Molecular sieve-based ammoxidation catalyst, method for preparing the same, and use thereof

By introducing copper complex precursors in situ and impregnating them during the molecular sieve synthesis process, an aluminum-rich molecular sieve-based catalyst was prepared. This solved the problems of byproduct generation and N₂ selectivity reduction in the ammonia oxidation process of noble metal catalysts, and achieved highly efficient selective catalytic oxidation of ammonia, which is suitable for treating mobile source waste gas.

CN123148987APending Publication Date: 2026-11-24JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611418120.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, noble metal catalysts are prone to generating byproducts such as N₂O and NOₓ during the selective catalytic oxidation of ammonia. Furthermore, when the copper loading is increased, CuO clusters enhance the oxidation step but weaken the SCR activity, resulting in a decrease in N₂ selectivity and making it difficult to balance the distribution of the two types of copper species.

Method used

In situ, copper complex precursors are introduced into the molecular sieve during the synthesis process. Combined with impregnation treatment, aluminum-rich molecular sieve-based catalysts are prepared. By controlling the distribution of copper and the second metal, an eight-membered ring channel structure is formed, achieving uniform distribution and functional differentiation of copper species.

Benefits of technology

It achieves efficient conversion of ammonia to N₂ at low temperatures while maintaining high N₂ selectivity, thus broadening the catalytic activity temperature window and making it suitable for treating ammonia oxidation reactions in motor vehicle, ship, and industrial waste gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148987A_ABST
    Figure CN123148987A_ABST
Patent Text Reader

Abstract

This invention discloses a molecular sieve-based ammonia oxidation catalyst, its preparation method, and its application, belonging to the field of catalytic materials technology. The preparation method of the molecular sieve-based ammonia oxidation catalyst includes: introducing a copper-containing complex precursor for crystallization during the synthesis of the molecular sieve to form an alumina-rich molecular sieve with an eight-membered ring channel structure; introducing copper species in situ into the alumina-rich molecular sieve during the crystallization process; impregnating the alumina-rich molecular sieve with a precursor solution containing a second metal, thereby loading the second metal onto the alumina-rich molecular sieve to obtain an impregnation product; and drying and calcining the impregnation product to obtain the molecular sieve-based ammonia oxidation catalyst. The catalyst prepared by this invention exhibits a uniform distribution of active components, demonstrates good catalytic activity and selectivity in the selective oxidation of ammonia, has wide applicability, and shows good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic materials technology, specifically relating to a molecular sieve-based ammonia oxidation catalyst, its preparation method, and its application. Background Technology

[0002] Selective catalytic oxidation of ammonia (NH3-SCO) is currently recognized as one of the effective methods to address ammonia slip from mobile sources. Noble metal catalysts are widely used in this field due to their excellent low-temperature catalytic activity. However, with increasingly stringent environmental emission standards, noble metal catalysts often produce N2O and NO2 due to over-oxidation in practical applications. x Byproducts such as these cause new environmental problems, challenging their applicability.

[0003] Compared to noble metal systems, copper-based species supported on molecular sieves exhibit differentiated catalytic functions. Among them, CuO or CuO x The clusters possess moderate oxidizing power, capable of selectively oxidizing some NH3 to NO; while isolated Cu within the molecular sieve framework or channels... 2+ These species possess the ability to catalyze the SCR reaction between NO and the remaining NH3. The two work synergistically to achieve the NH3→N2 conversion pathway (i.e., the i-SCR mechanism), thus maintaining high N2 selectivity while ensuring NH3 conversion. Molecular sieve supports, with their abundant and tunable Brønsted acid sites, are widely considered promising catalyst supports.

[0004] However, in existing technologies, increasing the copper loading to improve low-temperature activity often leads to the formation of large amounts of CuO clusters. While these species can enhance the oxidation process, they weaken isolated Cu atoms with SCR activity. 2+ The ratio leads to increased side reactions and a significant decrease in N2 selectivity. Therefore, how to effectively balance the distribution of the two copper species while increasing the copper loading remains a pressing technical challenge in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a molecular sieve-based ammonia oxidation catalyst, its preparation method, and its application, in order to solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the embodiments of the present invention provide the following technical solutions:

[0007] A method for preparing a molecular sieve-based ammonia oxidation catalyst includes the following steps:

[0008] In the process of synthesizing molecular sieves, copper-containing complex precursors are introduced for crystallization treatment to produce aluminum-rich molecular sieves with an eight-membered ring channel structure. During the crystallization treatment, copper species are introduced in situ into the aluminum-rich molecular sieves.

[0009] The aluminum-rich molecular sieve is impregnated with a precursor solution containing a second metal to load the second metal onto the aluminum-rich molecular sieve, thereby obtaining the impregnation product.

[0010] The impregnated product was dried and calcined to obtain a molecular sieve-based ammonia oxidation catalyst.

[0011] Furthermore, in the process of synthesizing molecular sieves, a step of introducing a copper-containing complex precursor for crystallization treatment is included, specifically:

[0012] An aluminum source, a silicon source, an alkali source, a copper-containing complex precursor, and a solvent are mixed to prepare a synthetic gel.

[0013] The synthetic gel was crystallized to obtain an aluminum-rich molecular sieve with an eight-membered ring pore structure; the crystallization treatment was carried out at a temperature of 100-200 °C for 12-216 hours.

[0014] Further, the aluminum source is selected from one or more of aluminum oxides, aluminum hydroxides, and aluminum salts, preferably boehmite, sodium aluminate, or aluminum hydroxide; the silicon source is selected from one or more of silica, silica sol, silica gel, tetraethyl orthosilicate, sodium silicate, and potassium silicate, preferably silica; the alkali source is potassium hydroxide and / or sodium hydroxide; the copper-containing complex precursor is selected from divalent copper and ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, or ammonia. One or more complexes are formed; the solvent is water; the molar ratios of the components in the synthetic gel are as follows: SiO2 / Al2O3=(4-40):1, preferably, SiO2 / Al2O3=(4-10):1; Na2O / SiO2=(0-0.8):1; K2O / SiO2=(0-0.5):1; H2O / SiO2=(4-60):1; Cu / SiO2=(0.01-0.12):1.

[0015] Furthermore, a structure-directing agent is added to the synthetic gel; depending on the topology of the target molecular sieve, the structure-directing agent may be selected from N,N-diethyl-3,5-dimethylpiperidinium hydroxide, 18-crown ether-6, hexamethylammonium divalent cation, pyrrolidine, N,N-dimethyl-1,4-diazabicyclo[2.2.2]octane divalent cation or N,N,N-trimethyl-1-adamantylammonium hydroxide, etc.; the alumina-rich molecular sieve has at least one topology selected from the following group: OFF / ERI symbiosis, CHA, AEI, AFX, FER, LEV, KFI, RTH, SFW and any combination or symbiotic structure thereof.

[0016] Furthermore, the topological structure of the alumina-rich molecular sieve is an OFF / ERI symbiotic structure, wherein the mass percentage of the ERI phase is 20%-80% and the mass percentage of the OFF phase is 80%-20%. Specifically, the mass percentage of the ERI and OFF phases can be controlled by adjusting the silica-alumina ratio, sodium-potassium ratio, alkalinity, amount of structure directing agent, type and amount of seed crystals, crystallization temperature and crystallization time of the synthesized gel.

[0017] Furthermore, the second metal is selected from at least one of Cu, Mn, Fe, Co, Ni, Ce, La, Pt, Pd, Ru, Rh, Ag, and Au; in the selective catalytic oxidation of ammonia, the second metal mainly provides low-temperature ammonia activation and oxygen activation sites, promoting NH3 oxidation; the copper species of the first metal mainly participates in the intermediate nitrogen-containing species or in-situ generation of NO. x Further conversion to improve N2 selectivity and reduce NO x Byproducts; the two types of metal sites constitute a tandem reaction or synergistic catalytic process, thus balancing low-temperature NH3 conversion activity and N2 selectivity. It should be noted that when selecting the second metal, a noble metal with strong oxidizing power is usually chosen, but over-oxidation may occur, leading to byproducts. Alternatively, a non-noble metal with less oxidizing power can be chosen.

[0018] Wherein, when the second metal is Cu, the precursor solution is an aqueous solution of one or more of copper nitrate, copper sulfate, copper acetate and copper chloride;

[0019] When the second metal is Mn and / or Ce, the precursor solution is an aqueous solution of one or more of manganese nitrate, manganese acetate, cerium nitrate, and cerium acetate.

[0020] Furthermore, the impregnation treatment is either equal-volume impregnation or excessive impregnation; the impregnation treatment time is 1-24 hours, and the temperature is 20-80 ℃; the drying temperature is 80-150 ℃, and the time is 4-24 hours; the calcination temperature is 400-650 ℃, and the time is 2-10 hours, and the calcination atmosphere is an oxygen-containing atmosphere (such as air or oxygen atmosphere).

[0021] Another object of the present invention is to provide a molecular sieve-based ammonia oxidation catalyst prepared by the above preparation method, wherein the active component comprises:

[0022] In situ introduction of copper species into the molecular sieve framework or channels during the crystallization process of alumina-rich molecular sieves; and

[0023] Second metal species loaded onto alumina-rich molecular sieves through impregnation post-treatment;

[0024] The total metal content in the molecular sieve-based ammonia oxidation catalyst is greater than 3 wt.% based on oxides, and the atomic ratio of total metal to Al is greater than 0.4; the molar ratio of copper species to the second metal species in the molecular sieve-based ammonia oxidation catalyst is 1:0.05-1:2.

[0025] Another object of the present invention is to provide the application of the above-mentioned molecular sieve-based ammonia oxidation catalyst in ammonia selective catalytic oxidation reaction, wherein the ammonia selective catalytic oxidation reaction is carried out in the presence of oxygen.

[0026] Furthermore, the space velocity of the selective catalytic oxidation reaction of ammonia is 5000-200000 h⁻¹. -1 The reaction temperature is 150-600 ℃; the ammonia selective catalytic oxidation reaction is used to treat ammonia-containing waste gas; the ammonia-containing waste gas is selected from at least one of motor vehicle exhaust, ship exhaust, industrial waste gas and stationary source flue gas.

[0027] The method for preparing a molecular sieve-based ammonia oxidation catalyst provided by this invention can yield a catalyst with a uniform distribution of active components. This catalyst exhibits good catalytic activity and selectivity in the selective oxidation of ammonia, has wide applicability, and shows promising application prospects. Compared with the prior art, this invention has at least the following beneficial effects:

[0028] (1) Copper-containing complex precursors participate in nucleation and crystal growth during molecular sieve crystallization, which helps to confine some copper species in the eight-membered ring channels, cages or exchange sites, and reduces uncontrolled aggregation that occurs when the post-loaded high copper content occurs.

[0029] (2) By combining two metal introduction methods, namely crystallization in situ introduction and impregnation post-treatment, the metal species inside the channel and near the outer surface can be controlled respectively, providing spatially adjacent but functionally different active sites for the ammonia oxidation step and subsequent transformation of nitrogen-containing intermediate products.

[0030] (3) The range of second metals is relatively wide. Cu, Mn, Ce, Fe or other metals can be selected according to the specific requirements of low temperature activity, N2 selectivity, water resistance or hydrothermal stability, and the ratio of Cu / second metal can be adjusted.

[0031] (4) The method of the present invention is applicable to various eight-membered ring molecular sieve topologies and can obtain molecular sieve-based ammonia oxidation catalysts with different pore environments by adjusting the silicon-aluminum ratio, alkali metal ratio, structure directing agent and crystallization conditions. Attached Figure Description

[0032] Figure 1 The XRD pattern of the molecular sieve sample synthesized for the example is shown.

[0033] Figure 2The graph shows the NH3 conversion rate of the catalysts prepared in the examples and comparative examples as a function of reaction temperature.

[0034] Figure 3 The graph shows the N2 selectivity of the catalysts prepared in the examples and comparative examples as a function of reaction temperature.

[0035] Figure 4 The graph shows the NO selectivity of the catalysts prepared in the examples and comparative examples as a function of reaction temperature.

[0036] Figure 5 The graph shows the NO2 selectivity of the catalysts prepared in the examples and comparative examples as a function of reaction temperature.

[0037] Figure 6 The graph shows the N2O selectivity of the catalysts prepared in the examples and comparative examples as a function of reaction temperature. Detailed Implementation

[0038] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0039] It should be noted that, in the embodiments of the present invention, the materials, reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0040] Example 1: This example provides a method for preparing an in-situ copper-post-impregnated copper / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst, the main steps of which are as follows:

[0041] (1) Add 25.00 g of deionized water to the reaction vessel, and add 2.122 g of sodium hydroxide with a mass fraction of 98%, 1.188 g of potassium hydroxide with a mass fraction of 85%, 1.500 g of boehmite and 6.008 g of silica in sequence under stirring. Continue stirring for 1 h to obtain a slurry. The molar ratio of SiO2 to Al2O3 in the slurry is 8:1, and the corresponding Si / Al atomic ratio is 4:1.

[0042] (2) Weigh 1.582 g of copper nitrate trihydrate and 0.787 g of ethylenediamine, and dissolve them separately in a small amount of deionized water; slowly add the ethylenediamine solution to the copper nitrate solution, and stir at 25 °C for 30 min to obtain Cu. 2+A copper-ethylenediamine complex solution with a molar ratio of approximately 1:2 to ethylenediamine was prepared. This complex solution was added to the slurry from step (1), and stirring was continued for 2 h. The mixture was then aged in a sealed container at 25 ℃ for 12 h to obtain a copper-containing synthetic gel. The SiO2 / Al2O3 molar ratio of the synthetic gel was 8:1, the corresponding nominal Si / Al atomic ratio was 4:1, and the Cu / SiO2 molar ratio was approximately 0.066:1.

[0043] (3) The above-synthesized gel was transferred to a polytetrafluoroethylene-lined reactor, with the liquid volume not exceeding 80% of the effective volume, and statically crystallized at 150 °C for 120 h. After cooling, it was filtered, washed with deionized water until the filtrate was nearly neutral, and dried at 110 °C for 12 h to obtain an OFF / ERI molecular sieve with an eight-membered ring pore structure containing in-situ copper species.

[0044] (4) Take 5.000 g of the above molecular sieve, dissolve 0.310 g of copper nitrate trihydrate in 50 mL of deionized water, add the molecular sieve powder, stir at 60 °C for 4 h, and then evaporate the water under reduced pressure at 70 °C. Dry the resulting solid at 110 °C for 12 h, raise the temperature to 550 °C at 2 °C / min and calcine in air for 6 h to obtain the in-situ copper-post-impregnated copper / OFF-ERI catalyst, denoted as Cu(in)-Cu(im) / OFF-ERI-1.

[0045] Example 2: This example provides a method for preparing an in-situ copper-post-impregnated manganese / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst, the main steps of which are as follows:

[0046] OFF / ERI molecular sieve raw powder containing in-situ copper species was prepared according to steps (1) to (3) of Example 1. The SiO2 / Al2O3 molar ratio of the molecular sieve raw powder was 8:1, and the corresponding nominal Si / Al atomic ratio was 4:1. 5.000 g of molecular sieve raw powder was taken, and 0.146 g of manganese nitrate tetrahydrate was dissolved in 50 mL of deionized water. The solution was impregnated in excess at 60 °C for 4 h, and then the water was removed by vacuum evaporation. The resulting solid was dried at 110 °C for 12 h and calcined in air at 500 °C for 4 h to obtain the in-situ copper-post-impregnated manganese / OFF-ERI catalyst, denoted as Cu(in)-Mn(im) / OFF-ERI-2.

[0047] Example 3: This example provides a method for preparing an in-situ copper-post-impregnated cerium / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst, the main steps of which are as follows:

[0048] OFF / ERI molecular sieve raw powder containing in-situ copper species was prepared according to steps (1) to (3) of Example 1. The SiO2 / Al2O3 molar ratio of the molecular sieve raw powder was 8:1, and the corresponding nominal Si / Al atomic ratio was 4:1. 5.000 g of molecular sieve raw powder was taken, and 0.127 g of cerium nitrate hexahydrate was dissolved in 50 mL of deionized water. The solution was impregnated in excess at 60 °C for 4 h, and then the water was removed by vacuum evaporation. The resulting solid was dried at 110 °C for 12 h and calcined in air at 500 °C for 4 h to obtain the in-situ copper-impregnated cerium / OFF-ERI catalyst, denoted as Cu(in)-Ce(im) / OFF-ERI-3.

[0049] Example 4: This example provides a method for preparing an in-situ copper-post-impregnated manganese / CHA molecular sieve-based ammonia oxidation catalyst, the main steps of which are as follows:

[0050] Based on 0.100 mol SiO2, silicon source (fumed silica), aluminum source (aluminum hydroxide), sodium hydroxide, N,N,N-trimethyl-1-adamantyl ammonium hydroxide (TMAdaOH), copper-tetraethylenepentamine complex (Cu-TEPA), and water were prepared to a molar composition (based on the molar ratio with SiO2) of SiO2:Al2O3:NaOH:TMAdaOH:Cu:H2O = 1:0.125:0.20:0.20:0.066:20, wherein the molar ratio of Cu to tetraethylenepentamine was 1:1. The SiO2 / Al2O3 molar ratio of the gel was 8:1, and the corresponding Si / Al atomic ratio was 4:1, consistent with Example 2. If fumed silica, aluminum hydroxide, and sodium hydroxide were used, the corresponding feed amounts would be 6.008 g, 1.950 g, and 0.800 g, respectively.

[0051] The synthesized gel was stirred at room temperature for 2 h and then transferred to a reactor for dynamic or static crystallization at 160 °C for 120 h. After filtration, washing, and drying at 110 °C for 12 h, CHA raw powder with an eight-membered ring channel structure containing in-situ copper species was obtained. 5.000 g of CHA raw powder was taken and impregnated with an excess of 0.146 g of manganese nitrate tetrahydrate according to the method in Example 2. After drying and calcination at 500 °C for 4 h, an in-situ copper-post-impregnated manganese / CHA catalyst was obtained, denoted as Cu(in)-Mn(im) / CHA-4.

[0052] Example 5: This example provides a method for preparing an in-situ copper-post-impregnated cerium / AEI molecular sieve catalyst, the main steps of which are as follows:

[0053] Based on 0.100 mol SiO2, silica, alumina, sodium hydroxide, N,N-diethyl-3,5-dimethylpiperidinium hydroxide (OSDA), copper-diethylenetriamine complex, and water were formulated to a molar composition (based on the molar ratio with SiO2) of SiO2:Al2O3:Na2O:OSDA:Cu:H2O = 1:0.125:0.25:0.15:0.066:30. The SiO2 / Al2O3 molar ratio of this AEI synthetic gel was 8:1, and the corresponding Si / Al atomic ratio was 4:1, consistent with Example 3. After crystallization at 140 °C for 100 h, solid-liquid separation, washing, and drying at 110 °C for 12 h yielded AEI raw powder with an eight-membered ring porous structure containing in-situ copper species. Take 5.000 g of AEI raw powder, impregnate it with 0.127 g of cerium nitrate hexahydrate according to the method of Example 3, dry it and calcine it at 500 °C for 4 h to obtain Cu(in)-Ce(im) / AEI-5.

[0054] Example 6: This example provides a method for preparing an in-situ copper-post-impregnated copper / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst.

[0055] Except for adjusting the amount of boehmite in step (1) of Example 1 from 1.500 g to 1.000 g, the other raw material types and amounts, preparation steps and process conditions are the same as in Example 1.

[0056] Based on the amount of feed, the initial SiO2 / Al2O3 molar ratio of the synthesized gel in this embodiment is 12:1, corresponding to a nominal Si / Al atomic ratio of 6:1. The resulting in-situ copper-post-impregnated copper / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst is denoted as Cu(in)-Cu(im) / OFF-ERI-6.

[0057] Example 7: This example provides a method for preparing an in-situ copper-post-impregnated copper / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst.

[0058] Except for adjusting the amount of boehmite in step (1) of Example 1 from 1.500 g to 0.600 g, the other raw material types and amounts, preparation steps and process conditions are the same as in Example 1.

[0059] Based on the amount of feed, the nominal SiO2 / Al2O3 molar ratio of the initial synthesized gel in this embodiment is 20:1, and the corresponding nominal Si / Al atomic ratio is 10:1. The resulting in-situ copper-post-impregnated copper / OFF-ERI symbiotic molecular sieve-based ammonia oxidation catalyst is denoted as Cu(in)-Cu(im) / OFF-ERI-7.

[0060] Comparative Example 1: This comparative example provides a method for preparing Cu-Mn / OFF-ERI molecular sieve catalysts using a stepwise impregnation method. The main steps are as follows:

[0061] Except for the absence of copper-ethylenediamine complex in the synthesized gel, the other raw material ratios and crystallization conditions were the same as in steps (1) and (2) of Example 1. After crystallization, solid-liquid separation, washing, and drying, an OFF / ERI molecular sieve support without in-situ copper species was obtained. X-ray diffraction characterization confirmed that the obtained support had the same OFF / ERI co-occurrence topology as in Example 1.

[0062] 5.000 g of the above OFF / ERI molecular sieve support was first impregnated with an aqueous copper nitrate solution. The amount of copper nitrate was calculated according to the target copper loading to ensure that the copper content in the resulting catalyst was close to that in the catalyst of Example 2. After impregnation, the catalyst was dried at 110 °C for 12 h to obtain the copper-impregnated intermediate product.

[0063] Subsequently, the intermediate product was impregnated a second time with an aqueous manganese nitrate solution. The amount of manganese nitrate used was calculated according to the target manganese loading, so that the manganese content in the resulting catalyst was close to that in the catalyst of Example 2. After impregnation, it was dried at 110 °C for 12 h and calcined at 550 °C for 6 h in air atmosphere to obtain a comparative catalyst impregnated with copper first and then with manganese, denoted as: Cu(im)-Mn(im) / OFF-ERI-D1.

[0064] Comparative Example 2: This comparative example provides a method for preparing an OFF / ERI molecular sieve catalyst with only in-situ copper, the main steps of which are as follows:

[0065] OFF / ERI molecular sieve raw powder containing in-situ copper species was prepared according to steps (1) to (3) of Example 1, but without second metal impregnation; the molecular sieve raw powder was directly calcined in air atmosphere at 550 °C for 6 h to obtain a comparative catalyst containing only in-situ copper species, denoted as Cu(in) / OFF-ERI-D2.

[0066] Comparative Example 3: This comparative example provides a method for preparing an in-situ copper-post-impregnated copper / ZSM-5 molecular sieve-based ammonia oxidation catalyst, using ZSM-5 molecular sieve instead of the OFF / ERI symbiotic molecular sieve in Example 1, as detailed below:

[0067] A copper complex precursor was added during the hydrothermal synthesis of ZSM-5 molecular sieve. After crystallization, solid-liquid separation, washing and drying, ZSM-5 molecular sieve raw powder containing in-situ copper species was obtained.

[0068] Take 5.000 g of the obtained molecular sieve raw powder and impregnate it with copper nitrate, dry it and calcine it according to the method described in step (4) of Example 1 to obtain the in-situ copper-post-impregnated copper / ZSM-5 molecular sieve-based ammonia oxidation catalyst, denoted as Cu(in)-Cu(im) / ZSM-5-D3.

[0069] Performance Testing: I. The XRD patterns of the molecular sieve samples synthesized in the above embodiments are as follows: Figure 1 As shown.

[0070] II. The metal-supported molecular sieve catalysts prepared in Examples 1-7 and Comparative Examples 1-2 were applied to the selective oxidation reaction of ammonia. The performance evaluation device for the catalysts consisted of a gas mixing and catalytic reaction experimental apparatus and a Fourier transform infrared spectrometer. The gas composition and concentration were: 500 ppm NH3, 20% O2, 5% H2O (when added), with N2 as the balance gas, a total gas flow rate of 250 mL / min, and a space velocity (GHSV) of 100,000 h⁻¹. -1 The catalyst sample content was 100 mg (40-60 mesh), and the NH3 conversion rate was ( N2 selectivity The NO selectivity, NO2 selectivity, and N2O selectivity are calculated as follows:

[0071]

[0072]

[0073]

[0074]

[0075]

[0076] Table 1. Comparison of NH3-SCO performance of catalysts prepared in the examples and comparative examples.

[0077] sample catalyst <![CDATA[Continuous temperature range with ≥95% NH3 conversion rate]]> <![CDATA[Continuous temperature range with ≥95% N₂ selectivity]]> Cu(in)-Cu(im) / OFF-ERI-1 250-500 ℃ 150-475 ℃ Cu(in)-Mn(im) / OFF-ERI-2 275-500 ℃ 150-300 ℃ With(in)-With(im) / OFF-ERI-3 225-500 ℃ 175-250 ℃ Cu(in)-Mn(im) / CHA-4 300-500 ℃ 200-300 ℃ Cu(in)-Ce(im) / AEI-5 225-500 ℃ 150-275 ℃ Cu(in)-Cu(im) / OFF-ERI-6 250-500 ℃ 150-300 ℃ Cu(in)-Cu(im) / OFF-ERI-7 250-500 ℃ 150-350 ℃ Cu(im)-Mn(im) / OFF-ERI-D1 250-500 ℃ 175-250 ℃ With / OFF-ERI-D2 275-500 ℃ 175-300 ℃ Cu(in)-Cu(im) / ZSM-5-D3 250-500 ℃ -

[0078] The test results are shown in Table 1 and Figure 2-Figure 6As shown in the figure. The Cu(in)-Cu(im) / OFF-ERI catalyst prepared in Example 1 exhibits a wide efficient reaction temperature window, with an NH3 conversion of no less than 95% in the range of 250-500 °C and an N2 selectivity of no less than 95% in the range of 150-475 °C. Therefore, both NH3 conversion and N2 selectivity of no less than 95% can be achieved simultaneously within the range of 250-475 °C. The Cu(in)-Mn(im) / OFF-ERI catalyst prepared in Example 2 exhibits an NH3 conversion of no less than 95% in the range of 275-500 °C and an N2 selectivity of no less than 95% in the range of 150-300 °C. The continuous temperature window in which both indicators simultaneously reach above 95% is 275-300 °C. The Cu(in)-Ce(im) / OFF-ERI catalyst prepared in Example 3 exhibits an NH3 conversion of no less than 95% in the temperature range of 225-500 °C and an N2 selectivity of no less than 95% in the temperature range of 175-250 °C. The continuous temperature window in which both indicators simultaneously reach 95% or higher is 225-250 °C. The Cu(in)-Mn(im) / CHA catalyst prepared in Example 4 achieves an NH3 conversion of no less than 95% and an N2 selectivity of no less than 95% in the temperature ranges of 300-500 °C and 200-300 °C, respectively. The temperature windows for these two indicators intersect at 300 °C. The Cu(in)-Ce(im) / AEI catalyst prepared in Example 5 exhibits an NH3 conversion of no less than 95% in the temperature range of 225-500 °C and an N2 selectivity of no less than 95% in the temperature range of 150-275 °C. The continuous temperature window in which both indicators simultaneously reach 95% or higher is 225-275 °C. The Cu(in)-Cu(im) / OFF-ERI catalysts prepared in Examples 6 and 7 exhibited NH3 conversion rates of no less than 95% within the temperature range of 250-500 °C, and N2 selectivity of no less than 95% within the temperature ranges of 150-300 °C and 150-350 °C, respectively. Therefore, the temperature ranges where both indicators simultaneously met the standards were 250-300 °C and 250-350 °C, respectively. Compared to Example 1, Examples 6 and 7 maintained the same temperature range for achieving the NH3 conversion standard, but the upper limit of the high N2 selectivity temperature range decreased, indicating that this data mainly reflects differences in selectivity retention capabilities.

[0079] In contrast, the Cu-Mn / OFF-ERI molecular sieve prepared by the stepwise impregnation method in Comparative Example 1 only simultaneously satisfies the requirement of NH3 conversion and N2 selectivity of not less than 95% around 250 °C; the continuous temperature window for simultaneously satisfying the above two indicators by only in-situ introducing copper OFF / ERI catalyst in Comparative Example 2 is 275-300 °C. Furthermore, comparing different pore structures, in the listed example data, both the OFF / ERI co-existing molecular sieve catalyst of Example 1 and the MFI-type ZSM-5 catalyst of Comparative Example 3 achieve NH3 conversion of not less than 95% in the range of 250-500 °C. However, the former maintains N2 selectivity of not less than 95% in the range of 250-475 °C, while the latter exhibits lower N2 selectivity. From the perspective of pore structure, the MFI-type molecular sieve has a larger pore size, which may facilitate the diffusion and escape of generated N2O, reducing the chance of it re-contacting with the active sites within the pores and undergoing subsequent transformation. In contrast, the octagonal ring pores and related cage environment may alter the residence time of nitrogen-containing intermediates and their contact probability with active sites through confinement and diffusion effects, thereby affecting product distribution. The above results indicate that the preparation method combining in-situ copper introduction via crystallization with subsequent metal impregnation can regulate catalyst activity and product selectivity. Specifically, the combination of in-situ and subsequent copper impregnation used in Example 1 resulted in highly dispersed Cu at the ion exchange sites of the molecular sieve. 2+ Nano-CuO / CuO formed by subsequent impregnation and calcination x It forms a bifunctional active center, achieving the widest overlapping temperature window with high conversion rate and high N2 selectivity.

[0080] Furthermore, low silica-to-alumina ratio molecular sieves possess a high framework Al density, providing more framework negative charges and potential cation exchange sites, which is beneficial for increasing the loading of metal species and regulating their dispersion state. In-situ introduction of copper during crystallization, combined with subsequent impregnation with a second metal, can further regulate the quantity, spatial distribution, and redox properties of metal species inside and outside the molecular sieve channels. This promotes the adsorption and activation of NH3, selective oxidation, and subsequent reactions between nitrogen-containing intermediates and remaining NH3, thereby broadening the reaction temperature window to achieve both high NH3 conversion and N2 selectivity.

[0081] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification.

Claims

1. A method for preparing a molecular sieve-based ammonia oxidation catalyst, characterized in that, Includes the following steps: In the process of synthesizing molecular sieves, copper-containing complex precursors are introduced for crystallization treatment to produce aluminum-rich molecular sieves with an eight-membered ring channel structure. During the crystallization treatment, copper species are introduced in situ into the aluminum-rich molecular sieves. The aluminum-rich molecular sieve is impregnated with a precursor solution containing a second metal to load the second metal onto the aluminum-rich molecular sieve, thereby obtaining the impregnation product. The impregnated product was dried and calcined to obtain a molecular sieve-based ammonia oxidation catalyst.

2. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 1, characterized in that, In the process of synthesizing molecular sieves, the step of introducing a copper-containing complex precursor for crystallization treatment specifically includes: An aluminum source, a silicon source, an alkali source, a copper-containing complex precursor, and a solvent are mixed to prepare a synthetic gel. The synthetic gel was crystallized to obtain an aluminum-rich molecular sieve with an eight-membered ring pore structure; the crystallization treatment was carried out at a temperature of 100-200 °C for 12-216 hours.

3. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 2, characterized in that, The aluminum source is selected from one or more of aluminum oxides, aluminum hydroxides, and aluminum salts; the silicon source is selected from one or more of silicon oxides and silicates; the alkali source is potassium hydroxide and / or sodium hydroxide; the copper-containing complex precursor is selected from complexes formed by divalent copper with one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and ammonia; the solvent is water; the molar ratios of the components in the synthetic gel are as follows: SiO2 / Al2O3=(4-40):1; Na2O / SiO2=(0-0.8):1; K2O / SiO2=(0-0.5):1; H2O / SiO2=(4-60):1; Cu / SiO2=(0.01-0.12):

1.

4. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 2, characterized in that, The synthetic gel also contains a structure-directing agent; the alumina-rich molecular sieve has at least one topological structure selected from the group consisting of: OFF / ERI symbiosis, CHA, AEI, AFX, FER, LEV, KFI, RTH, SFW and any combination or symbiotic structure thereof.

5. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 4, characterized in that, The alumina-rich molecular sieve has an OFF / ERI symbiotic topology, wherein the mass percentage of the ERI phase is 20%-80% and the mass percentage of the OFF phase is 80%-20%.

6. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 1, characterized in that, The second metal is selected from at least one of Cu, Mn, Fe, Co, Ni, Ce, La, Pt, Pd, Ru, Rh, Ag, and Au; When the second metal is Cu, the precursor solution is an aqueous solution of one or more of copper nitrate, copper sulfate, copper acetate, and copper chloride. When the second metal is Mn and / or Ce, the precursor solution is an aqueous solution of one or more of manganese nitrate, manganese acetate, cerium nitrate, and cerium acetate.

7. The method for preparing the molecular sieve-based ammonia oxidation catalyst according to claim 1, characterized in that, The impregnation treatment lasts for 1-24 hours at a temperature of 20-80°C; the drying temperature is 80-150°C for 4-24 hours; and the calcination temperature is 400-650°C for 2-10 hours in an oxygen-containing atmosphere.

8. A molecular sieve-based ammonia oxidation catalyst prepared by any one of claims 1-8, characterized in that, The active components in the molecular sieve-based ammonia oxidation catalyst include: In situ introduction of copper species into the molecular sieve framework or channels during the crystallization process of alumina-rich molecular sieves; and Second metal species loaded onto alumina-rich molecular sieves through impregnation post-treatment; The total metal content in the molecular sieve-based ammonia oxidation catalyst is greater than 3 wt.% based on oxides, and the atomic ratio of total metal to Al is greater than 0.4; the molar ratio of copper species to the second metal species in the molecular sieve-based ammonia oxidation catalyst is 1:0.05-1:

2.

9. The application of the molecular sieve-based ammonia oxidation catalyst as described in claim 8 in the selective catalytic oxidation of ammonia, characterized in that, The selective catalytic oxidation of ammonia is carried out in the presence of oxygen.

10. The application according to claim 9, characterized in that, The space velocity of the ammonia selective catalytic oxidation reaction is 5000-200000 h -1 The reaction temperature is 150-600 ℃; the ammonia selective catalytic oxidation reaction is used for treating ammonia-containing waste gas; and the ammonia-containing waste gas is selected from at least one of motor vehicle exhaust, ship exhaust, industrial waste gas and stationary source flue gas.