Preparation method of epoxidation molecular sieve catalyst and application thereof in synthesis of phosphomycin levomycin salt

The preparation method of EDTA-induced tungsten-supported molecular sieve catalyst solves the problem of poor tungsten source dispersion, achieves high efficiency and stability of the catalyst and multiple reuses, and reduces production costs and wastewater treatment burden.

CN123148984APending Publication Date: 2026-11-24HUBEI XUNDA PHARMA +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611315359.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, the tungsten source has poor dispersion in the catalyst, resulting in poor catalyst stability and catalytic performance. It cannot be repeatedly recycled and reused, which increases production costs and wastewater treatment burden.

Method used

The preparation method of EDTA-induced tungsten-supported molecular sieve catalyst, through hydrothermal crystallization and calcination, ensures that the tungsten source is highly dispersed in the molecular sieve channels, and the prepared catalyst maintains high efficiency and stability in multiple repeated uses.

Benefits of technology

The catalyst can still maintain more than 95% of the initial conversion rate after 8 reuses, which solves the problem of poor catalyst dispersibility, reduces production costs and simplifies wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148984A_ABST
    Figure CN123148984A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an epoxidation molecular sieve catalyst and its application in the synthesis of fosfomycin levozide phosphonium dimethylamine salt. The preparation includes: S1. Adding acid to an aqueous template agent solution, heating, and then adding a silicon source to obtain solution A; preparing an aqueous solution containing EDTA-2Na and a tungsten source to obtain solution B; S2. Adding solution B dropwise to solution A to allow for complete reaction; S3. Performing hydrothermal crystallization treatment on the reaction solution; S4. Washing, drying, and calcining the product after step S3 to obtain the molecular sieve catalyst. The catalyst is obtained by EDTA-induced tungsten loading, with metallic tungsten highly dispersed in the molecular sieve channels. It possesses good stability and regeneration capability for continuous catalysis, meeting the requirement that the conversion rate of the epoxidation reaction can be maintained at more than 95% of the initial use even after 8 repeated uses. It meets the requirements of multiple repeated recycling and performance considerations, and has significant application prospects for the industrial epoxidation preparation of fosfomycin levozide phosphonium dimethylamine salt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of compound catalytic synthesis technology, specifically to the preparation method of epoxidized molecular sieve catalysts and their application in the synthesis of fosfomycin levozide phosphamide salts. Background Technology

[0002] Fosfomycin is a broad-spectrum antibiotic first isolated in 1969 by Merck & Co. and CEPA from the fermentation broth of various Streptomyces. In vitro pharmacodynamic studies have confirmed that fosfomycin has high antibacterial activity against a variety of common clinical pathogens, especially Salmonella spp. Salmonella spp. ), Escherichia coli ( Escherichia coli ) and some Gram-positive bacteria such as Staphylococcus aureus ( Staphylococcus aureus All of these showed good sensitivity.

[0003] Early synthesis of levop-phosphorus-depressant ammonium salts mainly followed the method reported by Edward J. Glamkowski et al. in 1970. This method involved using tert-butyl as a protecting group and preparing the levop-phosphorus-depressant ammonium salt from phosphorus trichloride in six steps, requiring chiral resolution in the final step. This synthetic route was valuable at the time for its innovative integration of the protecting group strategy and the resolution process. However, its resolution steps were overly cumbersome, and the sodium tungstate and ethylenediaminetetraacetic acid (EDTA) used were single-use catalysts that could not be recycled, significantly increasing production costs.

[0004] In recent years, although the synthesis method of fosfomycin levophosphoric acid salts used in industrial production has been greatly simplified after multiple rounds of process improvements, it still uses a sodium tungstate and EDTA catalytic system. Patent document CN103113408A discloses the use of sodium tungstate and EDTA to catalyze the epoxidation of propylene phosphoric acid to obtain fosfomycin levophosphoric acid, followed by dynamic resolution to prepare fosfomycin levophosphoric acid salts. However, the problem of catalyst unrecoverability remains unresolved, resulting in a large amount of tungsten-containing wastewater during industrial production. Patent document CN113336791A discloses the use of tungsten / molybdenum supported ZSM-5 molecular sieves as a catalyst to catalyze the epoxidation reaction to synthesize fosfomycin levophosphoric acid salts, enabling catalyst recovery and reuse. However, the molecular sieve catalyst prepared by the impregnation method has tungsten and molybdenum only supported on the surface of ZSM-5 in the form of ion exchange, resulting in poor stability and dispersibility. It is easily lost during the epoxidation reaction, generating tungsten / molybdenum-containing wastewater while the catalyst's catalytic efficiency gradually decreases.

[0005] Therefore, it is necessary to solve the technical problem of poor dispersion of tungsten sources in catalysts, improve the stability and catalytic performance of catalysts, and enable them to be recycled and reused multiple times to reduce production costs. Summary of the Invention

[0006] This invention provides a method for preparing an epoxidized molecular sieve catalyst, which improves the stability and catalytic performance of the catalyst and meets the requirements for repeated recycling.

[0007] In view of this, the solution of the present invention is as follows: The first aspect of this invention is to provide a method for preparing an epoxidized molecular sieve catalyst, comprising the steps of: S1. Add acid to the template agent aqueous solution, heat and then add silicon source to obtain solution A; prepare an aqueous solution containing EDTA-2Na and tungsten source to obtain solution B; S2. Add solution B dropwise to solution A and allow it to react completely; S3. Perform hydrothermal crystallization treatment on the reaction solution; S4. The product after step S3 is washed, dried and then calcined to obtain a molecular sieve catalyst.

[0008] Furthermore, the molar ratio of the silicon source, EDTA-2Na, and tungsten source is (4-20):1:2; And / or, the amount of the template agent used is 5-10% of the molar amount of the silicon source.

[0009] Furthermore, in step S2, the reaction time is 20-30 hours.

[0010] Furthermore, in step S3, the hydrothermal crystallization treatment temperature is 100℃ and the time is 20-30h.

[0011] Further, in step S4, the calcination temperature is 550°C. The heating rate is 1-2 The roasting time is 4 to 6 hours.

[0012] A second aspect of the present invention is to provide a molecular sieve catalyst prepared by the preparation method described in the first aspect.

[0013] A third aspect of the invention is to provide an application of the molecular sieve catalyst described in the first aspect for the catalytic epoxidation preparation of fosfomycin levozide amine salt, wherein the preparation process recovers and reuses the molecular sieve catalyst.

[0014] A fourth aspect of the present invention is to provide a method for preparing fosfomycin levozide salt, the steps of which include: 1) Obtain or prepare a solution of dextrin phenylethylamine phosphate; 2) Add the molecular sieve catalyst described in the second aspect to the solution in step 1), and then add hydrogen peroxide solution dropwise until the reaction is complete; 3) The reaction product from step 2) was filtered to recover the molecular sieve catalyst, and the filtrate was purified by crystallization to obtain fosfomycin levozide salt.

[0015] Furthermore, in step 2), the reaction temperature is 50-60°C. pH=5-6, reaction time is 6 h; And / or, the molecular sieve catalyst recovered by filtration in step 3) is reused in step 2).

[0016] Preferably, the molecular sieve catalyst can maintain more than 95% of its initial catalytic activity after being recycled 8 times. After repeated use until the catalyst performance declines, its activity can be restored by calcination at 550°C.

[0017] The reaction equation for the preparation of fosfomycin levozide phosphatidylamine salt by molecular sieve catalyst-catalyzed epoxidation is as follows:

[0018] Compared with the prior art, the present invention has the following beneficial effects: The catalyst preparation method provided by this invention uses EDTA to induce tungsten-supported molecular sieve catalysts, in which metallic tungsten is highly dispersed in the molecular sieve channels. It has good stability and regeneration ability for continuous catalysis, and can maintain a conversion rate of more than 95% of the first use even after repeated use for 8 catalytic epoxidation reactions. It meets the requirements of multiple recycling and performance maintenance, and has significant application prospects for industrial epoxidation to prepare fosfomycin levozide phosphatidylcholine salt.

[0019] The catalyst preparation method provided by this invention yields a supported molecular sieve catalyst, which not only avoids the problems of difficult catalyst separation and large discharge of tungsten-containing wastewater in homogeneous catalysis, but also makes the recovery operation easier and has greater potential for large-scale production compared to the insoluble phosphotungstate system. Attached Figure Description

[0020] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the raw material in an embodiment of the present invention; Figure 2 This is the 1H NMR spectrum of the crude cis-propene phosphate dextrorotatory phenethylamine salt in an embodiment of the present invention; Figure 3 The 1H NMR spectrum of the crude fosfomycin levoprene salt prepared in Example 1 of this invention; Figure 4 The bar charts show the reaction conversion and selectivity of Examples 1-4 of the present invention after 10 catalyst cycles. Figure 5 The bar chart shows the catalyst recovery rate after 10 cycles of reaction in Examples 1-4 of this invention. Detailed Implementation

[0021] The technical solution of the present invention will now be clearly and completely described in conjunction with preferred embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] Preparation Example 1

[0023] Preparation method of EDTA-induced tungsten-supported molecular sieve catalyst A: Template agent P123 (5.5 g, 0.95 mmol) was added to 34 mL and stirred until dissolved. Concentrated hydrochloric acid (8 mL, 96 mmol) was added while stirring. The temperature was raised to 40 °C, and tetraethyl orthosilicate (3.5 mL, 16 mmol) was slowly added dropwise to obtain solution A. EDTA-2Na·2H2O (0.3 g, 0.8 mmol) and Na2WO4·2H2O (0.46 g, 1.6 mmol) were dissolved in deionized water to obtain solution B. Solution B was added dropwise to solution A, and the mixture was stirred for 24 h. The resulting reaction solution was poured into a polytetrafluoroethylene-lined container, placed in a hydrothermal synthesis reactor, and dried in an oven at 100 °C for 24 h. The mixture was then allowed to cool naturally to room temperature and filtered to obtain a filter cake. The filter cake was placed in a Soxhlet extractor and washed three times with deionized water and ethanol, each time for 6 h. It was then dried in a vacuum drying oven at 60 °C and ground to obtain a white powder. The white powder was then calcined in a muffle furnace at 550 °C with a heating rate of 2 °C / min to obtain catalyst A.

[0024] Preparation Example 2

[0025] Preparation method of EDTA-induced tungsten-supported molecular sieve catalyst B: Template agent P123 (5.5 g, 0.95 mmol) was added to 34 mL and stirred until dissolved. Concentrated hydrochloric acid (8 mL, 96 mmol) was added while stirring. The temperature was raised to 40 °C, and tetraethyl orthosilicate (3.5 mL, 16 mmol) was slowly added dropwise to obtain solution A. EDTA-2Na·2H2O (0.6 g, 1.6 mmol) and Na2WO4·2H2O (0.92 g, 3.2 mmol) were dissolved in deionized water to obtain solution B. Solution B was added dropwise to solution A, and the mixture was stirred for 24 h. The resulting reaction solution was poured into a polytetrafluoroethylene-lined container, placed in a hydrothermal synthesis reactor, and dried in an oven at 100 °C for 24 h. The mixture was then allowed to cool naturally to room temperature and filtered to obtain a filter cake. The filter cake was placed in a Soxhlet extractor and washed three times with deionized water and ethanol, each time for 6 h. It was then dried in a vacuum drying oven at 60 ℃ and ground to obtain a white powder. The white powder was then calcined in a muffle furnace at 550 ℃ with a heating rate of 2 ℃ / min to obtain catalyst B.

[0026] Preparation Example 3

[0027] Preparation method of EDTA-induced tungsten-supported molecular sieve catalyst C: Template agent P123 (5.5 g, 0.95 mmol) was added to 34 mL and stirred until dissolved. Concentrated hydrochloric acid (8 mL, 96 mmol) was added while stirring. The temperature was raised to 40 °C, and tetraethyl orthosilicate (3.5 mL, 16 mmol) was slowly added dropwise to obtain solution A. EDTA-2Na·2H2O (0.9 g, 2.4 mmol) and Na2WO4·2H2O (1.38 g, 4.8 mmol) were dissolved in deionized water to obtain solution B. Solution B was added dropwise to solution A, and the mixture was stirred for 24 h. The resulting reaction solution was poured into a polytetrafluoroethylene-lined container, placed in a hydrothermal synthesis reactor, and then placed in an oven at 100 °C. The reaction was carried out in a medium atmosphere for 24 hours, then naturally cooled to room temperature, and filtered to obtain a filter cake. The filter cake was placed in a Soxhlet extractor and washed three times with deionized water and ethanol, 6 hours each time, and then placed at 60°C. The powder was dried in a vacuum drying oven and then ground to obtain a white powder. The white powder was then placed at 550°C. Muffle furnace roasting, heating rate 2 / min, to obtain catalyst C.

[0028] Preparation Example 4

[0029] Preparation method of EDTA-induced tungsten-supported molecular sieve catalyst D: Template agent P123 (5.5 g, 0.95 mmol) was added to 34 mL and stirred until dissolved. Concentrated hydrochloric acid (8 mL, 96 mmol) was added while stirring. The temperature was raised to 40 °C, and tetraethyl orthosilicate (3.5 mL, 16 mmol) was slowly added dropwise to obtain solution A. EDTA-2Na·2H2O (1.2 g, 3.2 mmol) and Na2WO4·2H2O (1.84 g, 6.4 mmol) were dissolved in deionized water to obtain solution B. Solution B was added dropwise to solution A, and the mixture was stirred for 24 h. The resulting reaction solution was poured into a polytetrafluoroethylene-lined container, placed in a hydrothermal synthesis reactor, and then placed in an oven at 100 °C. In catalyst C, the reaction was carried out for 24 h, followed by natural cooling to room temperature, and the filter cake was obtained. The filter cake was placed in a Soxhlet extractor and washed three times with deionized water and ethanol, each time for 6 h. It was then dried in a vacuum drying oven at 60 °C and ground to obtain a white powder. The white powder was then calcined in a muffle furnace at 550 °C with a heating rate of 2 °C / min to obtain catalyst D.

[0030] Preparation Example 5

[0031] Preparation of EDTA-induced tungsten-supported molecular sieve catalyst E: Template agent P123 (5.5 g, 0.95 mmol) was added to 34 mL and stirred until dissolved. Concentrated hydrochloric acid (8 mL, 96 mmol) was added while stirring. The temperature was raised to 40 °C, and tetraethyl orthosilicate (3.5 mL, 16 mmol) was slowly added dropwise to obtain solution A. EDTA-2Na·2H2O (1.5 g, 4.0 mmol) and Na2WO4·2H2O (2.3 g, 8.0 mmol) were dissolved in deionized water to obtain solution B. Solution B was added dropwise to solution A, and the mixture was stirred for 24 h. The resulting reaction solution was poured into a polytetrafluoroethylene-lined container, placed in a hydrothermal synthesis reactor, and dried in an oven at 100 °C for 24 h. The mixture was then allowed to cool naturally to room temperature and filtered to obtain a filter cake. The filter cake was placed in a Soxhlet extractor and washed three times with deionized water and ethanol, each time for 6 h. It was then dried in a vacuum drying oven at 60 ℃ and ground to obtain a white powder. The white powder was then calcined in a muffle furnace at 550 ℃ with a heating rate of 2 ℃ / min to obtain catalyst E.

[0032] The following examples illustrate the preparation of fosfomycin levozide phosphodamine salt based on the molecular sieve catalyst obtained in the above preparation examples.

[0033] The preparation method of cis-propenyl phosphate dextrophenylethylamine salt in the examples is as follows: 63 mL of ethanolic solution of cis-propenyl phosphate was added to a three-necked flask, and the mixture was stirred continuously in an ice bath. Dextrorotatory phenylethylamine (26 mL, 204 mmol) was added dropwise. After the addition was complete, the mixture was transferred to an oil bath to continue the reaction and form a solution of dextrorotatory phenylethylamine salt of cis-propenyl phosphate. The reaction solution was cooled to 0 °C and allowed to stand for 24 h to crystallize. The crystals were filtered and recrystallized to obtain dextrorotatory phenylethylamine salt of cis-propenyl phosphate. The 1H NMR spectra of cis-propenyl phosphate and dextrorotatory phenylethylamine salt of cis-propenyl phosphate are shown below. Figure 1 , Figure 2 As shown.

[0034] Example 1

[0035] 50 g of dextrophenylethylamine cis-propenyl phosphate was added to a three-necked flask, dissolved in ethanol upon heating, followed by the addition of 0.5 g of catalyst A. After complete dissolution, 30% hydrogen peroxide solution was slowly added dropwise. The reaction was allowed to proceed for 6 h to obtain a solution of fosfomycin levophosphoric acid dextrophenylamine salt. The reaction solution was filtered while hot to recover the catalyst. The filtrate was cooled to 0 °C and allowed to stand for 24 h to crystallize. After filtration and recrystallization, fosfomycin levophosphoric acid dextrophenylamine salt was obtained. The conversion rate was 96.3%, and the selectivity was 95.2%. No tungsten ions were detected in the filtrate, indicating that metallic tungsten was not lost from the catalyst. The 1H NMR spectrum of the product fosfomycin levophosphoric acid dextrophenylamine salt is shown below. Figure 3 As shown.

[0036] Example 2

[0037] 50 g of dextrin phenylethylamine phosphate was added to a three-necked flask, dissolved in ethanol upon heating, followed by the addition of 0.5 g of catalyst B. After complete dissolution, 30% hydrogen peroxide solution was slowly added dropwise. The reaction was allowed to proceed for 6 h to obtain a solution of fosfomycin levophosphoric acid dextrin. The reaction solution was filtered while hot to recover the catalyst. The filtrate was cooled to 0 °C and allowed to stand for 24 h to crystallize. The crystallization was repeated after filtration to obtain fosfomycin levophosphoric acid dextrin. The conversion rate was 89%, and the selectivity was 97.1%. No tungsten ions were detected in the filtrate, indicating that metallic tungsten was not lost from the catalyst.

[0038] Example 3

[0039] 50 g of dextrin phenylethylamine phosphate was added to a three-necked flask, dissolved in ethanol upon heating, followed by the addition of 0.5 g of catalyst C. After complete dissolution, 30% hydrogen peroxide solution was slowly added dropwise. The reaction was allowed to proceed for 6 h to obtain a solution of fosfomycin levophosphoric acid dextrin. The reaction solution was filtered while hot to recover the catalyst. The filtrate was cooled to 0 °C and allowed to stand for 24 h to crystallize. The crystallization was repeated after filtration to obtain fosfomycin levophosphoric acid dextrin. The conversion rate was 98.1%, and the selectivity was 94.9%. No tungsten ions were detected in the filtrate, indicating that metallic tungsten was not lost from the catalyst.

[0040] Example 4

[0041] 50 g of dextrin phenylethylamine phosphate was added to a three-necked flask, dissolved in ethanol upon heating, followed by the addition of 0.5 g of catalyst D. After complete dissolution, 30% hydrogen peroxide solution was slowly added dropwise. The reaction was allowed to proceed for 6 h to obtain a solution of fosfomycin levophosphoric acid dextrin. The reaction solution was filtered while hot to recover the catalyst. The filtrate was cooled to 0°C and allowed to stand for 24 h to crystallize. The crystallization was repeated after filtration to obtain fosfomycin levophosphoric acid dextrin. The conversion rate was 96.9%, and the selectivity was 95.8%. No tungsten ions were detected in the filtrate, indicating that metallic tungsten was not lost from the catalyst.

[0042] Example 5

[0043] The molecular sieve catalysts from Examples 1-4 were recovered and reused, designated as group a, group b, group c, and group d, respectively. Ten cycles of experiments were repeated for each group, yielding conversion and selectivity data for each of the four catalyst groups after 10 cycles. The recovery rate data for each of the four catalyst groups are shown below. Figure 4 , Figure 5 As shown in the bar chart.

[0044] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an epoxidized molecular sieve catalyst, characterized in that the steps include... include: S1. Add acid to the template agent aqueous solution, heat it, and then add a silicon source to obtain solution A; An aqueous solution containing EDTA-2Na and a tungsten source was prepared to obtain solution B; S2. Add solution B dropwise to solution A and allow it to react completely; S3. Perform hydrothermal crystallization treatment on the reaction solution; S4. The product after step S3 is washed, dried and then calcined to obtain a molecular sieve catalyst.

2. The preparation method according to claim 1, characterized in that, The molar ratio of the silicon source, EDTA-2Na, and tungsten source is (4-20):1:2; And / or, the amount of the template agent used is 5-10% of the molar amount of the silicon source.

3. The preparation method according to claim 1, characterized in that, In step S2, the reaction time is 20-30 h.

4. The preparation method according to claim 1, characterized in that, In step S3, the hydrothermal crystallization treatment temperature is 100°C and the time is 20-30 h.

5. The preparation method according to claim 1, characterized in that, In step S4, the calcination temperature is 550°C, the heating rate is 1-2°C, and the calcination time is 4-6 hours.

6. A molecular sieve catalyst, characterized in that, It is prepared by the preparation method described in any one of claims 1-5.

7. The application of the molecular sieve catalyst according to claim 6, characterized in that, The application is the catalytic epoxidation preparation of fosfomycin levozide salt, and the preparation process recovers and reuses the molecular sieve catalyst.

8. A method for preparing fosfomycin levozide salt, characterized in that the step... include: 1) Obtain or prepare a solution of dextrin phenylethylamine phosphate; 2) Add the molecular sieve catalyst of claim 6 to the solution of step 1), and then add hydrogen peroxide solution dropwise to allow the reaction to proceed. 3) The reaction product from step 2) was filtered to recover the molecular sieve catalyst, and the filtrate was purified by crystallization to obtain fosfomycin levozide salt.

9. The preparation method according to claim 8, characterized in that, Step 2) The reaction temperature is 50-60℃, pH=5-6, and the reaction time is 6 h; And / or, the molecular sieve catalyst recovered by filtration in step 3) is reused in step 2).

Citation Information

Patent Citations

  • Novel method for preparing fosfomycin phenylethylamine

    CN103113408A

  • Production method of fosfomycin calcium bulk drug

    CN113336791A