Oxygen reduction reaction catalyst with surface negative field and preparation method and application thereof
By constructing a pyridine nitrogen-induced local negative electric field and a one-dimensional beaded hierarchical porous structure on the catalyst surface, the problem of insufficient activity and stability of non-precious metal oxygen reduction reaction catalysts in seawater systems due to chloride ion poisoning was solved, achieving simultaneous improvement in catalytic activity and chloride resistance.
Patent Information
- Application Number
- CN202611342433.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-24
AI Technical Summary
Existing non-precious metal oxygen reduction catalysts suffer from insufficient catalytic activity and stability in seawater systems due to chloride ion poisoning. Current strategies cannot effectively suppress chloride ion adsorption without sacrificing catalytic activity.
A localized negative electric field induced by pyridine nitrogen is constructed on the catalyst surface to suppress chloride ion adsorption using electrostatic repulsion. This, combined with a one-dimensional beaded structure and a hierarchical porous structure, ensures the accessibility of Fe-N₄ active sites and catalytic activity.
It significantly improves the catalyst's resistance to chlorine poisoning and long-term operational stability in seawater systems, while maintaining catalytic activity, thus solving the technical problem that traditional strategies cannot achieve both by sacrificing mass transfer or stability.
Smart Images

Figure CN123148977A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials synthesis technology, specifically relating to an oxygen reduction reaction catalyst with a negative surface electric field, its preparation method, and its application. Background Technology
[0002] The oxygen reduction reaction (ORR) is the core cathode reaction in electrochemical energy conversion devices such as fuel cells and metal-air batteries. Its reaction kinetics directly determine the energy conversion efficiency and output power level of the device. Seawater metal-air batteries use lightweight metals such as zinc, magnesium, and aluminum as anodes and air electrodes loaded with ORR catalysts as cathodes, and can use seawater as the electrolyte. They represent a new type of electrochemical energy storage device with great development potential. These batteries, relying on lightweight metal anodes, possess advantages such as high theoretical energy density and a wide range of raw material sources. Benefiting from their system advantages of high adaptability to marine conditions, these batteries can be widely used in special marine energy scenarios such as marine observation buoys, off-grid power supply for islands, small underwater vehicles, offshore emergency energy storage, and marine exploration equipment, possessing extremely high practical value and broad industrialization prospects.
[0003] Currently, the mainstream commercial oxygen reduction reaction catalysts are platinum-based noble metal catalysts (such as Pt / C). These catalysts have excellent ORR catalytic activity, but they have inherent defects such as scarce crustal reserves, high preparation costs, and extremely high cost barriers for large-scale application. These defects greatly limit the commercialization and large-scale promotion of seawater metal-air batteries and cannot meet the application requirements of low cost and large volume of marine energy storage devices.
[0004] To overcome the aforementioned drawbacks, non-precious metal catalysts have become a research focus. Among them, iron-based single-atom catalysts (Fe-NC) are considered the most promising alternative due to their well-defined Fe-N4 active centers, high atom utilization, and low cost. However, when Fe-NC catalysts are applied to seawater systems, Cl... - Chloride ions strongly adsorb onto the Fe-N4 active sites, competing with oxygen molecules for adsorption and thus clogging the active sites, leading to a decrease in catalytic activity. Therefore, chloride ion poisoning has become the core bottleneck restricting the stable operation of Fe-NC catalysts in seawater systems.
[0005] Regarding Cl - To address the poisoning problem, researchers have attempted strategies such as physical barrier coating, hydrophobic interface construction, and heteroatom doping. While physical barrier coating can block Cl... - Direct contact with the active site hinders oxygen diffusion and mass transfer, leading to a significant decrease in catalytic activity; while hydrophobic interface construction can utilize the hydrophobic effect to repel Cl... -However, the introduced hydrophobic functional groups or coatings lack stability in electrochemical environments, making them prone to peeling or detachment, thus compromising their resistance to Cl. - Performance decays rapidly; although heteroatom doping can adjust the charge density of Fe-N4 sites to reduce their influence on Cl... - While the adsorption affinity of Cl is strong, the actual controllability is limited by the distance between the doping sites and the active center, as well as the uniformity of doping, making it difficult to effectively suppress Cl. - Therefore, none of the above strategies can effectively inhibit Cl adsorption without sacrificing catalytic activity. - Adsorption.
[0006] To address the above problems, this invention is proposed. Summary of the Invention
[0007] To address the shortcomings of existing non-precious metal oxygen reduction catalysts in seawater systems, which suffer from insufficient catalytic activity and stability due to chloride ion poisoning, this invention provides an oxygen reduction catalyst with a negative surface electric field, its preparation method, and its applications. This invention utilizes the electrostatic repulsion effect to suppress the adsorption of chloride ions from seawater on the Fe-N4 active sites by constructing a localized negative electric field induced by pyridine nitrogen on the catalyst surface, thereby significantly improving the catalyst's stability and durability in seawater systems without sacrificing catalytic activity.
[0008] The present invention solves the technical problem by adopting the following technical solution:
[0009] The first aspect of the present invention provides an oxygen reduction reaction catalyst with a negative surface electric field, wherein the catalyst is a one-dimensional beaded structure composed of a carbon nanofiber skeleton connected in series with hollow carbon beads;
[0010] The hollow carbon beads have a carbon shell, and atomically dispersed Fe-N4 active sites are anchored within the carbon shell framework.
[0011] The carbon shell edge surface is enriched with pyridine nitrogen doping sites, and the pyridine nitrogen doping creates a local negative electric field on the carbon shell surface, which can suppress the adsorption of chloride ions on the Fe-N4 active site surface.
[0012] Preferably, the hollow carbon beads have a hierarchical porous structure, including micropores and mesopores.
[0013] A second aspect of this invention provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field, used to prepare the catalyst described in the first aspect, comprising the following steps:
[0014] (1) By introducing zinc source and iron source into the ZIF-8 synthesis system, Fe-doped ZIF-8 material was prepared, which was denoted as core Fe-ZIF-8 material;
[0015] (2) Using the core Fe-ZIF-8 material as the core and the nitrogen-containing polymer with the function of constructing a negative electric field on the surface as the shell, the electrospinning method is used to make the polymer shell simultaneously wrap and connect each Fe-ZIF-8 core, forming a precursor material with a one-dimensional beaded structure of Fe-ZIF-8 beads connected by a polymer fiber skeleton.
[0016] (3) The precursor material is subjected to high-temperature pyrolysis to carbonize the polymer to form a carbon nanofiber skeleton. The Fe-ZIF-8 beads are thermally collapsed to form hollow carbon beads. At the same time, Fe atoms are anchored in situ in the carbon skeleton to form Fe-N4 active sites. Nitrogen atoms in the polymer form pyridine nitrogen doping on the surface of the carbon shell edge. Finally, a one-dimensional hollow bead structure FeNCNFs oxygen reduction reaction catalyst with a negative surface electric field is obtained.
[0017] The hollow carbon beads have a hierarchical porous structure formed on their carbon shells, consisting of micropores and mesopores derived from ZIF-8 pyrolysis. The micropores provide anchoring sites for Fe-N4 active sites, while the mesopores provide rapid channels for material diffusion.
[0018] Preferably, the preparation process of the core Fe-ZIF-8 material in step (1) is as follows: zinc nitrate hexahydrate and iron acetylacetonate are dissolved together in methanol solvent and stirred evenly to obtain solution A;
[0019] Dimethylimidazole was dissolved in methanol to obtain solution B;
[0020] Solution B was slowly poured into solution A and stirred to react. After the reaction was completed, the precipitate was collected by centrifugation, washed repeatedly by centrifugation with methanol, and dried under vacuum overnight to obtain the Fe-ZIF-8 core material.
[0021] Preferably, in step (1), the zinc source is zinc nitrate hexahydrate, and the iron source is iron acetylacetonate; the mass ratio of zinc nitrate hexahydrate to iron acetylacetonate is 1.25:1 to 5:1, and the mass ratio of zinc nitrate hexahydrate to dimethylimidazole is 1:2 to 1:2.5; zinc nitrate hexahydrate and iron acetylacetonate are dissolved in methanol, dimethylimidazole is dissolved in methanol, and then the methanol solution of dimethylimidazole is slowly poured into the methanol solution of zinc nitrate hexahydrate and iron acetylacetonate, and the reaction is stirred at room temperature for 2 to 4 hours; after the reaction is completed, the precipitate is collected by centrifugation at 8000 to 12000 rpm, washed with methanol 2 to 4 times, and vacuum dried overnight to obtain the core Fe-ZIF-8 material.
[0022] Preferably, in step (2), the nitrogen-containing polymer is at least one of PAN, PVP, and PI; the electrospinning process parameters are: injection speed 0.08~0.12 mm / min, injector positive voltage 10~11kV, receiver negative voltage -2~-2.5kV; and the mass ratio of the core Fe-ZIF-8 material to the nitrogen-containing polymer is 1:1~1:1.4.
[0023] Preferably, the preparation process of the precursor material in step (2) is as follows: the core Fe-ZIF-8 material is dispersed in N,N-dimethylformamide solvent and ultrasonically dispersed evenly, then a nitrogen-containing polymer is added and stirred continuously overnight, followed by electrospinning, collecting the spun product and drying overnight to obtain the precursor material.
[0024] Preferably, in step (3), the high-temperature pyrolysis temperature is 950~1050 ℃, and the pyrolysis holding time is 1~2 h.
[0025] The third aspect of the present invention provides an application of an oxygen reduction reaction catalyst having a surface negative electric field, wherein the catalyst described in the first aspect or the catalyst prepared by the preparation method described in the second aspect is used as an air cathode oxygen reduction reaction catalyst in a seawater metal-air battery.
[0026] Preferably, the electrolyte of the seawater metal-air battery is alkaline seawater obtained by adding potassium hydroxide to natural seawater to precipitate calcium and magnesium ions and then filtering and precipitating the precipitate.
[0027] The present invention has the following beneficial effects:
[0028] 1. This invention constructs a stable local negative electric field by enriching pyridine nitrogen doping sites on the surface of a hollow carbon bead carbon shell. The principle is as follows: Pyridine nitrogen is a specific edge nitrogen configuration in nitrogen-doped carbon materials. The nitrogen atom is located at the edge of a six-membered ring and bonds with two carbon atoms, while retaining a pair of unbonded lone pairs of electrons. Because the electronegativity of nitrogen atoms is significantly higher than that of carbon atoms, after pyridine nitrogen is embedded in the carbon framework, the shared electron pair of the carbon-nitrogen bond shifts towards the nitrogen atom, significantly increasing the π electron cloud density around the pyridine nitrogen site. This forms a stable negative charge enrichment region on the carbon shell surface, i.e., the local negative electric field of this invention. Based on the physical mechanism of like charges repelling each other, this local negative electric field can significantly electrostatically repel negatively charged chloride ions in seawater, fundamentally preventing chloride ions from approaching and competing for adsorption at the Fe-N4 active sites. This effectively solves the problems of active site blockage and catalytic performance degradation caused by chloride ion poisoning in traditional Fe-NC single-atom catalysts in seawater systems, significantly improving the catalyst's resistance to chloride poisoning and long-term operational stability under seawater conditions.
[0029] 2. The one-dimensional hollow hierarchical porous synergistic structure constructed in this invention features a one-dimensional carbon fiber skeleton that runs through the entire catalyst, creating a long-range continuous electronic conduction pathway. This effectively reduces charge transfer resistance and accelerates electron transport during the reaction process. The internal cavity of the hollow carbon beads is interconnected with the micropores and mesopores on the shell wall, forming a multi-level material diffusion network. Specifically, the mesopores serve as rapid diffusion channels for oxygen and electrolyte, while the micropores act as sites for reactant enrichment and Fe-N4 active site anchoring. The synergy between the micropores and mesopores significantly reduces diffusion mass transfer resistance.
[0030] Meanwhile, pyridine nitrogen exists as lattice doping at the edge of the carbon shell, belonging to the inherent chemical composition of the carbon framework, rather than an external physical coating or hydrophobic coating. Therefore, it does not cover or block the Fe-N4 active sites or pore structure. More importantly, the lattice doping characteristics of pyridine nitrogen create a functional complementarity with the one-dimensional hollow bead structure: the carbon nanofiber framework ensures a continuous supply of electrons to the negative electric field, the hierarchical porous structure ensures high accessibility of the Fe-N4 active sites, and the negative electric field of pyridine nitrogen plays a role in electrostatically repelling Cl... - While exerting its effect, it does not add any additional diffusion resistance. Thanks to this, the present invention achieves excellent chlorine resistance while retaining the accessibility and catalytic activity of the Fe-N4 active sites, realizing a bidirectional simultaneous improvement in catalytic activity and chlorine resistance stability. This overcomes the technical problem in the prior art where strategies such as physical barrier coating and hydrophobic interface construction cannot achieve both due to the sacrifice of mass transfer or stability.
[0031] 3. This invention uses Fe-doped ZIF-8 as a precursor. Utilizing the unique microporous structure of ZIF-8 to spatially bind the metal precursor, Fe atoms are anchored in situ within the carbon framework during high-temperature pyrolysis, effectively suppressing Fe atom migration and aggregation, and ensuring the atomic-level dispersion of Fe-N4 active sites. Simultaneously, this invention employs electrospinning technology, using a nitrogen-containing polymer as the shell and Fe-ZIF-8 as the core, to obtain a one-dimensional beaded precursor consisting of a polymer fiber framework linked with Fe-ZIF-8 beads in a single spinning step. During subsequent high-temperature pyrolysis, taking advantage of the difference in thermal shrinkage rates between the polymer and ZIF-8 crystals, the precursor spontaneously evolves into a one-dimensional hollow beaded structure (the polymer shell carbonizes to form a carbon nanofiber framework). During high-temperature pyrolysis, the core of the Fe-ZIF-8 beads decomposes and shrinks, while the outer shell carbonizes and solidifies, thus forming hollow carbon beads. The entire preparation process requires no template removal or post-processing modification, has a simple process route, and is feasible for large-scale scaling. It can meet the industrialization needs of seawater metal-air batteries for the mass production and low-cost preparation of cathode catalysts. Attached Figure Description
[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0033] Figure 1 This is a flowchart illustrating the synthesis of the one-dimensional hollow beaded FeNCNFs catalyst with a negative surface electric field according to the present invention.
[0034] Figure 2 The image shows the X-ray diffraction (XRD) pattern of the one-dimensional hollow beaded FeNCNFs catalyst synthesized in Example 1 of this invention.
[0035] Figure 3 This is a transmission electron microscope (TEM) image of the one-dimensional hollow beaded FeNCNFs catalyst synthesized in Example 1 of the present invention;
[0036] Figure 4 This is an aberration-corrected transmission electron microscope (AC-TEM) image of the one-dimensional hollow beaded FeNCNFs catalyst synthesized in Example 1 of the present invention.
[0037] Figure 5 This is a comparison chart of the oxygen reduction reaction catalytic performance of the one-dimensional hollow beaded FeNCNFs catalyst synthesized in Example 1 of the present invention, the FeNC catalyst in Comparative Example 1, and the commercial Pt / C catalyst. Detailed Implementation
[0038] The present invention will be further described below through embodiments, but is not limited to these embodiments. Experimental methods not specifically described in the embodiments generally use conventional conditions and conditions described in manuals, or conditions recommended by the manufacturer. The general equipment, materials, reagents, etc., used are all commercially available unless otherwise specified.
[0039] Example 1
[0040] This embodiment provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field.
[0041] (1) Preparation of core Fe-ZIF-8 material:
[0042] 0.5 g of zinc nitrate hexahydrate and 0.2 g of ferric acetylacetone were dissolved together in 50 mL of methanol and stirred for 30 min, denoted as solution A. 1 g of dimethylimidazole was dissolved in 50 mL of methanol, denoted as solution B. Solution B was then slowly poured into solution A, and the reaction was carried out with slow stirring at room temperature for 3 h. After the reaction was complete, the precipitate was collected by centrifugation at 9000 rpm, washed three times with methanol, and the resulting product was dried overnight under vacuum to obtain a pale yellow solid, which was the core Fe-ZIF-8 material.
[0043] (2) Preparation of precursor materials:
[0044] 500 mg of the core Fe-ZIF-8 material obtained in step (1) was dispersed in 6 mL of N,N-dimethylformamide (DMF) and ultrasonically dispersed for 30 min until homogeneous. Then, 600 mg of polyacrylonitrile (PAN) was added, and stirring continued overnight to obtain a homogeneous spinning slurry. The spinning slurry was electrospun with the following parameters: injection speed 0.1 mm / min, injector positive voltage 10.2 kV, and receiver negative voltage -2.06 kV. The spun product was collected and dried overnight in a vacuum drying oven to obtain the precursor material (denoted as Fe-ZIF-8@PAN in this example). This precursor material exhibits a one-dimensional beaded structure consisting of a PAN fiber skeleton connected to Fe-ZIF-8 beads.
[0045] (3) High-temperature pyrolysis carbonization:
[0046] The precursor material obtained in step (2) was placed in a tube furnace and heated to 1000°C at a heating rate of 5°C / min under the protection of argon (Ar) atmosphere. It was then kept at the temperature for 2 h for pyrolysis and then naturally cooled to room temperature to obtain a one-dimensional hollow beaded FeNCNFs oxygen reduction reaction catalyst with a negative surface electric field.
[0047] Example 2
[0048] This embodiment provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field. The difference from Example 1 is that in step (2), polyacrylonitrile (PAN) is replaced with an equal mass of polyvinylpyrrolidone (PVP).
[0049] (1) Preparation of core Fe-ZIF-8 material:
[0050] The steps are exactly the same as those in Example 1 (1).
[0051] (2) Preparation of precursor materials:
[0052] 500 mg of the core Fe-ZIF-8 material obtained in step (1) was dispersed in 6 mL of N,N-dimethylformamide (DMF) and ultrasonically dispersed for 30 min until homogeneous. Then, 600 mg of polyvinylpyrrolidone (PVP) was added, and stirring was continued overnight to obtain a homogeneous spinning slurry. The spinning slurry was electrospun with the following parameters: injection speed 0.09 mm / min, injector positive voltage 10.1 kV, and receiver negative voltage -2.01 kV. The spun product was collected and dried overnight in a vacuum drying oven to obtain the precursor material (denoted as Fe-ZIF-8@PVP in this example).
[0053] (3) High-temperature pyrolysis carbonization:
[0054] The precursor material obtained in step (2) was placed in a tube furnace and heated to 1000°C at a heating rate of 5°C / min under the protection of argon (Ar) atmosphere. It was then kept at the temperature for 2 h for pyrolysis and then naturally cooled to room temperature to obtain a one-dimensional hollow beaded FeNCNFs oxygen reduction reaction catalyst with a negative surface electric field.
[0055] Example 3
[0056] This embodiment provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field. The difference from Example 1 is that in step (2), polyacrylonitrile (PAN) is replaced with an equal mass of polyimide (PI).
[0057] (1) Preparation of core Fe-ZIF-8 material:
[0058] The steps are exactly the same as those in Example 1 (1).
[0059] (2) Preparation of precursor materials:
[0060] 500 mg of the Fe-ZIF-8 core material obtained in step (1) was dispersed in 6 mL of N,N-dimethylformamide (DMF) and ultrasonically dispersed for 30 min until homogeneous. Then, 600 mg of polyimide (PI) was added, and stirring was continued overnight to obtain a homogeneous spinning slurry. The spinning slurry was electrospun with the following parameters: injection speed 0.11 mm / min, injector positive voltage 10.5 kV, and receiver negative voltage -2.16 kV. The spun product was collected and dried overnight in a vacuum drying oven to obtain the precursor material (denoted as Fe-ZIF-8@PI in this example).
[0061] (3) High-temperature pyrolysis carbonization:
[0062] The precursor material obtained in step (2) was placed in a tube furnace and heated to 1000°C at a heating rate of 5°C / min under the protection of argon (Ar) atmosphere. It was then kept at the temperature for 2 h for pyrolysis and then naturally cooled to room temperature to obtain a one-dimensional hollow beaded FeNCNFs oxygen reduction reaction catalyst with a negative surface electric field.
[0063] Example 4
[0064] This embodiment provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field. The difference from Example 1 is that in step (1), the mass ratio of zinc nitrate hexahydrate to iron acetylacetone is 2.5:1 (i.e., 0.5 g of zinc nitrate hexahydrate and 0.2 g of iron acetylacetone), and the mass ratio of zinc nitrate hexahydrate to dimethylimidazole is 1:2.3 (i.e., 0.5 g of zinc nitrate hexahydrate and 1.15 g of dimethylimidazole); in step (3), the pyrolysis temperature is 950℃, and the holding time is 2 h. The remaining steps and conditions are the same as in Example 1.
[0065] Example 5
[0066] This embodiment provides a method for preparing an oxygen reduction reaction catalyst with a negative surface electric field. The difference from Example 1 is that in step (1), the mass ratio of zinc nitrate hexahydrate to iron acetylacetone is 5:1 (i.e., 0.5 g of zinc nitrate hexahydrate and 0.1 g of iron acetylacetone), and the mass ratio of zinc nitrate hexahydrate to dimethylimidazole is 1:2.5 (i.e., 0.5 g of zinc nitrate hexahydrate and 1.25 g of dimethylimidazole); in step (3), the pyrolysis temperature is 1050℃, and the holding time is 1 h. The remaining steps and conditions are the same as in Example 1.
[0067] It should be noted that those skilled in the art should understand that the stirring reaction time in step (1) of the above embodiments can be adjusted in the range of 2 to 4 h, the centrifugation speed can be adjusted in the range of 8000 to 12000 rpm, and the number of methanol washing times can be adjusted in the range of 2 to 4 times, all of which can obtain core Fe-ZIF-8 materials and final catalysts with consistent morphology and catalytic performance; the heating rate in step (3) can also be adjusted in the range of 3 to 8 °C / min, all of which do not deviate from the protection scope of the present invention.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing a FeNC catalyst without a surface negative electric field, for comparison with the embodiments of the present invention, to verify the effect of the surface negative electric field of the present invention on improving the catalyst's resistance to chloride ion poisoning in seawater systems.
[0070] 0.5 g of zinc nitrate hexahydrate and 0.2 g of ferric acetylacetone were dissolved together in 50 mL of methanol and stirred for 30 min, denoted as solution A. 1 g of dimethylimidazole was dissolved in 50 mL of methanol, denoted as solution B. Solution B was then slowly poured into solution A, and the reaction was carried out with slow stirring at room temperature for 3 h. After the reaction was completed, the precipitate was collected by centrifugation at 9000 rpm, washed three times with methanol, and the resulting product was dried overnight under vacuum to obtain the Fe-ZIF-8 precursor. The Fe-ZIF-8 precursor was placed in a tube furnace and heated to 1000 °C at a heating rate of 5 °C / min under an argon (Ar) atmosphere, and held at this temperature for 2 h for pyrolysis. It was then naturally cooled to room temperature to obtain the FeNC catalyst.
[0071] Test Example 1
[0072] 1. Catalyst structural characterization
[0073] X-ray diffraction (XRD) analysis was performed on the FeNCNFs catalyst prepared in Example 1, and the results are as follows: Figure 2 As shown, only broad, diffuse diffraction peaks belonging to carbon materials were observed in the XRD pattern. No sharp diffraction peaks belonging to iron metals or iron compounds (such as Fe, Fe3C, Fe2O3, etc.) were observed, indicating that there are no iron-based nanoparticle aggregates in the catalyst prepared in Example 1, and that iron exists in a highly dispersed state in the carbon framework.
[0074] The FeNCNFs catalyst prepared in Example 1 was observed by transmission electron microscopy (TEM), and the results are as follows: Figure 3 As shown in the TEM image, the catalyst exhibits a one-dimensional beaded structure composed of hollow carbon beads connected in a carbon nanofiber framework. The carbon beads show obvious hollow features, and the shell walls are clearly visible, consistent with the structure described in claim 1 of this invention.
[0075] The FeNCNFs catalyst prepared in Example 1 was observed by aberration-corrected transmission electron microscopy (AC-TEM), and the results are as follows: Figure 4 As shown, numerous isolated bright spots can be clearly observed in the AC-TEM image, each corresponding to a single Fe atom. This indicates that Fe is dispersed in the carbon framework in the form of single atoms, without Fe atom clusters or nanoparticles, confirming the atomic-level dispersion of the Fe-N4 active sites.
[0076] 2. Catalyst performance testing
[0077] The catalytic performance of the FeNCNFs catalyst prepared in Example 1, the FeNC catalyst prepared in Comparative Example 1, and the commercial Pt / C catalyst for oxygen reduction reaction was tested using a three-electrode system. The test conditions were as follows: oxygen-saturated alkaline seawater was used as the electrolyte; the working electrode was a glassy carbon electrode with the catalyst supported; the counter electrode was a platinum sheet electrode; and the reference electrode was a Hg / HgO electrode. Linear sweep voltammetry (LSV) was performed at a scan rate of 5 mV / s and an electrode rotation speed of 1600 r / min.
[0078] Test results are as follows Figure 5 As shown in the figure, the FeNC catalyst of Comparative Example 1 exhibits significantly reduced oxygen reduction catalytic activity in the seawater system due to chloride ion poisoning, with both half-wave potential and limiting current density being lower. In contrast, the FeNCNFs catalyst prepared in Example 1 demonstrates excellent oxygen reduction catalytic activity in the seawater system, with both half-wave potential and limiting current density significantly superior to those of the FeNC catalyst of Comparative Example 1 and significantly superior to those of commercial Pt / C catalysts. This indicates that the present invention effectively suppresses the adsorption of chloride ions on the Fe-N4 active sites in seawater by constructing a pyridine nitrogen-induced local negative electric field on the catalyst surface, thereby significantly improving the catalytic performance of the catalyst in the seawater system for oxygen reduction. Meanwhile, the catalysts prepared in Examples 2-5, tested under the same conditions, all exhibited oxygen reduction catalytic activity comparable to that of Example 1.
[0079] The present invention has been described above by way of example. It should be noted that any simple modifications, alterations or other equivalent substitutions that can be made by those skilled in the art without creative effort without departing from the core of the present invention fall within the protection scope of the present invention.
Claims
1. A catalyst for oxygen reduction reaction with a negative surface electric field, characterized in that, The catalyst is a one-dimensional beaded structure composed of hollow carbon beads connected in series with a carbon nanofiber skeleton. The hollow carbon beads have a carbon shell, and atomically dispersed Fe-N4 active sites are anchored within the carbon shell framework. The carbon shell edge surface is enriched with pyridine nitrogen doping sites, and the pyridine nitrogen doping creates a local negative electric field on the carbon shell surface, which can suppress the adsorption of chloride ions on the Fe-N4 active site surface.
2. The oxygen reduction reaction catalyst with a negative surface electric field according to claim 1, characterized in that, The hollow carbon beads have a hierarchical porous structure, including micropores and mesopores.
3. A method for preparing an oxygen reduction reaction catalyst with a negative surface electric field, characterized in that, The preparation of the catalyst according to any one of claims 1 to 2 comprises the following steps: (1) By introducing zinc source and iron source into the ZIF-8 synthesis system, Fe-doped ZIF-8 material was prepared, which was denoted as core Fe-ZIF-8 material; (2) Using the core Fe-ZIF-8 material as the core and the nitrogen-containing polymer with the function of constructing a negative electric field on the surface as the shell, the electrospinning method is used to make the polymer shell simultaneously wrap and connect each Fe-ZIF-8 core, forming a precursor material with a one-dimensional beaded structure of Fe-ZIF-8 beads connected by a polymer fiber skeleton. (3) The precursor material is subjected to high-temperature pyrolysis to carbonize the polymer to form a carbon nanofiber skeleton. The Fe-ZIF-8 beads are thermally collapsed to form hollow carbon beads. At the same time, Fe atoms are anchored in situ in the carbon skeleton to form Fe-N4 active sites. Nitrogen atoms in the polymer form pyridine nitrogen doping on the surface of the carbon shell edge. Finally, a one-dimensional hollow bead structure FeNCNFs oxygen reduction reaction catalyst with a negative surface electric field is obtained.
4. The preparation method according to claim 3, characterized in that, The preparation process of the core Fe-ZIF-8 material in step (1) is as follows: zinc nitrate hexahydrate and iron acetylacetonate are dissolved together in methanol solvent and stirred evenly to obtain solution A; Dimethylimidazole was dissolved in methanol to obtain solution B; Solution B was slowly poured into solution A and stirred to react. After the reaction was completed, the precipitate was collected by centrifugation, washed repeatedly by centrifugation with methanol, and dried under vacuum overnight to obtain the Fe-ZIF-8 core material.
5. The preparation method according to claim 3, characterized in that, In step (1), the zinc source is zinc nitrate hexahydrate, and the iron source is iron acetylacetonate. The mass ratio of zinc nitrate hexahydrate to iron acetylacetonate is 1.25:1 to 5:1, and the mass ratio of zinc nitrate hexahydrate to dimethylimidazole is 1:2 to 1:2.
5. Zinc nitrate hexahydrate and iron acetylacetonate are dissolved in methanol, and dimethylimidazole is dissolved in methanol. The methanol solution of dimethylimidazole is then slowly poured into the methanol solution of zinc nitrate hexahydrate and iron acetylacetonate, and the mixture is stirred at room temperature for 2 to 4 hours. After the reaction is completed, the precipitate is collected by centrifugation at 8000 to 12000 rpm, washed 2 to 4 times with methanol, and vacuum dried overnight to obtain the core Fe-ZIF-8 material.
6. The preparation method according to claim 3, characterized in that, In step (2), the nitrogen-containing polymer is at least one of PAN, PVP, and PI; the electrospinning process parameters are: injection speed 0.08~0.12 mm / min, positive voltage of injector 10~11 kV, negative voltage of receiver -2~-2.5 kV; and the mass ratio of the core Fe-ZIF-8 material to the nitrogen-containing polymer is 1:1~1:1.
4.
7. The preparation method according to claim 6, characterized in that, The preparation process of the precursor material in step (2) is as follows: the core Fe-ZIF-8 material is dispersed in N,N-dimethylformamide solvent and ultrasonically dispersed evenly, then a nitrogen-containing polymer is added and stirred continuously overnight, followed by electrospinning, collecting the spun product and drying overnight to obtain the precursor material.
8. The preparation method according to claim 3, characterized in that, In step (3), the high-temperature pyrolysis temperature is 950~1050 ℃, and the pyrolysis holding time is 1~2 h.
9. The application of an oxygen reduction reaction catalyst with a negative surface electric field, characterized in that, The catalyst described in claim 1 or 2, or the catalyst prepared by the method described in any one of claims 3 to 8, is used as the oxygen reduction reaction catalyst for the air cathode of a seawater metal-air battery.
10. The application according to claim 9, characterized in that, The electrolyte of the seawater metal-air battery is alkaline seawater obtained by adding potassium hydroxide to natural seawater to precipitate calcium and magnesium ions and then filtering and precipitating the precipitate.