, Pr and Nd loaded on the surface of the support.

2. The chromium-free environmentally friendly catalyst according to claim 1, characterized in that, The molar ratio of Zr to Al in the composite carrier is 1:2~10.

3. The chromium-free environmentally friendly catalyst according to claim 1, characterized in that, The molar ratio of Ce, Pr, and Nd among the three rare earth elements is (0~1):(0~1):(0~1), and the amounts of Ce, Pr, and Nd are not simultaneously zero. The total rare earth loading is 2wt%~12wt% of the total mass of the catalyst.

4. The chromium-free environmentally friendly catalyst according to claim 1, characterized in that, The composite carrier is prepared by in-situ fluorination of zirconium aluminum composite oxide with ammonium fluoride, with ZrO2 as the continuous framework phase and AlF3 as the surface dispersed phase.

5. A method for preparing the chromium-free environmentally friendly catalyst according to any one of claims 1 to 4, characterized in that, Includes the following steps: (1) ZrO2-Al2O3 composite precursor was prepared by co-precipitation method: zirconium salt and aluminum salt were dissolved in deionized water to prepare mixed metal salt solution, and ammonia water was added dropwise in parallel to carry out co-precipitation. The pH of the system was controlled at 8.0~9.

0. After aging, filtration, washing and drying, zirconium aluminum composite oxide powder was obtained by pre-calcination at 450℃~550℃. (2) Fluorination modification to prepare ZrO2-AlF3 two-phase composite support: The obtained zirconium aluminum composite oxide powder was impregnated with an equal volume of ammonium fluoride solution at room temperature for 2h~6h, dried and then fluorinated and calcined to obtain a ZrO2-AlF3 composite support with two phases coexisting. (3) Loading rare earth active components: Ce, Pr and Nd nitrates are prepared into a uniform impregnation solution according to a preset ratio, and loaded onto the surface of ZrO2-AlF3 composite carrier by equal volume impregnation method. Impregnation is carried out at room temperature for 4h~9h, static curing is carried out for 8h~16h, and after drying, it is calcined at high temperature of 400℃~700℃ for 2h~6h to obtain rare earth modified ZrO2-AlF3 fluorination catalyst.

6. The method for preparing a chromium-free environmentally friendly catalyst according to claim 5, characterized in that, In step (1), the precipitation aging temperature is 30℃~100℃, the aging time is 1h~5h, and the pre-calcination heating rate is 1℃ / min~7℃ / min.

7. The method for preparing a chromium-free environmentally friendly catalyst according to claim 5, characterized in that, Step (2) The fluorination calcination temperature is 350℃~450℃, and the calcination time is 1h~3h.

8. The application of the chromium-free environmentally friendly catalyst according to any one of claims 1 to 4 in the one-step gas-phase fluorination of 1,1,1,3,3-pentachloropropane to prepare trans-1-chloro-3,3,3-trifluoropropene.

Citation Information

Patent Citations

  • Method for synthesizing trans1-chlorine-3,3,3-trifluoropropene, and preparation of catalyst thereof

    CN106748626A