Pure silica zeolite sigma hydrogenation catalyst, method of making and use
By using Sigma-2 type pure silica zeolite support and Pd-M alloy catalyst, the problems of low dispersion and poor stability of existing catalysts were solved, achieving a highly efficient selective hydrogenation reaction of acetylene and improving ethylene selectivity and catalyst stability.
Patent Information
- Application Number
- CN202611432073.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing α-Al₂O₃ supported Pd-based catalysts suffer from problems such as small specific surface area of the support, low Pd dispersion, easy sintering, poor stability, and insufficient ethylene selectivity in the selective hydrogenation of acetylene, leading to raw material waste and reduced economic benefits.
Using Sigma-2 type pure silica zeolite as a carrier, Pd-based components and auxiliary metals M (such as Cu, Zn, Fe, Ce, Ni, Ga, Ag, Au) are loaded. By controlling the ratio of Pd to M, Pd-M alloys are formed, which improves the dispersion of Pd and modulates its electronic state. Combined with the unique microporous structure and stacked pores, the mass transfer performance is optimized.
High acetylene conversion and high ethylene selectivity were achieved. The catalyst maintained good activity and stability under high space velocity conditions, reduced the side reaction of ethylene over-hydrogenation to ethane, and improved the overall performance of the catalyst.
Smart Images

Figure CN123148985A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydrogenation catalysis technology, specifically relating to a pure silica zeolite Sigma hydrogenation catalyst, its preparation method, and its application. Background Technology
[0002] Ethylene, hailed as the "mother of petrochemicals," is one of the world's largest-produced chemicals and holds an irreplaceable strategic position in the chemical industry chain. Ethylene is primarily produced through the steam cracking of higher hydrocarbons (ethane, propane, butane, naphtha, and gas oil). During the cracking process, a small amount of acetylene is produced as a byproduct, ranging from 0.2% to 3%. These trace amounts of acetylene can affect subsequent polyethylene processing, leading to a decrease in the quality of the polyethylene product. Therefore, it is required that the alkyne content in the raw ethylene be reduced to below a few ppm.
[0003] Currently, the mainstream industrial method for removing trace amounts of acetylene from ethylene feedstock is catalytic selective hydrogenation, which primarily uses Pd-based catalysts supported on α-Al₂O₃. While these catalysts offer advantages such as good reactivity at relatively low reaction temperatures, they also suffer from drawbacks including small support surface area, low Pd dispersion, sintering susceptibility, poor stability, and the need for improved ethylene selectivity. These issues lead to feedstock waste and reduced economic efficiency.
[0004] The core challenge of selective hydrogenation of acetylene lies in the competitive adsorption of acetylene and ethylene on the catalyst surface. It is necessary to ensure that trace amounts of acetylene preferentially adsorb onto the catalyst amidst a large amount of ethylene. Simultaneously, the activation energy for further hydrogenation of ethylene to ethane should be higher than the energy for ethylene desorption to avoid wasting ethylene feedstock. However, single-component Pd catalysts exhibit excessive adsorption strength for ethylene, easily leading to over-hydrogenation to ethane and carbon chain polymerization byproducts during the reaction. Consequently, they fail to meet ideal standards in terms of ethylene selectivity and resistance to carbon deposition.
[0005] Therefore, to address the aforementioned technical issues, it is necessary to provide a pure silica zeolite Sigma hydrogenation catalyst, its preparation method, and its application. Summary of the Invention
[0006] The purpose of this invention is to provide a pure silicon zeolite Sigma hydrogenation catalyst, its preparation method, and its application.
[0007] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution:
[0008] The pure silica zeolite Sigma hydrogenation catalyst comprises: a support, which is Sigma-2 type pure silica zeolite with pores formed on its outer surface (pores formed by the natural accumulation of substances generated during the support preparation process); and an active component loaded on the support, comprising a Pd-based component and an additive, wherein the metal element M in the additive is selected from Cu, Zn, Fe, Ce, Ni, Ga, Ag, Au, etc., wherein: the loading amount of the Pd-based component on the support, based on the mass of Pd, accounts for 0.05wt%-3.0wt% of the support mass; and the loading amount of the additive on the support, based on the mass of the metal element M, accounts for 0.05wt%-3.0wt% of the support mass. This invention utilizes Sigma-2 pure silica zeolite as an all-silica framework, free of acidic sites from aluminum, which can suppress olefin polymerization and carbon deposition side reactions during acetylene hydrogenation. The zeolite's intrinsic micropore size of 0.21 nm provides a molecular sieving effect, facilitating preferential acetylene adsorption and moderately weakening ethylene adsorption. The packing pores on the outer surface of the crystals improve mass transfer between reactants and products, reduce diffusion resistance, and maintain high activity under high space velocity conditions. The carrier crystallite particle size is controlled at 1-5 μm, ensuring both mechanical properties and sufficient exposure of active metal sites. The total specific surface area is controlled at 5-10 m². 2 / g, balancing mass transfer and molecular sieve structural stability; the pore size of the packing pores synergizes with the intrinsic micropores of the zeolite, avoiding catalyst deactivation caused by the retention of large molecular byproducts in the pores. Simultaneously, Pd is used as the main active site for acetylene hydrogenation in the active component. An appropriate Pd loading ensures hydrogenation activity; too low a loading results in insufficient activity, while too high a loading easily causes Pd particle agglomeration and sintering, reducing ethylene selectivity. The introduction of the auxiliary metal M allows for alloying with Pd, achieving electronic and geometric site effects: on the one hand, it improves Pd metal dispersion and inhibits high-temperature Pd sintering; on the other hand, it modulates the electronic state of Pd, weakening the ethylene adsorption strength on the catalyst surface, inhibiting the further hydrogenation of ethylene to ethane side reaction, and significantly improving ethylene selectivity. M is selected from the aforementioned metals, allowing for varying degrees of modification of the Pd sites.
[0009] In one or more embodiments of the present invention, the total specific surface area of the outer surface of the carrier is 5m². 2 / g-10m 2 / g; and / or, the intrinsic pore size of the outer surface of the carrier is less than 0.3 nm.
[0010] In one or more embodiments of the present invention, the particle size of the catalyst is 1 μm-5 μm.
[0011] In one or more embodiments of the present invention, a method for preparing a pure silicon zeolite Sigma hydrogenation catalyst includes: S1, mixing an appropriate amount of structure directing agent, silicon source, mineralizer and solvent to obtain a mixed solution; S2, mixing the mixed solution, Pd source, metal element M source and seed crystal to form a mixed system, and then crystallizing, filtering, washing, drying and calcining to obtain a pure silicon zeolite Sigma hydrogenation catalyst.
[0012] In one or more embodiments of the present invention, the structure directing agent in S1 is at least one of 1-adamantaneamine and ethylenediamine; and / or, the silicon source is at least one of silica sol and tetramethoxysilane; and / or, the mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride, wherein fluoride ions promote the rearrangement of silicon-oxygen bonds, which is beneficial to the crystallization of pure phase Sigma-2; and / or, the solvent is at least one of water and ethanol, which regulates the dissolution of the precursor and the dispersion of the metal salt.
[0013] In one or more embodiments of the present invention, the molar ratio of the structure directing agent to the silicon source in S1 is 1:(1-4); and / or, the molar ratio of the silicon source to the mineralizer is 1:(1-3); and / or, the molar ratio of deionized water to the silicon source is (20-100):1, to ensure the obtaining of pure phase Sigma-2 and avoid the formation of impurities.
[0014] In one or more embodiments of the present invention, the amount of seed crystal added in S2 is 0.1wt%-0.3wt% of the total mass of the mixed system. By inducing crystallization through seed crystal, the crystallization cycle is shortened, and zeolite grains with uniform morphology and a particle size of 1-5μm are obtained, thus inhibiting excessive grain growth; and / or, the molar ratio of palladium source to metal element M source is 1:(1-3).
[0015] In one or more embodiments of the present invention, crystallization in S2 is achieved by stirring at room temperature for 2-4 hours, followed by holding at 150°C-200°C for 1-3 days, thereby ensuring the complete formation of the Sigma-2 crystal phase.
[0016] In one or more embodiments of the present invention, the calcination conditions in S2 are: prior to calcination in an air atmosphere, at (2-10) °C·min. -1 The temperature is rapidly increased to 500℃-800℃ and held for 5-8 hours to remove the structure-directing agent and decompose the metal salt to obtain the metal oxide; then, under a hydrogen atmosphere, the temperature is increased at (5-10)℃·min. -1 The temperature is rapidly increased to 150℃-300℃ and held for 1-3 hours to reduce Pd and M oxides to metals, thus constructing active sites for the Pd-M alloy. During calcination, the heating rate is strictly controlled at different stages to prevent thermal collapse of the molecular sieve framework and to avoid sintering and agglomeration of metal particles.
[0017] In one or more embodiments of the present invention, the aforementioned application of the pure silica zeolite Sigma hydrogenation catalyst in the catalytic selective hydrogenation reaction of acetylene is used for the selective hydrogenation of trace amounts of acetylene from ethylene feedstock, at 150-250°C and high space velocities of 15000-45000 h⁻¹. -1 Under these conditions, it achieves high acetylene conversion while maintaining high ethylene selectivity; the pure silicon support inhibits carbon deposition, and the catalyst exhibits good operational stability; it maintains catalytic performance even under high space velocity conditions, and has great potential for industrial application.
[0018] Compared with existing technologies, the present invention provides a pure silicon zeolite Sigma hydrogenation catalyst, its preparation method, and its application. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 The X-ray diffraction intensity spectra (XRD) of the samples and standard cards in Examples 1-4 of this invention are shown.
[0021] Figure 2 The images shown are scanning electron microscope (SEM) images of the samples in Examples 1-4 of this invention, including the SEM images of (ab) Sigma crystal, (cd) Pd1Cu1 / Sigma-0.4, (ef) Pd1Cu2 / Sigma-0.4, and (gh) Pd1Cu3 / Sigma-0.4.
[0022] Figure 3 This is the N2 adsorption isotherm of the Pd1Cu2 / Sigma sample in Example 3 of the present invention;
[0023] Figure 4 This is a graph showing the changes in acetylene conversion and ethylene selectivity as a function of temperature in the acetylene catalytic hydrogenation experiment of the Pd1Cu2 / Sigma sample in Example 3 of this invention.
[0024] Figure 5 This is a stability test diagram of the Pd1Cu2 / Sigma sample at 230℃ in Example 3 of the present invention;
[0025] Figure 6 The Pd1Cu2 / Sigma sample in Example 3 of this invention was subjected to different space velocities (15000 h⁻¹). -1 30000h -1 45000h -1The curves showing the acetylene conversion rate and ethylene selectivity as a function of temperature. Detailed Implementation
[0026] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments disclosed herein. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.
[0027] Zeolite molecular sieves possess high specific surface area and regular pore structure, making them excellent supports for preparing highly dispersible and stable supported metal catalysts. The Sigma molecular sieve framework comprises silicon-aluminum-oxygen units, consisting of alternating five-membered rings (0.16 nm) and six-membered rings (0.28 nm), with an effective pore size of 0.21 nm. Notably, the crystallization process of Sigma is sensitive to the silicon-aluminum content of the precursor solution: without the addition of an aluminum source, the hydrothermal synthesis product transforms into the Sigma-2 crystalline phase. The Sigma used in this invention is actually a Sigma-2 type pure silica zeolite, without the introduction of an aluminum source, consisting solely of a silicon-oxygen framework. It possesses unique molecular sieving characteristics, resulting in high selectivity and high activity, enabling efficient removal of trace amounts of acetylene from ethylene.
[0028] The first aspect of this invention is to provide a Pd-supported Sigma molecular sieve hydrogenation catalyst. The catalyst uses Sigma molecular sieve as a support, with Pd element loaded on the support, to address the problems of low dispersion and poor stability in existing Pd-based catalysts. Based on the total weight of the catalyst, the mass percentage of Pd element is 0.05 wt%-3 wt%.
[0029] A second aspect of this invention is to provide a bimetallic PdM / Sigma hydrogenation catalyst formed by introducing an auxiliary metal element M, such as Cu (which can also be replaced by Zn, Fe, Ce, Ni, Ga, Ag, Au, etc.), to improve the selectivity and activity of ethylene and further solve the problem of insufficient ethylene selectivity. Taking a PdCu / Sigma hydrogenation catalyst as an example, in a pure silica zeolite Sigma hydrogenation catalyst, the mass percentage of metal element M is 0.05wt%-3wt%.
[0030] A third aspect of the present invention is to conduct experiments on the Sigma hydrogenation catalyst prepared according to the first and second aspects of the present invention to produce ethylene by acetylene semi-hydrogenation. By comparing monometallic and bimetallic Sigma catalysts, it is found that introducing an auxiliary agent improves the selectivity of ethylene and the conversion rate of acetylene.
[0031] In one or more embodiments of the present invention, the total specific surface area of the outer surface of the pure silica zeolite Sigma hydrogenation catalyst is 5 m². ² / g-10m 2 / g; and / or,
[0032] The pore size of the pure silica zeolite Sigma hydrogenation catalyst is less than 0.3 nm; and / or,
[0033] The particle size of the pure silica zeolite Sigma hydrogenation catalyst is 1μm-5μm.
[0034] According to the purpose of the invention, a method for preparing a pure silica zeolite Sigma hydrogenation catalyst is provided, which includes the following steps:
[0035] The structure-directing agent, silicon source, mineralizer and solvent are mixed to obtain a mixed solution; the mixed solution is mixed with seed crystals, and after crystallization, filtration, washing, drying and calcination, pure silicon zeolite Sigma hydrogenation catalyst is obtained.
[0036] In one or more embodiments of the present invention, the structure directing agent is at least one of 1-adamantaneamine and ethylenediamine; and / or,
[0037] The silicon source is at least one of silica sol and tetramethoxysilane; and / or,
[0038] The mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride; and / or,
[0039] The solvent is at least one of water and ethanol; and / or,
[0040] The seed crystal is a Sigma seed crystal.
[0041] In one or more embodiments of the present invention, the molar ratio of the structure-directing agent to the silicon source is 1:1 to 1:4; and / or,
[0042] The molar ratio of silicon source to mineralizer is 1:1 to 1:3; and / or,
[0043] The molar ratio of deionized water to silicon source is 20:1-100:1; and / or,
[0044] In one or more embodiments of the present invention, after the mixed solution and seed crystals are mixed, the mixture is stirred at room temperature for 2-4 hours, and then crystallized at 150°C-200°C for 1-3 days; and / or,
[0045] The washing procedure is as follows: wash with deionized water until neutral; and / or,
[0046] The drying conditions are: temperature 80℃-120℃, time 8h-12h; and / or,
[0047] The calcination conditions are as follows: first, under an air atmosphere, at 2℃·min- 1 -10℃·min -1 The temperature is rapidly increased to 500℃-800℃, and calcined for 5-8 hours; then, under a hydrogen atmosphere, the temperature is increased at 5℃·min. -1 -10℃·min -1 The temperature is increased rapidly to 150℃-300℃, and the calcination time is 1-3 hours.
[0048] According to a first aspect of the present invention, the technical solution provided by a specific embodiment is as follows:
[0049] A method for preparing a pure silica zeolite Sigma hydrogenation catalyst supported on Pd, the method comprising the following steps:
[0050] A mixed solution is obtained by mixing a structure-directing agent, a silicon source, a mineralizer, and a solvent.
[0051] The mixed solution, palladium source, and seed crystals were mixed, and then crystallized, filtered, washed, dried, and calcined to obtain a pure silicon zeolite Sigma hydrogenation catalyst.
[0052] In one or more embodiments of the present invention, the structure directing agent is at least one of 1-adamantaneamine and ethylenediamine; and / or,
[0053] The silicon source is at least one of silica sol and tetramethoxysilane; and / or,
[0054] The mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride; and / or,
[0055] The palladium source is at least one of palladium chloride, palladium nitrate, palladium acetate, palladium dichlorodiamine, palladium dichlorotetramine, and palladium oxalate; and / or,
[0056] The solvent is at least one of water and ethanol; and / or,
[0057] The seed crystal is a Sigma seed crystal.
[0058] In one or more embodiments of the present invention, the molar ratio of the structure-directing agent to the silicon source is 1:1 to 1:4; and / or,
[0059] The molar ratio of silicon source to mineralizer is 1:1 to 1:3; and / or,
[0060] The molar ratio of deionized water to silicon source is 20:1-100:1; and / or,
[0061] The amount of seed crystals added is 0.1wt%-0.3wt% of the total mass of the mixed solution and palladium source.
[0062] In one or more embodiments of the present invention, after mixing the mixed solution, palladium source, and seed crystals, the mixture is stirred at room temperature for 2-5 hours, and then crystallized at 150°C-200°C for 1-3 days; and / or,
[0063] The washing procedure is to wash with deionized water until neutral; and / or,
[0064] The drying conditions are: temperature 80℃-120℃, time 8h-12h; and / or,
[0065] The calcination conditions are as follows: first, under an air atmosphere, at 2℃·min -1 -10℃·min -1 The temperature is rapidly increased to 500℃-800℃ and calcined for 5-8 hours; then, under a hydrogen atmosphere, the temperature is increased at 5℃·min. -1 -10℃·min -1 The temperature is increased rapidly to 150℃-300℃, and the calcination time is 1-3 hours.
[0066] According to a second aspect of the present invention, specifically, taking Cu as an example, the technical solution provided by the specific embodiment is as follows:
[0067] A method for preparing a pure silica zeolite Sigma hydrogenation catalyst supported on Pd and Cu elements, the method comprising the following steps:
[0068] A mixed solution is obtained by mixing the structure-directing agent, silicon source, mineralizer and deionized water;
[0069] The mixed solution, palladium source, copper source and seed crystals were mixed, and then crystallized, filtered, washed, dried and calcined to obtain pure silicon zeolite Sigma hydrogenation catalyst.
[0070] In one or more embodiments of the present invention, the structure directing agent is at least one selected from 1-adamantanamine and ethylenediamine; and / or,
[0071] The silicon source is at least one of silica sol and tetramethoxysilane; and / or,
[0072] The mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride; and / or,
[0073] The palladium source is at least one of palladium chloride, palladium nitrate, palladium acetate, palladium dichlorodiamine, palladium dichlorotetramine, and palladium oxalate; and / or,
[0074] The copper source is at least one of copper nitrate trihydrate, copper chloride, and copper sulfate; and / or,
[0075] The solvent is at least one of water and ethanol; and / or,
[0076] The seed crystal is a Sigma seed crystal.
[0077] In one or more embodiments of the present invention, the molar ratio of the structure-directing agent to the silicon source is 1:1 to 1:4; and / or,
[0078] The molar ratio of silicon source to mineralizer is 1:1 to 1:3; and / or,
[0079] The molar ratio of deionized water to silicon source is 20:1-100:1; and / or,
[0080] The molar ratio of palladium source to copper source is 1:1 to 1:3; and / or,
[0081] The amount of seed crystals added is 0.1wt%-0.3wt% of the total mass of the mixed solution, palladium source and copper source.
[0082] In one or more embodiments of the present invention, after mixing the mixed solution, palladium source, copper source, and seed crystal, the mixture is stirred at room temperature for 2-4 hours, and then crystallized at 150°C-200°C for 1-3 days; and / or,
[0083] The washing procedure is to wash with deionized water until neutral; and / or,
[0084] The drying conditions are: temperature 80℃-120℃, time 8h-12h; and / or,
[0085] The calcination conditions are as follows: first, under an air atmosphere, at 2℃·min -1 -10℃·min -1 The temperature is rapidly increased to 500℃-800℃ and calcined for 5-8 hours; then, under a hydrogen atmosphere, the temperature is increased at 5℃·min. -1 -10℃·min -1 The temperature is increased rapidly to 150℃-300℃, and the calcination time is 1-3 hours.
[0086] According to a third aspect of the present invention, the technical solution provided by specific embodiments is as follows:
[0087] Application of the above-mentioned pure silica zeolite Sigma hydrogenation catalyst or the pure silica zeolite Sigma hydrogenation catalyst prepared by the above-mentioned method in the selective hydrogenation reaction of acetylene.
[0088] In one or more embodiments of the present invention, the pure silica zeolite Sigma hydrogenation catalyst is first pressed into tablets at a pressure of 10MPa-20MPa for 5min-10min, and then ground and sieved using a 40-60 mesh sieve to obtain 40-60 mesh catalyst particles. The catalyst particles are then used in the catalytic selective hydrogenation reaction of acetylene.
[0089] In one or more embodiments of the present invention, in the catalytic selective hydrogenation reaction of acetylene, the reactant gas is a mixture of H2, C2H2, and N2, and the volume hourly space velocity is 15000 h⁻¹. -1 -45000h -1 The reaction temperature is 150℃-250℃.
[0090] This invention selects Pd-based pure silica zeolite Sigma as the target catalyst because of its unique microporous structure and pure silica inert surface, which not only effectively avoids side reactions but also facilitates the dispersion and mass transfer of active components due to its small particle size. This invention employs a secondary seeding method to effectively synthesize pure-phase Sigma zeolite with short crystallization time and uniform crystal morphology. By adding Cu as an additive and controlling the Pd / Cu ratio, a Pd-Cu alloy is formed, improving the dispersion of Pd atoms and increasing the electron density of Pd through electronic modulation effects. This reduces the adsorption strength of ethylene on the catalyst surface, resulting in a Pd-based pure silica zeolite Sigma hydrogenation catalyst with excellent catalytic performance.
[0091] Based on this, the present invention combines the advantages of secondary seed synthesis method and palladium-copper catalyst, and successfully prepares a Pd-based pure silica zeolite Sigma hydrogenation catalyst with high selectivity and high activity by controlling the molar ratio of palladium and copper.
[0092] One specific embodiment of the present invention provides a pure silica zeolite Sigma hydrogenation catalyst, which uses Sigma molecular sieve as a support and loads Cu and Pd elements on the support; in the pure silica zeolite Sigma hydrogenation catalyst, the mass percentage of Pd element is 0.2wt%-0.6wt% and the mass percentage of Cu element is 0.2wt%-0.7wt%.
[0093] Specifically, by controlling the palladium-copper ratio to form a Pd-Cu alloy structure, the dispersion of Pd atoms is improved, and the electron density of Pd is increased through electronic regulation effect, thereby reducing the adsorption strength of ethylene on the catalyst surface and improving the catalytic activity and selectivity of the catalyst for selective hydrogenation of acetylene.
[0094] Furthermore, in the pure silica zeolite Sigma hydrogenation catalyst, the molar ratio of Pd to Cu is 1:1 to 1:3 on an atomic basis. By optimizing the palladium-copper ratio, the catalytic activity and selectivity of the catalyst are further improved.
[0095] Furthermore, the specific surface area of the pure silica zeolite Sigma hydrogenation catalyst is 5 m². 2 / g-10m 2 / g (based on N2 adsorption method), the pore size of the pure silica zeolite Sigma hydrogenation catalyst is less than 0.3nm, and the particle size of the pure silica zeolite Sigma hydrogenation catalyst is 1μm-5μm. The catalyst in this invention exhibits a pure phase and uniform crystal size.
[0096] Another specific embodiment of the present invention provides a method for preparing a pure silica zeolite Sigma hydrogenation catalyst, comprising the following steps:
[0097] Step 1: Mix the structure-directing agent, silicon source, mineralizer and deionized water to obtain a mixed solution.
[0098] Specifically, the structure-directing agent is at least one of 1-adamantaneamine and ethylenediamine; the silicon source is at least one of silica sol and tetramethoxysilane, with LUDOX®AS-30 silica sol being the preferred silicon source; the mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride, with anhydrous potassium fluoride (KF) being the preferred mineralizing agent. The molar ratio of the structure-directing agent to the silicon source is 1:1, 1:2, 1:3, or 1:4; the molar ratio of the silicon source to the mineralizing agent is 1:1, 1:2, or 1:3; and the molar ratio of deionized water to the silicon source is 20:1, 30:1, 40:1, 50:1, 70:1, 80:1, 90:1, 100:1, or 110:1.
[0099] During mixing, the system is stirred at a speed of 300 rpm to 500 rpm.
[0100] Step 2: Mix the mixed solution, palladium source, copper source and seed crystal, and then crystallize, filter, wash, dry and calcine to obtain pure silicon zeolite Sigma hydrogenation catalyst.
[0101] Specifically, palladium and copper sources are weighed in a certain proportion, placed in a beaker, dissolved in a small amount of ethanol, and sonicated until no obvious precipitate is observed. The palladium source is palladium chloride; the copper source is copper nitrate trihydrate. The molar ratio of palladium to copper source is 1:1 to 1:3, preferably 1:2.
[0102] Palladium and copper sources were pre-dissolved in ethanol, then mixed with the mixed solution and seed crystals, and stirred at room temperature for 2-4 hours. Crystallization was then carried out at 150-200℃ for 1-3 days. The mixture was then filtered and washed with deionized water until neutral. Finally, it was dried at 80-120℃ for 8-12 hours, and then placed in a muffle furnace with a programmed heating rate of 2℃·min. -1 -10℃·min -1 The sample was calcined in air at 500℃-800℃ for 5-8 hours. Then it was placed in a tube furnace with a heating rate of 5℃·min. -1 -10℃·min -1The catalyst is calcined in a hydrogen atmosphere at 150℃-300℃ for 1-3 hours. By controlling the heating rate and calcination temperature, a catalyst with regular morphology and uniform crystal size can be obtained. If the heating rate is too high, thermal runaway will occur, causing the catalyst structure to collapse and sinter, and the catalyst activity will also be reduced.
[0103] The preferred process parameters in step 2 are: stirring at room temperature for 2 hours followed by crystallization at 170°C for 2 days; drying at 80°C for 8 hours; and a programmed heating rate of 2°C / min. -1 The calcination temperature was set at 700℃ in an air atmosphere and the calcination time was 8 hours; the calcination temperature was set at 300℃ in a hydrogen atmosphere and the calcination time was 2 hours.
[0104] Furthermore, the amount of seed crystals added is 0.1wt%-0.3wt% of the total mass of the mixed solution, palladium source, and copper source.
[0105] The present invention will be further described in detail below with reference to specific embodiments.
[0106] Group 1
[0107] Example 1
[0108] The preparation of Sigma molecular sieves is as follows:
[0109] The reaction was carried out under vigorous stirring (300 rpm): 1.18 g of 1-adamantaneamine and 3.333 g of silicon source (LUDOX® AS-30 silica sol) were dissolved in 21.57 g of deionized water. After stirring for a short time, 0.965 g of KF was added to obtain a mixed solution. Approximately 0.03 g of Sigma seed crystals were added to the above mixture, and after stirring for 2 h, the mixture was transferred to a 200 mL hydrothermal reactor and crystallized at 170 °C for 2 days. The obtained sample was filtered and washed with deionized water until neutral, dried at 80 °C for 12 h, and then calcined in a muffle furnace at 700 °C for 8 h to obtain the Sigma molecular sieve sample.
[0110] The XRD pattern of the sample is shown below. Figure 1 The characterization diagram shows that characteristic diffraction peaks of Sigma molecular sieves appeared at 2θ = 8.9°, 19.7°, and 26.6°, indicating that the synthesized sample is a pure-phase Sigma molecular sieve; SEM images are shown below. Figure 2In (a) and (b), the Sigma molecular sieve crystals have clear outlines, regular morphology, and a polyhedral shape, with a grain size of approximately 1-5 μm. No impurities were observed, indicating that the synthesized sample is a pure-phase Sigma molecular sieve with uniform crystal size. XRD showed characteristic diffraction peaks of Sigma molecular sieves, with no impurities. SEM revealed a 1-5 μm polyhedral grain morphology. The total BET specific surface area was 6.7 m² / g, and the pore size was 0.21 nm. A well-formed, pure-phase Sigma-2 silica zeolite support was successfully synthesized, providing a basic framework for loading bimetallic active components. The support itself has no hydrogenation activity and requires loading with Pd-based active components.
[0111] Example 2
[0112] Pd1Cu1 / Sigma was prepared as follows:
[0113] Under vigorous stirring (300 rpm), 1.18 g of 1-adamantaneamine and 3.333 g of silicon source (LUDOX® AS-30 silica sol) were dissolved in 21.57 g of deionized water. After stirring briefly, 0.965 g of KF was added to obtain a mixed solution. Appropriate amounts of palladium chloride and copper nitrate trihydrate (molar ratio Pd:Cu = 1:1, calculated based on a final catalyst Pd loading of 0.4 wt%) were weighed, dissolved in 5 mL of ethanol, and sonicated until no obvious precipitate was observed before being added to the mixed solution. Approximately 0.03 g of Sigma seed crystals were added to the above mixture. After mixing and stirring for 2 h, the mixture was transferred to a 200 mL hydrothermal reactor and crystallized at 170 °C for 2 d. The obtained sample was filtered and washed with deionized water until neutral. It was dried at 80 °C for 8 h and then placed in a muffle furnace and calcined at 700 °C for 8 h at a programmed temperature rise rate of 2 °C / min. Finally, it was placed in a tube furnace and calcined at 300 °C for 2 h at a programmed temperature rise rate of 5 °C / min to obtain the sample Pd1Cu1 / Sigma.
[0114] The XRD pattern of the sample is shown below. Figure 1 The -Pd1Cu1 / Sigma sample, as shown in the characterization diagram, exhibits characteristic diffraction peaks of Sigma molecular sieves at 2θ = 8.9°, 19.7°, and 26.6°, indicating that the synthesized sample is a pure-phase Sigma molecular sieve. SEM images are shown below. Figure 2 In Figures (c) and (d), the Sigma hydrogenation catalyst crystals have clear outlines, regular morphology, and are polyhedral in shape. The crystal size is approximately 1 μm-5 μm, the total BET specific surface area is 6.8 m² / g, and the pore size is 0.20 nm. No impurities are present, indicating that the synthesized sample is a Sigma hydrogenation catalyst.
[0115] Example 3
[0116] The preparation of Pd1Cu2 / Sigma is as follows:
[0117] The preparation of the pure silicon zeolite Sigma hydrogenation catalyst in this embodiment is basically the same as in Example 2, except that the amounts of palladium chloride and copper nitrate trihydrate are adjusted so that the molar ratio of Pd to Cu is 1:2.
[0118] The XRD pattern of the sample is shown below. Figure 1 -Pd1Cu2 / Sigma, as shown in the characterization diagram, exhibits characteristic diffraction peaks of Sigma molecular sieve at 2θ = 8.9°, 19.7°, and 26.6°, indicating that the synthesized sample is a Sigma molecular sieve; SEM images are shown below. Figure 2 In samples (e) and (f), the morphology is regular, with grain size of approximately 1 μm-5 μm, total BET specific surface area of 6.7 m² / g, and pore size of 0.22 nm. The porosity test results (based on N₂ adsorption method) are shown in Table 1, and their specific surface area conforms to the characteristics of Sigma zeolite.
[0119] Table 1. Specific surface area and intrinsic pore size of Sigma and Pd1Cu2 / Sigma
[0120]
[0121] Example 4
[0122] Pd1Cu3 / Sigma was prepared as follows:
[0123] The preparation of the pure silicon zeolite Sigma hydrogenation catalyst in this embodiment is basically the same as in Example 2, except that the amounts of palladium chloride and copper nitrate trihydrate are adjusted so that the molar ratio of Pd to Cu is 1:3.
[0124] The XRD pattern of the sample is shown below. Figure 1 -Pd1Cu3 / Sigma, as shown in the characterization diagram, exhibits characteristic diffraction peaks of Sigma molecular sieve at 2θ = 8.9°, 19.7°, and 26.6°, indicating that the synthesized sample is a Sigma molecular sieve; SEM images are shown below. Figure 2 In the figures (g) and (h), the Sigma hydrogenation catalyst crystals have clear outlines, regular morphology, and are polyhedral in shape, with a grain size of approximately 1 μm-5 μm; no impurities are present, indicating that the synthesized sample is a Sigma hydrogenation catalyst.
[0125] The XRD patterns of Examples 2-4 show that all samples retain the characteristic XRD diffraction peaks of Sigma-2, indicating that the introduction of metal does not disrupt the zeolite crystal framework; the grain size remains 1-5 μm with a regular morphology. Example 3 shows that the Pd1Cu2 / Sigma has a total specific surface area of 7.2 m² / g and a pore size maintained at 0.21 nm, indicating that the molecular sieve pore structure is preserved after metal loading. Catalytic evaluation: Pd1Cu2 / Sigma at 230 °C and a space velocity of 30000 h⁻¹... -1Under the given conditions, the acetylene conversion rate was 99% and the ethylene selectivity was 94.5%. In contrast, in Comparative Example 1, the single-metal Pd / Sigma had an acetylene conversion rate of 100% and an ethylene selectivity of only 85-90%. In Comparative Example 2, the single-metal Cu / Sigma had an acetylene conversion rate of only 9.6% and a selectivity of 97%, but its activity was severely insufficient.
[0126] The above comparison shows that single Pd catalysts have high activity, but severe side reactions of ethylene over-hydrogenation and low selectivity; single Cu catalysts have almost no hydrogenation activity; Pd-Cu bimetallic catalysts have a significant synergistic effect; a Pd / Cu molar ratio of 1:2 has the best overall performance; if the Cu content is too low, the alloy modification is insufficient and the selectivity improvement is limited; if the Cu content is too high, it dilutes the active sites of Pd and causes a decrease in acetylene conversion.
[0127] The Pd1Cu2 / Sigma sample from Example 3 was selected for the following performance evaluation:
[0128] (1) Performance evaluation of catalysts for selective hydrogenation of acetylene
[0129] The Pd1Cu2 / Sigma catalyst prepared in Example 3 was applied to the catalytic selective hydrogenation of acetylene. Specific reaction conditions were as follows: Catalyst performance evaluation was conducted in a fixed-bed continuous flow quartz reactor. The catalyst particle size was 40-60 mesh, and the dosage was 0.1 g. The reactant gas was a ternary mixture of H2 / C2H2 / N2 with a volume ratio of 2:2:96, with N2 as the equilibrium gas. The reaction volume hourly space velocity (VHSV) was 30,000 h⁻¹. -1 The catalytic reaction was carried out at 150℃-240℃, and activity data were collected after the reaction reached equilibrium. The products were analyzed by online gas chromatography (GC8860), and the C2H2 conversion and C2H4 selectivity were calculated using the following formulas.
[0130] ;
[0131] ;
[0132] Wherein, C2H2 (inlet) is the acetylene inlet; C2H2 (outlet) is the acetylene outlet; C2H4 (outlet) is the ethylene outlet; Others (outlet) is the outlet of other by-products, including ethane, n-butene, isobutene, 1,3-butadiene, etc.
[0133] The above experiments show that the Pd1Cu2 / Sigma catalyst prepared in this invention exhibits good catalytic performance (C2H2 conversion, C2H4 selectivity) in the catalytic selective hydrogenation of acetylene, as shown in the following results. Figure 4The Pd1Cu2 / Sigma catalyst exhibits excellent catalytic hydrogenation performance, with C2H2 conversion reaching 99% and C2H4 selectivity reaching 94.5% at 230℃. 230℃ was selected as the optimal reaction temperature.
[0134] (2) Evaluation of catalyst stability
[0135] The stability performance of the Pd1Cu2 / Sigma catalyst prepared in Example 3 was evaluated. The test apparatus and catalyst dosage were the same as those used in (1) the performance evaluation of selective hydrogenation of acetylene catalyst. The reactant gas was a ternary mixture of H2 / C2H2 / N2 with a volume ratio of 2:2:96, with N2 as the equilibrium gas, and the reaction volume hourly space velocity was 30000 h⁻¹. -1 The catalytic reaction was carried out at 230℃ for 35 h.
[0136] This invention utilizes online gas chromatography (GC8860) to test the catalytic selective hydrogenation stability of Pd1Cu2 / Sigma catalyst for acetylene, and the results are shown in the appendix. Figure 5 As shown in the figure, the catalyst of this invention exhibits good stability. With prolonged reaction time, catalyst agglomeration occurs on the outer surface of the support, and the active sites are covered by green oil products, resulting in a slight decrease in activity. Ethylene selectivity remains high for an extended period; acetylene conversion gradually decreases with operating time, presumably due to a small amount of carbon deposits covering the active sites. Compared to traditional alumina-supported Pd catalysts, the pure silicon support in this system has low acidity, suppresses carbon deposition rates, and exhibits better overall stability than traditional industrial support systems.
[0137] (3) Evaluation of the catalytic performance of catalysts for selective hydrogenation of acetylene at different space velocities
[0138] The Pd1Cu2 / Sigma catalyst prepared in Example 3 was applied at different space velocities (15000 h⁻¹). -1 30000h -1 45000h -1 In the catalytic selective hydrogenation reaction of acetylene, the test apparatus and catalyst dosage were the same as in Example 5. The reactant gas was a ternary mixture of H2 / C2H2 / N2 in a volume ratio of 2:2:96, with N2 as the equilibrium gas, and the gas space velocity was 15000 h⁻¹. -1 30000h -1 45000h -1 The reaction temperature was 150℃-240℃, and the results are shown in the appendix. Figure 6 As can be seen from the figure, the catalyst of this invention maintains high catalytic activity even at high space velocities. The catalyst exhibits high catalytic activity at a high space velocity of 45,000 h⁻¹. -1It maintains a high acetylene conversion rate and ethylene selectivity, thanks to the optimized mass transfer of the Sigma-2 grains with stacked pores on the outer surface. The grain size is suitable, and the active sites can efficiently contact the reactants, making it suitable for high-space-velocity industrial operations.
[0139] Comparative Example 1
[0140] The catalyst preparation process in this comparative example is basically the same as in Example 3, except that copper nitrate trihydrate is not added. The resulting sample is denoted as Pd / Sigma.
[0141] In the performance evaluation of the pure silica zeolite Sigma hydrogenation catalyst prepared in this comparative example, the C2H2 conversion rate was 100% and the C2H4 selectivity was in the range of 85%-90% in the catalytic selective hydrogenation of acetylene.
[0142] Comparative Example 2
[0143] The catalyst preparation process in this comparative example is basically the same as in Example 3, except that palladium chloride is not added. The resulting sample is denoted as Cu / Sigma.
[0144] In the performance evaluation of the pure silica zeolite Sigma hydrogenation catalyst prepared in this comparative example, the C2H2 conversion rate was 9.6% and the C2H4 selectivity was within the range of 97%.
[0145] Comparative Examples 1 and 2 show that loading only palladium or only copper is not conducive to optimizing the catalyst performance. However, loading both palladium and copper simultaneously can significantly improve the catalyst performance through their synergistic effect, making it suitable for the thermocatalytic hydrogenation reaction to remove trace amounts of acetylene from ethylene.
[0146] Group 2: The only difference from Example 2 is the use of different carriers (fixed Pd-Cu active component, Pd:Cu=1:2, Pd loading 0.4wt%).
[0147] serial number sample Carrier Description Example 1-1 <![CDATA[Pd1Cu2 / Sigma-2-2]]> After crystallization at 170℃ for 1.5 days, the total specific surface area was 5 m² / g. Examples 1-2 <![CDATA[Pd1Cu2 / Sigma-2-3]]> Approximately 0.02 g of Sigma seed crystals were added to the mixed system, resulting in a total specific surface area of 9.5 m² / g. Compare with Example 1-1 <![CDATA[Pd1Cu2 / α-Al2O3]]> The mixed solution of commercially available α-alumina carriers with the same specific surface area was replaced with a dispersion containing an equal mass of carrier. Compare with Examples 1-2 <![CDATA[Pd1Cu2 / Silicalite-1]]> The difference from Comparative Example 1-1 is that the support was replaced with an all-silica MFI zeolite (Silicalite-1) support. Compare with Examples 1-3 <![CDATA[Pd1Cu2 / Sigma-Al]]> The difference from Comparative Example 1-1 is that the support was replaced with an aluminum-containing Sigma molecular sieve (non-Sigma-2) support.
[0148] The comparison results show that the Sigma-2 support group of this invention has both high acetylene conversion and high ethylene selectivity; the aluminum-containing Sigma support has acidic sites, which increases carbon deposition and decreases selectivity; the α-Al2O3 metal has poor dispersion and low selectivity, with an acetylene conversion of 56.9% and a selectivity of 80.5% under the same reaction conditions; the Silicalite-1 has a different pore structure, weak sieving effect, and lower selectivity than Sigma-2.
[0149] Group 3: The only difference from Example 2 is that the additive M is different and the Pd / M molar ratio is different (the carrier is uniformly Sigma-2, and the Pd loading is 0.4wt%).
[0150] Group A: Fixed Pd, but different additives M were used, with a molar ratio of Pd:M = 1:2
[0151]
[0152] This comparative study shows that Cu, Zn, and Ga can all improve selectivity as additives; the Pd:Cu ratio of 1-3 exhibits the best overall performance; too low a Cu ratio results in insufficient modification; too high a Cu ratio dilutes the active sites of Pd, leading to a decrease in acetylene conversion; single Pd exhibits poor selectivity; single Cu shows almost no activity. The addition of Na increases acidity, causing active sites to aggregate and reducing activity.
[0153] Group 4: The only differences from Example 2 are: the in-situ crystallization process versus the impregnation method; and the comparison of key process parameters.
[0154] The embodiments in this group used Sigma-2 carrier, with a target Pd:Cu ratio of 1:2 and a Pd loading of 0.4 wt%.
[0155]
[0156] The comparison results show that the in-situ seeding method yields catalysts with higher metal dispersion and better catalytic activity and selectivity than the post-impregnation method; the seedless synthesis sample has more impurities and uneven grain size; lacking hydrogen reduction, the metal exists in the form of oxides, and the hydrogenation activity is significantly reduced.
[0157] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within this disclosure. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0158] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A pure silica zeolite Sigma hydrogenation catalyst, comprising: The carrier is Sigma-2 type pure silica zeolite with deposited pores formed on its outer surface; An active ingredient, loaded on a carrier, comprises a Pd-based component and an auxiliary agent. The metal element M in the auxiliary agent is selected from Cu, Zn, Fe, Ce, Ni, Ga, Ag, and Au, wherein: The loading of Pd-based components on the support, based on the mass of Pd, accounts for 0.05 wt% to 3.0 wt% of the support mass; The loading of the additives on the carrier, based on the mass of the metal element M, accounts for 0.05wt%-3.0wt% of the carrier mass.
2. The pure silica zeolite Sigma hydrogenation catalyst according to claim 1, characterized in that, The total specific surface area of the outer surface of the carrier is 5m². 2 / g-10m 2 / g; and / or, The intrinsic pore size of the outer surface of the carrier is less than 0.3 nm.
3. The pure silica zeolite Sigma hydrogenation catalyst according to claim 1, characterized in that, The catalyst has a particle size of 1μm-5μm.
4. The method for preparing the pure silica zeolite Sigma hydrogenation catalyst according to any one of claims 1-3, comprising: S1. Mix appropriate amounts of structure directing agent, silicon source, mineralizer and solvent to obtain a mixed solution; S2. The mixed solution, Pd source, metal element M source and seed crystal are mixed to form a mixed system. After crystallization, filtration, washing, drying and calcination, pure silicon zeolite Sigma hydrogenation catalyst is obtained.
5. The preparation method according to claim 4, characterized in that, The structure-directing agent described in S1 is at least one of 1-adamantaneamine and ethylenediamine; and / or, The silicon source is at least one of silica sol and tetramethoxysilane; and / or, The mineralizing agent is at least one of anhydrous potassium fluoride and anhydrous sodium fluoride; and / or, The solvent is at least one of water and ethanol.
6. The preparation method according to claim 4, characterized in that, The molar ratio of the structure directing agent to the silicon source described in S1 is 1:(1-4); and / or, The molar ratio of the silicon source to the mineralizer is 1:(1-3); and / or, The molar ratio of the deionized water to the silicon source is (20-100):
1.
7. The preparation method according to claim 4, characterized in that, The amount of seed crystals added in S2 is 0.1wt%-0.3wt% of the total mass of the mixed system; and / or, The molar ratio of the palladium source to the metal element M source is 1:(1-3).
8. The preparation method according to claim 4, characterized in that, The crystallization described in S2 involves stirring at room temperature for 2-4 hours, followed by holding at 150℃-200℃ for 1-3 days.
9. The preparation method according to claim 4, characterized in that, The calcination conditions described in S2 are: first, under an air atmosphere, at (2-10) °C·min. -1 The temperature was increased to 500℃-800℃ and held for 5-8 hours; then heated at (5-10)℃·min under a hydrogen atmosphere. -1 Increase the temperature at a rate of 150℃-300℃ and maintain it for 1-3 hours.
10. The application of the pure silica zeolite Sigma hydrogenation catalyst according to any one of claims 1-3 in the catalytic selective hydrogenation reaction of acetylene.