Preparation method and application of fly ash-based porous fiber denitration catalyst
By employing techniques such as ionic liquid ball milling, coaxial spinning, and two-stage pyrolysis, a porous fiber denitrification catalyst was constructed, which solved the problems of insufficient low-temperature activity and poor stability of fly ash-based denitrification catalysts, and achieved efficient low-temperature denitrification and low-cost preparation.
Patent Information
- Application Number
- CN202611437296.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-24
AI Technical Summary
Existing fly ash-based denitrification catalysts suffer from insufficient denitrification activity at low temperatures, high manufacturing costs, and poor stability. Furthermore, traditional processes are energy-intensive and subject to severe interference from impurities, making it difficult to meet the flue gas treatment needs of non-power industries.
A porous fiber denitration catalyst was constructed using techniques such as ionic liquid ball milling synergistic activation, coaxial spinning coupled liquid nitrogen flash freezing, and two-stage temperature- and atmosphere-controlled pyrolysis. The low-temperature activity and stability of the catalyst were improved by ultrasonic alkali dissolution with sodium hydroxide, dielectric barrier discharge plasma treatment, and ammonia nitrogen etching to regulate surface sites.
It achieves high efficiency and low-temperature denitrification performance, the catalyst preparation process is simple, cost-effective, and has good application and promotion value.
Smart Images

Figure CN123148981A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing and applying a fly ash-based porous fiber denitrification catalyst, belonging to the field of air pollution control. Background Technology
[0002] The large-scale stockpiling of fly ash not only occupies land resources but also poses environmental risks such as dust pollution and groundwater contamination. Currently, the mainstream disposal methods for fly ash are still mainly low-value-added applications such as building material admixtures and roadbed filling, resulting in low unit product value and difficulty in effectively covering transportation and processing costs. The total content of SiO2 and Al2O3 in fly ash is generally above 70%, giving it a natural advantage as a framework for inorganic porous materials. Converting fly ash into a catalyst carrier for flue gas denitrification can, on the one hand, replace some commercial silicon-aluminum sources and reduce catalyst manufacturing costs, and on the other hand, explore new paths for the high-value-added resource utilization of fly ash, thus possessing significant research value and industrialization potential.
[0003] Currently, research on the preparation of denitrification catalysts using fly ash as a silica-alumina source has made some progress. At the support construction level, there are two main technical routes: alkali fusion-hydrothermal synthesis of molecular sieve supports and acid leaching-sol-gel preparation of amorphous silica-alumina supports. The former can obtain crystalline zeolite structures such as ZSM-5 and Y-type, while the latter is more suitable for constructing mesoporous oxide-supported systems. However, these technologies still have limitations in practical applications. The alkali fusion-hydrothermal method has high energy consumption and a long crystallization cycle, and impurities such as Fe2O3 and CaO in fly ash can interfere with zeolite crystallization, resulting in low crystallinity and insufficient acidic site density in the product, making it difficult to meet the denitrification activity requirements of non-power industry flue gas treatment at low temperatures (<200 ℃). The acid leaching-sol-gel method consumes a large amount of strong acid, has high wastewater treatment costs, and the surface acidity of the amorphous silica-alumina support is relatively weak, making it prone to agglomeration and sintering after loading of active components, resulting in poor long-term catalyst stability. Summary of the Invention
[0004] The purpose of this invention is to address the current status and existing problems of low-temperature denitrification in non-electric industries, and to propose a method for preparing and applying a fly ash-based porous fiber denitrification catalyst.
[0005] A fly ash-based porous fiber denitrification catalyst, the preparation method of which is as follows:
[0006] (1) Ionic liquid ball milling synergistic activation to construct spinning sizing agent
[0007] Weigh out fly ash, sodium hydroxide, and deionized water, mix them evenly, then perform ultrasonic alkali dissolution in a water bath, filter, wash with water, and dry to obtain modified fly ash powder. Then, mix the modified fly ash powder and polyvinylpyrrolidone evenly and place them in a dielectric barrier discharge plasma reactor. Discharge treatment is performed under argon gas to obtain activated powder.
[0008] Weigh out activated powder, 1-ethyl-3-methylimidazolium diethyl phosphate, and deionized water, mix them, and stir them in a constant temperature water bath to obtain a mixed slurry. After centrifugation, retain the lower layer sol. Then mix the lower layer sol, nano aluminum sol, citric acid, vanadium salt, tungsten salt, manganese salt, and cerium salt, and stir them in a constant temperature water bath to obtain a composite sol.
[0009] The composite sol, polyvinyl alcohol, polyether P123, polymethyl methacrylate monodisperse microsphere solution, bacterial cellulose dispersion, deionized water, and anhydrous ethanol were mixed and placed in a planetary ball mill for continuous ball milling. After ball milling, a spinning slurry was obtained.
[0010] (2) Construction of network precursors by coaxial spinning coupled with liquid nitrogen flash freezing
[0011] Weigh out polystyrene, N,N-dimethylformamide and polymethyl methacrylate monodisperse microspheres and mix them evenly to form an inner fluid. Use the spinning slurry obtained in step (1) as the outer fluid. Use a coaxial spinneret to spin the microfluidic electrostatic osmosis machine. At the same time, place a stainless steel tray collector directly below the spinning nozzle and pre-inject liquid nitrogen into the collector. During the spinning process, continuously add liquid nitrogen to maintain the liquid nitrogen level. After spinning, place the filamentous ice crystals in the liquid nitrogen in a freeze dryer and freeze dry to obtain the network precursor.
[0012] (3) Preparation of catalyst matrix by pyrolysis coupled in-situ steam activation
[0013] The network precursor obtained in step (2) is placed in a tube atmosphere furnace, heated to 350-450°C and held for 3-4 hours under nitrogen gas conditions, and then nitrogen gas is first introduced into a constant temperature bubbling water bath so that the mixture of nitrogen gas and water vapor is introduced into the tube atmosphere furnace, heated to 600-700°C and held for 4-8 hours to obtain a porous catalyst matrix;
[0014] (4) Ammonia nitrogen etching to regulate surface sites
[0015] The porous catalyst matrix obtained in step (3) is placed in a dielectric barrier discharge plasma reactor, a mixture of ammonia and argon is introduced, and then discharged. After the discharge is completed, a porous fiber denitrification catalyst is obtained.
[0016] In the above method: the mass ratio of fly ash, sodium hydroxide and deionized water in step (1) is 1:(3~5):(10~20), the temperature of water bath ultrasonic alkali dissolution is 70~90℃, the power of water bath ultrasonic alkali dissolution is 500~700W, the time of water bath ultrasonic alkali dissolution is 2~4h, the drying temperature is 80~100℃, the drying time is 6~12h, the mass ratio of modified fly ash powder and polyvinylpyrrolidone is 1:(0.2~0.4), the rate of argon gas introduction is 60~80mL / min, the power of discharge treatment is 200~300W, and the discharge treatment time is 30~60min.
[0017] In the above method: the CAS number of 1-ethyl-3-methylimidazolium diethyl phosphate mentioned in step (1) is 848641-69-0, the model of the nano aluminum sol is JR14W, purchased from Xuancheng Jingrui New Materials Co., Ltd., the vanadium salt is ammonium metavanadate, the tungsten salt is ammonium metatungstate, the manganese salt is manganese nitrate hexahydrate or manganese chloride, the cerium salt is cerium nitrate hexahydrate or cerium chloride, and the mass ratio of activated powder, 1-ethyl-3-methylimidazolium diethyl phosphate, and deionized water is as follows: The mass ratio of the lower sol, nano-aluminum sol, citric acid, vanadium salt, tungsten salt, manganese salt, and cerium salt is 1:(0.1~0.15):(0.06~0.12):(0.02~0.04):(0.04~0.06):(0.04~0.06):(0.03~0.05). The temperature of the constant temperature water bath is 60~80℃, and the stirring time is 2~4h.
[0018] In the above method: the polyvinyl alcohol mentioned in step (1) has a CAS number of 9002-89-5 and a weight-average molecular weight of 13,000~50,000; the polyether P123 has a CAS number of 9003-11-6 and a weight-average molecular weight of 5,800; the polymethyl methacrylate monodisperse microspheres have a diameter of 1~2 μm; the concentration of the polymethyl methacrylate monodisperse microspheres is 25 mg / mL; and the content of the bacterial cellulose dispersion is 2.5~5%. The mass ratio of the sol, polyvinyl alcohol, polyether P123, polymethyl methacrylate monodisperse microspheres, bacterial cellulose dispersion, deionized water, and anhydrous ethanol was 1:(0.02~0.04):(0.01~0.03):(0.03~0.06):(0.05~0.1):(0.3~0.6):(0.3~0.6). The ball milling speed was 300~500 rpm, and the ball milling time was 3~6 h.
[0019] In the above method: the CAS number of the polystyrene mentioned in step (2) is 9003-53-6, the weight average molecular weight is 280,000~350,000, the diameter of the polymethyl methacrylate monodisperse microspheres is 300~500nm, the concentration of the polymethyl methacrylate monodisperse microspheres is 25mg / mL, and the mass ratio of N,N-dimethylformamide, polystyrene and polymethyl methacrylate monodisperse microspheres is 1:(0.1~0.2):(0.05~0.1).
[0020] In the above method: the injection rate of the inner layer fluid in the spinning process described in step (2) is 0.2~0.3mL / h, the injection rate of the outer layer fluid is 0.6~0.9mL / h, the voltage is 15~25kV, the size of the stainless steel tray collector is 30cm×20cm×8cm, the height of the injected liquid nitrogen is 1 / 2~4 / 5 of the stainless steel tray collector, the freeze-drying temperature is -50~-40℃, and the freeze-drying time is 36~72h.
[0021] In the above method: the nitrogen gas introduction rate in step (3) is 200~300mL / min, and the temperature of the constant temperature bubbling water bath is 80~90℃.
[0022] In the above method: the rates of ammonia and argon introduced in step (4) are 10~15mL / min and 90~140mL / min, respectively; the voltage during the discharge process is 15~20kV; and the processing time is 20~40min.
[0023] The catalyst prepared by the above method is used in low-temperature denitrification.
[0024] The above-mentioned denitrification is a selective catalytic reduction of nitrogen oxides.
[0025] The experimental conditions for evaluating the catalyst activity of this invention are as follows: 0.5 mL of 40-60 mesh catalyst is poured into a quartz tube with an inner diameter of 8 mm, fixed with quartz wool and wire mesh, and placed in a tube furnace. The temperature of the catalytic reaction is adjusted by controlling the heating temperature of the tube furnace. The inlet gas components are: NO (500 ppm), NH3 (500 ppm), O2 (10 vol.%), and the remainder is N2. The total gas flow rate is 400 mL / min, and the temperature is controlled at 150-270℃. The temperature is maintained at 30℃ for 30 min. The NO concentration is measured using a flue gas analyzer. The denitrification efficiency of the catalyst is higher than 90% within the temperature range of 180-240℃.
[0026] Beneficial effects:
[0027] (1) Traditional fly ash activation often uses high-temperature alkali melting (800~850℃) followed by acid leaching or hydrothermal crystallization. Such methods are energy-intensive, consume large amounts of acid and alkali, and the melt is prone to forming a glassy body after cooling, requiring secondary crushing and grinding, which easily introduces impurities and causes uneven condensation degree of silicon and aluminum species. This invention utilizes a three-stage progressive activation strategy of ultrasonic alkali dissolution of sodium hydroxide-plasma treatment-ionic liquid stripping. First, the OH generated by sodium hydroxide... - Under ultrasonic cavitation, the Si-O-Si and Si-O-Al bridging bonds in the fly ash glass network are broken, causing it to initially depolymerize into oligomeric aluminosilicate units. Then, argon DBD plasma activation is introduced, utilizing the oxygen vacancies and dangling bonds generated by high-energy electron collisions with oxygen lattice on the fly ash surface to increase surface free energy and hydroxyl density, providing active sites for subsequent intercalation and exfoliation by ionic liquids. Next, 1-ethyl-3-methylimidazolium diethyl phosphate is selected, and through the strong coordination tendency of the phosphate anion with aluminum species, the insoluble mullite phase in the fly ash is further dissociated, while the phosphate ion acts as a mineralization agent. In subsequent pyrolysis, the agent is in situ incorporated into a silicon-aluminum framework to form PO-Si / Al bonds, enhancing the acidity and hydrothermal stability of the carrier. Finally, the activated sol, nano-aluminum sol, active component precursor, spinning aid PVA, mesoporous soft template P123, macroporous hard template PMMA microspheres, and bacterial cellulose nanofibers are placed in a planetary ball mill for mechanochemical ball milling. The high-speed collision and shearing of zirconia balls completes the nano-homogenization of sol particles, the uniform dispersion of templates, and the in-situ construction of the rheological network of spinning slurry, providing homogenization guarantee for subsequent multifunctional slurries with excellent spinnability.
[0028] (2) Fibers prepared by traditional uniaxial electrospinning or centrifugal spinning are usually solid cylindrical and tightly packed. There are no large pores between the fibers, and the gas transfer along the fiber axis is severely hindered while the radial diffusion is severely blocked. Moreover, the fibers are easy to melt and form a dense film after calcination. In this invention, coaxial electrospinning is used, with fly ash-based composite sol as the inner fluid to ensure the continuity of the carrier skeleton as the main fiber body. Polystyrene / DMF solution containing PMMA microspheres is used as the outer fluid. The PS is completely removed during the pyrolysis process to form a continuous hollow core cavity. The embedded PMMA microspheres first occupy the space in the inner layer. After pyrolysis, nanopores are left on the inner wall of the fiber, so that the hollow core cavity is connected with the shell mesoporous network. The receiving end uses a stainless steel tray continuously filled with liquid nitrogen instead of a conventional rotating drum, so that the coaxial jet undergoes three coordinated steps during flight: electric field stretching, partial solvent evaporation, and liquid nitrogen quenching. The flying liquid filaments solidify instantly upon contact with liquid nitrogen, and the water inside the fibers rapidly nucleates into tiny ice crystals. The ice crystals serve as an in-situ dynamic template to open and freeze the overlapping nodes between fibers, avoiding the problems of uncontrollable pore size and fiber fusion caused by ice crystal coarsening in the pre-freezing step of traditional freeze-drying methods. Finally, a three-dimensional network block is formed by ice-welded nodes. After freeze-drying, the large pores between fibers left by the in-situ sublimation of ice crystals and the hollow core cavity formed by the removal of the PS core layer are spatially interwoven and connected, constructing a three-dimensional interconnected channel topology.
[0029] (3) When treating catalyst precursors containing template agents using traditional high-temperature calcination methods, organic matter is usually removed by one-step calcination in air atmosphere. However, rapid oxidation and exothermic reactions can lead to local overburning, causing fiber melting and collapse and active phase sintering. Moreover, template removal creates pores of a single type, which cannot simultaneously connect mesopores and macropores. This invention utilizes a two-stage temperature and atmosphere controlled pyrolysis strategy. First, low-temperature pre-carbonization is carried out under nitrogen protection, allowing organic components such as PVA, P123, and bacterial cellulose to slowly decompose into residual carbon skeletons under anaerobic conditions. This residual carbon layer can support the fiber morphology and prevent premature densification and shrinkage of silicon and aluminum species. Then, nitrogen is first introduced into a constant-temperature bubbling water bath to carry water vapor. At high temperature, a triple reaction of water vapor physical activation, complete template removal, and in-situ generation of active components is carried out simultaneously. Water vapor, as a green and mild etching agent, can react with the residual carbon skeleton to react C + H2O → CO + The H2 water-gas reaction results in residual carbon gasification and escape, leaving behind worm-like mesopores in situ. Simultaneously, water vapor molecules etch the Si-O-Si bonds in the fly ash silica-alumina network, creating new micro-mesopores. The superposition of these two processes causes the mesopores to extend from inter-chain nanopores to the fiber walls. Three templates are used to create a hierarchical porous network consisting of PMMA microspheres (macropores), PS (hollow core), P123 (mesopores), and bacterial cellulose (nanopores). Furthermore, the active component precursor decomposes in the water vapor oxidizing atmosphere, releasing a composite oxide active phase. The presence of water vapor also inhibits the high-temperature over-oxidation of vanadium species and the excessive growth of WO3 grains, allowing the active component to be highly dispersed at the nanoscale and firmly anchored to the mesopore-macropore walls. This effectively avoids the problems of pore blockage and uneven distribution of active components in the traditional method of first preparing the carrier and then impregnating.
[0030] (4) Traditional methods to improve the surface acidity of denitrification catalysts often involve impregnation with sulfuric acid or phosphoric acid followed by secondary calcination. Such wet modification is prone to partial collapse of multi-level channels due to liquid surface tension, and capillary condensation of acid in nanopores can cause channel blockage and redistribution of active components. In this invention, ammonia nitrogen dielectric barrier discharge plasma surface treatment is used to utilize the high-energy electrons generated by DBD discharge to collide with the mixed gas, causing ammonia to dissociate into highly active nitrogen-containing free radicals, which selectively react with hydroxyl groups such as Si-OH, V-OH, and W-OH on the catalyst surface to undergo the substitution reaction M-OH + NH2• → M-NH2 + H2O, converting the hydroxyl sites of weak Brønsted acids into more basic -NH2 groups. These amino groups can adsorb reaction molecules to form intermediates in the SCR reaction, enhancing the surface enrichment capacity and reactivity of reaction molecules. In addition, the ion bombardment in the plasma simultaneously generates a surface lattice oxygen etching effect, introducing new oxygen vacancy defect states in the fiber subsurface layer, increasing the density of unsaturated coordinated metal cations (Lewis acid sites).
[0031] Therefore, the catalyst prepared by this invention not only has excellent low-temperature denitrification performance, but also has a simple preparation process, high cost performance, and strong application and promotion value. Attached Figure Description
[0032] Figure 1 This is a field emission scanning electron microscope image of the catalyst prepared in Example 1;
[0033] Figure 2 The diagram shows the denitrification efficiency of the catalysts prepared in Examples 1-2. Detailed Implementation
[0034] The present invention will be further described below with reference to the embodiments. The embodiments are implemented under the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given. However, the protection scope of the present invention is not limited to the following embodiments.
[0035] The bacterial cellulose dispersion involved in the embodiments or comparative examples of this invention is BC bacterial cellulose produced by Qihong Technology Co., Ltd.; the nano aluminum sol is model JR14W and was purchased from Xuancheng Jingrui New Materials Co., Ltd.
[0036] The polymethyl methacrylate monodisperse microsphere solution is a commercially available product, and its purchase sources include, but are not limited to, the following: https: / / e.tb.cn / h.8NvKpIoRtIZ9Hpm?tk=M0poTUir61J
[0037] Example 1
[0038] (1) Ionic liquid ball milling synergistic activation to construct spinning sizing agent
[0039] Weigh 20g of fly ash, 60g of sodium hydroxide, and 100g of deionized water and mix them evenly. Then, ultrasonically dissolve the mixture in a water bath at 70℃ (the power of alkali dissolution is 500W) for 4 hours. After alkali dissolution, filter, wash with water, and dry at 80℃ for 12 hours to obtain modified fly ash powder. Then, weigh 10g of modified fly ash powder and 2g of polyvinylpyrrolidone and mix them evenly. Place the mixture in a dielectric barrier discharge plasma reactor and discharge it under argon gas conditions (argon gas introduction rate is 60mL / min) (discharge treatment power is 200W, discharge treatment time is 60min) to obtain activated powder.
[0040] Weigh 10g of activated powder, 4g of 1-ethyl-3-methylimidazolium diethyl phosphate, and 20g of deionized water, mix them, and stir in a 60℃ constant temperature water bath for 4 hours to obtain a mixed slurry. After centrifugation, retain the lower layer sol. Then, mix 10g of the lower layer sol, 1g of nano aluminum sol, 0.6g of citric acid, 0.2g of ammonium metavanadate, 0.4g of ammonium metatungstate, 0.4g of manganese nitrate hexahydrate, and 0.3g of cerium nitrate hexahydrate, and stir in a 60℃ constant temperature water bath for 4 hours to obtain a composite sol.
[0041] 12.9g of composite sol, 0.258g of polyvinyl alcohol (weight average molecular weight of 13000), 0.129g of polyether P123, 0.387g of polymethyl methacrylate monodisperse microsphere solution (diameter of 1μm, concentration of 25mg / mL), 0.645g of bacterial cellulose dispersion (content of 2.5%), 3.87g of deionized water, and 3.87g of anhydrous ethanol were mixed and placed in a planetary ball mill and continuously ball-milled at 300rpm for 6h. After ball milling, spinning slurry was obtained.
[0042] (2) Construction of network precursors by coaxial spinning coupled with liquid nitrogen flash freezing
[0043] Weigh out 1g of polystyrene (weight average molecular weight 280,000) and 10g of... N,N-dimethylformamide and 0.5g polymethyl methacrylate monodisperse microsphere solution (diameter 300nm, concentration 25mg / mL) were mixed evenly to form an inner fluid. The spinning slurry obtained in step (1) was used as the outer fluid. Spinning was performed using a microfluidic electrostatic integrated machine with a coaxial spinneret (the injection rate of the inner fluid during spinning was 0.2mL / h, the injection rate of the outer fluid was 0.6mL / h, the voltage was 15kV, and the injection of the inner fluid stopped synchronously after the outer fluid was consumed). At the same time, a stainless steel tray collector (size 30cm×20cm×8cm) was placed directly below the spinning nozzle, and liquid nitrogen was pre-injected into the collector (the height of the liquid nitrogen injection was 1 / 2 of the stainless steel tray collector). Liquid nitrogen was continuously added during spinning to maintain the liquid nitrogen height. After spinning, the filamentous ice crystals in the liquid nitrogen were placed in a freeze dryer and freeze-dried at -50℃ for 36h to obtain the network precursor.
[0044] (3) Preparation of catalyst matrix by pyrolysis coupled in-situ steam activation
[0045] The network precursor obtained in step (2) was placed in a tube atmosphere furnace and heated to 350°C and held for 4 hours under nitrogen gas conditions (nitrogen gas rate of 200 mL / min). Then, nitrogen gas (nitrogen gas rate of 200 mL / min) was first introduced into an 80°C constant temperature bubbling water bath to introduce the mixture of nitrogen gas and water vapor into the tube atmosphere furnace, heated to 600°C and held for 8 hours to obtain a porous catalyst matrix.
[0046] (4) Ammonia nitrogen etching to regulate surface sites
[0047] The porous catalyst matrix obtained in step (3) was placed in a dielectric barrier discharge plasma reactor, and a mixture of ammonia and argon was introduced (the rates of ammonia and argon were 10 mL / min and 140 mL / min, respectively). Then, it was subjected to discharge treatment (the voltage during the discharge treatment was 15 kV, and the treatment time was 40 min). After the treatment, a porous fiber denitrification catalyst was obtained (the FE-SEM image of the catalyst is shown in the figure). Figure 1 (as shown)
[0048] (5) Catalytic activity test
[0049] Take 0.5 mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8 mm. Fix it with quartz wool and wire mesh. Place the quartz tube in a tube furnace and adjust the temperature of the catalytic reaction by controlling the heating temperature of the tube furnace. The inlet gas components are: NO (500 ppm), NH3 (500 ppm), O2 (10 vol.%), and the remainder is N2. The total gas flow rate is 400 mL / min. The temperature is controlled at 150-270℃, and the temperature is maintained at 30℃ for 30 min. The NO concentration is measured using a flue gas analyzer. The denitrification efficiency of the catalyst is higher than 90% in the temperature range of 180-240℃.
[0050] Example 2
[0051] (1) Ionic liquid ball milling synergistic activation to construct spinning sizing agent
[0052] Weigh 20g of fly ash, 100g of sodium hydroxide, and 400g of deionized water and mix them evenly. Then, ultrasonically dissolve the mixture in a 90℃ water bath (700W power for alkali dissolution) for 2 hours, filter and wash with water, and dry at 100℃ for 6 hours to obtain modified fly ash powder. Then, weigh 10g of modified fly ash powder and 4g of polyvinylpyrrolidone and mix them evenly. Place the mixture in a dielectric barrier discharge plasma reactor and discharge it under argon gas conditions (argon gas introduction rate of 80mL / min) (discharge power of 300W, discharge time of 30min) to obtain activated powder.
[0053] Weigh 10g of activated powder, 6g of 1-ethyl-3-methylimidazolium diethyl phosphate, and 40g of deionized water, mix them, and stir in an 80℃ constant temperature water bath for 2 hours to obtain a mixed slurry. After centrifugation, retain the lower layer sol. Then, mix 10g of the lower layer sol, 1.5g of nano aluminum sol, 1.2g of citric acid, 0.4g of ammonium metavanadate, 0.6g of ammonium metatungstate, 0.6g of manganese hexachloride, and 0.5g of cerium chloride, and stir in an 80℃ constant temperature water bath for 2 hours to obtain a composite sol.
[0054] 14.8g of composite sol, 0.592g of polyvinyl alcohol (weight average molecular weight 50000), 0.444g of polyether P123 (weight average molecular weight 5800), 0.888g of polymethyl methacrylate monodisperse microsphere solution (diameter 2μm, concentration 25mg / mL), 1.48g of bacterial cellulose dispersion (content 5%), 8.88g of deionized water, and 8.88g of anhydrous ethanol were mixed and placed in a planetary ball mill and continuously ball-milled at 500rpm for 3h. After ball milling, spinning slurry was obtained.
[0055] (2) Construction of network precursors by coaxial spinning coupled with liquid nitrogen flash freezing
[0056] Weigh out 4g of polystyrene (weight average molecular weight 350,000) and 20g of... N,N-dimethylformamide and 2g of polymethyl methacrylate monodisperse microsphere solution (diameter 500nm, concentration 25mg / mL) were mixed evenly to form an inner fluid. The spinning slurry obtained in step (1) was used as the outer fluid. Spinning was performed using a microfluidic electrostatic integrated machine with a coaxial spinneret (the injection rate of the inner fluid during spinning was 0.3mL / h, the injection rate of the outer fluid was 0.9mL / h, the voltage was 25kV, and the injection of the inner fluid stopped synchronously after the outer fluid was consumed). At the same time, a stainless steel tray collector (size 30cm×20cm×8cm) was placed directly below the spinning nozzle, and liquid nitrogen was pre-injected into the collector (the height of the liquid nitrogen injection was 4 / 5 of the stainless steel tray collector). Liquid nitrogen was continuously added during the spinning process to maintain the liquid nitrogen height. After spinning, the filamentous ice crystals in the liquid nitrogen were placed in a freeze dryer and freeze-dried at -40℃ for 72h to obtain the network precursor.
[0057] (3) Preparation of catalyst matrix by pyrolysis coupled in-situ steam activation
[0058] The network precursor obtained in step (2) was placed in a tube atmosphere furnace and heated to 450°C and held for 3 hours under nitrogen gas conditions (nitrogen gas rate of 300 mL / min). Then, nitrogen gas (nitrogen gas rate of 300 mL / min) was first introduced into a 90°C constant temperature bubbling water bath to introduce the mixture of nitrogen gas and water vapor into the tube atmosphere furnace, heated to 700°C and held for 4 hours to obtain a porous catalyst matrix.
[0059] (4) Ammonia nitrogen etching to regulate surface sites
[0060] The porous catalyst matrix obtained in step (3) was placed in a dielectric barrier discharge plasma reactor, and a mixture of ammonia and argon was introduced (the rates of ammonia and argon were 15 mL / min and 90 mL / min, respectively). Then, it was discharged (the voltage during the discharge process was 20 kV and the treatment time was 20 min). After the treatment, a porous fiber denitrification catalyst was obtained.
[0061] (5) Catalytic activity test
[0062] Take 0.5 mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8 mm. Fix it with quartz wool and wire mesh. Place the quartz tube in a tube furnace and adjust the temperature of the catalytic reaction by controlling the heating temperature of the tube furnace. The inlet gas components are: NO (500 ppm), NH3 (500 ppm), O2 (10 vol.%), and the remainder is N2. The total gas flow rate is 400 mL / min. The temperature is controlled at 150-270℃, and the temperature is maintained at 30℃ for 30 min. The NO concentration is measured using a flue gas analyzer. The denitrification efficiency of the catalyst is higher than 90% in the temperature range of 180-240℃.
[0063] Comparative Example 1
[0064] (1) Catalyst preparation
[0065] Except for step (1) of catalyst preparation, which does not use the water bath ultrasonic alkaline dissolution step, the other conditions are the same as in Example 1;
[0066] (2) Catalytic activity test
[0067] Take 0.5 mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8 mm. Fix it with quartz wool and wire mesh. Place the quartz tube in a tube furnace and adjust the temperature of the catalytic reaction by controlling the heating temperature of the tube furnace. The inlet gas components are: NO (500 ppm), NH3 (500 ppm), O2 (10 vol.%), and the remainder is N2. The total gas flow rate is 400 mL / min. The temperature is controlled between 150 and 270℃, and the temperature is maintained at 30℃ for 30 min. The NO concentration is measured using a flue gas analyzer. The catalyst denitrification efficiency at 180℃ is 54.1%.
[0068] (3) Comparison effect
[0069] Compared with Example 1, the catalyst preparation step (1) does not use the water bath ultrasonic alkali dissolution step. The fly ash retains the original micron-sized dense particle morphology. Even after plasma treatment and ionic liquid intercalation, it is difficult to effectively peel off its inert skeleton. As a result, the dense glass microsphere structure of fly ash cannot be opened, the dissolution of Si and Al is hindered, the surface hydroxyl density is reduced, which leads to the failure of subsequent plasma and ionic liquid synergistic activation and the decrease in the stability of the sol system. In addition, the metal active components are unevenly dispersed due to the lack of anchoring points. The fiber wall pores are poorly developed and the specific surface area is significantly reduced, which severely restricts the mass transfer of flue gas and ultimately leads to a significant decrease in NO conversion rate.
[0070] Comparative Example 2
[0071] (1) Catalyst preparation
[0072] Except for step (3) of catalyst preparation, in which a mixture of nitrogen and water vapor is directly introduced into a tubular atmosphere furnace, heated to 700°C and held for 4 hours, instead of using two-stage calcination, the other conditions are the same as in Example 2.
[0073] (2) Catalytic activity test
[0074] Take 0.5 mL of 40-60 mesh catalyst and pour it into a quartz tube with an inner diameter of 8 mm. Fix it with quartz wool and wire mesh. Place the quartz tube in a tube furnace and adjust the temperature of the catalytic reaction by controlling the heating temperature of the tube furnace. The inlet gas components are: NO (500 ppm), NH3 (500 ppm), O2 (10 vol.%), and the remainder is N2. The total gas flow rate is 400 mL / min. The temperature is controlled at 150-270℃, and the temperature is maintained at 30℃ for 30 min. The NO concentration is measured using a flue gas analyzer. The denitrification efficiency of the catalyst at 180℃ is 28.6%.
[0075] (3) Comparison effect
[0076] Compared with Example 2, in the catalyst preparation step (3), a mixture of nitrogen and water vapor was directly introduced into a tubular atmosphere furnace, heated to 700°C and held for 4 hours, instead of using two-stage calcination. During the heating process, the organic template agent rapidly pyrolyzes and releases a large amount of gas, causing the fiber wall to rupture due to the sudden increase in internal gas pressure, and the three-dimensional network skeleton to collapse and pulverize. At the same time, the metal precursor decomposes directly at high temperature before forming a stable inorganic skeleton, and the active components are prone to migration, aggregation and sintering. In addition, the simultaneous activation of water vapor and removal of organic matter leads to uneven pore development, a significant decrease in specific surface area and pore volume, and ultimately results in the loss of mechanical strength of the catalyst and a significant decrease in denitrification activity.
Claims
1. A method for preparing a fly ash-based porous fiber denitrification catalyst, characterized in that: The catalyst is prepared as follows: (1) Ionic liquid ball milling synergistic activation to construct spinning sizing agent Fly ash, sodium hydroxide, and deionized water are mixed evenly, then ultrasonically dissolved in a water bath, filtered, washed with water, and dried to obtain modified fly ash powder. The modified fly ash powder and polyvinylpyrrolidone are then mixed evenly and placed in a dielectric barrier discharge plasma reactor, and discharged under argon gas to obtain activated powder. The activated powder, 1-ethyl-3-methylimidazolium diethyl phosphate, and deionized water were mixed and stirred in a constant temperature water bath to obtain a mixed slurry. After centrifugation, the lower layer of sol was retained. Then, the lower layer of sol, nano aluminum sol, citric acid, vanadium salt, tungsten salt, manganese salt, and cerium salt were mixed and stirred in a constant temperature water bath to obtain a composite sol. The composite sol, polyvinyl alcohol, polyether P123, polymethyl methacrylate monodisperse microsphere solution, bacterial cellulose dispersion, deionized water, and anhydrous ethanol were mixed and placed in a planetary ball mill for continuous ball milling. After ball milling, a spinning slurry was obtained. (2) Construction of network precursors by coaxial spinning coupled with liquid nitrogen flash freezing Weigh out polystyrene, N,N-dimethylformamide and polymethyl methacrylate monodisperse microsphere solution and mix them evenly to form an inner fluid. Use the spinning slurry obtained in step (1) as the outer fluid. Use a coaxial spinneret to spin the microfluidic electrostatic osmosis machine. At the same time, place a stainless steel tray collector directly below the spinning nozzle and pre-inject liquid nitrogen into the collector. During the spinning process, continuously add liquid nitrogen to maintain the liquid nitrogen level. After spinning, place the filamentous ice crystals in the liquid nitrogen in a freeze dryer and freeze dry to obtain the network precursor. (3) Preparation of catalyst matrix by pyrolysis coupled in-situ steam activation The network precursor obtained in step (2) is placed in a tube atmosphere furnace, heated to 350-450°C and held for 3-4 hours under nitrogen gas conditions, and then nitrogen gas is first introduced into a constant temperature bubbling water bath so that the mixture of nitrogen gas and water vapor is introduced into the tube atmosphere furnace, heated to 600-700°C and held for 4-8 hours to obtain a porous catalyst matrix; (4) Ammonia nitrogen etching to regulate surface sites The porous catalyst matrix obtained in step (3) is placed in a dielectric barrier discharge plasma reactor, a mixture of ammonia and argon is introduced, and then discharged. After the discharge is completed, a porous fiber denitrification catalyst is obtained.
2. The preparation method according to claim 1, characterized in that: The mass ratio of fly ash, sodium hydroxide, and deionized water in step (1) is 1:(3~5):(10~20); the temperature of ultrasonic alkaline dissolution in water bath is 70~90℃, the power of ultrasonic alkaline dissolution in water bath is 500~700W, and the time of ultrasonic alkaline dissolution in water bath is 2~4h. The drying temperature was 80~100℃ and the drying time was 6~12h. The mass ratio of modified fly ash powder to polyvinylpyrrolidone is 1:(0.2~0.4). The argon gas introduction rate is 60~80mL / min, the discharge treatment power is 200~300W, and the discharge treatment time is 30~60min.
3. The preparation method according to claim 1, characterized in that: The nano-aluminum sol used in step (1) is model JR14W, purchased from Xuancheng Jingrui New Materials Co., Ltd. The vanadium salt is ammonium metavanadate, the tungsten salt is ammonium metatungstate, the manganese salt is manganese nitrate hexahydrate or manganese chloride, and the cerium salt is cerium nitrate hexahydrate or cerium chloride. The mass ratio of activated powder, 1-ethyl-3-methylimidazolium diethyl phosphate, and deionized water is 1:(0.4~0.6):(2~4); the mass ratio of lower sol, nano-aluminum sol, citric acid, vanadium salt, tungsten salt, manganese salt, and cerium salt is 1:(0.1~0.15):(0.06~0.12):(0.02~0.04):(0.04~0.06):(0.04~0.06):(0.03~0.05). The temperature of the constant temperature water bath for stirring is 60~80℃, and the stirring time is 2~4h.
4. The preparation method according to claim 1, characterized in that: The polyvinyl alcohol mentioned in step (1) has a weight-average molecular weight of 13,000 to 50,000, the polymethyl methacrylate monodisperse microspheres have a diameter of 1 to 2 μm, the concentration of the polymethyl methacrylate monodisperse microsphere solution is 25 mg / mL, and the content of the bacterial cellulose dispersion is 2.5% to 5%. The mass ratio of the composite sol, polyvinyl alcohol, polyether P123, polymethyl methacrylate monodisperse microsphere solution, bacterial cellulose dispersion, deionized water, and anhydrous ethanol was 1:(0.02~0.04):(0.01~0.03):(0.03~0.06):(0.05~0.1):(0.3~0.6):(0.3~0.6). The ball milling speed was 300~500 rpm, and the ball milling time was 3~6 h.
5. The preparation method according to claim 1, characterized in that: The polystyrene mentioned in step (2) has a weight-average molecular weight of 280,000 to 350,000, the polymethyl methacrylate monodisperse microspheres have a diameter of 300 to 500 nm, the polymethyl methacrylate monodisperse microsphere solution has a concentration of 25 mg / mL, and the mass ratio of N,N-dimethylformamide, polystyrene, and polymethyl methacrylate monodisperse microsphere solution is 1:(0.1 to 0.2):(0.05 to 0.1).
6. The preparation method according to claim 1, characterized in that: In step (2), the injection rate of the inner fluid during the spinning process is 0.2~0.3 mL / h, the injection rate of the outer fluid is 0.6~0.9 mL / h, the voltage is 15~25 kV, the height of the injected liquid nitrogen is 1 / 2~4 / 5 of the collector, the freeze-drying temperature is -50~-40℃, and the freeze-drying time is 36~72 h.
7. The preparation method according to claim 1, characterized in that: The nitrogen gas introduction rate in step (3) is 200~300mL / min, and the temperature of the constant temperature bubbling water bath is 80~90℃.
8. The preparation method according to claim 1, characterized in that: In step (4), the rates of ammonia and argon gas introduced are 10-15 mL / min and 90-140 mL / min, respectively. The voltage during the discharge process is 15-20 kV, and the processing time is 20-40 min.
9. A fly ash-based porous fiber denitrification catalyst, characterized in that, The catalyst was prepared by the method described in any one of claims 1 to 8.
10. The application of the catalyst prepared by the method of claim 1 in low-temperature denitrification, wherein the denitrification is preferably selective catalytic reduction of nitrogen oxides.