Fine grinding and activation method of a gasification slag environmental governance repair material
By adding tannic acid and dicyandiamide to the fine coal gasification slag and calcining it under a nitrogen atmosphere, a structure is formed in which iron is combined with nitrogen-containing sites, which solves the problem of unstable internal iron binding in the fine coal gasification slag and improves the stability of catalytic activity.
Patent Information
- Application Number
- CN202611654126.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the bonding state between endogenous iron and the matrix in coal gasification fine slag is unstable, which leads to the attenuation of catalytic activity during repeated use due to the migration or dissolution of iron species.
By mixing coal gasification slag with tannic acid and dicyandiamide in water and then calcining it under a nitrogen atmosphere, a local structure is formed in which iron is combined with nitrogen-containing sites, thus fixing the endogenous iron and reducing its migration and dissolution during use.
It improves the catalytic activity and stability of the coal gasification fine slag environmental remediation material, reduces the migration and dissolution of iron species, and maintains the long-term reactivity of the material.
Smart Images

Figure CN123148983A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gasification slag resource utilization and iron-containing catalytic material preparation technology, and discloses a fine grinding and activation method for gasification slag environmental remediation materials. Background Technology
[0002] Coal gasification slag contains residual carbon, silica-alumina minerals, and iron-containing components, which can be used as raw materials for catalytic materials in water pollution control. The residual carbon and mineral components form a composite matrix, while the iron-containing components participate in oxidant activation. CN119793461A employs high-energy ball milling to refine particles through the impact and shearing of the grinding media, breaking down some of the silica-alumina minerals' encapsulation of the iron components. Tannic acid is then added for complexation, causing the endogenous iron to migrate and redistribute. The mixture is dried and calcined to obtain an iron-containing carbon-mineral composite material. In use, it is added together with persulfate to water containing phenolic pollutants to activate the oxidant, generate reactive species, and degrade the pollutants. After the reaction, the solid is separated and recovered. This route utilizes the iron and residual carbon within the slag itself to connect particle dissociation, iron species migration, and composite material preparation.
[0003] The above treatments can alter the exposure and distribution of iron-containing components, but the new surface formed by fine grinding and the pre-complex structure formed by tannic acid do not directly determine the bonding state between iron and the surrounding matrix after calcination. When tannic acid decomposes thermally, iron species also undergo migration and phase transformation, and some iron may form weakly bonded surface particles. After repeated contact with oxidants and polluted water, this portion of iron may dissolve from the solid surface or re-migrate and aggregate, causing changes in the number and distribution of the original active sites. Therefore, there is still a difference between the initial reactivity resulting from particle exposure and pre-complexation and the bonding state after thermal transformation and the stability during continuous use.
[0004] Even if a material exhibits some pollutant degradation capability in the initial reaction, its activity may decline during subsequent use. Current approaches link fine grinding, iron species distribution adjustment, and heat treatment, but the stability of the bond between iron and the surrounding matrix after heat treatment remains a challenge. The technical dilemma lies in the fact that exposure of active components facilitates contact with reactants, while weakly bonded surface iron is prone to migration and dissolution during use, affecting the retention of active sites. Therefore, the required technical improvement is to strengthen the bond between endogenous iron and the matrix during the fine grinding and heat treatment process to form the composite material. This would allow the iron species to maintain a relatively stable solid-phase distribution under continuous reaction and repeated use conditions, and preserve the conditions for its participation in surface catalytic reactions. Summary of the Invention
[0005] To address the problem that the bonding state between endogenous iron and the matrix in existing coal gasification fine slag is unstable, and that catalytic activity may decrease during repeated use due to iron species migration or dissolution, this invention provides a fine grinding and activation method for gasification slag environmental remediation materials. By combining tannic acid, dicyandiamide, and coal gasification fine slag, and calcining under a nitrogen atmosphere, the fixation state of endogenous iron in the resulting remediation material is improved.
[0006] The term "gasification slag" as used in this application specifically refers to the fine slag-like solid byproduct produced during the coal gasification process, which contains residual carbon, silicon-aluminum minerals, and endogenous iron. It refers to the same applicable raw material as "coal gasification fine slag" in the text. Its scope of application is further limited by the following raw material selection conditions.
[0007] To address the aforementioned technical problems, this invention provides a fine grinding and activation method for a gasification slag environmental remediation material. The method involves ball milling coal gasification slag containing residual carbon and endogenous iron, then mixing it with tannic acid and dicyandiamide in water. The resulting mixture is dried and calcined under a nitrogen atmosphere to obtain the remediation material. Based on the total dry basis mass of all solid raw materials before calcination, the tannic acid comprises 8-12%, and the dicyandiamide comprises 8-14%. The total dry basis mass is the sum of the masses of all solid raw materials before calcination after deducting free water; water used during the mixing process is not included in the total dry basis mass. The mass percentages represent the raw material input ratio and do not directly represent the composition ratio of the remediation material obtained after calcination.
[0008] In practice, ball milling refines the coal gasification slag through the impact and shearing of the grinding media, exposing some of the iron-containing components encapsulated by minerals. The ball-milled coal gasification slag then contacts tannic acid and dicyandiamide in water. The oxygen-containing groups of tannic acid can coordinate with exposed or migrating iron species, while dicyandiamide is distributed between the coal gasification slag particles and on their surface during the mixing process. After drying, tannic acid, dicyandiamide, and the coal gasification slag together enter the roasting process. Tannic acid participates in carbon structure formation, and dicyandiamide provides nitrogen-containing precursors. The residual carbon and the carbon components formed by thermal conversion together constitute the matrix surrounding the iron-containing components, which is conducive to the formation of local structures where iron and nitrogen-containing sites are combined. A nitrogen atmosphere limits the impact of air oxidation on the residual carbon and the thermal conversion process. When the resulting remediation material comes into contact with polluted water, the iron-containing components fixed in the matrix participate in surface catalytic reactions, which is expected to reduce the activity decay caused by iron detachment from the solid phase. The specific binding form of the iron phase and nitrogen-containing sites depends on the actual thermal conversion process and is not determined solely by the feed ratio.
[0009] Furthermore, in the above technical solution, the solid raw material is composed of the coal gasification fine slag, the tannic acid and the dicyandiamide, with the coal gasification fine slag being the remainder, and the total mass percentage of the three is 100%.
[0010] In practical implementation, this scheme uses coal gasification fine slag to simultaneously provide residual carbon, mineral components, and endogenous iron. Tannic acid and dicyandiamide participate in the coordination of iron species and the formation of nitrogen-containing carbon structures, respectively. During batching, the mass percentages of tannic acid and dicyandiamide are first determined within the specified range, and then the coal gasification fine slag is used to bring the total to 100%. The combined ratio of tannic acid and dicyandiamide is 16-26%, and the corresponding proportion of coal gasification fine slag is 84-74%. These values are interrelated to avoid adding coal gasification fine slag at a fixed ratio when the precursor dosage changes, which would cause inconsistencies between the total batch size and the measurement standard.
[0011] Furthermore, in the above technical solution, the mixing includes: dissolving the tannic acid in water, adding the ball-milled coal gasification fine slag to the obtained tannic acid aqueous solution and stirring, then adding the dicyandiamide and continuing to stir.
[0012] In practice, tannic acid is contacted in aqueous solution with the ball-milled coal gasification slag, allowing the dissolved tannic acid to distribute onto the particle surface. Stirring ensures continuous contact between the coal gasification slag and the tannic acid aqueous solution, providing conditions for coordination between the tannic acid and exposed iron-containing components. Dicyandiamide is then added and stirring continues, allowing the dicyandiamide to enter the mixture already containing the coal gasification slag and tannic acid, providing a mixing basis for subsequent co-drying and roasting. This order of addition arranges the contact between tannic acid and the coal gasification slag before the addition of dicyandiamide, and does not require the two precursors to be simultaneously dispersed in a dry powder state.
[0013] Furthermore, in the above technical solution, the calcination and subsequent cooling are both carried out under the nitrogen atmosphere.
[0014] In practice, the dried mixture is heated under a nitrogen atmosphere, where tannic acid and dicyandiamide undergo thermal conversion, and residual carbon and iron-containing components in the coal gasification slag undergo roasting. The nitrogen atmosphere limits the consumption of carbon components by oxygen in the air and reduces interference from the oxidizing atmosphere on the conversion state of iron-containing components. After roasting, cooling continues under a nitrogen atmosphere to reduce further oxidation that occurs when high-temperature materials are in direct contact with air, ensuring that the cooling process uses the same atmospheric conditions as the roasting process.
[0015] Furthermore, in the above technical solution, the solid raw material also includes conductive carbon black added to the mixture before drying; based on the total dry weight, the dicyandiamide is 8-10%, the conductive carbon black is 2-4%, and the two together are 12%. This solution is another component solution that adds conductive carbon black to the overall technical solution, and is not applicable in combination with the aforementioned three-component solution consisting only of coal gasification fine slag, tannic acid, and dicyandiamide.
[0016] In practice, conductive carbon black is added to the mixture before drying, and undergoes drying and calcination together with coal gasification slag, tannic acid, and dicyandiamide. This allows the conductive carbon black to distribute between particles and form contact with the carbon components in the material. Dicyandiamide continues to provide nitrogen-containing precursors, while conductive carbon black replenishes the conductive carbon components. These two components respectively correspond to the binding of iron to nitrogen-containing sites and electron transfer between particles. The values of dicyandiamide and conductive carbon black are linked: as the proportion of conductive carbon black increases, the proportion of dicyandiamide decreases accordingly, and the two always total 12% to limit the substitution relationship between the nitrogen-containing precursor and the conductive carbon components.
[0017] Furthermore, in the above technical solution, the dry basis mass percentage of the solid raw materials in the aforementioned three-component composition scheme is: 78% of the coal gasification fine slag, 10% of the tannic acid, and 12% of the dicyandiamide.
[0018] In its specific implementation, the formula fixes the input ratio of coal gasification fine slag at 78% to provide residual carbon, mineral components, and endogenous iron; tannic acid and dicyandiamide are added at 10% and 12% respectively, followed by mixing, drying, and calcination according to the overall technical plan. The total of these three components is 100%, ensuring that the amounts of tannic acid and dicyandiamide are determined relative to the total dry weight. This ratio defines the input relationship between the two precursors and the coal gasification fine slag during co-thermal conversion, and does not equate the amount of precursors input with the carbon and nitrogen retention in the finished product.
[0019] Furthermore, in the above technical solution, the dicyandiamide is added in the form of an aqueous solution in the aforementioned mixing scheme with a defined addition order; the mixture is not subjected to solid-liquid separation before drying, and the drying is the overall evaporation of the mixture to remove water.
[0020] In practice, dicyandiamide is added in the form of an aqueous solution to a mixture already containing coal gasification slag and tannic acid, and distributed in the liquid phase and around the particles with stirring. The mixture is then evaporated to remove water, allowing the solid particles and dissolved or dispersed non-volatile substances in the liquid phase to enter the dried product together. No solid-liquid separation is performed before drying to avoid carrying away dicyandiamide, tannic acid, and iron species that have migrated into the liquid phase during discharge, allowing these components to enter the subsequent roasting process together.
[0021] Furthermore, in the above technical solution, the roasting temperature in the aforementioned scheme of roasting and cooling in a nitrogen atmosphere is 800°C, and the cooling after roasting is to cool to room temperature in the furnace under the nitrogen atmosphere.
[0022] In practice, the dried mixture is calcined at 800°C under a nitrogen atmosphere. Tannic acid, dicyandiamide, and relevant components from the coal gasification slag undergo thermal transformation under the same temperature conditions, providing conditions for the co-formation of nitrogen-containing carbon structures and iron-containing components. After calcination, the material is kept under a nitrogen atmosphere and cooled to room temperature as the furnace temperature decreases, reducing air contact caused by material transfer during the high-temperature stage. The stated temperature refers to specific calcination conditions and does not imply that the resulting repair material necessarily possesses a particular iron phase or a specific iron-nitrogen coordination structure.
[0023] Furthermore, in the above technical solution, the solid raw material in the aforementioned composition scheme containing conductive carbon black is composed of the coal gasification fine slag, the tannic acid, the dicyandiamide and the conductive carbon black; based on the total dry weight, the tannic acid is 10% and the coal gasification fine slag is 78%.
[0024] In practice, the coal gasification slag and tannic acid together account for 88%, while the remaining 12% is composed of dicyandiamide and conductive carbon black. When dicyandiamide is in the range of 8-10%, the conductive carbon black is in the corresponding range of 4-2%, with the four solid raw materials totaling 100%. When using the same batch of coal gasification slag, this compositional relationship maintains a constant input of coal gasification slag and tannic acid, ensuring that the source of endogenous iron and the amount of tannic acid do not change with the substitution of dicyandiamide and conductive carbon black. The compositional adjustment is concentrated between the nitrogen-containing precursor and the conductive carbon component.
[0025] Furthermore, in the above technical solution, the dry basis mass percentage of the solid raw materials in the aforementioned four-component composition scheme is as follows: 78% of the coal gasification fine slag, 10% of the tannic acid, 9% of the dicyandiamide, and 3% of the conductive carbon black.
[0026] In practice, this formulation fixes the total ratio of dicyandiamide and conductive carbon black at 12%, with the four solid raw materials totaling 100%. Compared to the aforementioned three-component formulation, the ratio of coal gasification slag and tannic acid remains unchanged, while dicyandiamide is adjusted from 12% to 9%, and 3% conductive carbon black is added accordingly. After co-drying and calcining, the mixture allows dicyandiamide to participate in the formation of nitrogen-containing structures, and conductive carbon black to participate in the contact between carbon components. This is expected to supplement electron transport pathways while retaining the nitrogen-containing precursor, thus ensuring that the fixation of endogenous iron and its participation in surface catalytic reactions are mutually compatible.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Adding dicyandiamide to the feedstock system of coal gasification slag and tannic acid allows for the adjustment of iron species distribution and the formation of nitrogen-containing carbon structures to occur simultaneously during the heat treatment of the same mixture. Tannic acid participates in iron complexation, while dicyandiamide provides nitrogen-containing precursors. Both are dried together with the slag and calcined under a nitrogen atmosphere, which facilitates the formation of local structures where iron and nitrogen-containing sites are combined, providing additional fixation sites for endogenous iron. This is expected to reduce the migration and dissolution of weakly bound iron species during use. The input ratio of tannic acid and dicyandiamide is limited based on the total dry weight of all solid raw materials, ensuring a clear feeding relationship between the two precursors and the slag. The mixture is evaporated as a whole to remove water, preventing the removal of precursors and migrating iron species from the liquid phase during solid-liquid separation before drying. Cooling in nitrogen after calcination reduces the impact of air oxidation during the cooling stage on the state of the resulting iron-containing components.
[0028] 2. Conductive carbon black was added to the dicyandiamide-containing formulation, with the sum of the dry weight percentages of dicyandiamide and conductive carbon black limited to 12%. This ensures that the introduction of the conductive carbon component is accompanied by a partial replacement of the nitrogen source. The conductive carbon black was added to the mixture before drying, undergoing drying and calcination together with the fine slag and precursor. This facilitates increased contact between carbon particles and provides electron transport pathways for the dispersed iron-containing components. In a formulation with 78% fine slag, 10% tannic acid, 9% dicyandiamide, and 3% conductive carbon black, the input amounts of fine slag and tannic acid are consistent with the representative formulation without carbon black, maintaining the same endogenous iron source and complexing component input. This compositional adjustment, while retaining the nitrogen-containing precursor, supplements the conductive carbon component, which is expected to alleviate the impact of limited local electron transport on the catalytic reaction, allowing the fixed iron sites to participate more fully in oxidant activation. Attached Figure Description
[0029] Figure 1 This is a comparison diagram of particle morphology after fine grinding and recycling according to the present invention.
[0030] Figure 2 This is a comparison diagram of the iron local neighbor structure before and after cycling according to the present invention.
[0031] Figure 3 This is a comparison diagram of the nitrogen 1s spectrum in the nitrogen-containing environment of the present invention.
[0032] Figure 4 This is an AC impedance diagram corresponding to the carbon black addition method of the present invention.
[0033] Figure 5 This diagram illustrates the phenol removal process and reuse of the present invention. Detailed Implementation
[0034] In the following examples, unless otherwise stated, the coal gasification slag was derived from the same batch of coal gasification solid by-products containing residual carbon and endogenous iron, dried to constant weight at 105°C, and measured on a dry basis. Tannic acid and dicyandiamide were analytical grade reagents, conductive carbon black was conductive grade powder, water was deionized water, and nitrogen purity was 99.999%. Phenol used in the tests was analytical grade reagent, persulfate was a composite salt containing potassium persulfate and measured as effective persulfate, methanol and acetonitrile were chromatographic grade, and nitric acid and iron standard solution were used for iron content detection. The preparation process used a ball mill, stirring device, evaporation drying device, and tube furnace. The resulting dry powder was stored in a sealed container, and independent samples were used for three parallel tests for quantitative analysis. Spectroscopic and morphological analysis were performed according to the test instructions for each item. All solid feed ratios were calculated based on the total dry weight of the raw materials before calcination; mixed water was not included, and the finished product quality was determined by weighing the cooled dry powder.
[0035] The gasification slag used in this method is selected according to the following conditions: based on the mass of the gasification slag after drying to constant weight at 105℃, the dry basis fixed carbon content is 20-35%, the dry basis ash content is 60-75%; the total iron content is 5-10% based on Fe2O3, the silicon content is 25-40% based on SiO2, and the aluminum content is 10-20% based on Al2O3. The above parameters are used to limit the raw materials entering the preparation process, distinguishing them from the formulation percentages of coal gasification fine slag, tannic acid, dicyandiamide, and conductive carbon black relative to the total solid feed.
[0036] Fixed carbon and ash content are determined according to industrial analysis methods. The total mass percentage of fixed carbon, ash, and volatile matter on a dry basis is 100%, and the values of each indicator should be consistent with each other. Fixed carbon is not directly replaced by loss on ignition or total carbon in elemental analysis. Silicon, aluminum, and iron can be determined by calibrated X-ray fluorescence spectrometry. When using ash samples and normalizing their oxide content to 100% for reporting, the content must be multiplied by the dry basis ash mass fraction of the original gasification slag, converted to the original dry slag benchmark, and compared with the above range. Total iron can also be determined after the sample is completely decomposed and converted according to w(Fe2O3 equivalent) = w(Fe) × M(Fe2O3) / [2M(Fe)]. Total iron, calculated as Fe, is approximately 0.6994 times the Fe2O3 equivalent.
[0037] The silica-aluminate inorganic components in the raw materials may include aluminosilicate glass phases and crystalline phases such as quartz, feldspar, and pyroxene; endogenous iron refers to iron-containing components inherent in the raw materials, combined with or encapsulated by their inorganic framework. Mineral composition and crystalline iron-containing phases are identified using X-ray diffraction combined with scanning electron microscopy and energy dispersive spectroscopy. The equivalent amount of oxides is not equated to the phase content of the corresponding free oxides, nor is the total iron content used to infer a single iron phase. Iron-containing phases appearing after calcination are not inferred to be the same phase already present in the raw materials.
[0038] Example 1: This example is a preferred embodiment of a fine grinding and activation method for a gasification slag environmental remediation material.
[0039] Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 9.000g dicyandiamide and 3.000g conductive carbon black, with a total dry weight of 100.000g; 1000.00mL of water for mixing.
[0040] Preparation process: S1. Weigh 78.000g of dry coal gasification fine slag, and use zirconium oxide grinding media to dry ball mill for 120min at a ball-to-material mass ratio of 10:1 and 400r / min. Recover all 78.000g of ball-milled fine slag as solid input for S2.
[0041] S2. Dissolve 10.000g of tannic acid in 800.00mL of deionized water, add all the ball milled residue from S1 at 25℃, stir at 500r / min for 60min to obtain a complex suspension containing 88.000g of dry solids, and send it all to S3; in this step, the liquid phase is not discharged and the pH of the suspension is not adjusted.
[0042] S3. Dissolve 9.000g of dicyandiamide in 200.00mL of deionized water at 60℃, add all the complexed suspension from S2, then add 3.000g of conductive carbon black, and continue stirring at 60℃ and 500r / min for 60min to obtain a total mixture containing 100.000g of dry solids and 1000.00mL of mixed water, and send it all to S4.
[0043] S4. The entire mixture of S3 is evaporated at 80℃ for 240 min to remove water, and then dried at 105℃ for 120 min to constant weight. 100.000 g of dried precursor is collected. No solid-liquid separation is performed before drying. The non-volatile precursor and iron species in the liquid phase are retained together with the solid and sent to S5.
[0044] S5. All the dried precursors from S4 are loaded into a tube furnace and purged with nitrogen at 200 mL / min for 30 min. The temperature is increased from 25°C to 800°C at 5°C / min, and calcined at 800°C for 120 min. The volatile components are discharged with the tail gas, while all the calcined solids are retained and then directly enter S6 without solids separation.
[0045] S6. Continue to purge with nitrogen at 200 mL / min, cool with the furnace for 300 min to 25°C, collect 81.748 g of repair material, lightly grind and store in a sealed container; the mass difference from 100.000 g of dried precursor to this dry powder is the component that leaves the solid phase during thermal conversion.
[0046] Example 2: The difference between this example and Example 1 is as follows: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 12.000g dicyandiamide, total dry weight 100.000g; the grade of other raw materials and the amount of water used are as described in Example 1.
[0047] Preparation process: S1, referring to S1 of Example 1, all 78.000g of the coal gasification fine slag in this example are ball-milled and recovered, and then sent to S2.
[0048] S2, referring to S2 of Example 1, dissolve 10.000g of tannic acid in 800.00mL of water and mix it with the fine residue obtained in S1 of this example; 88.000g of dry solids in this step are sent to S3 in full.
[0049] S3, referring to S3 of Example 1, dissolve 12.000g of dicyandiamide in 200.00mL of water and then add the suspension obtained in S2 of this example. No conductive carbon black is added in this example; the total mixture contains 100.000g of dry solids, and the stirring conditions remain unchanged.
[0050] S4-S6, referring sequentially to S4, S5 and S6 of Example 1, 100.000g of the dried precursor obtained by total evaporation was treated under the same nitrogen, heating, heat preservation and furnace cooling conditions; in this example, 79.176g of repair material was finally collected.
[0051] Example 3: The difference between this example and Example 1 is as follows: Formula: 84.000g coal gasification fine slag, 8.000g tannic acid, 8.000g dicyandiamide, total dry weight 100.000g; the grade of other raw materials and the amount of water used are as described in Example 1.
[0052] Preparation process: S1, referring to S1 of Example 1, all 84.000g of the coal gasification fine slag in this example are ball-milled and recovered, and sent to S2.
[0053] S2. Referring to S2 of Example 1, 8.000g of tannic acid in this example is dissolved in 800.00mL of water and mixed with the fine residue obtained in S1 of this example; 92.000g of dry solids in this step are sent to S3 in full.
[0054] S3, referring to S3 of Example 1, dissolve 8.000g of dicyandiamide in 200.00mL of water and then add the suspension obtained in S2 of this example. No conductive carbon black is added in this example; the total mixture contains 100.000g of dry solids, and the stirring conditions remain unchanged.
[0055] S4-S6, referring sequentially to S4, S5 and S6 of Example 1, 100.000g of the dried precursor obtained by total evaporation was treated under the same nitrogen, heating, heat preservation and furnace cooling conditions; in this example, 83.556g of repair material was finally collected.
[0056] Example 4: The difference between this example and Example 1 is as follows: Formula: 74.000g coal gasification fine slag, 12.000g tannic acid, 14.000g dicyandiamide, total dry weight 100.000g; the grade of other raw materials and the amount of water used are as described in Example 1.
[0057] Preparation process: S1, referring to S1 of Example 1, all 74.000g of the coal gasification fine slag in this example are ball-milled and recovered, and sent to S2.
[0058] S2. Referring to S2 of Example 1, 12.000g of tannic acid in this example is dissolved in 800.00mL of water and mixed with the fine residue obtained in S1 of this example; 86.000g of dry solids in this step are sent to S3 in full.
[0059] S3, referring to S3 of Example 1, dissolve 14.000g of dicyandiamide in 200.00mL of water and then add the suspension obtained in S2 of this example. No conductive carbon black is added in this example; the total mixture contains 100.000g of dry solids, and the stirring conditions remain unchanged.
[0060] S4-S6, referring sequentially to S4, S5 and S6 of Example 1, 100.000g of the dried precursor obtained by total evaporation was treated under the same nitrogen, heating, heat preservation and furnace cooling conditions; in this example, 76.661g of repair material was finally collected.
[0061] Example 5: The difference between this example and Example 1 is as follows: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 10.000g dicyandiamide, 2.000g conductive carbon black, total dry weight 100.000g; the grade of other raw materials and the amount of water are as described in Example 1.
[0062] Preparation process: S1, referring to S1 of Example 1, all 78.000g of the coal gasification fine slag in this example are ball-milled and recovered, and then sent to S2.
[0063] S2, referring to S2 of Example 1, dissolve 10.000g of tannic acid in 800.00mL of water and mix it with the fine residue obtained in S1 of this example; 88.000g of dry solids in this step are sent to S3 in full.
[0064] S3. Referring to S3 of Example 1, 10.000g of dicyandiamide in this example was dissolved in 200.00mL of water and then the suspension obtained in S2 of this example was added, followed by 2.000g of conductive carbon black; the total mixture contained 100.000g of dry solids, and the stirring conditions remained unchanged.
[0065] S4-S6, referring to S4, S5 and S6 of Example 1 in sequence, 100.000g of the dried precursor obtained by total evaporation was treated under the same nitrogen, heating, heat preservation and furnace cooling conditions; in this example, 80.929g of repair material was finally collected.
[0066] Example 6: The difference between this example and Example 1 is as follows: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 8.000g dicyandiamide, 4.000g conductive carbon black, total dry weight 100.000g; the grade of other raw materials and the amount of water are as described in Example 1.
[0067] Preparation process: S1, referring to S1 of Example 1, all 78.000g of the coal gasification fine slag in this example are ball-milled and recovered, and then sent to S2.
[0068] S2, referring to S2 of Example 1, dissolve 10.000g of tannic acid in 800.00mL of water and mix it with the fine residue obtained in S1 of this example; 88.000g of dry solids in this step are sent to S3 in full.
[0069] S3. Referring to S3 of Example 1, 8.000g of dicyandiamide in this example was dissolved in 200.00mL of water and then the suspension obtained in S2 of this example was added, followed by 4.000g of conductive carbon black; the total mixture contained 100.000g of dry solids, and the stirring conditions remained unchanged.
[0070] S4-S6, referring sequentially to S4, S5 and S6 of Example 1, 100.000g of the dried precursor obtained by total evaporation was treated under the same nitrogen, heating, heat preservation and furnace cooling conditions; in this example, 82.472g of repair material was finally collected.
[0071] Comparative Example 1: The difference between this comparative example and Example 1 is that: Formula: 78.000g of coal gasification fine slag, 10.000g of tannic acid, total dry weight 88.000g; no dicyandiamide or conductive carbon black added.
[0072] Preparation process: S1-S2, referencing S1 and S2 of Example 1, keep the absolute feed amounts of coal gasification slag and tannic acid and their contact conditions unchanged.
[0073] S3. Add 200.00 mL of deionized water to the suspension containing 88.000 g of dry solids obtained in S2 of this example, without adding dicyandiamide and conductive carbon black; stir at the temperature, speed and time of Example 1, and feed the entire volume into S4.
[0074] S4-S6, following the corresponding steps of Example 1, 88.000g of the dried precursor was collected by total evaporation, and then calcined and cooled according to the same nitrogen program to obtain 77.027g of repair material. This comparative example is used for baseline comparison of existing routes that simultaneously remove nitrogen-containing precursors and conductive carbon black; when compared with Example 2, the difference is concentrated in the introduction of dicyandiamide.
[0075] Comparative Example 2: The difference between this comparative example and Example 1 is that: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 9.000g dicyandiamide and 3.000g conductive carbon black, total dry weight 100.000g.
[0076] Preparation process: S1-S2, referring to S1 and S2 of Example 1.
[0077] S3. Following the method described in Example 1, dicyandiamide aqueous solution is added, but conductive carbon black is not added at this time, resulting in a mixture containing 97.000g of dry solids and 1000.00mL of water, which is then fed into S4 in its entirety.
[0078] S4-S5, following the corresponding processing conditions of Example 1, 97.000g of dried precursor was obtained by total evaporation and then completely calcined with nitrogen.
[0079] S6. After cooling the furnace under nitrogen conditions as in Example 1, 78.691g of the calcined product was collected first, and then 3.000g of conductive carbon black was added and lightly ground and mixed to finally obtain 81.691g of material. This comparative example only changed the timing of carbon black addition; the carbon black did not undergo drying and calcination together with the precursor.
[0080] Comparative Example 3: The difference between this comparative example and Example 1 is that: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 9.000g dicyandiamide and 3.000g conductive carbon black, total dry weight 100.000g.
[0081] Preparation process: S1-S5, referencing all the corresponding raw materials, quantities, and steps of Example 1.
[0082] S6. After calcination, nitrogen flow was stopped, and the furnace was cooled to 25°C in air atmosphere for 300 minutes. 81.714g of repair material was collected. The remaining post-treatment followed S6 of Example 1. This comparative example only cut off the nitrogen cooling condition after calcination.
[0083] Comparative Example 4: The difference between this comparative example and Example 1 is that: Formula: 78.000g coal gasification fine slag, 10.000g tannic acid, 9.000g dicyandiamide and 3.000g conductive carbon black, total dry weight 100.000g.
[0084] Preparation process: S1. Weigh 78.000g of dry coal gasification fine slag, do not ball mill it, and send all the un-ball milled fine slag directly into S2.
[0085] S2-S6, except that the un-ball-milled fine slag obtained in S1 of this example was used instead of the ball-milled fine slag, all the corresponding steps, raw materials, amounts and conditions of Example 1 were used, and 81.651g of repair material was finally collected. This comparative example only cuts off the pretreatment of particle refinement and exposure of iron-containing components.
[0086] Test method: Phenol removal rate: For each 0.200g sample, 100.00mL of a 20.00mg / L phenol aqueous solution was added. The reaction was initiated with 0.100mmol of effective persulfate at 25℃, initial pH 7.00, and consistent stirring conditions. Reaction solutions were collected at 0, 10, 20, and 30 min. The catalyst was first removed using a 0.22μm membrane, and then 1.00mL of the filtrate was mixed with 1.00mL of methanol to terminate the reaction. The concentration dilution factor was 2. Phenol was determined by HPLC using a reversed-phase C18 column, a mobile phase of water to acetonitrile (65:35), a flow rate of 1.0mL / min, a column temperature of 30℃, a detection wavelength of 270nm, an injection volume of 10μL, and sampling intervals of 0-4 min. The retention time of phenol was approximately 2.64 min, with an integration interval of 2.18–3.30 min. Local baselines were determined by signals at 2.00–2.12 min and 3.35–3.50 min. Using a 100 mg / L phenol standard stock solution, 0, 0.02, 0.10, 0.50, 2.00, 5.00, 10.00, and 12.00 mL of stock solution were measured in 100 mL volumetric flasks and diluted to volume, forming a series of 0, 0.02, 0.10, 0.50, 2.00, 5.00, 10.00, and 12.00 mg / L concentrations. Each series was injected three times. A linear regression was performed between peak area (mAU·min) and concentration. The original reaction solution concentration was calculated as (peak area – intercept) ÷ slope × 2, and the removal rate was calculated as (initial concentration – 30 min concentration) ÷ initial concentration × 100%. Each sample was replicated in triplicate. The conclusion only applies to the disappearance of phenol and does not equate the removal rate with the total organic carbon mineralization rate.
[0087] Cyclic activity retention rate: The above phenol removal method was used for 5 consecutive cycles. After each 30-minute cycle, all catalytic solids were separated and recovered. The solution was washed with water and re-introduced into 100.00 mL of freshly prepared phenol solution from the same batch. The same amount of oxidant was added, but no additional catalytic material was added. The initial concentration was the same as the HPLC value at 0 min of the same batch solution. The concentration was recorded after 30 min of each cycle. The recovery and recycling were carried out independently for 3 groups. Cyclic activity retention rate = phenol removal rate of the 5th cycle ÷ phenol removal rate of the 1st cycle × 100%. The average of the calculations for each group was taken; the unit is %, which compares the degree of retention of the removal rate.
[0088] Iron dissolution concentration: Liquid phase from each cycle for 30 min was filtered through a 0.22 μm membrane. 5.00 mL of the filtrate was added to 1.00 mL of 10% (v / v) nitric acid solution, and then diluted to 10.00 mL with water. Iron signals were read at 238.204 nm using ICP. A 1.000 mg / L iron working solution was used as the standard. 0, 0.50, 2.00, 5.00, 10.00, 20.00, 50.00, and 100.00 mL of the working solution were measured in 100 mL volumetric flasks to obtain standards of 0, 0.005, 0.020, 0.050, 0.100, 0.200, 0.500, and 1.000 mg / L, with three signals for each level. The standard and the sample use the same acidity. The concentration is linearly calibrated according to the signal (count / s). The iron concentration in the reaction solution = (sample signal - intercept) ÷ slope × 2. The result unit is mg / L. The result table lists the value of the first cycle. The average of 3 parallel samples is taken. The standard range covers all treated samples.
[0089] Charge transfer resistance: 5.000 mg of material was dispersed in an equal volume mixture of 0.50 mL of water and ethanol. Using 0.1% perfluorosulfonic acid resin as a film-forming aid, 2.00 μL of the dispersion was deposited onto a glassy carbon electrode with an effective area of 0.071 cm², along with 20 μg of the same dry-based material. The electrode was then dried at room temperature. Using a platinum counter electrode and an Ag / AgCl reference electrode, an AC perturbation of 5 mV was applied at the open-circuit potential in 0.1 mol / L Na₂SO₄. 81 points were collected at logarithmic intervals from 100,000 Hz to 0.1 Hz. An equivalent circuit was constructed using the solution resistance, charge transfer resistance, and capacitance in parallel. The semicircle diameter was fitted using the real and imaginary impedances. The unit of charge transfer resistance is Ω. The average value was calculated after fitting the values for three independent film-forming electrodes. With consistent electrode materials and film-forming conditions, this value was only used for electron transfer comparison within the same test system.
[0090] Local coordination: Freshly prepared material and the dried solid after the 5th cycle were used. Iron K-edge absorption spectra were recorded for the 7050-7700 eV incident and fluorescence channels, with a 0.5 eV interval between 7112-7160 eV and a 2 eV interval for the remaining intervals. Energy alignment was performed with reference to the 7112 eV iron K-edge. Absorption spectra were extracted from the ratio of fluorescence to incident signal, and the background at the leading edge and the background of smoothing edge transitions were subtracted. The wavelengths were then analyzed in the range of 2.5-12 Å. - ¹The range was squared and weighted, and Fourier transform was performed using a Hanning window. The relative changes in the contributions of the first light element's nearest neighbor shell and the more distant iron nearest neighbor were interpreted. Radial coordinates were not phase-corrected and were not directly used as bond lengths. Additionally, the nitrogen 1s spectrum was read using XPS with binding energies of 409-391 eV and a step size of 0.1 eV. The same energy calibration and counting scale were used to interpret the nitrogen-containing signal in the 398-402 eV region. Both characterizations support the presence of a nitrogen-containing environment and localized iron nearest neighbor variations. Light element scattering cannot independently distinguish between nitrogen and oxygen, and therefore, a unique coordination number, single-atom structure, or iron phase is not assigned based on this. The results are classified qualitatively.
[0091] Particle morphology: SEM was used to observe the freshly prepared material and the material after the 5th cycle in the same dry state. A 5μm scale and the same magnification scale were used. Three dispersed fields of view were selected for each state. Qualitative judgment was made based on whether the particles were refined, whether the pore outline was preserved, and whether local coarse aggregates appeared. Figure 1 The top row shows the fresh state of Example 1 and Comparative Example 4, and the bottom row shows the state of Example 1 and Comparative Example 1 after the 5th cycle, corresponding to the ball milling pretreatment and nitrogen-containing precursor intervention, respectively; the images are not used to determine iron-nitrogen chemical bonds or the only iron phase.
[0092] The test results are shown in Table 1.
[0093] Table 1 Performance test results of each embodiment and comparative example
[0094] Results analysis: Depend on Figure 1 It can be seen that the newly prepared material in Example 1 of the upper row is a finer, irregular porous particle, while the unmilled material in Comparative Example 4 retains coarser angular fragments; Example 1 of the lower row still maintains the pore outline after 5 cycles, while Comparative Example 1 shows coarser local aggregation when dicyandiamide is lacking.
[0095] Depend on Figure 2 As can be seen, the left figure shows the newly prepared material, and the right figure shows the material after 5 cycles. Examples 1 and 2 retain the light element nearest neighbor contribution at an apparent radial distance of about 1.6 Å, while Comparative Example 1 has a more obvious distant iron nearest neighbor contribution around about 2.4 Å. The difference is still discernible after cycling.
[0096] Depend on Figure 3It can be seen that the nitrogen 1s signal in Examples 1 and 2 shows a distinguishable peak group in the 398-402 eV region, while the signal in the same region is weaker in Comparative Example 1 when dicyandiamide is not added. All curves use the same counting scale and are not independently normalized; the differences in peak shape and count correspond to the addition of nitrogen-containing precursors.
[0097] Depend on Figure 4 It can be seen that the impedance semicircle of Example 1 is smaller than that of Example 2 without carbon black and Comparative Example 2 with carbon black added after cooling; the charge transfer resistances obtained by fitting the three independent electrodes are 139.1, 198.6 and 191.3 Ω, respectively. The curves use the same frequency range and measurement conditions, which shows that the method of drying and calcining carbon black together with the precursor is consistent with the improvement of interparticle transfer.
[0098] Depend on Figure 5 As can be seen, in the left figure, the relative phenol concentration of Example 1 decreased with reaction time, and the removal rate was 90.30% after 30 minutes; in the right figure, its activity retention rate after 5 cycles was 95.43%, which was higher than that of Comparative Example 1 (58.26%) and Comparative Example 3 (81.75%). Example 2 and the control with carbon black added simultaneously showed different removal rates. The curves, along with the iron dissolution and impedance results, jointly support the coordination of precursor fixation and transport conditions. The disappearance of phenol is not equivalent to complete mineralization.
[0099] In Example 1, the phenol removal rate was 90.30%, the cycle activity retention rate was 95.43%, and the charge transfer resistance was 139.1 Ω. In the three-component Example 2, the resistance was 198.6 Ω, and the removal rate was 86.47%; the improvement in particle contact path after introducing co-heat-treated carbon black was consistent with the decrease in resistance. In Examples 5 and 6, 2% and 4% carbon black were used to replace part of the dicyandiamide, respectively, resulting in resistances of 155.6 Ω and 126.4 Ω, and removal rates of 89.39% and 91.34%. The iron leaching in Example 6 was 0.049 mg / L, higher than the 0.034 mg / L in Example 5, indicating a trade-off between the conductive path and the nitrogen-containing fixation environment. The removal rates of the three-component boundary examples 3 and 4 were 83.33% and 87.17%, respectively, not showing simultaneous optimality across all indicators; the ingredient window corresponds to the compositional relationship rather than a unique performance extreme value.
[0100] Comparative Example 1, with dicyandiamide removed and no carbon black added, showed a weakened nitrogen signal accompanied by a strong contribution from neighboring iron, resulting in localized aggregation after cycling. Its iron dissolution was 0.435 mg / L, and the cycle activity retention rate was only 58.26%, compared to 0.031 mg / L and 95.76% in Example 2. Comparative Example 2, by simply adding carbon black after cooling, saw its resistivity rise to 191.3 Ω, and the removal rate decrease to 86.32%, while the iron dissolution of 0.042 mg / L was close to that of Example 1, indicating that the timing of carbon black addition mainly affects contact and transfer. Comparative Example 3, retaining the ingredients and nitrogen roasting but replacing it with air cooling, had a resistivity of 138.0 Ω, still close to that of Example 1, but the iron dissolution increased to 0.195 mg / L, and the cycle retention rate decreased to 81.75%, corresponding to changes in the solid phase state during the cooling stage. Comparative Example 4, by eliminating ball milling, saw coarse particles and localized encapsulation reduce the removal rate to 81.84%, affecting both the fixed environment and reaction contact.
Claims
1. A fine grinding activation method of a gasification slag environmental governance remediation material, characterized in that, include: S1. Grind the gasification slag containing residual carbon, silicon-aluminum minerals and endogenous iron into balls; S2. Mix the gasification residue after ball milling with tannic acid and dicyandiamide in water; S3. After adding conductive carbon black to the obtained mixture, dry the mixture. S4. The dried mixture is calcined under a nitrogen atmosphere to obtain the repair material; The gasification slag is fine coal gasification slag; based on the mass of the gasification slag after drying to constant weight at 105℃, its dry basis fixed carbon content is 20-35%, dry basis ash content is 60-75%, total iron (calculated as Fe2O3) is 5-10%, silicon (calculated as SiO2) is 25-40%, and aluminum (calculated as Al2O3) is 10-20%. Based on the total dry weight of all solid raw materials before calcination, the mass percentage of tannic acid is 8-12%, the mass percentage of dicyandiamide is 8-10%, the mass percentage of conductive carbon black is 2-4%, and the sum of the mass percentages of dicyandiamide and conductive carbon black is 12%.
2. The method according to claim 1, wherein the method is characterized by, The mixing process includes: dissolving the tannic acid in water; adding the gasified residue after ball milling to the resulting tannic acid aqueous solution and stirring; then adding the dicyandiamide and continuing to stir.
3. The method according to claim 1, wherein the method is characterized by, The roasting and subsequent cooling were both carried out under a nitrogen atmosphere.
4. The fine grinding and activation method for a gasification slag environmental remediation material according to claim 2, characterized in that, The dicyandiamide is added in the form of an aqueous solution; the mixture is not separated into solid and liquid before drying, and the drying is a process of evaporating the mixture as a whole to remove water.
5. The fine grinding and activation method for a gasification slag environmental remediation material according to claim 3, characterized in that, The roasting temperature is 800°C, and the cooling after roasting is carried out in a nitrogen atmosphere and cooled to room temperature in the furnace.
6. The fine grinding and activation method for a gasification slag environmental remediation material according to claim 1, characterized in that, The solid raw materials consist of gasification slag, tannic acid, dicyandiamide, and conductive carbon black. Based on the total dry weight of all solid raw materials before roasting, the gasification slag accounts for 78%, tannic acid for 10%, dicyandiamide for 8-10%, and conductive carbon black for 2-4%. The sum of the mass percentages of dicyandiamide and conductive carbon black is 12%, and the total mass percentage of the four is 100%.
7. The fine grinding and activation method for a gasification slag environmental remediation material according to claim 6, characterized in that, The dry basis mass percentages of the solid raw materials are: 78% gasification slag, 10% tannic acid, 9% dicyandiamide, and 3% conductive carbon black.
Citation Information
Patent Citations
Method for preparing magnetic coal gasification slag composite material through mechanochemical method and application of magnetic coal gasification slag composite material
CN119793461A