A copper-based catalyst, a preparation method and application thereof

By preparing a copper-based catalyst and employing co-precipitation crystallization and in-situ calcination carbonization techniques, a Cu⁰-Cu⁺-Lewis alkaline site synergistic catalytic system was constructed. This solved the problems of heavy metal pollution and harsh reaction conditions associated with chromium-based catalysts, and enabled the efficient, green, and stable hydrogenation reaction of dimethyl 1,4-cyclohexanedicarboxylate, which is suitable for industrial applications.

CN123148975APending Publication Date: 2026-11-24ZHEJIANG HENGYI PETROCHEMICAL RES INST CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611079240.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing chromium-based catalysts for the hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate to 1,4-cyclohexanediethanol present problems such as heavy metal pollution, harsh reaction conditions, complex preparation processes, and difficulties in product separation, making it difficult to achieve efficient and green production.

Method used

Using a copper-based catalyst, a copper nanoparticle catalyst containing a composite metal oxide support of divalent magnesium and trivalent iron and a nitrogen-doped porous carbon coating was prepared through co-precipitation crystallization, in-situ calcination carbonization, and reduction treatment. This formed a Cu⁰-Cu⁺-Lewis alkaline site synergistic catalytic system, enabling highly efficient hydrogenation reactions.

Benefits of technology

The catalyst achieves efficient hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate under mild conditions, with a feed conversion rate of ≥99%, a product selectivity of ≥98%, and excellent catalyst stability, making it suitable for continuous industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148975A_ABST
    Figure CN123148975A_ABST
Patent Text Reader

Abstract

The application provides a copper-based catalyst, a preparation method and application thereof. The copper-based catalyst comprises a substrate and a nitrogen-doped porous carbon coating layer coated on at least part of the surface of the substrate, the substrate comprises a composite carrier and an active component loaded on the composite carrier; the composite carrier comprises a composite metal oxide containing a divalent magnesium element and a trivalent iron element; the active component comprises copper nanoparticles, the copper nanoparticles comprise Cu 0 and Cu + . The copper-based catalyst is green and chromium-free, can realize efficient hydrogenation of 1,4-cyclohexane dimethyl dicarboxylate under mild conditions, has raw material conversion rate of no less than 99%, product selectivity of no less than 98%, high trans / cis ratio, excellent catalyst stability, long service life and is suitable for industrialized continuous production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst preparation, and more particularly to a copper-based catalyst, its preparation method, and its application. Background Technology

[0002] 1,4-Cyclohexanediethanol (CHDM) is a key monomer for synthesizing modified polyesters such as poly(1,4-cyclohexanediethanol) terephthalate (PCT), polyethylene terephthalate-1,4-cyclohexanediethanol (PETG), and poly(1,4-cyclohexanediethanol) isophthalate (PCTA). Its molecular structure exhibits excellent symmetry, and the polymer materials derived from it possess superior thermal stability, transparency, impact resistance, abrasion resistance, and corrosion resistance compared to conventional polyesters (PET) and polybutylene terephthalate (PBT). It has been widely used in the manufacturing of high-end products such as advanced liquid crystal materials, medical devices, electrical appliances, and high-performance shrink films.

[0003] In recent decades, CHDM has gradually replaced ethylene glycol in the synthesis of high-heat-resistant polyesters due to its comprehensive performance advantages, becoming a preferred key chemical intermediate in the industry. Currently, the mainstream technical route for industrial-scale CHDM production involves using a chromium trioxide-modified copper-based (Cu-Cr2O3) heterogeneous catalyst for the catalytic hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate (DMCD). To optimize this catalytic system, scholars both domestically and internationally have conducted extensive research, but the following technical bottlenecks remain to be addressed: traditional Cu-Cr2O3 catalysts contain highly toxic chromium components, causing severe heavy metal pollution during production, use, and disposal, which does not meet the requirements of green chemical development. To date, the only reported feasible CHDM preparation route on an industrial scale is the catalytic hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate (DMCD) using a Cr2O3-promoted copper-based (Cu-Cr2O3) heterogeneous catalyst. However, these chromium-containing catalysts have a certain degree of toxicity, and although they exhibit good activity, they cause serious environmental pollution. Therefore, developing green, chromium-free catalysts with high activity and selectivity for the hydrogenation reaction of DMCD has always been a challenge.

[0004] In recent years, researchers both domestically and internationally have conducted extensive studies on the modification of catalysts for the hydrogenation of DMCD to CHDM. Hu et al. (J. Mol. Catal. A 2015, 397, 134-141) synthesized a highly dispersed and stable supported copper-based catalyst using a Cu-Zn-Al layered double hydroxide (LDH) precursor for the gas-phase hydrogenation of DMCD to CHDM, achieving a high CHDM yield of 95.6%. The high activity was attributed to the presence of highly dispersed and stable active copper species, as well as an appropriate amount of Cu. +The species promoted the activation of the ester groups in the reactants, but the hydrogen-to-oil ratio of the reaction was too high (H2 / DMCD=406 (mol / mol)), resulting in excessive hydrogen consumption.

[0005] Chang et al. (J. Mater. Chem. A, 2025, 13, 16759) prepared a highly stable Cu / MgO@SiO2 catalyst for the hydrogenation reaction of BHCD (diethylene terephthalate) using modified CuMg-MOF-74 material. The results showed that the conversion rate of BHCD and the CHDM selectivity reached 99.2% and 97.1%, respectively, which were superior to Cu / MgO and other Cu-SiO2 catalysts. The better activity of this catalyst is attributed to its larger specific surface area and pore volume, higher dispersion of metallic Cu, and abundant basic sites. However, the reaction temperature is too high (240~260℃), which is not conducive to the long-term stability of the catalyst. In addition, the preparation of this catalyst is complicated and difficult to apply industrially.

[0006] Luo et al. (Appl. Catal. A2020, 602, 117669) modified the structure and chemical properties of the catalyst by loading 5 wt% Re onto the surface of activated carbon, and used it for the liquid-phase hydrogenation reaction of DMCD. Under the conditions of 220 °C and 10 MPa pressure, the CHDM yield was 66%, but the CHDM yield was still low due to the high reaction pressure.

[0007] Patent document CN104888789A discloses a catalyst for preparing 1,4-cyclohexanediethanol. This catalyst is prepared by dissolving zinc nitrate and aluminum nitrate in water containing polyethylene glycol to form a complex, which is then co-precipitated with copper nitrate and an auxiliary metal nitrate. When used to prepare 1,4-cyclohexanediethanol, the highest recission-to-cis ratio is 3.82:1. However, the above method for preparing the catalyst generates organic wastewater due to the presence of polyethylene glycol, making the preparation process complex. It also fails to mention intermediates with similar boiling points to the product. Although the selectivity is high, it is not conducive to subsequent separation and purification.

[0008] Therefore, how to solve the problems of existing catalyst toxicity pollution, harsh reaction conditions, complex preparation process, difficult product separation and low CHDM-cis ratio in the reaction system for the catalytic hydrogenation of 1,4-cyclohexanedicarboxylate to prepare 1,4-cyclohexanedimethylethanol is a technical challenge that urgently needs to be overcome in this field. Summary of the Invention

[0009] This invention provides a copper-based catalyst, its preparation method, and its application. The copper-based catalyst provided by this invention is green and chromium-free, and can achieve efficient hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate under mild conditions. The feed conversion rate is ≥99%, the product selectivity is ≥98%, the reaction-cis ratio is high, the catalyst has excellent stability, and a long service life, making it suitable for continuous industrial production.

[0010] This invention provides a copper-based catalyst, comprising a matrix and a nitrogen-doped porous carbon coating layer covering at least a portion of the surface of the matrix. The matrix includes a composite support and an active component loaded on the composite support. The composite support comprises a composite metal oxide containing divalent magnesium and trivalent iron. The active component comprises copper nanoparticles, wherein the copper nanoparticles include Cu. 0 and Cu + .

[0011] According to one embodiment of the present invention, the average particle size of the copper nanoparticles is 5 nm to 8 nm.

[0012] According to one embodiment of the present invention, based on the total mass of the copper-based catalyst, the mass percentage of copper in the copper nanoparticles is 14% to 37%.

[0013] According to one embodiment of the present invention, based on the total mass of the copper-based catalyst, the mass percentage of nitrogen in the nitrogen-doped porous carbon coating layer is 2% to 5%.

[0014] According to one embodiment of the present invention, based on the total mass of the copper-based catalyst, the mass percentage of carbon in the nitrogen-doped porous carbon coating layer is 5% to 10%.

[0015] In another aspect, the present invention provides a method for preparing a copper-based catalyst, comprising the following steps: mixing a mixed solution of metal salts containing copper, magnesium, and iron salts with a mixed alkaline solution to obtain a mixed suspension; crystallizing the mixed suspension to obtain a copper-based ternary layered double hydroxide precursor; mixing the copper-based ternary layered double hydroxide precursor with a nitrogen-containing carbon material and calcining it in an inert atmosphere to obtain a copper-based catalyst precursor; and reducing the copper-based catalyst precursor in a hydrogen atmosphere to obtain the copper-based catalyst.

[0016] According to one embodiment of the present invention, the copper salt includes one or more of copper nitrate, copper acetate, and copper chloride.

[0017] According to one embodiment of the present invention, the magnesium salt includes one or more of magnesium nitrate, magnesium acetate, and magnesium chloride.

[0018] According to one embodiment of the present invention, the iron salt includes one or more of ferric nitrate, ferric acetate, and ferric chloride.

[0019] According to one embodiment of the present invention, in the metal salt mixed solution, Cu 2+ The concentration is 0.05 mol / L~0.15 mol / L, Mg 2+The concentration is 0.05 mol / L~0.75 mol / L, Fe 3+ The concentration is 0.03 mol / L to 0.3 mol / L.

[0020] According to one embodiment of the present invention, in the metal salt mixed solution, the Cu 2+ With the Mg 2+ The molar ratio is (0.2~1):1.

[0021] According to one embodiment of the present invention, the Cu 2+ With the Mg 2+ The total number of moles and the Fe 3+ The molar ratio is (2~4):1.

[0022] According to one embodiment of the present invention, the mixed alkaline solution comprises a sodium hydroxide solution and a sodium carbonate solution.

[0023] According to one embodiment of the present invention, the crystallization treatment is performed at a temperature of 30°C to 60°C for a time of 6 hours to 24 hours.

[0024] According to one embodiment of the present invention, the nitrogen-containing carbon material includes one or more of melamine, cyanamide, polyaniline, polypyrrole, and urea.

[0025] According to one embodiment of the present invention, the mass ratio of the copper-based ternary layered double hydroxide precursor to the nitrogen-containing carbon material is 1:(0.1~2).

[0026] According to one embodiment of the present invention, the calcination treatment is carried out at a temperature of 350°C to 550°C for a time of 3 hours to 6 hours.

[0027] According to one embodiment of the present invention, the reduction treatment is performed at a temperature of 250°C to 350°C for a time of 1 hour to 4 hours.

[0028] In another aspect, the present invention provides a method for preparing 1,4-cyclohexanediethanol, comprising the following steps: hydrogenating dimethyl 1,4-cyclohexanedicarboxylate in the presence of a catalyst to obtain the 1,4-cyclohexanediethanol; wherein the catalyst comprises the copper-based catalyst described above, or a copper-based catalyst prepared according to the method described above.

[0029] The implementation of this invention has at least the following beneficial effects: The copper-based catalyst provided by this invention is green and chromium-free, and can achieve efficient hydrogenation of dimethyl 1,4-cyclohexanedicarboxylate under mild conditions, with a feed conversion rate of ≥99%, a product selectivity of ≥98%, a high cis-to-reverse ratio, excellent catalyst stability, and a long service life, making it suitable for continuous industrial production. Attached Figure Description

[0030] Figure 1 The X-ray diffraction pattern of the copper-based catalyst provided in Example 1 of this application;

[0031] Figure 2 The X-ray photoelectron spectrum of the copper-based catalyst provided in Example 1 of this application;

[0032] Figure 3 This is a transmission electron microscope image of the copper-based catalyst provided in Example 1 of this application;

[0033] Figure 4 The performance evaluation curve of the copper-based catalyst for DMCD hydrogenation reaction provided in Example 1 of this application is shown. Detailed Implementation

[0034] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. The specific embodiments listed below are merely descriptions of the principles and features of this invention, and the examples given are only for explaining this invention and are not intended to limit the scope of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0035] This invention provides a copper-based catalyst, comprising a matrix and a nitrogen-doped porous carbon coating layer covering at least a portion of the surface of the matrix. The matrix includes a composite support and an active component supported on the composite support. The composite support comprises a composite metal oxide containing divalent magnesium and trivalent iron. The active component comprises copper nanoparticles, wherein the copper nanoparticles include Cu. 0 and Cu + .

[0036] According to the inventors' research, the copper-based catalyst provided by this invention constructs a surface-interface Cu through an integrated structural design of "composite support - dual-valent active component - nitrogen-doped porous carbon coating layer". 0 -Cu + - A highly efficient catalytic system with synergistic effects of Lewis basic sites. Specifically, it involves a composite metal oxide containing divalent magnesium and trivalent iron, obtained through a topological transformation of a ternary layered oxide precursor formed by the co-precipitation of copper, magnesium, and iron. The unique microstructure of the layered precursor allows for uniform distribution of the metal elements, fostering strong metal-support interactions and resulting in the formation of abundant Cu at the interface. + The stable structure of -OM (M stands for magnesium / iron) replaces traditional chromium-containing catalysts from the source, avoiding heavy metal pollution; at the same time, the composite support has intrinsic Lewis basic sites, which can synergistically activate ester carbonyl groups and promote the hydrogenation of C=O bonds.

[0037] The active component uses Cu 0 and Cu + Copper nanoparticles, in which Cu 0 This refers to metallic copper, which is responsible for the efficient dissociation of hydrogen gas to generate active hydrogen species; the interface state Cu. + It can interact with the lone pair electrons of the oxygen atom in the carbonyl group of the ester group to polarize the C=O bond, thereby activating the ester group. The two are spatially close to each other to form a synergistic catalytic system, which can achieve high catalytic activity under mild reaction conditions. Moreover, it can precisely affect the cis-trans isomerization process of CHDM by regulating the electronic microenvironment at the interface, thereby improving the trans-cis ratio of the product.

[0038] Furthermore, the nitrogen-doped porous carbon coating layer, which covers at least a portion of the substrate surface, is generated through in-situ pyrolysis, eliminating the need for complex post-coating processes. This allows it to exert a physical spatial confinement effect, inhibiting the sintering and growth of copper nanoparticles and extending the catalyst's lifespan. Nitrogen atom doping significantly enhances the Lewis base site density on the catalyst surface, further modifying the electronic state of copper species and effectively promoting Cu... + Speciation occurs, and additional basic sites are introduced, Cu 0 -Cu + The synergistic effect among the three basic sites (Lewis, Lewis, and Lewis) enables the catalyst to exhibit excellent ester hydrogenation performance.

[0039] Specifically, iron ions (Fe 3+ It can form a stable ternary layered double hydroxide structure with magnesium and copper ions; its oxide has strong alkalinity and thermal stability, which can further enhance the Lewis alkalinity of the support and strengthen the interaction with copper species.

[0040] In some embodiments, the average particle size of the copper nanoparticles can be 5 nm to 8 nm, for example, a range consisting of 5 nm, 6 nm, 6.5 nm, 7 nm, 8 nm, or any combination thereof. An average particle size of not less than 5 nm helps reduce the tendency for excessively fine particles to aggregate; an average particle size of not more than 8 nm helps maintain a high active specific surface area and provides sufficient active sites. Controlling the average particle size of the copper nanoparticles within the above range is beneficial for balancing the hydrogenation activity and anti-sintering stability of the catalyst, solving the technical problem that existing catalysts struggle to simultaneously achieve both activity and stability.

[0041] In some embodiments, based on the total mass of the copper-based catalyst, the mass percentage of copper in the copper nanoparticles can be 14% to 37%, for example, a range of 14%, 20%, 25%, 30%, 37%, or any two of these. Copper is the core active component in catalytic hydrogenation. A mass percentage of copper not less than 14% helps provide sufficient hydrogenation active sites and ensures the conversion rate of the reaction; a mass percentage of copper not more than 37% helps maintain the high dispersibility of copper and inhibit particle agglomeration. Controlling the mass percentage of copper within the above range is beneficial for balancing the activity and stability of the catalyst, solving the problem that excessive copper content in existing catalysts easily leads to agglomeration, reducing dispersibility and stability.

[0042] In some embodiments, based on the total mass of the copper-based catalyst, the mass percentage of nitrogen in the nitrogen-doped porous carbon coating layer can be 2% to 5%, for example, 2%, 3%, 3.5%, 4%, 5%, or any combination thereof. Nitrogen atoms help introduce nitrogen-containing functional groups such as pyridine nitrogen and pyrrole nitrogen, providing additional Lewis basic sites and regulating the electronic structure of copper species. A nitrogen mass percentage of not less than 2% helps introduce sufficient basic sites and electronic effects, enhancing the ester activation ability and Cu. + Qualitatively, nitrogen content not exceeding 5% by mass helps maintain the structural integrity and stability of the carbon layer.

[0043] In some embodiments, based on the total mass of the copper-based catalyst, the mass percentage of carbon in the nitrogen-doped porous carbon coating layer can be 5% to 10%, for example, 5%, 6%, 7%, 8%, 9%, 10%, or any combination thereof. Carbon constitutes the framework structure of the coating layer. A carbon mass percentage of not less than 5% helps to form a continuous porous carbon coating layer and exert a spatial confinement effect; a carbon mass percentage of not more than 10% helps to avoid increased mass transfer resistance caused by an excessively thick coating layer; controlling the carbon mass fraction within the above range is beneficial for balancing the confinement effect of the coating layer and the mass transfer efficiency.

[0044] In summary, the copper-based catalyst of this invention is green and chromium-free, with good dispersibility and uniform particle size of copper nanoparticles. 0 With interface state Cu + The synergistic effect is significant. The nitrogen-doped porous carbon coating can effectively inhibit copper sintering. The catalyst has excellent stability and the preparation process is simple and easy to scale up industrially.

[0045] This invention also provides a method for preparing the above-mentioned copper-based catalyst, comprising the following steps: mixing a mixed solution of metal salts containing copper, magnesium, and iron salts with a mixed alkaline solution to obtain a mixed suspension; crystallizing the mixed suspension to obtain a copper-based ternary layered double hydroxide precursor; mixing the copper-based ternary layered double hydroxide precursor with a nitrogen-containing carbon material and calcining it in an inert atmosphere to obtain a copper-based catalyst precursor; and reducing the copper-based catalyst precursor in a hydrogen atmosphere to obtain the copper-based catalyst.

[0046] According to the inventors' research, the above-mentioned preparation method achieves green and efficient catalyst preparation through a three-step process of "co-precipitation crystallization to prepare the precursor - in-situ calcination carbonization - reduction treatment". Specifically, it uses a mixed solution of copper salt, magnesium salt and iron salt and a mixed alkaline solution for co-precipitation, which allows the three metal ions to hydrolyze simultaneously and self-assemble to form a ternary layered double hydroxide precursor (commonly known as ternary hydrotalcite), achieving uniform distribution of metal elements. This avoids the problems of local enrichment and uneven dispersion of active components that exist in traditional impregnation methods and physical mixing methods from the source. At the same time, it replaces the traditional preparation system of chromium-containing catalysts, eliminating the risk of heavy metal pollution.

[0047] By directly mixing the precursor with nitrogen-containing carbon materials and calcining them in an inert atmosphere, the topological transformation of the precursor to generate a composite metal oxide carrier, the in-situ generation of copper species, and the pyrolytic carbonization of the nitrogen-containing carbon materials can be achieved simultaneously. This results in the in-situ formation of a porous nitrogen-doped carbon layer coating the surface of the carrier and the active component, eliminating the need for complex post-coating processes and solving the problems of uneven coating and easy detachment of carbon layers in traditional post-coating methods.

[0048] Finally, a controlled reduction is performed under a hydrogen atmosphere, allowing for precise control of the valence state distribution of copper species, resulting in a product that combines Cu... 0 With interface state Cu + The dual active centers construct a highly efficient synergistic catalytic system, achieving high catalytic activity and a high product recission ratio under mild reaction conditions. At the same time, the spatial confinement effect of the porous nitrogen-doped carbon layer can inhibit the sintering of copper nanoparticles and improve the long-term stability of the catalyst.

[0049] In some embodiments, the copper salts described above include one or more of copper nitrate, copper acetate, and copper chloride. All of these copper salts are water-soluble inorganic copper salts, capable of completely dissociating into copper ions and corresponding anions in water, ensuring a uniform distribution of copper ions in the metal salt mixture solution. Their anions (e.g., nitrate, acetate, chloride ions) do not form stable, insoluble compounds with metal ions during co-precipitation, nor do they interfere with the nucleation and growth process of the ternary layered double hydroxide precursor. Furthermore, they can be completely decomposed or removed during subsequent calcination, leaving no harmful impurities in the catalyst.

[0050] In some embodiments, the magnesium salt comprises one or more of magnesium nitrate, magnesium acetate, and magnesium chloride. The magnesium salt exhibits excellent water solubility, and its anions match those of the copper salt, which helps to ensure consistent precipitation rates of the various metal ions in the co-precipitation system, achieving synchronous precipitation and thus allowing magnesium ions to be uniformly embedded in the lattice of the ternary layered double hydroxide precursor. Simultaneously, no impurity ions affecting catalytic performance are introduced.

[0051] In some embodiments, the iron salt includes one or more of ferric nitrate, ferric acetate, and ferric chloride. This helps to achieve uniform doping of iron ions, forming a pure-phase and structurally stable ternary hydrotalcite precursor.

[0052] In some embodiments, in the above-described metal salt mixed solution, Cu 2+ The concentration is 0.05 mol / L~0.15 mol / L, Mg 2+ The concentration is 0.05 mol / L~0.75 mol / L, Fe 3+ The concentration of metal ions is 0.03 mol / L to 0.3 mol / L. The concentration of metal ions directly affects the rate of coprecipitation reaction and the nucleation and growth process of precipitate particles. Controlling the concentration of metal ions within the above range is beneficial to obtaining precursors with good crystallinity and uniform elemental distribution, laying the foundation for the subsequent preparation of highly dispersed, highly active, and highly stable copper-based catalysts. This solves the problem of poor precursor quality and large fluctuations in catalytic performance caused by improper concentration control in existing coprecipitation processes.

[0053] For example, Cu 2+ The concentration can be from 0.05 mol / L to 0.15 mol / L, for example, 0.05 mol / L, 0.07 mol / L, 0.09 mol / L, 0.11 mol / L, 0.15 mol / L, or any combination thereof. 2+ A concentration of not less than 0.05 mol / L helps ensure the basic content of copper active components in the final catalyst, providing sufficient hydrogenation active sites and avoiding low feed conversion rates due to insufficient active sites; Cu 2+ A concentration not exceeding 0.15 mol / L helps avoid local oversaturation in the coprecipitation reaction system, prevents rapid aggregation of copper ions to form amorphous copper hydroxide impurities, and maintains atomically uniform dispersion of copper species in the hydrotalcite layer; Cu 2+ Controlling the concentration within the above range is beneficial for balancing the activity of the catalyst and the dispersibility of copper species, thus solving the problem of insufficient activity or severe agglomeration caused by improper control of copper concentration in the traditional co-precipitation method.

[0054] For example, the above-mentioned Mg 2+The concentration can be from 0.05 mol / L to 0.75 mol / L, for example, 0.05 mol / L, 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.75 mol / L, or any combination thereof. Mg 2+ A concentration of not less than 0.05 mol / L helps to construct a complete and stable layered framework structure of the double hydroxide, providing sufficient lattice sites for copper and iron ions, and enhancing the anchoring effect of the subsequently formed composite support on copper species; Mg 2+ A concentration not exceeding 0.75 mol / L helps to avoid a decrease in catalytic activity due to an excessively low relative proportion of copper ions, while also preventing the formation of a single magnesium hydroxide impurity phase that could disrupt the pure phase structure of the copper-based ternary layered double hydroxide precursor.

[0055] For example, Fe 3+ The concentration can be from 0.03 mol / L to 0.3 mol / L, for example, 0.03 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, or any combination thereof. Fe 3+ An ion concentration of not less than 0.03 mol / L helps maintain the charge balance of the layered structure, ensures the stable existence of interlayer carbonate anions, and promotes the formation of pure-phase copper-based ternary layered double hydroxide precursors; Fe 3+ An ion concentration not exceeding 0.3 mol / L helps avoid increased side reactions caused by excessive Lewis alkalinity on the support surface, while also preventing the precipitation of iron oxide impurities that weaken the interaction between copper and the support; Fe 3+ Controlling the ion concentration within the above range is beneficial for obtaining a pure-phase precursor with good crystallinity, laying the foundation for the subsequent preparation of high-performance catalysts and solving the Fe... 3+ Inappropriate content can lead to unstable precursor structure and increased byproducts.

[0056] In some embodiments, in the above-described metal salt mixed solution, Cu 2+ With Mg 2+ The molar ratio can be (0.2~1):1, for example, 0.2:1, 0.4:1, 0.6:1, 0.8:1, 1:1, or any combination thereof. Cu 2+ With Mg 2+ The molar ratio of Cu to copper is not less than 0.2:1, which helps to ensure that the catalyst contains sufficient copper active components and provides ample hydrogenation active sites; 2+ With Mg 2+ The molar ratio should not exceed 1:1, which helps maintain the high dispersibility of copper species and inhibits particle agglomeration; controlling the molar ratio within the above range is beneficial to balancing the activity and stability of the catalyst.

[0057] In some embodiments, the Cu described above 2+ With Mg 2+ The total number of moles of Fe and the above 3+ The molar ratio can be (2~4):1, for example, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, or any combination thereof. A molar ratio not lower than 2:1 helps maintain the positive charge balance of the layered structure and ensures the stable existence of interlayer anions; a molar ratio not higher than 4:1 helps avoid Fe... 3+ The insufficiency leads to instability in the layered structure; controlling the molar ratio within the above range is beneficial for generating a pure-phase and structurally stable copper-based ternary layered double hydroxide precursor.

[0058] In some embodiments, the aforementioned mixed alkaline solution includes a sodium hydroxide solution and a sodium carbonate solution. Sodium hydroxide completely dissociates into hydroxide ions in aqueous solution, which can act as a precipitant in co-precipitation reactions, causing metal ions to hydrolyze and form hydroxide precipitates. The carbonate ions dissociated from sodium carbonate act as balancing anions between the layers of the hydrotalcite, neutralizing the positive charge on the layers and stabilizing the layered structure. Simultaneously, the binding force between carbonate ions and the layers is moderate, allowing for complete decomposition into carbon dioxide gas during subsequent calcination, preventing impurities from remaining in the catalyst. Using sodium hydroxide alone as a precipitant fails to form a stable layered double hydroxide structure; using other anions (such as chloride or sulfate ions) as interlayer anions results in excessively strong binding forces, making removal during calcination difficult and affecting catalyst performance.

[0059] Specifically, in the above-mentioned mixed alkaline solution, the molar concentration of sodium hydroxide can be from 0.25 mol / L to 2.4 mol / L, for example, 0.25 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.4 mol / L, or any combination thereof. A molar concentration of sodium hydroxide not less than 0.25 mol / L helps to provide sufficient hydroxide ions, enabling the simultaneous precipitation of copper, magnesium, and iron ions, maintaining the pH of the reaction system stable within the target range, and avoiding incomplete precipitation of metal ions due to insufficient hydroxide ions. A molar concentration of sodium hydroxide not more than 2.4 mol / L helps to avoid a sudden increase in local pH during the dropwise addition process, preventing the dissolution of amphoteric copper hydroxide and iron hydroxide, reducing the formation of amorphous precipitates and impurities, and reducing the amount of alkaline residue in the subsequent washing process. The concentration of sodium carbonate can be from 0.06 mol / L to 0.6 mol / L, for example, 0.06 mol / L, 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.6 mol / L, or any combination thereof. A sodium carbonate concentration of not less than 0.06 mol / L helps to provide sufficient carbonate ions as balancing anions between the layers of hydrotalcite, neutralize the positive charge of the layers, stabilize the layered structure of the hydroxide precursor, and avoid the formation of a single hydroxide impurity phase. A sodium carbonate concentration of not more than 0.6 mol / L helps to avoid the formation of carbonate precipitates by excessive carbonate ions and metal ions, while also preventing excessive structural collapse during precursor calcination due to excessive interlayer anions.

[0060] The molar concentration of sodium hydroxide in the mixed alkaline solution is twice that of Cu. 2+ Mg 2+ and Fe 3+ The total molar concentration, i.e., [NaOH] = 2([Cu] 2+ ]+[Mg 2+ ]+[Fe 3+ The molar concentration of sodium carbonate is twice that of Fe. 3+ Molar concentration, i.e., [Na₂CO₃] = 2[Fe 3+ ].

[0061] Specifically, the molar concentration of sodium hydroxide can be from 0.25 mol / L to 2.4 mol / L, for example, a range of 0.25 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.4 mol / L, or any combination thereof.

[0062] Specifically, the molar concentration of sodium carbonate can be from 0.06 mol / L to 0.6 mol / L, for example, 0.06 mol / L, 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, or any combination thereof.

[0063] In addition, the pH of the mixed suspension was controlled to be 10-11 by adding a mixed alkaline solution dropwise. Maintaining the pH of the mixed suspension within this range helps to promote the simultaneous and complete precipitation of copper, magnesium, and iron ions, avoiding a low elemental ratio due to incomplete precipitation of some metal ions, and providing a suitable alkaline environment for the nucleation and growth of copper-based ternary layered double hydroxide precursors.

[0064] In some embodiments, the crystallization temperature can be 30°C to 60°C, for example, a range of 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, or any combination thereof; the crystallization time can be 6 hours to 24 hours, for example, 6 hours, 10 hours, 14 hours, 18 hours, 22 hours, 24 hours, or any combination thereof. The crystallization process is a process of growth, structural refinement, and increased crystallinity of the copper-based ternary layered double hydroxide precursor. A crystallization temperature not lower than 30°C and a time not lower than 6 hours help to ensure sufficient growth and structural refinement of the precursor, thereby increasing its crystallinity. A crystallization temperature not higher than 60°C and a time not higher than 24 hours help to avoid excessive crystal growth, maintaining a smaller particle size and a larger specific surface area. Controlling the crystallization conditions within the above range is beneficial for obtaining copper-based ternary layered double hydroxide precursors with good crystallinity and suitable particle size.

[0065] The preparation method of copper-based catalysts also includes: obtaining a crystallization solution containing a copper-based ternary layered double hydroxide precursor after crystallization treatment; centrifuging the crystallization solution, washing it with deionized water until the pH of the washing solution is neutral, and drying it to obtain the copper-based ternary layered double hydroxide precursor.

[0066] Specifically, the temperature of the drying process can be 70℃~100℃, for example, 70℃, 80℃, 85℃, 90℃, 100℃ or any combination thereof; the time of the crystallization process can be 12h~24h, for example, 12h, 14h, 16h, 18h, 20h, 22h, 24h or any combination thereof.

[0067] In some embodiments, the aforementioned nitrogen-containing carbon materials include one or more of melamine, cyanamide, polyaniline, polypyrrole, and urea. These materials are all nitrogen-rich organic compounds with high nitrogen content, and can generate a carbon coating layer with a high nitrogen content during pyrolysis in an inert atmosphere. Simultaneously, these materials decompose during pyrolysis to produce large amounts of gases such as ammonia and carbon dioxide, which can act as in-situ pore-forming agents, forming abundant mesoporous and microporous structures within the carbon coating layer, thereby enhancing the modification effect.

[0068] In some embodiments, the mass ratio of the copper-based ternary layered double hydroxide precursor to the nitrogen-containing carbon material can be 1:(0.1~2), for example, a range consisting of 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, or any two of these. A mass ratio of copper-based ternary layered double hydroxide precursor to nitrogen-containing carbon material of not less than 1:0.1 helps to form a continuous carbon coating layer, exerting spatial confinement and electronic regulation effects; a mass ratio of not more than 1:2 helps to avoid increased mass transfer resistance and active site coverage caused by excessively thick carbon coating layers; controlling this mass ratio within the above range is beneficial for obtaining a carbon coating layer with suitable thickness and excellent performance, solving the technical problem of poor performance caused by improper ratio control in existing coating processes.

[0069] In some embodiments, the calcination temperature can be 350°C to 550°C, for example, a range of 350°C, 400°C, 450°C, 500°C, 550°C, or any combination thereof; the calcination time is 3h to 6h, for example, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or any combination thereof. The calcination process is a coupled process of topological transformation of the copper-based ternary layered double hydroxide precursor and pyrolytic carbonization of the nitrogen-containing carbon material. A calcination temperature not lower than 350°C and a time not lower than 3h facilitate complete decomposition of the precursor and sufficient carbonization of the nitrogen-containing carbon material; a calcination temperature not higher than 550°C and a time not higher than 6h help suppress the sintering of copper nanoparticles and the destruction of the carbon coating structure; controlling the calcination conditions within the above range is beneficial for obtaining a copper-based ternary layered double hydroxide precursor with excellent structure and performance.

[0070] The heating rate from room temperature to the calcination temperature can be 2℃ / min to 10℃ / min, for example, a range of 2℃ / min, 4℃ / min, 6℃ / min, 8℃ / min, 10℃ / min or any combination thereof.

[0071] The above-mentioned roasting process is carried out in an inert atmosphere, which includes one or more of helium, nitrogen, and argon.

[0072] In some embodiments, the temperature of the reduction treatment can be 250°C to 350°C, for example, a range of 250°C, 270°C, 290°C, 310°C, 350°C, or any combination thereof; the time of the reduction treatment can be 1 hour to 4 hours, for example, a range of 1 hour, 2 hours, 2.5 hours, 3 hours, 4 hours, or any combination thereof. The reduction process is a key step in regulating the valence state of copper species and affects the Cu content in the catalyst. 0 and Cu + The proportion and distribution of copper species, with a reduction temperature not lower than 250℃ and a time not lower than 1 hour, help to fully reduce copper oxide and form sufficient active sites; a reduction temperature not higher than 350℃ and a time not higher than 4 hours help to precisely control the valence state distribution of copper species and maintain a suitable Cu content. 0 and Cu + The ratio is adjusted to inhibit particle sintering; controlling the reduction conditions within the above range is beneficial for obtaining copper-based catalysts with suitable valence distribution and good dispersion.

[0073] Specifically, the space velocity for the reduction of the aforementioned 10% H2 / N2 mixture is 300 h⁻¹. -1 ~1000h -1 For example, 300h -1 500h -1 700h -1 900h -1 1000h -1 or a range consisting of any two of them.

[0074] In specific implementation, copper salt, magnesium salt, iron salt, and deionized water are mixed to obtain a mixed metal salt solution; the mixed metal salt solution is stirred and mixed with a mixed alkaline solution to obtain a mixed suspension; the mixed suspension is crystallized to obtain a crystallized solution containing a copper-based ternary layered double hydroxide precursor; the crystallized solution is centrifuged, and the precipitate is washed with deionized water until the pH of the washing solution is neutral, and then dried to obtain a copper-based ternary layered double hydroxide precursor; the copper-based ternary layered double hydroxide precursor is mixed with a nitrogen-containing carbon material and calcined in an inert atmosphere to obtain a copper-based catalyst precursor; the copper-based catalyst precursor is reduced in a hydrogen atmosphere to obtain the copper-based catalyst.

[0075] In summary, the copper-based catalyst prepared by the above method is green and chromium-free. It can operate under mild conditions in the hydrogenation reaction of dimethyl 1,4-cyclohexanedicarboxylate, with a feed conversion rate of ≥99%, a selectivity of ≥98% for 1,4-cyclohexanediethanol, a high product cis-to-reverse ratio, and excellent long-term stability, making it suitable for continuous industrial production.

[0076] This invention also provides a method for preparing 1,4-cyclohexanediethanol, comprising the following steps: hydrogenating 1,4-cyclohexanedicarboxylate under the action of a catalyst to obtain the above-mentioned 1,4-cyclohexanediethanol; wherein the above-mentioned catalyst includes the above-mentioned copper-based catalyst, or a copper-based catalyst prepared according to the above-mentioned catalyst preparation method.

[0077] According to the inventors' research, the copper-based catalyst of this invention integrates highly dispersed copper nanoparticles and stable interfacial Cu... + It possesses multiple structural advantages, including abundant Lewis basic sites and a nitrogen-doped porous carbon coating. When applied to the hydrogenation reaction of dimethyl 1,4-cyclohexanedicarboxylate, it achieves highly efficient hydrogenation of 1,4-cyclohexanedicarboxylate under relatively low reaction pressure and hydrogen-to-oil ratio conditions. The resulting catalyst exhibits high feed conversion, good selectivity for the target product 1,4-cyclohexanediethanol, a high recission ratio, and excellent long-term operational stability. This solves the technical problems of existing catalysts in this reaction, such as chromium contamination, harsh reaction conditions, excessively high hydrogen-to-oil ratio, low recission ratio, and poor stability, thus meeting the requirements for continuous industrial production.

[0078] Specifically, the temperature of the hydrogenation reaction can be 210℃~250℃, for example, 210℃, 220℃, 230℃, 240℃, 250℃ or any combination thereof; the pressure of the hydrogenation reaction can be 1MPa~3MPa, for example, 1MPa, 1.5MPa, 2MPa, 2.5MPa, 3MPa or any combination thereof.

[0079] In some embodiments, the space velocity of the above-mentioned dimethyl 1,4-cyclohexanedicarboxylate can be 0.3 h⁻¹. -1 ~0.7h -1 For example, 0.3h -1 0.4h -1 0.5h -1 0.6h -1 0.7h -1 Or a range consisting of any two of them. Airspeed not less than 0.3 h / h -1 This helps increase the amount of raw materials processed per unit catalyst, improve production efficiency, and reduce equipment investment and operating costs for industrial production; the space velocity should not exceed 0.7 h⁻¹. -1 This helps ensure that the raw materials have sufficient residence time in the catalyst bed, allowing for the complete hydrogenation and conversion of dimethyl 1,4-cyclohexanedicarboxylate, and avoiding a decrease in raw material conversion rate and an increase in by-products due to incomplete reaction. Controlling the space velocity within the above range is beneficial for balancing the catalyst's production efficiency with the reaction's conversion rate and selectivity, thus meeting the needs of continuous industrial production.

[0080] The space velocity (H₂O) of dimethyl 1,4-cyclohexanedicarboxylate refers to the mass of dimethyl 1,4-cyclohexanedicarboxylate catalyzed by one gram of catalyst per unit time, expressed in h₂O. -1 .

[0081] In some embodiments, the molar ratio of hydrogen to dimethyl 1,4-cyclohexanedicarboxylate can be (120~200):1, for example, 120:1, or any combination thereof.

[0082] In practice, the catalyst is loaded into a fixed-bed reactor. Inert magnetic rings are installed at the upper and lower ends of the catalyst bed to ensure uniform distribution of the reaction gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate is pumped into the reaction apparatus and thoroughly mixed with hydrogen before being introduced into the catalyst bed for hydrogenation. The reaction product is condensed and the liquid phase is collected. Quantitative analysis is performed using gas chromatography to obtain 1,4-cyclohexanediethanol.

[0083] The present invention will be further described below through specific embodiments.

[0084] The raw materials used in the following examples and comparative examples can all be obtained by conventional means in the art, such as commercial purchases.

[0085] Example 1

[0086] S1, Preparation of copper-based catalysts

[0087] S1-1. Mix and dissolve 12.08g of Cu(NO3)2·3H2O, 25.64g of Mg(NO3)2·6H2O, 20.20g of Fe(NO3)3·9H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0088] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 0.5:1, Cu 2+ With Mg 2+ Total number of moles and Fe 3 + The molar ratio is 3:1;

[0089] S1-2, 16.00g sodium hydroxide and 10.60g anhydrous sodium carbonate were dissolved in 500mL deionized water to obtain a mixed alkaline solution; the mixed metal salt solution and the mixed alkaline solution were added dropwise to a beaker and stirred to obtain a mixed suspension, the pH of which was controlled at 10.5; the mixed suspension was crystallized in a 40℃ water bath for 12h to obtain a crystallized solution containing a copper-based ternary layered double hydroxide precursor; the crystallized solution was centrifuged, and the precipitate was washed with deionized water until the pH of the washing solution reached 7; the solution was dried at 70℃ for 12h to obtain the copper-based ternary layered double hydroxide precursor;

[0090] S1-3. The copper-based ternary layered double hydroxide precursor powder and melamine were mixed at a mass ratio of 0.5:1 and calcined at 400°C for 4 hours in a nitrogen atmosphere to obtain the copper-based catalyst precursor.

[0091] S1-4. Under a 10% H2 / Ar mixed gas atmosphere (the volume fraction of hydrogen in the mixed gas is 10%), the copper-based catalyst precursor was reduced at 300℃ (heating rate 5℃ / min) for 2 hours to obtain the copper-based catalyst.

[0092] In the copper-based catalyst prepared in Example 1, the average particle size of the copper nanoparticles was 8.2 nm as measured by the XDR Scherrer equation; the average particle size of the copper nanoparticles was 5.2 nm as measured by TEM. The Cu loading was 24.0%, the C content was 6.8%, and the N content was 3.2%.

[0093] Preparation of S2 and 1,4-cyclohexanediethanol:

[0094] A copper-based catalyst was loaded into a fixed-bed reactor. The reaction tube had an inner diameter of 20 mm and contained 20 g of copper-based catalyst. Inert magnetic rings were installed at the top and bottom of the catalyst bed to ensure uniform distribution of the reactant gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) was added at a rate of 0.4 h⁻¹. -1 The mixture was transported to the reaction apparatus at space velocity and thoroughly mixed with H2 before being introduced into the catalyst bed. The molar ratio of H2 to DMCD was 160:1. The hydrogenation reaction was carried out at 225°C and a reaction pressure of 2.5 MPa. The pipeline was kept at a constant temperature throughout. The reaction product was condensed and the liquid phase was collected. Quantitative analysis was performed by gas chromatography to obtain 1,4-cyclohexanediethanol.

[0095] Example 2

[0096] S1, Preparation of copper-based catalysts

[0097] S1-1. Mix and dissolve 18.12g of Cu(NO3)2·3H2O, 19.23g of Mg(NO3)2·6H2O, 20.20g of Fe(NO3)3·9H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0098] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 1:1, Cu 2+ With Mg 2+ Total number of moles and Fe 3+ The molar ratio is 3:1;

[0099] The remaining preparation conditions were the same as in Example 1.

[0100] In the copper-based catalyst prepared in Example 2, the average particle size of the copper nanoparticles was 6.5 nm as measured by TEM, the Cu loading was 33.2%, the C content was 6.3%, and the N content was 3.1%.

[0101] Example 3

[0102] S1, Preparation of copper-based catalysts

[0103] S1-1. Mix and dissolve 6.04g of Cu(NO3)2·3H2O, 32.05g of Mg(NO3)2·6H2O, 20.20g of Fe(NO3)3·9H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0104] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 0.2:1, Cu 2+ With Mg 2+ Total number of moles and Fe 3 + The molar ratio is 3:1;

[0105] The remaining preparation conditions were the same as in Example 1.

[0106] In the copper-based catalyst prepared in Example 3, the average particle size of the copper nanoparticles was 7.3 nm as measured by TEM, the Cu loading was 13.1%, the C content was 6.7%, and the N content was 3.8%.

[0107] Example 4

[0108] S1, Preparation of copper-based catalysts

[0109] S1-1. Mix and dissolve 9.98g of Cu(CH3COO)2·H2O, 21.4g of Mg(CH3COO)2·4H2O, 15.25g of Fe(CH3COO)3·4H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0110] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 0.5:1, Cu 2+ With Mg 2+ Total number of moles and Fe 3 + The molar ratio is 3:1;

[0111] The remaining preparation conditions were the same as in Example 1.

[0112] In the copper-based catalyst prepared in Example 4, the average particle size of the copper nanoparticles was 6.2 nm as measured by TEM, the Cu loading was 24%, the C content was 6.7%, and the N content was 3.2%.

[0113] Example 5

[0114] S1, Preparation of copper-based catalysts

[0115] S1-1. Mix and dissolve 8.52g of CuCl2·2H2O, 20.30g of MgCl2·6H2O, 13.53g of FeCl3·6H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0116] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 0.5:1, Cu 2+ With Mg 2+ Total number of moles and Fe 3 + The molar ratio is 3:1;

[0117] The remaining preparation conditions were the same as in Example 1.

[0118] In the copper-based catalyst prepared in Example 5, the average particle size of the copper nanoparticles was 7.3 nm as measured by TEM, the Cu loading was 24%, the C content was 6.1%, and the N content was 3.3%.

[0119] Example 6

[0120] S1, Preparation of copper-based catalysts

[0121] S1-3. The copper-based ternary layered double hydroxide precursor powder and melamine were mixed at a mass ratio of 1:0.25 and calcined at 400°C for 4 hours in a nitrogen atmosphere to obtain the copper-based catalyst precursor.

[0122] The remaining preparation conditions were the same as in Example 1.

[0123] In the copper-based catalyst prepared in Example 6, the average particle size of the copper nanoparticles was 6.7 nm as measured by TEM, the Cu loading was 25.3%, the C content was 3.2%, and the N content was 1.4%.

[0124] Example 7

[0125] S1-3. The copper-based ternary layered double hydroxide precursor powder and melamine were mixed at a mass ratio of 1:1 and calcined at 400°C for 4 hours in a nitrogen atmosphere to obtain the copper-based catalyst precursor.

[0126] The remaining preparation conditions were the same as in Example 1.

[0127] In the copper-based catalyst prepared in Example 7, the average particle size of the copper nanoparticles was 7.5 nm as measured by TEM, the Cu loading was 21.3%, the C content was 12.2%, and the N content was 6.3%.

[0128] The difference between Comparative Example 1 and Example 1 is that melamine was not added; the other preparation conditions were the same as in Example 1.

[0129] In the copper-based catalyst prepared in Comparative Example 1, the average particle size of the copper nanoparticles was 8.4 nm as measured by TEM, the Cu loading was 26.7%, the C content was 0%, and the N content was 0%.

[0130] Comparative Example 2

[0131] S1, Preparation of copper-based catalysts

[0132] S1-1. Mix and dissolve 12.08g of Cu(NO3)2·3H2O, 6.73g of Fe(NO3)3·9H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0133] Cu in the metal salt mixed solution 2+ with Fe 3+ The molar ratio is 3:1;

[0134] The remaining preparation conditions were the same as in Example 1.

[0135] In the copper-based catalyst prepared in Comparative Example 2, the average particle size of copper nanoparticles was 11.5 nm as measured by TEM, the Cu loading was 43.2%, the C content was 7.1%, and the N content was 3.3%.

[0136] Comparative Example 3

[0137] S1, Preparation of copper-based catalysts

[0138] S1-1. Mix and dissolve 12.08g of Cu(NO3)2·3H2O, 25.64g of Mg(NO3)2·6H2O and 500mL of deionized water to obtain a mixed solution of metal salts.

[0139] Cu in the metal salt mixed solution 2+ With Mg 2+ The molar ratio is 0.5:1;

[0140] S1-2, 16.00g of sodium hydroxide was dissolved in 500mL of deionized water to obtain an alkaline solution;

[0141] The remaining preparation conditions were the same as in Example 1.

[0142] In the copper-based catalyst prepared in Comparative Example 3, the average particle size of copper nanoparticles was 13.6 nm as measured by TEM, the Cu loading was 36.1%, the C content was 7.2%, and the N content was 3.2%.

[0143] The following are the testing methods used in the implementation of the embodiments and comparative examples of this invention:

[0144] (1) Transmission electron microscopy and particle size determination of copper-based catalysts: Transmission electron microscopy images were determined using a transmission electron microscope (JEM2100F). The specific determination method is as follows: The copper-based catalyst sample prepared in Example 1 was placed in an agate mortar and ground thoroughly into a fine powder. The ground powder was added to anhydrous ethanol and ultrasonically treated for 20 minutes to fully disperse the sample and form a stable suspension. One drop of the above suspension was pipetted onto a copper mesh covered with a carbon film and placed in a dust-free and ventilated environment until the anhydrous ethanol evaporated completely. The mesh was then placed on the transmission electron microscope sample stage for testing. The test acceleration voltage was set to 200kV. Multiple fields of view were randomly selected in different areas of the sample, and clear and non-overlapping transmission electron microscopy images were taken to observe the microstructure, dispersion state, and particle size distribution of the copper-based catalyst prepared in Example 1. Figure 3 As shown.

[0145] (2) Determination of X-ray diffraction (XRD) of copper-based catalyst: The X-ray diffraction pattern was determined using an X-ray diffractometer (RigakuSmartLab). The specific determination method is as follows: The copper-based catalyst sample prepared in Example 1 was placed in an agate mortar and ground thoroughly until it became a uniform fine powder with a particle size of less than 200 mesh. The ground powder was spread evenly in the groove of the sample stage and gently pressed flat with a glass slide to make the sample surface flush with the sample stage surface. The sample stage was then placed in the sample chamber of the diffractometer for testing. The test used a Cu target Kα radiation source (λ=0.15406nm), with the tube voltage set to 40kV, the tube current set to 40mA, the scanning range to 10°~80°, the scanning step size to 0.02°, and the scanning speed to 5° / min. Data was collected using continuous scanning mode. Finally, the X-ray diffraction pattern of the copper-based catalyst prepared in Example 1 was obtained, as shown below. Figure 1 As shown.

[0146] (3) Determination of X-ray photoelectron spectroscopy of copper-based catalysts: X-ray photoelectron spectroscopy was performed using an X-ray photoelectron spectrometer (KratosAxisUltraDLD). The specific determination method is as follows: The copper-based catalyst sample prepared in Example 1 was placed in an agate mortar and ground thoroughly into a uniform fine powder. The powder was then evenly adhered to the surface of the conductive adhesive. Loose powder that was not firmly adhered was gently blown away with a rubber bulb. The sample was then placed in the sample chamber of the spectrometer and heated under a vacuum degree better than 1×10^ -7 The test was conducted under the condition of Pa; an AlKα monochromatic excitation source (hν = 1486.6 eV) was used, and the binding energy was calibrated using the C1s binding energy of contaminated carbon (284.8 eV) as an internal standard. The full spectrum scanning range was 0–1200 eV with a step size of 1.0 eV, and the high-resolution spectral scanning step size was 0.05 eV. The acquired data were processed using XPSPeak software for peak fitting, and the X-ray photoelectron spectrum of the copper-based catalyst prepared in Example 1 was finally obtained, as shown below. Figure 2 As shown.

[0147] (4) Quantitative analysis by gas chromatography: The liquid phase sample obtained in the preparation process of 1,4-cyclohexanediethanol was filtered through an organic filter membrane and injected into a gas chromatograph (Agilent 8860). It was separated by a capillary column (HP-5) with hydrogen as the carrier gas and equipped with a flame ionization detector (FID). The conversion rate of 1,4-cyclohexanedicarboxylate, the selectivity and yield of 1,4-cyclohexanediethanol were calculated by the external standard method to achieve accurate quantification of the product components.

[0148] Table 1

[0149]

[0150] The results of Examples 1-3 in Table 1 show that when the Cu loading is too low, it affects the adsorption and dissociation of hydrogen by the catalyst, leading to a decrease in the DMCD conversion rate. Conversely, a higher Cu loading results in larger Cu particles and poorer dispersion, which also weakens the adsorption and dissociation capacity for hydrogen. An appropriate Cu loading (Example 1) achieves the highest DMCD conversion rate and CHDM selectivity, with a CHDM trans proportion exceeding 80%, indicating that Cu is more uniformly dispersed in this system and that the catalyst contains more Cu. + The presence of alkaline sites allows for the formation of a richer Cu-metal oxide interface. The results of Examples 4 and 5 further demonstrate that the nitrogen-doped carbon-modified copper-based catalyst synthesized from nitrate exhibits the highest activity. Examples 6 and 7 further indicate that excessively low or high nitrogen-carbon doping levels can affect the yield of the target product, CHDM. Combined with the results of Example 1, the highest CHDM yield was achieved when the mixing ratio of copper-based composite metal oxide to melamine was 1:0.5.

[0151] The results of Comparative Example 1 show that the nitrogen-doped carbon-modified copper-based catalyst has higher activity than the unmodified catalyst. This is because the introduction of nitrogen-carbon materials enhances the Lewis base sites on the catalyst surface and effectively promotes the surface Cu... + Speciation promotes the hydrogenation of DMCD. The results of Comparative Examples 2 and 3 indicate that, compared to the copper-based catalysts with Mg and Fe added in the co-precipitation double titration, the copper dispersion is less uniform, the interaction between the metal support is weaker, and fewer Cu-metal oxide interfaces are formed, resulting in a lower concentration of Cu in the catalyst. + The low content of basic sites resulted in both low DMCD conversion rate and low CHDM selectivity.

[0152] The copper-based catalysts prepared in Examples 1 to 7 have similar X-ray diffraction patterns, X-ray photoelectron spectra, transmission electron microscope images, and hydrogenation reaction performance evaluation curves. Example 1 is used as an example for illustration.

[0153] like Figure 1 As shown, Figure 1The X-ray diffraction patterns of the copper-based catalyst provided in Example 1 before and after calcination are shown. The copper-based ternary layered double hydroxide precursor (CuMgFe-LDH) sample before calcination showed characteristic diffraction peaks (JCPDS37-0630) corresponding to the (003), (006), (012), (015), (018), (100), and (113) crystal planes of hydrotalcite, indicating that the synthesized precursor has a high hydrotalcite crystal structure. After doping with nitrogen-containing carbon materials and calcination reduction, the characteristic diffraction peaks of hydrotalcite in the copper-based catalyst sample (NC-CuMgFe) disappeared, and characteristic diffraction peaks of metallic Cu and MgO appeared. No characteristic diffraction peaks of the Fe2O3 phase appeared, indicating that Fe2O3 exists in an amorphous form. The average size of the copper nanoparticles was calculated to be 8.2 nm using the Scherrer equation. This is because the introduction of melamine can inhibit the growth of copper nanoparticles, thereby preventing the aggregation of copper nanoparticles during the reduction process.

[0154] like Figure 2 As shown, Figure 2 The X-ray photoelectron spectrum of the copper-based catalyst provided in Example 1 is shown. The two peaks obtained by fitting are located at 915.8 eV and 918.2 eV, corresponding to Cu... + and Cu 0 Species, Cu + / (Cu + +Cu 0 The ratio of 0.44 indicates a strong metal-support interaction in the copper-based catalyst. + Cu at the interface + -OM (M=Mg / Fe) or Cu + -Exists in NC form.

[0155] Figure 3 Transmission electron microscopy image of the copper-based catalyst provided in Example 1. Figure 3 As shown, copper nanoparticles are uniformly dispersed on a metal oxide carrier, with uniform particle size and an average particle size of 5 nm to 8 nm.

[0156] Figure 4 The DMCD hydrogenation reaction performance evaluation curve of the copper-based catalyst provided in Example 1 is shown below. Figure 4 The results show that the catalyst prepared by this invention has small copper particle size and strong interaction with the metal support, exhibiting excellent catalytic performance and outstanding stability during a reaction lasting up to 2000 hours. At the same time, the catalyst preparation method of this invention is quick and simple, with low energy consumption, and does not use organic solvents or toxic metal Cr during the preparation process, making it more environmentally friendly and suitable for industrial production.

[0157] Taking the copper-based catalyst prepared in Example 1 as an example, the conversion rate of the copper-based catalyst to dimethyl 1,4-cyclohexanedimethyl ester was verified by controlling different reaction conditions during the preparation of 1,4-cyclohexanedimethyl methanol.

[0158] (1) Different temperatures for controlling the hydrogenation reaction: Copper-based catalyst was loaded into a fixed-bed reactor with an inner diameter of 20 mm. 20 g of copper-based catalyst was loaded, and inert magnetic rings were installed at the upper and lower ends of the catalyst bed to ensure uniform distribution of the reaction gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) was added at a rate of 0.4 h. -1 The H2 was transported to the reaction apparatus at a space velocity and thoroughly mixed with H2 before being introduced into the catalyst bed. The molar ratio of H2 to DMCD was 160:1. The hydrogenation reaction was carried out at 210℃~250℃ and a reaction pressure of 2.5MPa, with the pipeline kept at a constant temperature. The reaction products were collected after condensation and quantitatively analyzed by gas chromatography. The results are shown in Table 2. The byproducts in the preparation process are as follows: 4-methylcyclohexane methanol (MCHM); methyl 4-methylcyclohexane carboxylate (MMCHC); 4-methoxymethylcyclohexane methanol (MOMCM); methyl 4-hydroxymethylcyclohexane carboxylate (HMCHC); and methyl 4-(hydroxymethyl)cyclohexanecarboxylate-[4-hydroxymethylcyclohexyl]methyl ester (HMCME).

[0159] Table 2. Catalytic effects of the copper-based catalyst in Example 1 at different hydrogenation reaction temperatures.

[0160]

[0161] Table 2 shows that at a reaction pressure of 2.5 MPa and a DMCD space velocity of 0.4 h⁻¹, -1 Under a hydrogen-to-oil ratio of 160:1, the selectivity of the over-hydrogenation product MCHM and the etherification product MOMCM gradually increased with increasing temperature, while the selectivity of the intermediate hydrogenation products HMCHC and HMCME gradually decreased. This indicates that excessively high reaction temperatures can lead to over-hydrogenation and side reactions, while excessively low reaction temperatures can result in incomplete hydrogenation of the intermediate products. These results demonstrate that the copper-based catalyst prepared in this invention exhibits excellent catalytic activity over a wide temperature range of 210℃ to 250℃.

[0162] (2) Different space velocities for DMCD: Copper-based catalyst was loaded into a fixed-bed reactor with an inner diameter of 20 mm. 20 g of copper-based catalyst was loaded, and inert magnetic rings were installed at the upper and lower ends of the catalyst bed to ensure uniform distribution of the reaction gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) was added at a space velocity of 0.3 h⁻¹. -1 ~0.7h -1The H2 was transported to the reaction device at a space velocity and thoroughly mixed with H2 before being introduced into the catalyst bed. The molar ratio of H2 to DMCD was 160:1. The hydrogenation reaction was carried out at 225℃ and a reaction pressure of 2.5MPa. The pipeline was kept at a constant temperature throughout. The reaction products were collected as liquid components after condensation and quantitatively analyzed by gas chromatography. The results are shown in Table 3.

[0163] Table 3. Catalytic effect of copper-based catalyst in Example 1 at different DMCD space velocities.

[0164]

[0165] Table 3 shows that under the conditions of 225℃, 2.5MPa, and a hydrogen-to-oil ratio of 160:1, the effect of space velocity increasing from 0.3h... -1 Rise to 0.7h -1 The DMCD conversion rate gradually decreased, while the CHDM selectivity first increased and then decreased, at 0.4h. -1 The peak value reached 98.6%. The copper-based catalyst prepared in this invention was tested at a DMCD space velocity of 0.4 h⁻¹. -1 It exhibits excellent catalytic performance, balancing high feed conversion rate, target product selectivity, and production capacity per unit catalyst, making it suitable for continuous industrial production.

[0166] (3) Different pressures for controlling the hydrogenation reaction: Copper-based catalysts are loaded into a fixed-bed reactor with an inner diameter of 20 mm and 20 g of copper-based catalyst. Inert magnetic rings are installed at the upper and lower ends of the catalyst bed to ensure uniform distribution of the reaction gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) is added at a pressure of 0.4 h. -1 The H2 was transported to the reaction device at a space velocity and thoroughly mixed with H2 before being introduced into the catalyst bed. The molar ratio of H2 to DMCD was 160:1. The hydrogenation reaction was carried out at 225℃ and a reaction pressure of 1MPa~3MPa. The pipeline was kept warm throughout. The reaction products were collected as liquid components after condensation and quantitatively analyzed by gas chromatography. The results are shown in Table 4.

[0167] Table 4. Catalytic effects of the copper-based catalyst in Example 1 under different hydrogenation reaction pressures.

[0168]

[0169] Table 4 shows that as the reaction pressure increases, the selectivity of the intermediate hydrogenation products HMCHC and HMCME gradually decreases, while the selectivity of the over-hydrogenation product MCHM slightly increases. When the reaction pressure exceeds 2.5 MPa, the improvement in DMCD conversion and CHDM selectivity significantly decreases. These results indicate that the copper-based catalyst prepared in this invention can achieve high catalytic performance at relatively low reaction pressures, effectively reducing equipment investment and operating costs for industrial production.

[0170] (4) Different hydrogen-to-oil ratios for controlling the hydrogenation reaction: A copper-based catalyst is loaded into a fixed-bed reactor with an inner diameter of 20 mm. 20 g of copper-based catalyst is loaded, and inert magnetic rings are installed at the upper and lower ends of the catalyst bed to ensure uniform distribution of the reaction gas and support the catalyst bed. Dimethyl 1,4-cyclohexanedicarboxylate (DMCD) is added at a rate of 0.4 h⁻¹. -1 The H2 was transported to the reaction device at a space velocity and thoroughly mixed with H2 before being introduced into the catalyst bed. The molar ratio of H2 to DMCD was 120~200:1. The hydrogenation reaction was carried out at 225℃ and 2.5MPa. The pipeline was kept warm throughout. The reaction products were collected after condensation and quantitative analysis was performed by gas chromatography. The results are shown in Table 5.

[0171] Table 5. Catalytic effect of copper-based catalyst in Example 1 at different hydrogen-to-oil ratios in hydrogenation reactions.

[0172]

[0173] Table 5 shows that the reaction temperature was 225℃, the reaction pressure was 2.5MPa, and the DMCD space velocity was 0.4h. -1 Under the specified conditions, as the hydrogen-to-oil ratio increased from 120:1 to 200:1, the conversion rate of DMCD first increased from 98.0% to 99.8% and then gradually decreased to 98.9%, while the selectivity of CHDM first increased from 98.1% to 98.6% and then gradually decreased to 98.2%, achieving the best catalytic effect at a hydrogen-to-oil ratio of 160:1. When the hydrogen-to-oil ratio was below 160:1, the amount of hydrogen was insufficient to meet the hydrogenation requirements of the feedstock and intermediate products, leading to an increase in the selectivity of intermediate products HMCHC and HMCME. When the hydrogen-to-oil ratio was above 160:1, excess hydrogen reduced the residence time of the reactants, preventing the intermediate products from being converted in time, and also increased the energy consumption of hydrogen recycling. The above results indicate that the copper-based catalyst prepared in this invention has stable catalytic performance and good operational flexibility over a wide range of hydrogen-to-oil ratios.

[0174] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A copper-based catalyst, characterized in that, The system includes a substrate and a nitrogen-doped porous carbon coating layer covering at least a portion of the surface of the substrate. The substrate includes a composite support and an active component loaded on the composite support. The composite support comprises a composite metal oxide containing divalent magnesium and trivalent iron. The active component comprises copper nanoparticles, wherein the copper nanoparticles include Cu. 0 and Cu + .

2. The copper-based catalyst according to claim 1, characterized in that, The average particle size of the copper nanoparticles is 5 nm to 8 nm.

3. The copper-based catalyst according to claim 1 or 2, characterized in that, Based on the total mass of the copper-based catalyst, the mass percentage of copper in the copper nanoparticles is 14% to 37%.

4. The copper-based catalyst according to claim 1, characterized in that, Based on the total mass of the copper-based catalyst, the mass percentage of nitrogen in the nitrogen-doped porous carbon coating layer is 2% to 5%.

5. The copper-based catalyst according to claim 1 or 4, characterized in that, Based on the total mass of the copper-based catalyst, the mass percentage of carbon in the nitrogen-doped porous carbon coating layer is 5% to 10%.

6. A method for preparing a copper-based catalyst according to any one of claims 1 to 5, characterized in that, Includes the following steps: A mixed solution of metal salts containing copper, magnesium, and iron salts is mixed with a mixed alkaline solution to obtain a mixed suspension; the mixed suspension is then subjected to crystallization treatment to obtain a copper-based ternary layered double hydroxide precursor. The copper-based ternary layered double hydroxide precursor was mixed with a nitrogen-containing carbon material and calcined in an inert atmosphere to obtain a copper-based catalyst precursor. The copper-based catalyst precursor was reduced under a hydrogen atmosphere to obtain the copper-based catalyst.

7. The method for preparing the copper-based catalyst according to claim 6, characterized in that, The copper salt includes one or more of copper nitrate, copper acetate, and copper chloride; And / or, the magnesium salt includes one or more of magnesium nitrate, magnesium acetate, and magnesium chloride; And / or, the iron salt includes one or more of ferric nitrate, ferric acetate, and ferric chloride.

8. The method for preparing the copper-based catalyst according to claim 6 or 7, characterized in that, In the metal salt mixed solution, Cu 2+ The concentration is 0.05 mol / L~0.15 mol / L, Mg 2+ The concentration is 0.05 mol / L~0.75 mol / L, Fe 3+ The concentration is 0.03 mol / L to 0.3 mol / L; And / or, in the metal salt mixed solution, the Cu 2+ With the Mg 2+ The molar ratio is (0.2~1):1; And / or, the Cu 2+ With the Mg 2+ The total number of moles and the Fe 3+ The molar ratio is (2~4):

1.

9. The method for preparing the copper-based catalyst according to claim 6, characterized in that, The mixed alkaline solution includes sodium hydroxide solution and sodium carbonate solution; And / or, the crystallization treatment is performed at a temperature of 30°C to 60°C for a time of 6 hours to 24 hours; And / or, the nitrogen-containing carbon material includes one or more of melamine, cyanamide, polyaniline, polypyrrole, and urea; And / or, the mass ratio of the copper-based ternary layered double hydroxide precursor to the nitrogen-containing carbon material is 1:(0.1~2). And / or, the calcination treatment is carried out at a temperature of 350℃~550℃ for a time of 3h~6h; And / or, the reduction treatment is performed at a temperature of 250℃~350℃ for a time of 1h~4h.

10. A method for preparing 1,4-cyclohexanediethanol, characterized in that, Includes the following steps: Dimethyl 1,4-cyclohexanedicarboxylate is hydrogenated in the presence of a catalyst to obtain 1,4-cyclohexanediethanol; wherein the catalyst comprises a copper-based catalyst according to any one of claims 1 to 5, or a copper-based catalyst prepared according to the method for preparing a copper-based catalyst according to any one of claims 6 to 9.

Citation Information

Patent Citations

  • Catalyst for preparing 1,4-cyclohexanedimethanol

    CN104888789A