Preparation method and application of a bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion
By preparing the Co@ZrO₂-CN catalyst, the problems of insufficient low-temperature activity, tandem reaction adaptability and cycle life of existing catalysts were solved, realizing the efficient conversion of CO₂ into aromatic amines, and improving production efficiency and resource utilization.
Patent Information
- Application Number
- CN202611412363.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-24
AI Technical Summary
Existing catalysts have shortcomings in low-temperature catalytic activity, tandem reaction compatibility, and cycle life, resulting in low production efficiency and lengthy process flow.
Using a Co@ZrO₂-CN catalyst, UiO-66 material was synthesized by reacting zirconium oxychloride, terephthalic acid, and cobalt nitrate with 4,4-bipyridine under specific conditions. The resulting material was then calcined to form a porous octahedral structure, enabling one-step tandem catalysis of CO₂ and nitro aromatic compounds.
It significantly improves the low-temperature catalytic activity and stability of the catalyst, increases the reaction rate and yield, achieves efficient resource utilization, and reduces energy consumption and cost.
Smart Images

Figure CN123148979A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of CO2 utilization and conversion technology, specifically to a method for preparing and applying a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2. Background Technology
[0002] With the continuous development of industry and human activities, the massive consumption of non-renewable fossil fuels has led to the generation of large amounts of CO2, causing serious environmental problems such as global warming and ocean acidification. Carbon neutrality has been widely recognized as an important goal for future sustainable development. Therefore, developing effective CO2 capture and conversion technologies is crucial. As an abundant, readily available, and non-toxic C1 compound, CO2 is increasingly being considered for conversion into useful fuels and high-value-added chemicals to achieve carbon cycling, a field that has received considerable attention in recent years. Among the many reported conversion pathways, the N-formylation reaction of aromatic amines with CO2 to construct new CN bonds is one of the most attractive and promising strategies for CO2 conversion. The resulting formamide is an important intermediate in the synthesis of pharmaceuticals, pesticides, dyes, and fragrances, making this method highly attractive. However, due to the extremely high thermodynamic stability of CO2 molecules, designing efficient catalysts to activate CO2 remains a highly challenging yet attractive research area.
[0003] Current processes commonly use aromatic amines directly as reactants to undergo N-formylation with CO2. However, aromatic amines are chemically unstable, requiring strict temperature and light-protection conditions for storage and transportation. Post-reaction separation and purification are cumbersome, significantly increasing energy consumption and material loss, resulting in poor overall atom economy. Existing traditional composite catalysts used in small-scale nitroaromatic tandem catalytic systems still suffer from several performance drawbacks in practical applications: First, limited catalytic activity; the yield of the target formamide product is low under mild conditions, often requiring high temperature, high pressure, and long reaction times to achieve acceptable conversion levels, leading to low production efficiency. Second, active metal particles are prone to agglomeration, and the support has a simple pore structure, resulting in weak substrate and CO2 adsorption and activation capabilities and slow reaction kinetics. Third, the catalyst exhibits poor cyclic stability; its activity rapidly declines after multiple recycling and reuse, failing to meet the demands of continuous mass production. Fourth, the support lacks synergistic activation sites, making it difficult to simultaneously enhance the two-step tandem reaction of nitro hydrogenation and CO2 activation, preventing one-step conversion of nitroaromatics and necessitating the staged preparation and separation of aromatic amine intermediates, resulting in a lengthy process.
[0004] Therefore, the low-temperature catalytic activity, tandem reaction adaptability, cycle life, and economic efficiency of existing catalysts still need to be improved simultaneously. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing and applying a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2, thereby solving the following technical problems:
[0006] Existing catalysts still suffer from poor synergy in low-temperature catalytic activity, tandem reaction compatibility, and cycle life.
[0007] The objective of this invention can be achieved through the following technical solutions:
[0008] A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 includes the following steps:
[0009] S1: Mix zirconium oxychloride solution and terephthalic acid solution and stir for 25-35 min to obtain mixture A;
[0010] S2: Add acetic acid to mixture A, stir, react at 90-120℃ for 18-26h, centrifuge, wash 3 times with anhydrous ethanol, and dry to obtain UiO-66 material;
[0011] S3: The UiO-66 material was dispersed in a non-aqueous solvent and ultrasonically dispersed. Then, cobalt nitrate and 4,4-bipyridine solution were added and stirred to react. After centrifugation and drying, the mixture was calcined under a nitrogen atmosphere and cooled to obtain a bifunctional Co@ZrO2-CN catalyst.
[0012] Preferably, the zirconium oxychloride solution in S1 is made from N,N-dimethylformamide and zirconium oxychloride, and the mass ratio of zirconium oxychloride to N,N-dimethylformamide is 1:100.
[0013] The terephthalic acid solution described in S1 is made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40.
[0014] The ratio of zirconium oxychloride solution to terephthalic acid solution is 1:1.
[0015] Preferably, the ratio of mixture A to acetic acid in S2 is 2.5:1.
[0016] Preferably, the reaction temperature during the stirring reaction in S3 is 45°C, the reaction time is 30 h, and the CO2 pressure is 0.3 MPa.
[0017] Preferably, the mass ratio of UiO-66 material, cobalt nitrate, and 4,4-bipyridine in S3 is 1:1:1-2.
[0018] Preferably, the calcination treatment in S3 is performed at a temperature of 600-800℃ for 4 hours.
[0019] Preferably, in step S3, the mass ratio of UiO-66 material to non-aqueous solvent is 0.1-0.2:16.
[0020] The beneficial effects of this invention are:
[0021] This invention provides a method for preparing and applying a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2. The invention simultaneously improves the low-temperature catalytic activity, tandem reaction adaptability, and cycle life of the catalyst through the following method.
[0022] (1) The present invention significantly improves the performance of the catalyst: by using metal Co as the active site, ZrO2 with alkaline sites as the CO2 carrier, and the three-level synergy of porous nanocomposite, the porous octahedral structure and uniform loading of Co nanoparticles of MOFs-derived Co@ZrO2-CN composite material are realized. At a reaction temperature of 45℃, a reaction time of 30h, and a CO2 pressure of 0.3MPa, the yield reaches 99.8%. After 7 cycles, the yield does not decrease, and it has high stability, which is far superior to traditional composite materials.
[0023] (2) This invention achieves efficient resource utilization: It innovatively uses nitro aromatic compounds as raw materials and utilizes the in-situ hydrogenation reaction of nitro aromatic compounds to generate aromatic amines. Then, in the same reactor, the N-formylation reaction of amines and carbon dioxide is used to realize a one-step tandem catalytic process, which can minimize the separation, purification, storage and transportation of intermediate aromatic amines, improve the overall yield, reduce costs and energy consumption, achieve atom economy, and promote the development of green materials.
[0024] (3) The present invention improves the reaction rate and stability: the hierarchical octahedral pore structure and the active sites of Co with uniform and small particle size significantly improve the reaction kinetics and stability of the catalyst material.
[0025] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description
[0026] Figure 1 The XRD patterns of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1 and four materials prepared by physical mixing, namely Co / ZrO2-CN, Co-CN, and ZrO2 / C, are shown in comparison.
[0027] Figure 2 The N2 adsorption-desorption isotherm comparison curves of the Co / ZrO2-CN material prepared by physical mixing of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1 and the catalyst in Example 1 are shown.
[0028] Figure 3Raman spectra of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1, the Co / ZrO2-CN material prepared by physical mixing, the Co-CN material, and the Zr-CN material;
[0029] Figure 4 XPS fine spectra of the Co 2p orbitals of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1, the Co / ZrO2-CN material prepared by physical mixing, the Co-CN material, and the Zr-CN material;
[0030] Figure 5 XPS fine spectra of Zr 3d orbitals of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1, the Co / ZrO2-CN material prepared by physical mixing, the Co-CN material, and the Zr-CN material;
[0031] Figure 6 The XPS fine spectra of the O 1s orbitals of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1, the Co / ZrO2-CN material prepared by physical mixing, the Co-CN material, and the Zr-CN material are shown.
[0032] Figure 7 Comparison curves of CO2 temperature-programmed desorption (CO2-TPD) of the bifunctional Co@ZrO2-CN catalyst prepared in Example 1 and the Co / ZrO2-CN material prepared by physical mixing.
[0033] Figure 8 The bifunctional Co@ZrO2-CN catalyst prepared in Example 1, the Co / ZrO2-CN material prepared by physical mixing, and the performance of Co-CN material in the tandem N-formylation reaction of nitroaromatic compounds with CO2 are described. Detailed Implementation
[0034] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. The embodiments described below are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0035] Example 1: A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 is as follows:
[0036] S1: Mix 9.5g of zirconium oxychloride solution (made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:100) and 9.5g of terephthalic acid solution (made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40) and stir for 25min to obtain mixture A;
[0037] S2: Add 10g of acetic acid to 25g of mixture A, stir and react at 90℃ for 18h. After centrifugation, wash three times with anhydrous ethanol and dry to obtain UiO-66 material.
[0038] S3: 0.1g of UiO-66 material was dispersed in methanol and ultrasonically dispersed. Then, 0.1g of cobalt nitrate and 0.1g of 4,4-bipyridine were added and the mixture was stirred at 45℃ and CO2 pressure of 0.3MPa for 30h. The mixture was then centrifuged and dried, followed by calcination at 700℃ under a nitrogen atmosphere for 4h. After cooling, a bifunctional Co@ZrO2-CN catalyst was obtained.
[0039] Example 2: A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 is as follows:
[0040] S1: Mix 9.5g of zirconium oxychloride solution (made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:100) and 9.5g of terephthalic acid solution (made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40) and stir for 30min to obtain mixture A;
[0041] S2: Add 10g of acetic acid to 25g of mixture A, stir, react at 105℃ for 22h, centrifuge, wash three times with anhydrous ethanol, and dry to obtain UiO-66 material;
[0042] S3: 0.1g of UiO-66 material was dispersed in methanol and ultrasonically dispersed for 30min. Then, 0.1g of cobalt nitrate and 0.1g of 4,4-bipyridine were added and stirred for 30h at 45℃ and CO2 pressure of 0.3MPa. The mixture was then centrifuged and dried, followed by calcination at 800℃ under nitrogen atmosphere for 4h. After cooling, the bifunctional Co@ZrO2-CN catalyst was obtained.
[0043] Example 3: A method for preparing a bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion is as follows:
[0044] S1: Mix 9.5g of zirconium oxychloride solution (made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:100) and 9.5g of terephthalic acid solution (made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40) and stir for 35min to obtain mixture A;
[0045] S2: Add 10g of acetic acid to 25g of mixture A, stir, react at 120℃ for 26h, centrifuge, wash three times with anhydrous ethanol, and dry to obtain UiO-66 material;
[0046] S3: 0.1g of UiO-66 material was dispersed in methanol and ultrasonically dispersed for 30min. Then, 0.1g of cobalt nitrate and 0.2g of 4,4-bipyridine were added and stirred for 30h at 45℃ and CO2 pressure of 0.3MPa. The mixture was then centrifuged and dried, followed by calcination at 700℃ under a nitrogen atmosphere for 4h. After cooling, a bifunctional Co@ZrO2-CN catalyst was obtained.
[0047] Comparative Example 1: A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 is as follows:
[0048] S1: Mix 9.5g of zirconium oxychloride solution (made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:100) and 9.5g of terephthalic acid solution (made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40) and stir for 10min to obtain mixture A;
[0049] S2: Add 10g of acetic acid to 25g of mixture A, stir and react at 90℃ for 18h. After centrifugation, wash three times with anhydrous ethanol and dry to obtain UiO-66 material.
[0050] S3: 0.2g of UiO-66 material was dispersed in methanol and ultrasonically dispersed. Then, 0.1g of cobalt nitrate and 0.1g of 4,4-bipyridine were added and the mixture was stirred and reacted at 45℃ and CO2 pressure of 0.3MPa for 30h. The mixture was then centrifuged and dried, followed by calcination at 700℃ under nitrogen atmosphere for 4h. After cooling, the bifunctional Co@ZrO2-CN catalyst was obtained.
[0051] Comparative Example 2: A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 is as follows:
[0052] S1: Mix 9.5g of zirconium oxychloride solution (made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:100) and 9.5g of terephthalic acid solution (made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:40) and stir for 10min to obtain mixture A;
[0053] S2: Add 10g of acetic acid to 25g of mixture A, stir and react at 90℃ for 18h. After centrifugation, wash three times with anhydrous ethanol and dry to obtain UiO-66 material.
[0054] S3: 0.2g of UiO-66 material was dispersed in methanol and ultrasonically dispersed for 30min. Then, 0.2g of cobalt nitrate and 0.1g of 4,4-bipyridine were added and stirred for 30h at 45℃ and CO2 pressure of 0.3MPa. The mixture was then centrifuged and dried, followed by calcination at 600℃ under nitrogen atmosphere for 4h. After cooling, the bifunctional Co@ZrO2-CN catalyst was obtained.
[0055] Performance testing:
[0056] The yields (%) of the preparation processes of Examples 1-3 and Comparative Examples 1-2 were determined, and the results are shown in Table 1.
[0057] Table 1: Performance test results of Examples 1-3 and Comparative Examples 1-2
[0058] project Yield / % Example 1 99.8 Example 2 95.8 Example 3 92.6 Comparative Example 1 85.3 Comparative Example 2 80.6
[0059] Effect Analysis:
[0060] Combined with Table 1 Figures 1 to 8 It can be seen that the preparation method of the present invention has excellent yield of bifunctional Co@ZrO2-CN catalyst; at the same time, the prepared bifunctional Co@ZrO2-CN catalyst also has excellent catalytic rate boosting ability, catalytic activity and stability.
[0061] like Figure 1 As shown, the structure and composition of the Co@ZrO2-CN, Co / ZrO2-CN, Co-CN, and ZrO2 / C catalysts were investigated by XRD. The diffraction peaks observed at 30.2°, 35.0°, 50.4°, and 60.2° correspond to the crystal planes of ZrO2, respectively. The (222) crystal plane of Co was observed at 44.3°.
[0062] like Figure 2As shown, the specific surface area and pore volume of the MOF-derived Co@ZrO2-CN prepared in Example 1 of this invention are significantly higher than those of the Co / ZrO2-CN prepared by physical mixing. This indicates that the Co@ZrO2-CN material prepared in this example facilitates the effective transfer of substrate and catalyst. This characteristic improves the catalytic activity and stability of the material.
[0063] like Figure 3 As shown, compared with the Co / ZrO2-CN material prepared by physical mixing, the MOFs-derived Co@ZrO2-CN prepared in Example 1 of this invention has more oxygen vacancies and structural defects on its surface.
[0064] like Figure 4-6 As shown, the XPS results further indicate that the Co@ZrO2-CN material prepared in Example 1 has more oxygen vacancies and Lewis basic sites, as well as electron transfer between Co and ZrO2, compared to the Co / ZrO2-CN material prepared by physical mixing. This further demonstrates that the Co@ZrO2-CN material prepared in this example is more conducive to promoting CO2 adsorption and activation, as well as the adsorption of the substrate nitrobenzene, thereby significantly improving the reaction efficiency. This indicates that the Co@ZrO2-CN prepared in this example is more conducive to adsorbing and activating CO2, and thus has the potential to increase the catalytic rate during the catalytic reaction.
[0065] like Figure 7 As shown, compared with the Co / ZrO2-CN prepared by physical mixing, the temperature of the CO2 desorption peak in the MOFs-derived Co@ZrO2-CN material prepared in Example 1 of this invention shifts slightly to a higher temperature. Simultaneously, Co@ZrO2-CN not only has the highest total number of basic sites, but also the highest content of medium-strong and strong basic sites. This indicates that the Co@ZrO2-CN material prepared in this example has a higher content of basic sites, which is beneficial for promoting the formation of intermediates during the reaction of CO2 with nitroaromatics, thereby improving the reactivity.
[0066] like Figure 8 As shown, under the conditions of reaction temperature of 45℃, reaction time of 30h, and CO2 pressure of 0.3MPa, the yield of Example 1 reached 99.8%, which is significantly higher than that of Co / ZrO2-CN material.
[0067] The above results indicate that the Co@ZrO2-CN catalyst prepared in Example 1 exhibits higher performance.
[0068] The foregoing has provided a detailed description of one embodiment of the present invention, but this description is merely a preferred embodiment and should not be construed as limiting the scope of the invention. All equivalent variations and modifications made within the scope of the claims of this invention should still fall within the patent coverage of this invention.
Claims
1. A method for preparing a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2, characterized in that, Includes the following steps: S1: Mix zirconium oxychloride solution and terephthalic acid solution and stir for 25-35 min to obtain mixture A; S2: Add acetic acid to mixture A, stir, react at 90-120℃ for 18-26h, centrifuge, wash 3 times with anhydrous ethanol, and dry to obtain UiO-66 material; S3: The UiO-66 material was dispersed in a non-aqueous solvent and ultrasonically dispersed. Then, cobalt nitrate and 4,4-bipyridine solution were added and stirred to react. After centrifugation and drying, the mixture was calcined under a nitrogen atmosphere and cooled to obtain a bifunctional Co@ZrO2-CN catalyst.
2. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, The zirconium oxychloride solution described in S1 is made from N,N-dimethylformamide and zirconium oxychloride, with a mass ratio of zirconium oxychloride to N,N-dimethylformamide of 1:
100. The terephthalic acid solution described in S1 is made from N,N-dimethylformamide and terephthalic acid, with a mass ratio of terephthalic acid to N,N-dimethylformamide of 1:
40. The ratio of zirconium oxychloride solution to terephthalic acid solution is 1:
1.
3. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, The ratio of mixture A to acetic acid in S2 is 2.5:
1.
4. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, The reaction temperature during the stirring reaction described in S3 is 45℃, the reaction time is 30h, and the CO2 pressure is 0.3MPa.
5. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, The mass ratio of UiO-66 material, cobalt nitrate, and 4,4-bipyridine in S3 is 1:1:1-2.
6. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, The calcination treatment described in S3 is performed at a temperature of 600-800℃ for a duration of 4 hours.
7. The preparation method of the bifunctional Co@ZrO2-CN catalyst for direct CO2 conversion according to claim 1, characterized in that, In step S3, the mass ratio of UiO-66 material to non-aqueous solvent is 0.1-0.2:
16.
8. A bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2, characterized in that, The catalyst, prepared by any one of claims 1-7, achieves a target N-phenylformamide yield of 99.8% under reaction conditions of 45°C and CO2 pressure of 0.3 MPa. The catalyst exhibits excellent cycle stability with no significant decrease in catalytic yield after 7 cycles of recycling.
9. The application of a bifunctional Co@ZrO2-CN catalyst for the direct conversion of CO2 according to any one of claims 1-7, characterized in that, The bifunctional Co@ZrO2-CN catalyst can be applied to multi-step tandem catalytic reactions, CO2 cycloaddition reactions, and the formylation reaction of CO2 with nitrobenzene.