Cobalt-based electrospun fiber catalysts induced by hydrogen peroxide and methods of making and using the same
By combining in-situ growth with defect engineering, the cobalt-based electrospun fiber catalyst prepared solves the problems of insufficient stability and activity of MOF catalysts, and achieves the effect of efficient degradation of organic pollutants.
Patent Information
- Application Number
- CN202611663878.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-27
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional MOFs suffer from insufficient exposure of active sites, limited electron transport efficiency, and poor stability in catalysts. They are particularly prone to detachment in liquid-phase reactions, resulting in poor catalytic performance.
In-situ growth combined with defect engineering was employed to prepare cobalt-based electrospun fiber catalysts via electrospinning technology. Hydrogen peroxide was used to etch controllable hollow open defect structures, and the molar ratio of europium to cobalt was controlled at 1:5~20. Hydrogen peroxide was added in batches to form stable defect structures, thereby enhancing the stability and activity of the catalyst.
The catalyst's stability and catalytic activity have been improved, enabling it to effectively degrade a variety of organic pollutants. In particular, under the conditions of pH=7.3 and temperature of 25℃, the cobalt-based electrospun fiber catalyst can degrade 95.41% of norfloxacin within 20 minutes and maintain good degradation performance under different environments.
Smart Images

Figure CN123148996A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst preparation technology, specifically relating to a cobalt-based electrospun fiber catalyst induced by hydrogen peroxide corrosion, its preparation method, and its application. Background Technology
[0002] Metal-organic frameworks (MOFs) are porous materials formed by the self-assembly of metal ions or metal clusters with organic ligands through coordination bonds. They possess ultra-high specific surface area, tunable pore structure, and abundant active sites, showing great promise for applications in catalysis, adsorption, and environmental remediation. However, traditional MOFs often face challenges in practical applications, such as insufficient exposure of active sites and limited electron transport efficiency.
[0003] In the engineering applications of MOFs, electrospinning technology provides an effective approach for preparing easily separable and highly stable catalytic materials. Currently, the main method for preparing MOF / polymer composite fibers is direct growth spinning, which involves directly mixing MOF crystals with polymer spinning solutions and then spinning the resulting composite fibers. While direct growth spinning is simple to operate, it suffers from several drawbacks: the polymer matrix easily coats the MOF particles, clogging pores and masking active sites. Furthermore, in the prepared catalytic materials, the MOF crystals and fibers are only physically attached, resulting in weak interfacial bonding. This makes them prone to detachment in actual catalytic reactions, especially liquid-phase reactions, leading to poor stability and recyclability, ultimately affecting catalytic performance. Summary of the Invention
[0004] To address the problems existing in the prior art, this invention provides a hydrogen peroxide-induced corrosion cobalt-based electrospun fiber catalyst, its preparation method, and its application. By employing in-situ growth combined with defect engineering, the catalytic performance and catalyst stability are effectively improved. The specific technical solution is as follows.
[0005] A method for preparing a hydrogen peroxide-induced corrosion cobalt-based electrospun fiber catalyst includes the following steps: The cobalt-based precursor spinning solution is electrospun to obtain precursor electrospun fibers; the cobalt-based precursor spinning solution contains europium and cobalt in a molar ratio of 1:5~20. Precursor electrospun fibers are placed in a solution containing organic ligands and undergo a coordination reaction for 6 to 22 hours to obtain MOF / polymer composite fibers; the mass ratio of precursor electrospun fibers to ligands is 1:1 to 2. MOF / polymer composite fibers were placed in an aqueous system, and hydrogen peroxide was added as an etchant to form defects, thus obtaining the cobalt-based electrospun fiber catalyst. The mass-to-volume ratio of the MOF / polymer composite fibers to the hydrogen peroxide was 0.15 g: 60 μL~180 μL. The hydrogen peroxide was added in batches, with no less than two additions, and the interval between each addition was 80 min~160 min.
[0006] This invention addresses the challenges of improving catalytic performance and enhancing material stability by combining defect-engineered unsaturated metal sites with electrospun fiber structures. Hydrogen peroxide is a commonly used etchant in defect engineering, and its dosage or etching time is controlled to manage defect formation. However, during experiments, this invention found that existing methods of controlling hydrogen peroxide can lead to defect collapse, resulting in decreased stability and metal leakage, thus affecting catalyst activity. This invention prepares bimetallic CoEu-MOF precursor fibers using Co and Eu as metal sources. By adding hydrogen peroxide in batches at least twice, it not only controllably etches the coordination bonds in the MOF to form hollow, open, but non-collapsed defect structures, effectively increasing the number of active sites, but also further enhancing the catalyst's catalytic activity. Simultaneously, the introduction of rare earth Eu, while maintaining a europium to cobalt molar ratio of 1:5 to 20, not only improves the stability of the electrospun matrix catalyst but also further inhibits Co leaching, increasing recyclability and achieving the goal of degrading various organic pollutants.
[0007] In another preferred embodiment, the batch addition is performed 2 to 4 times, with the same volume added each time.
[0008] In another preferred embodiment, the parameters for electrospinning are as follows: The feed rate is 0.8 mL / h, and the voltage is 16 kV~20 kV.
[0009] In another preferred embodiment, the cobalt-based precursor spinning solution further contains polyvinylpyrrolidone and polyacrylonitrile, wherein the mass ratio of polyvinylpyrrolidone to cobalt is 0.25~0.26:1; The mass ratio of the polyacrylonitrile to the cobalt is 1:1 to 1.1.
[0010] In another preferred embodiment, the cobalt is derived from cobalt nitrate, the europium is derived from europium nitrate, and the ligand is 2-methylimidazole.
[0011] In another preferred embodiment, the reaction time for the defect is 16h to 18h.
[0012] In another preferred embodiment, the solvent in the solution containing the organic ligand is methanol.
[0013] The second aspect of the present invention provides a cobalt-based electrospun fiber catalyst prepared by the method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst.
[0014] The third aspect of the present invention provides the application of the cobalt-based electrospun fiber catalyst in the degradation of organic pollutants in water, characterized in that the organic pollutant is any one of levofloxacin, sulfamethoxazole, norfloxacin, rhodamine B, and tetracycline.
[0015] Compared with the prior art, the present invention has the following beneficial effects: This invention employs in-situ growth combined with defect engineering to effectively improve catalytic performance and enhance catalyst stability. By introducing rare earth element Eu, and under Europium and cobalt molar ratios of 1:5~20, Co leaching can be suppressed, increasing the number of cycles and improving stability. Furthermore, by combining hydrogen peroxide etching treatment, and through controlled dosage and batch addition of hydrogen peroxide, the coordination bonds in the MOF are etched in a controlled manner to form hollow, open, and non-collapsed defect structures, thereby controlling the morphology of the MOF material and effectively increasing the number of active sites. Simultaneously, it can further enhance the catalytic activity of the cobalt-based electrospun fiber catalyst. Experimental results show that this invention is effective at pH 7.3, temperature 25℃, and a cobalt-based electrospun fiber catalyst dosage of 0.1 g·L⁻¹. -1 Persulfate concentration 0.3 g·L -1 Under these conditions, the cobalt-based electrospun fiber catalyst can degrade 95.41% of norfloxacin within 20 minutes, with a cobalt ion leaching concentration of only 0.16 mg·L⁻¹. -1 The results demonstrate that the method described in this invention can effectively improve the stability of cobalt-based electrospun fiber catalysts, thereby enabling recycling. Furthermore, the cobalt-based electrospun fiber catalysts exhibit significant degradation effects on various recalcitrant pollutants, and maintain good degradation performance under different anionic environments and actual water quality conditions. Quenching experiments and electron paramagnetic resonance analysis show that •OH plays a major role in the degradation process. 1 O2 and SO4 •- The contribution is secondary. This invention, by combining defect-engineered unsaturated metal sites with electrospun fiber structures, provides experimental evidence for the development of efficient, stable, and easily recyclable MOF-based environmental functional materials. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the H2O2 etching process for manufacturing Eu-ZIF-67 / PAN or Eu-Co-BTC / PAN.
[0017] Figure 2 SEM images of Eu-ZIF-67 treated with different concentrations of H2O2: (a) 60 μL, (b) 120 μL, (c) 180 μL; the right column in the figure is a further magnified version of the left column.
[0018] Figure 3 SEM images of Eu-ZIF-67 under different single-drop H2O2 treatment volumes: (a) 40 μL × 3, (b) 120 μL × 1, (c) 30 μL × 4, (d) 60 μL × 2.
[0019] Figure 4 Scanning electron microscope images of different products; (a) and (b) are images of Eu. 3+ -Co 2+ Scanning electron microscope (SEM) images of 1:10-Eu-ZIF-67 / PAN at different magnifications: (c) and (d) at different magnifications for 6 h; (e) and (f) at different magnifications for 1:10-Eu-ZIF-67 / PAN at 14 h; (g) and (h) at different magnifications for 1:10-Eu-ZIF-67 / PAN at 22 h.
[0020] Figure 5 Scanning electron microscope images and EDS elemental mappings of different products; (a) for Eu 3+ -Co 2+ (a) Scanning electron microscope image of PAN, (b) Scanning electron microscope image of EZ-10H, (c) Scanning electron microscope image of EZP-10, (d) EDS elemental mapping of EZP-10H, (e) EDS elemental mapping of EZP-10H.
[0021] Figure 6 Scanning electron microscope (SEM) images of different products: (a) and (b) SEM images of ECP-10 at different magnifications, and (c) SEM image of ECP-10H.
[0022] Figure 7 XRD patterns of different products: (a) ZIF-67 / PAN, 1:20 Eu-ZIF-67 / PAN, 1:10 Eu-ZIF-67 / PAN, 1:5 Eu-ZIF-67 / PAN, (b) EZP-10H after H2O2 etching, (c) Co-BTC / PAN, 1:10 Eu-Co-BTC / PAN, (d) ECP-10H after H2O2 etching.
[0023] Figure 8High-resolution XPS spectra of different catalysts ZP-H, EZP-10, and EZP-10H: (a) full spectrum, (b) N 1s, (c) Co 2p, and (d) Eu 3d.
[0024] Figure 9 High-resolution XPS spectra of different catalysts CP-H, ECP-10, and ECP-10H: (a) full spectrum, (b) O 1s, (c) Co 2p, and (d) Eu 3d.
[0025] Figure 10 Figure 1 shows the catalytic effects of different catalysts on NOR; (a) the degradation effect of different EZP-10H / PMS on NOR, (c) the degradation effect of different ECP-10H / PMS on NOR and the changes in related reaction rate constants and degradation rates in (b) and (d); the reaction conditions were catalyst = 0.10 g·L⁻¹. -1 NOR = 10 mg·L -1 PMS = 0.30 g·L -1 Initial pH = 7.3, reaction temperature = 25℃.
[0026] Figure 11 Figures showing the catalytic effect analysis results; (a) different catalytic systems, (c) initial pH, (e) EZP-10H dosage, (g) effect of PMS dosage on NOR removal and related reaction rate constants, (b), (d), (f), (h), and (i) comparison of catalyst performance with previously reported catalysts; reaction conditions: catalyst = 0.10 g·L⁻¹ -1 NOR = 10 mg·L -1 PMS = 0.30 g·L -1 The initial pH was 7.3, and the reaction temperature was 25°C. The experiment was repeated three times for error analysis.
[0027] Figure 12 Figure 1 shows the results of the analysis of the effect of quencher on the degradation of NOR in the EZP-10H / PMS system; (a) effect of quencher on the degradation of NOR in the EZP-10H / PMS system, (b) change in degradation rate, and (c) different catalytic systems. 1 EPR spectrum of O2, (d) EPR spectrum of •OH and SO4 in different catalytic systems •- EPR spectra, (e) O2 in different catalytic systems •- EPR spectrum.
[0028] Figure 13 Possible pathways for NOR degradation in the EZP-10H / PMS system.
[0029] Figure 14Figure 1 shows the analytical results of NOR and its intermediates; (a) bioaccumulation factor, (b) LC-12 of Daphnia magna. 50 (c) Fish LC 50 (d) Mutagenicity and (e) Developmental toxicity.
[0030] Figure 15 Figures show the analytical results of organic matter degradation in different systems; (a) and (b) the effect of different anion doping on NOR degradation efficiency, (c) and (d) the degradation of different organic pollutants by the EZP-10H / PMS system, and (e) and (f) the degradation effect of the EZP-10H / PMS / NOR system in different aqueous media; reaction conditions: CIP, TC, LEV, SMX = 10 mg·L -1 RhB = 300 mg·L -1 Catalyst = 0.10 g·L -1 NOR = 10 mg·L -1 PMS = 0.30 g·L -1 Initial pH = 7.3, reaction temperature = 25℃.
[0031] Figure 16 Figures showing the analysis results of the stability of different systems: (a) Leaching concentration of Co in EZ-10H / PMS and EZP-10H / PMS systems, (b) Leaching concentration of Co in EZP-10H / PMS system under different pH conditions, (c) TOC removal efficiency of EZP-10H and ECP-10H at 5 min, 10 min, 15 min and 20 min of reaction, and (d) Cyclic data chart.
[0032] Figure 17 XRD patterns and XPS spectra of freshly prepared and used EZP-10H catalysts; (a) XRD patterns and XPS spectra; (b) N 1s, (c) Co 2p, (d) Eu 3d. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0034] Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0035] Defect engineering, by controllably introducing ligand absences, metal vacancies, or unsaturated coordination sites, can modulate the electronic structure and surface properties of MOFs, thereby enhancing their catalytic performance. In recent years, H2O2 etching has attracted considerable attention due to its mild and controllable characteristics. It can selectively oxidize ligands or metal nodes, generating abundant defect sites while maintaining framework integrity. The main purpose of H2O2 etching is to form hollow spherical structures, typically using a one-time addition or constant-flow dripping method to increase the number of defects and activity. However, the defect structures formed in this way can lead to defect collapse and decreased stability, resulting in metal leakage. Existing techniques usually control defect formation by changing the H2O2 concentration or etching time, but these methods cannot truly solve the problems of defect collapse and reduced stability.
[0036] This invention utilizes electrospinning combined with in-situ growth technology to prepare bimetallic CoEu-MOF precursor fibers using Co and Eu as metal sources. Controllable defects are induced by H₂O₂ etching to construct a defect-type CoEu-MOF electrospun fiber catalyst. Experiments revealed that the method of H₂O₂ addition significantly affects the etching-induced defects. Batch addition allows for controllable etching of surface coordination bonds, forming an open defect structure that does not collapse, further preventing Co leaching and improving catalytic efficiency. This material combines unsaturated metal sites generated by defect engineering with the three-dimensional network structure of electrospun fibers for activating PMS to degrade norfloxacin, providing experimental evidence for the development of efficient, stable, and easily recyclable MOF-based environmental functional materials.
[0037] 1. Preparation of cobalt-based electrospun fiber catalysts induced by hydrogen peroxide corrosion.
[0038] 1.1 x-Eu 3+ -Co 2+ Preparation of PAN precursor fibers.
[0039] 1.0 g of cobalt nitrate hexahydrate and europium nitrate hexahydrate were dissolved and ultrasonically dispersed in 10 mL of N,N-dimethylformamide. Then, under ultrasonication, 1 g of polyacrylonitrile with a molecular weight of 150,000 and 0.25 g of polyacrylonitrile with a molecular weight of 1.3 × 10⁻⁶ were added. 6 Polyvinylpyrrolidone was continuously stirred for 24 hours. The well-stirred viscous solution was poured into a 10 mL plastic syringe connected to a 19G needle and then connected to a high-voltage power supply. Electrospinning was performed at room temperature, with a 20 cm gap between the aluminum foil receiver and the needle tip. The feed rate was controlled at 0.8 mL / h using a syringe pump. -1 The voltage was set to 16kV. Precursor electrospun fibers x-Eu were obtained. 3 + -Co2+ / PAN, where x represents the molar ratio of cobalt nitrate hexahydrate to europium nitrate hexahydrate during the synthesis process, yielding 1:20-Eu 3+ -Co 2+ / PAN、1:10-Eu 3+ -Co 2+ / PAN and 1:5-Eu 3+ -Co 2+ / PAN.
[0040] 1.2 Synthesis of Eu-ZIF-67 / PAN and Eu-Co-BTC / PAN.
[0041] Synthesis of x-Eu-ZIF-67 / PAN-y: 0.1 g of the precursor electrospun fibers obtained in step 1.1 was immersed in 15 mL of methanol solution containing 0.1 g of 2-methylimidazole and soaked at room temperature for a certain period of time. It was then washed twice with ethanol to finally obtain the x-Eu-ZIF-67 / PAN-y composite material; precursors 1:20-Eu-ZIF-67 / PAN-y, 1:10-Eu-ZIF-67 / PAN-y, and 1:5-Eu-ZIF-67 / PAN-y were obtained, where y represents different soaking times in methanol, 6 h, 14 h, and 22 h, respectively. ZIF-67 / PAN was prepared without the addition of Eu(NO3)3·6H2O.
[0042] In Eu-Co-BTC / PAN, BTC stands for pyromellitic acid and PAN stands for polyacrylonitrile. Using these as a comparison, the preparation process of Eu-Co-BTC / PAN is as follows: Synthesis of 1:10-Eu-Co-BTC / PAN: 1:10-Eu-Co-BTC / PAN was prepared by a solvothermal method. 1:10-Eu... 3+ -Co 2+ PAN and trimesic acid were dissolved in 50 mL of anhydrous ethanol at a molar ratio of 2:1, and the mixture was stirred continuously for 15 min until completely dissolved. The solution was then transferred to a 100 mL high-pressure reactor lined with polytetrafluoroethylene (PTFE), sealed, and placed in an oven at 150 °C for 24 h. After the reaction was complete and cooled to room temperature, the resulting electrospun fibers were washed several times with ethanol and finally treated in a vacuum oven at 120 °C for 12 h.
[0043] 1.3 Preparation of x-Eu-ZIF-67 / PAN-y by H2O2 etching.
[0044] 150 mg of the precursors 1:10-Eu-ZIF-67 / PAN-22h and 1:10-Eu-Co-BTC / PAN were weighed and dispersed in conical flasks containing 100 mL of high-purity water, respectively. 60 μL, 120 μL, and 180 μL of different volumes of 30.0 vol% hydrogen peroxide solution were added with stirring. During the reaction, the electrospun fibers gradually turned brownish-black, accompanied by the generation of a large amount of oxygen. The detailed preparation process is as follows... Figure 1 As shown. During the dropwise addition process, H2O2 was added dropwise in portions; taking 120 μL as an example, it was divided into 30 μL × 4 times, 40 μL × 3 times, 60 μL × 2 times, and 120 μL × 1 time, in order to precisely control the generation of defects and the changes in catalyst morphology during the etching process. After reacting for 18 h, it was washed several times with deionized water and dried under vacuum at 60 °C to obtain multiple catalyst samples, abbreviated as EZP-10H and ECP-10H; among them, EZP-10H is the catalyst prepared by 1:10-Eu-ZIF-67 / PAN-22h, and ECP-10H is the catalyst prepared by 1:10-Eu-Co-BTC / PAN. For comparison, two catalysts without electrospun fibers as the matrix were prepared: 1:10-Eu-ZIF-67 (EZ-10H) etched with H2O2, and 1:10-Eu-BTC (EC-10H) etched with H2O2. During this process, the color of the mixed solution gradually deepened by adjusting the amount of H2O2 added and the volume of each drop. The etched catalyst precipitate was collected by centrifugation and washed multiple times with deionized water; other synthesis steps remained consistent with the above.
[0045] 2. Characterization of the structure and morphology of the catalyst.
[0046] Scanning electron microscopy was used to characterize the microstructure and structure of the precursor and catalyst. To clarify the effects of different H₂O₂ concentrations and single-drop volume on the morphology, etching experiments were first performed on the catalyst not supported on electrospun fibers. Figure 2 As shown, when the H2O2 dosage was 60 μL, EZ-10H partially transformed from an initial dodecahedral structure into an open hollow structure. When the H2O2 dosage was increased to 120 μL, almost all the dodecahedrons transformed into open hollow structures, with larger and more pronounced openings, but with slight agglomeration. Further increasing the H2O2 dosage to 180 μL caused the dodecahedral shape of the MOF to collapse, indicating that excessive concentration led to overly rapid etching, damaging the structural integrity of the material. Furthermore, Figure 2 The color of the sample deepened with increasing H2O2 concentration, further confirming the intensified etching process. In summary, to balance structural integrity and catalytic stability, 120 μL was selected as the appropriate amount of H2O2.
[0047] The effect of different single-drop volume on MOF morphology is as follows: Figure 3 As shown, when 120 μL of H2O2 was added all at once, only the surface of the material underwent peeling, and the basic dodecahedral morphology was preserved. Adding it in two separate drops resulted in significant agglomeration, making the original dodecahedral structure difficult to discern. This may be due to the large single drop volume, causing localized contact between H2O2 and the material, leading to uneven etching. When added in three separate drops, EZ-10H essentially transformed into an open hollow structure, with relatively uniform etching, although some agglomeration still existed. Increasing the number of drops to four resulted in partial collapse of the catalyst morphology. Therefore, the etching condition of three drops of 120 μL H2O2 was ultimately determined for subsequent morphology studies of the EZP-10H catalyst supported on electrospun fibers.
[0048] like Figure 4 As shown in a, Eu 3+ -Co 2+ / PAN is a continuous, uniform, and smooth electrospun fiber. ZIF-67, with a dodecahedral morphology, grows on the surface of electrospun fibers immersed in 2-methylimidazole. This can be achieved by controlling the immersion time in 2-methylimidazole. Figure 4 The results showed that the amount of ZIF-67 grown on the fiber surface was relatively small after soaking for 6 h and 14 h. As the soaking time increased, the number of dodecahedrons on the fiber surface increased. To ensure that ZIF-67 was evenly dispersed on the fiber surface, a soaking condition of 22 h in methanol was selected to obtain a ratio of 1:10-Eu-ZIF-67 / PAN-22h. Since the soaking time was selected for 22 h in subsequent experiments, the suffix 22h was not added to the catalyst in subsequent experiments.
[0049] like Figure 5 As shown in b, the H2O2-etched 1:10-Eu-ZIF-67 catalyst without electrospun fiber support exhibits a notched dodecahedral structure with significant particle agglomeration; while the catalyst prepared using electrospun fiber as the matrix, such as Figure 5 In the matrix, c and d, ZIF-67-derived dodecahedrons are uniformly dispersed on the fiber surface, effectively increasing the specific surface area of the material. After H2O2 etching, the material surface becomes rough and forms a hollow porous structure, consistent with the expected material design. Furthermore, EDS energy dispersive spectroscopy analysis results are as follows... Figure 5 The figure shows that Co, Eu, C and N elements are present on the catalyst surface and are relatively uniformly distributed, indicating that the metal components are well dispersed in the material.
[0050] Figure 6The morphology of the 1:10-Eu-Co-BTC / PAN material is shown. Spherical BTC MOF materials with smooth surfaces are grown on electrospun fibers. After being etched by H2O2, the spherical structure of ECP-10H is destroyed and transformed into flower-like fragments, which to some extent increases the specific surface area of the material and is beneficial to enhancing the contact effect with pollutants during subsequent catalytic degradation.
[0051] Figure 7 X-ray diffraction patterns of catalysts with different Co:Eu molar ratios are shown. For example... Figure 7 As shown in Figure a, the diffraction peaks of the 1:10-Eu-ZIF-67 / PAN precursor are completely consistent with the standard spectrum of ZIF-67 with a zeolite imidazole ester framework structure, indicating its high crystallinity and typical ZIF structure. XRD comparisons with different Eu doping concentrations show that the introduction of Eu did not change the crystal framework of ZIF-67, and the materials maintained their intact crystal form. Simultaneously, the diffraction peaks of the 1:10-Eu-Co-BTC / PAN precursor also show high agreement with the standard spectrum of Co-BTC MOF. Figure 7 As shown in c in the figure. After H2O2 etching, regardless of the concentration of H2O2 or the volume of a single drop, the diffraction peaks of both precursors basically disappeared, and no obvious crystal phase diffraction signal was observed. Figure 7 As shown in b and d, the final catalyst has an amorphous structure.
[0052] To further investigate the electronic structure and chemical composition of the materials, X-ray photoelectron spectroscopy was used to analyze ZP-H, EZP-10, and EZP-10H. The results are as follows: Figure 8 As shown, high-resolution spectra of the full spectrum, N 1s, Co 2p, and Eu 3d are presented. In the full spectrum... Figure 8 As shown in Figure a, all three catalysts contain characteristic peaks of C 1s, N 1s, O 1s, and Co 2p, and the Eu-doped samples all exhibit Eu 3d characteristic peaks, indicating that Eu has been successfully introduced into the material system. A comparison of the N 1s peaks of EZP-10 and EZP-10H is shown below. Figure 8 As shown in b, the content of pyridine nitrogen at 398.9 eV in the material decreased significantly before and after etching, indicating that H2O2 caused partial breakage of the Co-N coordination bond. At the same time, the pyrrole nitrogen peak at 400.4 eV broadened, indicating that the imidazole ring structure was disturbed. EZP-10 indicates that it was not etched by H2O2. Figure 8 In the figure, 'c' represents the high-resolution XPS spectra of Co 2p for the three samples. The peaks at 787.1 eV and 803.2 eV are satellite peaks, while the binding energy peaks at 780.2 eV and 795.9 eV belong to Co. 3+ The peaks at 782.1 eV and 798.3 eV correspond to Co. 2+This indicates that Co is present in the material. 3+ and Co 2+ Peaks representing two valence states. A comparison shows that after H2O2 etching, the Co content in the catalyst... 3+ The relative content of EZP-10 increased, from 34.54% to 42.4% (EZP-10H), indicating that the strong oxidizing property of H2O2 partially reduced the content of Co. 2+ Oxidized to Co 3+ Compared to undoped ZP-10H, the peak positions of EZP-10H are shifted towards directions with lower binding energies. Furthermore, in the high-resolution Eu 3d spectrum... Figure 8 Eu 3d can be observed in d. 5 / 2 and Eu 3d 3 / 2 The two characteristic peaks further confirm that Eu mainly exists in the +3 valence state, and that the peak position of EZP-10H shows a certain positive shift relative to ZP-H. The existence of this shift phenomenon proves that there is a certain interaction between Co and Eu, and that there is a certain amount of electron transfer between them.
[0053] Similarly, XPS was used to analyze the full spectrum, O 1s, Co 2p, and Eu 3d high-resolution spectra of CP-H, ECP-10, and ECP-10H, such as... Figure 9 As shown, ECP-10 indicates catalysts obtained without H2O2 etching, and CP-H indicates catalysts without Eu, obtained by electrospinning only Co and PAN, followed by H2O2 etching. Similar to the previous discussion, the full spectrum is as follows... Figure 9 As shown in Figure a, all three catalysts contain characteristic peaks of C 1s, N 1s, O 1s, and Co 2p, and the Eu-doped sample exhibits a Eu 3d characteristic peak, indicating successful Eu doping. Figure 9 As shown in b, the O 1s spectrum of ECP-10 includes carboxylate oxygen (Co-OC=O), ligand carbonyl oxygen (C=O), and surface-adsorbed oxygen (H2O / OH). - Three characteristic peaks were observed. After H₂O₂ etching, the O 1s spectrum of ECP-10H showed three characteristic peaks at 530.0 eV, 531.9 eV, and 533.5 eV, corresponding to newly generated Co₃O₄ lattice oxygen, surface hydroxylated species and residual carboxylate groups, and oxidized ligand fragments and adsorbed oxygen, respectively. The main peak at 531.9 eV indicates that the sample surface is dominated by hydroxylated MOFs, while the weakest peak at 530.0 eV confirms that only localized conversion to cobalt oxides occurred, indicating a limited overall oxidation degree. This is consistent with the etching-reconstruction mechanism of MOFs by H₂O₂. Figure 9 In the figure, 'c' represents the high-resolution XPS spectra of Co 2p for the three samples. The binding energy peaks at 780.1 eV and 795.6 eV are attributed to Co. 3+The peaks at 782.0 eV and 797.9 eV are attributed to Co. 2+ This indicates that Co is present in the material. 3+ and Co 2+ Comparing ECP-10 with CP-H and ECP-10H reveals that after H2O2 etching, the Co content in the catalyst... 3+ The relative content of Eu increased to some extent, from 44.18% in ECP-10 to 76.5% in CP-H and 61.65% in ECP-10H, indicating that the presence of Eu can reduce the active site Co. 2+ The oxidation level is adjusted to promote subsequent catalytic degradation reactions. The peak position of ECP-10H shows a certain negative shift compared to CP-10H. Furthermore, compared to CP-H, ECP-10H contains higher levels of Eu 3d... 5 / 2 and Eu 3d 3 / 2 The binding energy peak shows a positive shift, such as Figure 9 As shown in d, the shift phenomenon is the same as the change phenomenon between ZP-10 and EZP-10H, proving that a certain electron transfer occurred between Eu and Co.
[0054] 3. Degradation performance study.
[0055] To evaluate the catalytic activity of the prepared catalysts, norfloxacin (NOR) was used as a model pollutant. The performance differences of EZP-10H and ECP-10H obtained after etching with different H2O2 concentrations and single-drop volumes in the degradation of NOR by activated persulfate (PMS) were compared. Under conditions where the catalyst and PMS coexisted, EZP-10H treated with different etching conditions all exhibited high catalytic activity. Figure 10 The degradation effects of 'a' and 'b' in the formula are as follows: 120 μL: 40 μL × 3 times > 120 μL: 60 μL × 2 times > 120 μL: 30 μL × 4 times > 60 μL: 30 μL × 2 times > 180 μL: 30 μL × 6 times > 120 μL: 120 × 1 time. With the same total volume of 120 μL, the catalyst with the best performance was obtained by adding 40 μL three times in three separate additions, with an intrinsic rate constant as high as 0.4332 min. -1 Among the comparisons of different concentrations, the material obtained by etching under the condition of 120μL:30μL×4 times showed the highest activity, with a rate constant of 0.3943min within 4min. -1 .
[0056] In contrast, ECP-10H also exhibits certain catalytic activity under different etching conditions, such as... Figure 10The reaction rates of c and d were both NOR degradation rates below 90%, and their order of effectiveness was: 120 μL: 30 μL × 4 times > 120 μL: 60 μL × 2 times > 120 μL: 120 μL × 1 time > 180 μL: 30 μL × 6 times > 120 μL: 40 μL × 3 times > 60 μL: 30 μL × 2 times. The optimal reaction rate constant was 0.1428 min. -1 The performance was significantly lower than that of EZP-10H under the 120μL:40μL×3 etching conditions. Therefore, subsequent experiments used EZP-10H and 120μL:40μL×3 etching conditions as the research object to further explore the influence of various factors on the NOR degradation effect.
[0057] The process of NOR degradation by PMS activated by EZP-10H catalyst is affected by multiple reaction parameters. A single-variable method was used to investigate the effects of different catalytic systems, initial solution pH, catalyst dosage, and PMS dosage on the NOR removal efficiency. Without the addition of PMS, EZP-10H can remove approximately 27.0% of NOR through adsorption alone. Figure 11 As shown in Figure a, this is mainly attributed to the physical retention of pollutants by the electrospun fiber matrix. Simultaneously, due to the low decomposition rate of PMS itself, the PMS system alone cannot effectively degrade NOR. Therefore, the subsequent removal of NOR in the system can be entirely attributed to the activation and degradation process of PMS by the catalyst. After reacting for 30 min under the same reaction conditions, the degradation rates of NOR by the four catalysts ZP-H, EZP-20H, EZP-10H, and EZP-5H were 92.02%, 93.92%, 95.41%, and 91.54%, respectively. The differences in degradation performance may be related to factors such as the structure, dispersibility, and surface uniformity of the catalysts. The degradation process of each system conforms to a first-order reaction kinetic model. Further comparison of catalytic activity was achieved by calculating the reaction rate constant, as shown in the figure. Figure 11 As shown in b in the figure. Under the same conditions, the four catalysts... K Obs The values were 0.3687 min. -1 0.3619min -1 0.4332min -1 and 0.3085min -1 Among them, ECP-10H exhibited the highest catalytic activity. Therefore, this catalyst was selected as a representative activator in this study to investigate subsequent influencing factors and degradation mechanisms.
[0058] To investigate the effect of initial pH on the catalytic performance of EZP-10H, degradation experiments were conducted within the pH range of 3.0–11.0. The results are as follows: Figure 11Figures c and d show the results. Within the pH range of 3.0–9.0, the NOR removal rate of the system consistently remained above 75%, indicating that the catalyst exhibits good PMS activation ability over a wide pH range. Under acidic conditions at pH 3.0, the NOR removal rate decreased to 76.18%, which may be due to the low pH environment and the presence of Co. 2+ The generation of Co is suppressed, while Co 2+ It is the main active species for activating PMS, and its reduced content leads to insufficient surface active sites. Furthermore, high concentrations of H... + It also inhibits SO4 •- The generation of •OH radicals reduces the reaction rate. When the pH increases to 11.0, the NOR degradation efficiency also decreases significantly, possibly because PMS undergoes deprotonation under strongly alkaline conditions, affecting its activation process. In summary, EZP-10H can efficiently activate PMS to degrade NOR within a pH range of 3.0–9.0, indicating that this catalytic system has a wide pH applicability and good application potential in practical wastewater treatment.
[0059] To investigate the effect of catalyst dosage on degradation performance, a dosage of 0.05 g·L⁻¹ was tested. -1 0.10 g·L -1 0.15 g·L -1 and 0.20 g·L -1 The catalytic degradation effect of four different concentrations of EZP-10H on NOR. Figure 11 As shown in e and f, the NOR degradation efficiency under different catalyst dosages within 20 min and the apparent rate constant at 4 min are... K Obs No significant differences were observed, with only a slight increase with increasing dosage. This may be due to slight catalyst agglomeration at high concentrations, leading to a reduction in exposed effective active sites, which in turn affects its sufficient contact with PMS and the efficiency of free radical generation. It is worth noting that when the catalyst dosage was 0.10 g·L⁻¹... -1 At that time, the NOR degradation rate was close to 90% after only 8 minutes of reaction. To avoid the reaction being too rapid and detrimental to mechanism studies, and also considering economic efficiency, subsequent experiments used a concentration of 0.10 g·L⁻¹. -1 The appropriate concentration of the catalyst.
[0060] like Figure 11 As shown in g, different PMS dosages of 0.25 g·L⁻¹ were studied. -1 0.30 g·L -1 0.35 g·L -1 and 0.40 g·L -1The effect on NOR degradation performance. Within a 30-minute reaction time, the removal rates of NOR by the EZP-10H / PMS system reached 93.52%, 95.41%, 94.36%, and 93.50%, respectively. According to... Figure 10 The reaction rate constant calculated from h shows that the degradation rate increases with increasing PMS concentration, but only in the low PMS dosage range (≤0.30 g·L⁻¹). -1 The NOR removal rate increased with increasing PMS dosage, possibly because the adsorption sites on the catalyst surface were not completely occupied by PMS. However, when the PMS dosage continued to increase (>0.30 g·L⁻¹), the removal rate decreased further. -1 At that time, the removal efficiency decreased slightly, which may be due to the limited number of active sites on the catalyst surface, restricting the continuous generation of free radicals, and may also be related to the self-quenching of free radicals initiated by excessive PMS. Therefore, 0.30 g·L⁻¹ was selected. -1 The PMS dosage concentration was used as a reference for subsequent experiments.
[0061] Figure 11 By comparing the EZP-10H / PMS system with existing catalytic systems, the results show that the new system can achieve higher pollutant degradation efficiency and a higher reaction rate constant in a shorter reaction time, demonstrating excellent catalytic activity and promising application prospects in antibiotic wastewater treatment.
[0062] Based on the above experimental results, the optimal reaction conditions for this system were determined to be: catalyst dosage of 0.10 g·L⁻¹. -1 The PMS concentration was 0.3 g·L⁻¹. -1 Initial pH = 7.3.
[0063] 4. Degradation mechanism research.
[0064] Identification of reactive oxygen species. To determine the main reactive oxygen species (ROS) involved in NOR degradation in the EZP-10H / PMS system, a series of quenching experiments were conducted, such as... Figure 12 a and b in the text. Methanol (MeOH) and tert-butanol (TBA) were used as sulfate radicals (SO4), respectively. •- It is a scavenger of hydroxyl radicals (•OH). When 100 mM excess TBA and 100 mM MeOH were added, a decrease in the overall degradation rate was observed. Based on the change in the degradation rate, it is indicated that •OH is the main contributor to the degradation process, and SO42- •- It plays a minor role in the degradation process. Subsequently, chloroform and L-histidine (L-His) are used as superoxide radicals (O2). •- and singlet oxygen 1 O2 quenchers. The addition of chloroform had only a slight inhibitory effect on degradation. In contrast, the presence of L-His inhibited the degradation of NOR to some extent, reducing the removal efficiency to 48.49%.
[0065] To directly demonstrate the generation of ROS, electron paramagnetic resonance spectroscopy experiments were performed using DMPO and TEMP as trapping agents, capturing SO42-. •- •OH, O2 •- and 1 The signal of O2. For example... Figure 12 As shown in c, TEMP- 1 The traditional triple signal peak ratio of O2, 1:1:1, proves the effectiveness of the EZP-10H / PMS system. 1 The generation of O2. Figure 10 The observation of peaks with a ratio of 1:2:1:2:1:2:1 in d and e indicates that DMPO underwent oxidative cleavage. The signal peak of the DMPO oxidation product DMPOX indirectly confirms the presence of SO4 in the catalytic system. •- The generation of •OH species was determined. Methanol was used as a solvent to determine whether O2 was generated during the degradation process. •- No DMPO-O2 detected •- Characteristic peaks. Combined with quenching experimental results, •OH plays a major role in the EZP-10H / PMS / NOR system. 1 O2 and SO4 ·- It plays a supporting role.
[0066] Furthermore, electrochemical impedance spectroscopy was performed in a 0.1 M K3[Fe(CN)6] solution to investigate changes in the catalyst's ion and charge transfer resistance, further studying the catalyst's kinetics. Based on the impedance model of the equivalent circuit, the diameter of the semicircle represents the charge transfer resistance Rct; the smaller Rct is, the greater the charge transfer rate and the faster the catalytic kinetics. The H2O2-etched-1:10-Eu / ZIF-67@PAN catalyst exhibited the lowest resistance, indicating that the Eu-doped H2O2-etched-1:10-Eu / ZIF-67@PAN / PMS / NOR system has a faster charge transfer rate.
[0067] 5. Degradation pathway and toxicological studies.
[0068] The possible degradation pathways of NOR were deduced using liquid chromatography-mass spectrometry (LC-MS / MS), such as... Figure 13As shown. The degradation intermediates of NOR at 2 min, 4 min, 8 min, 12 min, and 20 min were detected, revealing three possible pathways for NOR degradation. Pathway I: The initial step involves the direct addition of hydrogen peroxide to the NOR molecule, generating a highly oxidized intermediate P1, m / z=352. Subsequently, P1 undergoes the removal of a C2O2 fragment, Δm=-56, or a similar small molecule fragment, transforming into P2, m / z=296. Pathway II: First, NOR undergoes oxidative dehydrogenation to generate P3, m / z=35. The piperazine ring of P3 then undergoes ring-opening and the removal of a CO molecule, Δm=-28, forming P4, m / z=322. Subsequently, P4 undergoes CN bond cleavage, removing an isocyanate-NCO, Δm=-43, or an equivalent fragment, generating P5, m / z=279. P5 can further remove a fluorine molecule, Δm=-18, ultimately producing the small molecule fragment P6, m / z=261.
[0069] Pathway III: This is a transformation pathway that initially competes with Pathway II but leads to a different outcome. NOR is also initially oxidized to P7 (m / z = 350), an isomer of P3. P7 then transforms into P8 (m / z = 322) via another ring-opening mechanism, such as the removal of CH2=CH2 (Δm = -28). The quinolone nucleus of P8 undergoes cleavage under oxidative attack, removing a CO or HCO fragment (Δm = -28) to generate P9 (m / z = 294). P9 continues to degrade, eventually forming P10 (m / z = 251) through the removal of a CH3CO fragment (Δm = -43) or a similar process. Finally, as the reaction continues, NOR completely decomposes into smaller inorganic molecules, such as CO2, H2O, and F. - and NO3 - .
[0070] The toxicity of NOR and its degradation intermediates was theoretically predicted using TEST software. Figure 14 As shown in 'a', among the ten intermediates, the bioaccumulation factors of all intermediate products decreased to some extent, indicating that they are more difficult to accumulate in organisms than NOR. Acute toxicity LC-MS in fish was then used... 50 Acute toxicity LC of water fleas 50 As an indicator for biotoxicity evaluation, such as Figure 14 For items b and c, the biotoxicity classification standard is: highly toxic < 1, 1 < toxic < 10, 10 < harmful < 100, 100 < harmless, unit: mg·L -1 The toxicity of most intermediate products to different organisms gradually decreases, and as the degradation reaction proceeds, they gradually transform from toxic to harmful, until finally harmless. Figure 14As shown in d and e, the developmental toxicity of the intermediate products gradually decreases as the reaction proceeds. Simultaneously, the initially generated intermediate products exhibit the same level of mutagenicity as NOR. Overall, the EZP-10H / PMS system is a highly efficient and pollution-free method. The toxicity of intermediate products during NOR degradation is effectively reduced, and as the degradation process continues, NOR is ultimately degraded into non-toxic small molecules, CO2 and H2O.
[0071] To evaluate the application potential of this catalytic system in real-world water bodies, the effects of common water components on NOR degradation were investigated. Anions and dissolved organic matter (DOM), prevalent in real-world water bodies, may participate in or interfere with free radical chain reactions, thus affecting degradation efficiency. For example... Figure 15 As shown in a and b, Cl was added to the EZP-10H / PMS / NOR reaction system respectively. - SO4 2- H2PO4 - Anions were used, and humic acid (HA) was used to represent natural organic matter to investigate their effect on NOR degradation. The results showed that 5 mM SO4... 2- and 5mM H2PO4 - It has little impact on the NOR degradation rate. K Obs The time decreased to 0.3332 min. -1 and 0.3724min -1 And 5mM Cl - This significantly inhibits the degradation process. K Obs Decreased to 0.2175 min -1 This may be due to Cl - With SO4 •- The reaction generates chlorine free radicals with weak oxidizing power, such as Cl• and Cl2. •- This reduces the overall oxidation efficiency of the system. Furthermore, DOM, which is widely present in water, also has a significant impact on catalytic oxidation. When 20 mg·L⁻¹ is added... -1 During HA, K Obs It further decreased to 0.144 min. -1 The inhibition mechanism may include: on the one hand, the functional groups such as carboxyl and phenolic hydroxyl groups contained in HA adsorb onto the catalyst surface, covering the active sites and hindering the generation of free radicals; on the other hand, HA competes with NOR to consume active free radicals, thereby leading to a decrease in the degradation rate.
[0072] Actual wastewater contains various recalcitrant organic pollutants, most of which contain benzene ring structures, making them difficult to remove effectively using traditional water treatment processes. To further investigate the oxidation performance of the EZP-10H catalyst for different pollutants, this study selected several representative recalcitrant organic compounds as target pollutants for degradation experiments. Figure 15 c and d in the figure. The results showed that the catalytic system exhibited good degradation effects on various dyes and antibiotics within 20 min: Rhodamine B (RhB) could be completely removed, and the degradation rates of ciprofloxacin (CIP), tetracycline (TC), levofloxacin (LEV), and sulfamethoxazole (SMX) remained above 80%. This indicates that the catalyst has good versatility in activating PMS to degrade various recalcitrant organic compounds and has application potential in practical wastewater treatment. Its excellent catalytic performance may be related to the use of electrospun fibers as a carrier. The fiber matrix promotes uniform dispersion of catalyst particles, effectively increasing the contact area between the catalyst and pollutants, thereby improving the overall efficiency of the heterogeneous catalytic reaction.
[0073] To evaluate the applicability of the EZP-10H / PMS system in actual water bodies, this paper used tap water and Yellow River water as water matrices to investigate the degradation of NOR in them. The results are as follows: Figure 15 As shown in e and f, the degradation rates of NOR in tap water and Yellow River water were 71.84% and 69.87%, respectively, which were lower than those in the deionized water system. The inhibition of degradation performance may be due to the high concentrations of organic matter and inorganic anions in the actual water body, which compete with the active sites on the catalyst surface for adsorption or consume the active free radicals generated during the reaction, thus affecting the degradation efficiency of the catalytic system. These results indicate that although the composition of the actual water body may have a certain inhibitory effect on the catalytic process, this system still has the potential for application in practical water treatment.
[0074] The leaching concentration of Co during catalytic degradation was determined by inductively coupled plasma mass spectrometry (ICP-MS) to evaluate the catalyst's stability and practical application potential. Compared with the fiber-free EZ-10H catalyst, the Co leaching amount of the fiber-containing EZP-10H catalyst was 0.16 mg·L⁻¹. -1 Compared to the 2.3 mg·L of EZ-10H electrostatically atomized spinning matrix. -1 The concentration of Co leaching was significantly lower, indicating that electrospun fibers can significantly improve the structural stability of MOF materials during etching and reaction processes. In the EZP-10H / PMS / NOR system, the Co leaching concentration was far below the limit specified in the "Groundwater Quality Standard" GB / T 14848-2017, indicating that the system has low environmental risk and good application safety. The effect of solution pH on Co leaching was further investigated. Figure 16In section b, within the acidic to neutral pH range of 3-7.3, the surface hydroxylation layer (Co-OH) generated by H2O2 etching becomes more stable as the pH value increases; under acidic conditions, H... + Attacks on the Co-O bond prompted Co 2+ The dissolution of Co is most efficient at pH 7.3, where the Co-OH / Co-O structure is most compact, effectively preventing the release of Co and resulting in minimal leaching. High concentrations of OH- in the alkaline range (pH 7.3–11) are also beneficial. - It will undergo coordination substitution with the Co site, disrupting the Co-O bridging bond and generating soluble [Co(OH)4]. 2- Or [Co(OH)3] - The alkaline environment weakened the coordination stability of the Co-N complex, causing partial collapse of the framework and a significant increase in Co leaching. In summary, the system was most stable at pH 7.3, with the lowest Co leaching. Within the pH range of 3 to 11, the Co leaching concentration met the groundwater quality limits, indicating that the catalytic system has a wide adaptability to the actual pH of the water body.
[0075] Complete mineralization of pollutants is an important indicator for evaluating the degradation capacity of a catalytic system. Therefore, a total organic carbon (TOC) removal experiment was conducted to compare and analyze the mineralization performance of the EZP-10H / PMS and ECP-10H / PMS systems for NOR. Figure 16 c. During the reaction, TOC values were measured every 5 minutes to calculate the removal rate. The results showed that after 20 minutes of reaction, the TOC removal rate of the EZP-10H / PMS system for NOR reached 56.88%, while that of the ECP-10H / PMS system was only 44.98%. This further demonstrates that EZP-10H has a better catalytic effect on activating PMS and promoting the deep mineralization of pollutants.
[0076] In the catalyst recycling experiment, the EZP-10H catalyst after the reaction was recovered, washed, dried, and then used in the next round of degradation experiments to examine its stability and reusability. Figure 16 As shown in d, after four cycles, although the catalyst activity decreased slightly, the removal rate of NOR remained above 90%. With increasing cycle number, the degradation efficiency showed a slow decreasing trend, which may be attributed to two reasons: first, intermediate products generated during the reaction adsorbed or deposited on the catalyst surface, covering some active sites; second, the active component Co ions gradually leach out during recycling, leading to a reduction in the number of effective active sites, thus causing a slow decline in catalytic performance.
[0077] Figure 17Figure 'a' shows the XRD pattern before and after using EZP-10H. The characteristic peaks of the catalyst remained basically unchanged after use, and there were still no obvious diffraction peaks, indicating that the catalyst has good stability.
[136] The chemical states of freshly prepared and used EZP-10H catalysts were compared using XPS. The N1s spectra after five cycles of H2O2 etching are shown below. Figure 17 The peak b in the figure shows a trend of weakening of the main peak, strengthening of the oxidation peak, and decrease in total nitrogen. Crucially, the peak intensity at 402 eV is enhanced to some extent, indicating deep oxidation of the imidazole ring structure, which simultaneously produces the deep oxidation product NO. X The valence state of Co changes on the material surface, indicating its participation in the oxidation process. This can be seen from the fine spectrum of Co, such as... Figure 17 As can be seen from c, compared with freshly prepared EZP-10H, the Co content in this catalyst is lower. 2+ / Co 3+ The ratio increased from 0.72 to 1.17, and Figure 15 The peak intensity of Eu in d was only slightly reduced, confirming that EZP-10H still possesses a certain catalytic degradation effect after recycling. In conclusion, the reproducibility and wide applicability of EZP-10H indicate that this catalyst has certain development potential in practical applications.
[0078] This invention successfully prepared an EZP-10H catalyst by in-situ growth of Eu-ZIF-67 / PAN as a precursor on the surface of electrospun fibers, combined with hydrogen peroxide etching. The morphology of the MOF material can be controlled by adjusting the concentration and single-drop volume of hydrogen peroxide. The material with the most regular morphology and optimal catalytic performance was obtained when 120 μL of H₂O₂ was added dropwise in three portions. Experimental results show that the optimal conditions are achieved at pH 7.3, temperature 25℃, and catalyst dosage of 0.1 g·L⁻¹. -1 Persulfate PMS concentration 0.3 g·L -1 Under the specified conditions, the EZP-10H / PMS system can degrade 95.41% of norfloxacin (NOR) within 20 min (10 mg·L⁻¹). -1 The cobalt ion leaching concentration was only 0.16 mg·L⁻¹. -1 This result demonstrates the crucial role of electrospun fibers in material stability. Furthermore, the EZP-10H / PMS system exhibits significant degradation effects on various recalcitrant pollutants, maintaining good degradation performance under different anionic environments and actual water quality conditions. Quenching experiments and electron paramagnetic resonance analysis indicate that •OH plays a major role in the degradation process. 1 O2 and SO4 •-It contributes a secondary role. This invention combines defect-engineered unsaturated metal sites with electrospun fiber structures, providing experimental evidence for the development of efficient, stable, and easily recyclable MOF-based environmental functional materials.
[0079] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, it is intended to include any modifications and variations that fall within the scope of the claims and their equivalents.
Claims
1. A method for preparing a hydrogen peroxide-induced corrosion cobalt-based electrospun fiber catalyst, characterized in that, Includes the following steps: The cobalt-based precursor spinning solution is electrospun to obtain precursor electrospun fibers; the cobalt-based precursor spinning solution contains europium and cobalt in a molar ratio of 1:5~20. Precursor electrospun fibers are placed in a solution containing organic ligands and subjected to a coordination reaction for 6 to 22 hours to obtain MOF / polymer composite fibers. The mass ratio of precursor electrospun fibers to ligands is 1:1~2; MOF / polymer composite fibers were placed in an aqueous system, and hydrogen peroxide was added to form defects to obtain the cobalt-based electrospun fiber catalyst. The mass-to-volume ratio of the MOF / polymer composite fibers to the hydrogen peroxide was 0.15 g: 60 μL~180 μL. The hydrogen peroxide was added in batches, with no less than two additions, and the interval between each addition was 80 min~160 min.
2. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The addition is done in batches 2 to 4 times, with the same volume added each time.
3. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The parameters for electrospinning are as follows: The feed rate is 0.8 mL / h, and the voltage is 16 kV~20 kV.
4. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The cobalt precursor spinning solution also contains polyvinylpyrrolidone and polyacrylonitrile, wherein the mass ratio of polyvinylpyrrolidone to cobalt is 0.25~0.26:1; The mass ratio of the polyacrylonitrile to the cobalt is 1:1 to 1.
1.
5. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The cobalt is derived from cobalt nitrate, the europium is derived from europium nitrate, and the ligand is 2-methylimidazole.
6. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The reaction time of the defect is 16h~18h.
7. The method for preparing the hydrogen peroxide-induced cobalt-based electrospun fiber catalyst according to claim 1, characterized in that, The solvent in the solution containing the organic ligand is methanol.
8. A cobalt-based electrospun fiber catalyst prepared by the method for preparing a cobalt-based electrospun fiber catalyst induced by hydrogen peroxide corrosion as described in claims 1 to 7.
9. The application of the cobalt-based electrospun fiber catalyst of claim 8 in the degradation of organic pollutants in water, characterized in that, The organic pollutant is any one of levofloxacin, sulfamethoxazole, norfloxacin, rhodamine B, and tetracycline.