A MIP-209 Ti / Cu9S5 heterojunction photocatalyst, its preparation method and application

By constructing a heterojunction structure of MIP-209 Ti and Cu₉S₅, the problems of narrow spectral absorption range of single-component MIP-209 Ti and small specific surface area of ​​Cu₉S₅ were solved, achieving efficient and stable degradation of organic pollutants.

CN123148997APending Publication Date: 2026-11-24中国市政工程西北设计研究院有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611666254.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The single-component MIP-209 Ti has a narrow spectral absorption range and rapid photogenerated charge recombination. Its Cu₉S₅ has a small specific surface area and insufficient exposure of active sites, resulting in a low removal rate of organic pollutants.

Method used

By constructing a heterojunction structure of MIP-209 Ti and Cu₉S₅, and utilizing the step-matching of their band structures and interfacial self-assembly, the rapid separation of photogenerated carriers is promoted, and the synergistic adsorption, enrichment and catalysis are achieved to efficiently degrade organic pollutants.

Benefits of technology

It broadens the light response range to the full visible and near-infrared spectrum, extends the lifetime of active carriers, improves the degradation efficiency and stability of organic pollutants, and maintains catalytic performance after multiple cycles of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123148997A_ABST
    Figure CN123148997A_ABST
Patent Text Reader

Abstract

This invention discloses a MIP-209 Ti / Cu9S5 heterojunction photocatalyst, its preparation method, and its applications, belonging to the field of photocatalysts. The photocatalyst is constructed from a composite of MIP-209 Ti and Cu9S5 nanomaterials. In preparation, Cu9S5 is first prepared via a hydrothermal reaction using copper acetate, thiourea, PVP, and PEG400 as raw materials; then, MIP-209 Ti is prepared via a hydrothermal reaction using 2-nitroterephthalic acid, tetraisopropyl titanate, and glacial acetic acid as raw materials; finally, MIP-209 Ti and Cu9S5 are added to a dispersion medium, ultrasonically dispersed, stirred, and subjected to interfacial self-assembly. After washing and drying, the MIP-209 Ti / Cu9S5 photocatalyst is obtained. This photocatalyst possesses broad-spectrum light-harvesting capability, rapid interfacial charge separation efficiency, and excellent molecular adsorption and enrichment characteristics, enabling efficient degradation of organic pollutants in water and exhibiting excellent cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalysts, specifically relating to a MIP-209 Ti / Cu9S5 heterojunction photocatalyst, its preparation method, and its application. Background Technology

[0002] With the rapid development of the pharmaceutical, dyeing, and chemical industries, large quantities of emerging organic pollutants such as antibiotics, azo dyes, phenols, and perfluorinated compounds have entered the aquatic environment. These pollutants are chemically stable, difficult to biodegrade, and bioaccumulate, making them difficult to completely eliminate using conventional biological treatment and physical adsorption processes. Solar photocatalytic advanced oxidation technology based on semiconductor materials can utilize light excitation to generate photogenerated carriers and induce the generation of hydroxyl radicals (·OH) and superoxide radicals (·O2). - ) and singlet oxygen ( 1 Highly reactive oxygen species such as O2 completely mineralize organic pollutants in water into water, carbon dioxide, and inorganic small molecules, offering significant advantages such as being green and mild, causing no secondary pollution, and having low energy consumption.

[0003] Metal-organic frameworks (MOFs) are porous crystalline materials formed by the self-assembly of inorganic metal cluster nodes and multidentate organic ligands. They have attracted considerable attention due to their high specific surface area, uniformly tunable pore channels, and abundant coordination-unsaturated active sites. A novel titanium-based MOF material, MIP-209Ti, is composed of high-core Ti... 12 O 15 The MOF, constructed from a metal-oxygen cluster and a 2-nitroterephthalic acid ligand, exhibits a one-dimensional nanoporous structure with hexagonal symmetry. This structure is regular and possesses excellent thermal stability and resistance to aqueous chemical degradation. Its regular nanoporous channels provide ample adsorption and enrichment space and diffusion pathways for the reaction substrate. However, the single-component MIP-209 Ti has a wide bandgap, with its main light absorption bands concentrated in the ultraviolet and near-ultraviolet bands. It exhibits extremely weak absorption of visible and near-infrared light, which constitute the largest portion of the solar spectrum. Furthermore, the recombination rate of photogenerated electron-hole pairs after photoexcitation is extremely fast, resulting in low photon efficiency when using this MOF material alone. This limits its application in practical water treatment for the degradation of organic pollutants.

[0004] Non-stoichiometric transition metal sulfides, such as Cu9S5, possess a narrow bandgap (approximately 1.36 eV) and good metallic conductivity. Due to their internal localized surface plasmon resonance effect, they exhibit excellent light-harvesting capabilities and efficient photothermal energy conversion characteristics across the entire visible to near-infrared wavelength range. However, pure-phase Cu9S5 has a relatively small specific surface area, limiting its ability to adsorb and concentrate low-concentration organic pollutants, and its photogenerated carrier lifetime is also limited when used alone. Summary of the Invention

[0005] The purpose of this invention is to provide a method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst to solve the problems of narrow spectral absorption range and rapid photogenerated charge recombination of single-component MIP-209 Ti, and low organic pollutant removal rate due to small specific surface area and insufficient exposure of active sites of Cu9S5.

[0006] Another object of the present invention is to provide a MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0007] A third objective of this invention is to provide an application of the MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0008] The technical solution of this invention is: (one)

[0010] A MIP-209 Ti / Cu9S5 heterojunction photocatalyst is constructed by combining titanium-based metal-organic framework material MIP-209 Ti with Cu9S5 nanomaterials with a broad spectral response to form a heterojunction structure. (two)

[0012] A method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst includes the following steps:

[0013] A. Preparation of Cu9S5: Copper acetate monohydrate, thiourea and polyvinylpyrrolidone were added sequentially to polyethylene glycol 400, stirred evenly, and then transferred to a high-pressure reactor with a polytetrafluoroethylene substrate for hydrothermal reaction. After the reaction was completed, the mixture was cooled to room temperature, filtered and collected, washed several times with deionized water and anhydrous ethanol, and then vacuum dried at 60°C to obtain Cu9S5 nanomaterials.

[0014] B. Preparation of MIP-209 Ti: 2-nitroterephthalic acid and glacial acetic acid were added to a polytetrafluoroethylene reactor and stirred at room temperature to form a uniformly dispersed suspension; tetraisopropyl titanate was added to the suspension in one go and stirred to make the system uniformly mixed. Then the reaction system was placed in an oven for hydrothermal reaction. After cooling, it was repeatedly washed with ethanol and dried to obtain MIP-209 Ti.

[0015] C. Assembly and preparation of MIP-209 Ti / Cu9S5 heterojunction: The Cu9S5 nanomaterials obtained in step A and the MIP-209 Ti obtained in step B were added to a dispersion medium (selected from at least one of anhydrous ethanol, isopropanol, and methanol), ultrasonically dispersed for 20-40 minutes and then stirred. Subsequently, the mixture was placed at 20-60℃ for interfacial self-assembly. After the reaction was completed, the solid product was collected by centrifugation, washed and vacuum dried to obtain the MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0016] As a further improvement of the present invention, in step A, the hydrothermal reaction temperature is 120-180°C and the hydrothermal reaction time is 12-24 hours.

[0017] As a further improvement of the present invention, in step A, the molar ratio of copper acetate monohydrate to thiourea is 1:0.8-1.5; the number average molecular weight of polyvinylpyrrolidone is 8000; and the mass ratio of polyvinylpyrrolidone to the volume ratio of polyethylene glycol 400 is 0.3-0.5 g:30 mL.

[0018] As a further improvement of the present invention, in step B, the hydrothermal reaction temperature is 120-150°C and the hydrothermal reaction time is 30-48 hours.

[0019] As a further improvement of the present invention, in step B, the molar ratio of 2-nitroterephthalic acid to tetraisopropyl titanate is 2.5-3.5:1; the molar amount of 2-nitroterephthalic acid to the volume ratio of glacial acetic acid is 0.005-0.007 mol:5 mL.

[0020] As a further improvement of the present invention, in step C, the mass ratio of MIP-209 Ti to Cu9S5 is 3-25:1. (three)

[0022] A MIP-209 Ti / Cu9S5 heterojunction photocatalyst is prepared by the above-mentioned method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst. (Four)

[0024] Application of the above-mentioned MIP-209 Ti / Cu9S5 heterojunction photocatalyst in the photocatalytic degradation of organic pollutants in water.

[0025] Furthermore, the organic pollutant is at least one of the following: antibiotic pollutants, organic dye pollutants, phenolic compounds, and fluorine-containing organic pollutants.

[0026] This invention achieves heterogeneous composite of the large specific surface area titanium-based microporous framework MIP-209 Ti and the Cu9S5 micro / nano structure with broad spectral response characteristics at the molecular and nanoscale. By leveraging the stepwise matching of their band structures, the rapid separation of photogenerated carriers at the interface is promoted. At the same time, the adsorption, enrichment and targeted catalysis of the two are synergistic, providing an ideal solution for the efficient degradation of organic pollutants in water.

[0027] Compared with the prior art, the present invention has the following advantages:

[0028] In terms of spectral absorption, the introduction of narrow bandgap Cu9S5 effectively breaks through the limitation that titanium-based MOF materials can only respond to ultraviolet and near-ultraviolet light, significantly broadening the photoresponse range of the composite catalytic system to the visible and near-infrared full spectrum region, enabling the catalyst to efficiently collect and utilize solar energy.

[0029] In terms of carrier dynamics, the energy level structure of MIP-209 Ti and Cu9S5 is staggered and matched. The built-in electric field formed after the heterojunction contacts drives the directional migration of photogenerated charges, which effectively suppresses the ineffective spontaneous recombination of electrons and holes and is beneficial to prolonging the lifetime of active carriers.

[0030] In terms of the synergistic degradation mechanism, the porous framework of MIP-209 Ti provides abundant channels for the adsorption and mass transfer of organic pollutants. The high-density exposed Ti active centers on its surface efficiently activate water and dissolved oxygen to generate a variety of reactive oxygen species. Meanwhile, the potential local photothermal heating effect of Cu9S5 helps to reduce the reaction activation energy of organic chemical bond cleavage. The adsorption concentration, photocatalytic oxidation and local thermal activation work together to promote the efficient degradation and complete mineralization of organic pollutants.

[0031] The preparation method of this invention adopts a three-step stepwise synthesis and a neutral and mild liquid phase interface assembly strategy, which effectively overcomes the technical defects of the traditional in-situ one-step hydrothermal process, such as the chemical erosion and dissolution of copper sulfide phase by high temperature and strong acid environment and the homogeneous rapid crystallization of tetraisopropyl titanate. By stepwise independent control, the crystal phase purity and micromorphology of the two components are optimized, and the mild liquid phase interface assembly promotes the formation of dense chemical bond contact channels between the two phases.

[0032] Furthermore, the heterojunction catalyst of this invention possesses both excellent aqueous chemical stability and mechanical structural tolerance. After repeated cycles of use, its catalytic performance and framework structure remain highly stable, demonstrating promising application prospects. Attached Figure Description

[0033] Figure 1 The image shows a SEM image of the MIP-209 Ti / Cu9S5 prepared in Example 1.

[0034] Figure 2 The XRD patterns of MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 are shown.

[0035] Figure 3 The UV diffuse reflectance spectra of MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 are shown.

[0036] Figure 4The graph shows a comparison of the visible light catalytic degradation performance of tetracycline by MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2.

[0037] Figure 5 The diagram shows the cyclic experiment of visible light catalytic degradation of tetracycline by MIP-209 Ti / Cu9S5 prepared in Example 1. Detailed Implementation

[0038] To make the technical solution, synthesis process and beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments.

[0039] Example 1

[0040] A method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst includes the following steps:

[0041] A. Preparation of Cu9S5: 1 mmol of copper acetate monohydrate, 1 mmol of thiourea, and 0.4 g of polyvinylpyrrolidone (number-average molecular weight 8000) were weighed and added sequentially to 30 mL of polyethylene glycol 400 (PEG400) solvent. The mixture was magnetically stirred at room temperature for 30 minutes until homogeneous. The solution was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel high-pressure reactor, sealed, and placed in an oven at 150 °C for a hydrothermal reaction for 18 hours. After the reaction, the reactor was allowed to cool naturally to room temperature. The black precipitate was collected by filtration, washed several times by alternating centrifugation with anhydrous ethanol and deionized water, and finally dried in a vacuum drying oven at 60 °C for 12 hours to obtain hexagonal phase Cu9S5 powder nanomaterials.

[0042] B. Preparation of MIP-209 Ti: 1.25 g (0.006 mol) of 2-nitroterephthalic acid and 5 mL of glacial acetic acid were added to a 23 mL polytetrafluoroethylene reactor. The mixture was magnetically stirred at room temperature for 20 minutes to fully disperse the solid powder and form a uniform suspension. Then, 0.59 mL (0.002 mol) of tetraisopropyl titanate (CAS: 546-68-9) was added rapidly in one go using a pipette. Vigorous stirring was continued for 10 minutes to ensure thorough coordination and mixing of the precursors. The sealed reactor was then placed in a preheated oven at 150 °C for hydrothermal reaction for 30 hours. After the reaction, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation, repeatedly washed with anhydrous ethanol overnight, and finally vacuum dried at room temperature to obtain white microcrystalline pure-phase MIP-209 Ti powder.

[0043] C. Assembly and preparation of MIP-209 Ti / Cu9S5 heterojunction: Weigh 0.50 g of MIP-209 Ti powder and 0.05 g of Cu9S5, and place them together in a round-bottom flask containing 50 mL of anhydrous ethanol. First, place the flask in an ultrasonic cleaner for ultrasonic oscillation treatment for 30 minutes. The ultrasonic dispersion effect fully deaggregates the two phase particles and fully wets and contacts the microscopic surfaces. Then, turn on magnetic stirring and carry out a mild interface-induced assembly reaction at 60 °C. This promotes the spontaneous induced bonding of the two phase surfaces due to the coordination unsaturated sites to form a tight interface. The resulting solid product is washed and vacuum dried to obtain the tightly bonded MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0044] Figure 1 This is a scanning electron microscope (SEM) image of the MIP-209 Ti / Cu9S5 prepared in this embodiment. The results show that the well-ordered microcrystalline nanoparticles of MIP-209 Ti are tightly covered on the surface of the Cu9S5 sheets, and the interface between the two phases is dense.

[0045] Comparative Example 1

[0046] Preparation of pure-phase MIP-209 Ti: 1.25 g (0.006 mol) of 2-nitroterephthalic acid and 5 mL of glacial acetic acid were added to a 23 mL polytetrafluoroethylene reactor. The mixture was magnetically stirred at room temperature for 20 minutes to form a homogeneous suspension. Then, 0.59 mL (0.002 mol) of tetraisopropyl titanate was added rapidly in one go. After stirring for 10 minutes, the reactor was sealed and placed in a preheated oven at 150 °C for a solvothermal reaction for 30 hours. After cooling to room temperature, the white precipitate was collected by centrifugation at 10,000 rpm for 3 minutes. The precipitate was repeatedly washed with anhydrous ethanol overnight and then vacuum dried at room temperature to obtain pure-phase MIP-209 Ti powder.

[0047] Comparative Example 2

[0048] Preparation of pure phase Cu9S5: 1 mmol (0.1996 g) of copper acetate monohydrate, 1 mmol (0.0761 g) of thiourea, and 0.4 g of polyvinylpyrrolidone were weighed and added to 30 mL of polyethylene glycol 400. After stirring for 30 minutes, the mixture was transferred to a 50 mL autoclave with a polytetrafluoroethylene substrate and reacted at 150 °C for 18 hours. After cooling, the mixture was filtered, washed with anhydrous ethanol and deionized water, and dried under vacuum at 60 °C to obtain pure phase Cu9S5 powder.

[0049] Figure 2The X-ray powder diffraction (XRD) patterns of MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2 are shown. The XRD diffraction peaks of Cu9S5 are consistent with the standard diffraction pattern (PDF#47-1748) of orthorhombic chalcopyrite, indicating that Cu9S5 has good crystallinity. Characteristic diffraction peaks at 27.83°, 29.25°, 32.22°, 46.28°, and 54.82° can be observed, corresponding to the (0015), (107), (1010), (110), and (1115) planes of Cu9S5, respectively. For MIP-209 Ti, the three peaks at 4.44°, 6.86°, and 7.74° are consistent with the standard single-crystal electron diffraction data (DOI:10.1002 / aenm.202500211). Furthermore, the retention of characteristic diffraction peaks in MIP-209 Ti / Cu9S5 further demonstrates the successful composite of the materials.

[0050] Figure 3 The images show the UV diffuse reflectance spectra of MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2. It can be observed that the light absorption cutoff edge of a single MIP-209 Ti material is approximately 367 nm. In contrast, Cu9S5's light absorption covers the entire visible light wavelength range, theoretically effectively compensating for the insufficient light absorption of MIP-209 Ti. After successful composite formation, the overall visible light absorption performance of the MIP-209 Ti / Cu9S5 material is improved, with a light absorption cutoff edge of approximately 390 nm. Crucially, it retains a sufficiently broad absorption tail peak to effectively capture visible light.

[0051] Example 2

[0052] A MIP-209 Ti / Cu9S5 heterojunction photocatalyst and its preparation method, comprising the following steps:

[0053] A. Preparation of Cu9S5: 1 mmol of copper acetate monohydrate, 0.8 mmol of thiourea, and 0.3 g of polyvinylpyrrolidone (number-average molecular weight 8000) were weighed and added sequentially to 30 mL of polyethylene glycol 400 (PEG400) solvent. The mixture was magnetically stirred at room temperature for 30 minutes until homogeneous. The solution was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel high-pressure reactor, sealed, and placed in an oven at 120 °C for 24 hours. After the reaction, the reactor was allowed to cool naturally to room temperature. The black precipitate was collected by filtration, washed several times by alternating centrifugation with anhydrous ethanol and deionized water, and finally dried in a vacuum drying oven at 60 °C for 12 hours to obtain hexagonal phase Cu9S5 powder nanomaterials.

[0054] B. Preparation of MIP-209 Ti: 0.005 mol of 2-nitroterephthalic acid and 5 mL of glacial acetic acid were added to a 23 mL polytetrafluoroethylene reactor. The mixture was magnetically stirred at room temperature for 20 minutes to fully disperse the solid powder and form a uniform suspension. Then, 0.59 mL (0.002 mol) of tetraisopropyl titanate (CAS: 546-68-9) was added rapidly in one go using a pipette. Vigorous stirring was continued for 10 minutes to ensure thorough coordination and mixing of the precursors. The sealed reactor was then placed in a preheated oven at 150°C and kept at that temperature for 30 hours. After the reaction, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation, repeatedly washed with anhydrous ethanol overnight, and finally vacuum dried at room temperature to obtain white microcrystalline pure-phase MIP-209Ti powder.

[0055] C. Assembly and preparation of MIP-209(Ti) / Cu9S5 heterojunction: 0.3 g of MIP-209 Ti powder and 0.1 g of Cu9S5 were weighed and placed together in a round-bottom flask containing 50 mL of anhydrous ethanol. The flask was first subjected to ultrasonic oscillation for 20 minutes in an ultrasonic cleaner. Ultrasonic dispersion was used to fully deagglomerate the two phases and ensure thorough wetting and collision of the microscopic surfaces. Then, magnetic stirring was turned on, and a mild interface-induced assembly reaction was carried out at 20°C. This induced spontaneous bonding of the two phase surfaces due to coordination unsaturated sites, resulting in a tight interface. The obtained solid product was washed and vacuum dried to obtain the tightly bonded MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0056] Example 3

[0057] A MIP-209 Ti / Cu9S5 heterojunction photocatalyst and its preparation method, comprising the following steps:

[0058] A. Preparation of Cu9S5: 1 mmol of copper acetate monohydrate, 1.5 mmol of thiourea, and 0.5 g of polyvinylpyrrolidone (number average molecular weight 8000) were weighed and added sequentially to 30 mL of polyethylene glycol 400 (PEG400) solvent. The mixture was magnetically stirred at room temperature for 30 minutes until homogeneous. The solution was then transferred to a 50 mL polytetrafluoroethylene-lined stainless steel high-pressure reactor, sealed, and placed in an oven at 180 °C for 12 hours. After the reaction, the reactor was allowed to cool naturally to room temperature. The black precipitate was collected by filtration, washed several times by alternating centrifugation with anhydrous ethanol and deionized water, and finally dried in a vacuum drying oven at 60 °C for 12 hours to obtain hexagonal phase Cu9S5 powder nanomaterials.

[0059] B. Preparation of MIP-209 Ti: 0.007 mol of 2-nitroterephthalic acid and 5 mL of glacial acetic acid were added to a 23 mL polytetrafluoroethylene reactor. The mixture was magnetically stirred at room temperature for 20 minutes to fully disperse the solid powder and form a uniform suspension. Then, 0.59 mL (0.002 mol) of tetraisopropyl titanate (CAS: 546-68-9) was added rapidly in one go using a pipette. Vigorous stirring was continued for 10 minutes to ensure thorough coordination and mixing of the precursors. The sealed reactor was then placed in a preheated oven at 120°C and kept at that temperature for 48 hours. After the reaction, the mixture was allowed to cool naturally to room temperature. The white precipitate was collected by centrifugation, repeatedly washed with anhydrous ethanol overnight, and finally vacuum dried at room temperature to obtain white microcrystalline pure-phase MIP-209Ti powder.

[0060] C. Assembly and preparation of MIP-209(Ti) / Cu9S5 heterojunction: 2.5g of MIP-209 Ti powder and 0.1g of Cu9S5 were weighed and placed together in a round-bottom flask containing 50mL of anhydrous ethanol. The flask was first subjected to ultrasonic oscillation for 40 minutes in an ultrasonic cleaner. Ultrasonic dispersion was used to fully deagglomerate the two phases and ensure thorough wetting and collision of the microscopic surfaces. Then, magnetic stirring was turned on, and a mild interface-induced assembly reaction was carried out at 45℃. This induced spontaneous bonding of the two phase surfaces due to coordination unsaturated sites, resulting in a tight interface. The obtained solid product was washed and vacuum dried to obtain the tightly bonded MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

[0061] (I) Evaluation of photocatalytic activity:

[0062] Tetracycline degradation experiments were conducted on the photocatalysts MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2, respectively, using the following methods:

[0063] Using tetracycline hydrochloride (TC), a recalcitrant organic pollutant in water, as a model, the photocatalytic oxidation degradation activity of the above-mentioned catalyst was evaluated. The degradation experiment was conducted in a photochemical reactor equipped with a quartz window and a water bath for temperature control (25℃). A 300 W xenon lamp with a visible light filter (λ > 420 nm) was used as a simulated light source, with an irradiance of 200 mW / cm². 50 mL of a 20 mg / L tetracycline hydrochloride aqueous solution was placed in the reactor, and 25 mg of the above-mentioned catalyst was added. Before switching on the light source, the mixture was continuously magnetically stirred for 30 minutes in the dark to reach adsorption-desorption equilibrium of the pollutant on the catalyst surface. The photoreaction was initiated by switching on the light source. Every 10 minutes, 3 mL of the reaction solution was aspirated and filtered through a 0.22 μm polytetrafluoroethylene microporous membrane to remove catalyst powder. The absorbance change of the reaction filtrate at the characteristic absorption peak of 357 nm was detected using a UV-Vis spectrophotometer, and the tetracycline removal rate was calculated.

[0064] Figure 4 This is a comparison of the visible light catalytic degradation performance of tetracycline by MIP-209 Ti / Cu9S5, MIP-209 Ti, and Cu9S5 prepared in Example 1 and Comparative Examples 1 and 2. Figure 4 As shown, the adsorption efficiency of single MIP-209 Ti for tetracycline was 71.64% within 30 min, reaching 78.09% after 30 min with the lamp on, indicating that the removal of tetracycline by MIP-209 Ti is mainly adsorption. In contrast, the adsorption efficiency of Cu9S5 for tetracycline was 1.94% within 30 min, reaching 41.35% after 30 min with the lamp on, indicating that the removal of tetracycline by Cu9S5 is mainly photodegradation. The MIP-209 Ti / Cu9S5 heterojunction composite material constructed in Example 1 showed an adsorption efficiency of 67.44% for tetracycline within 30 min, and the removal rate successfully increased to 95.23% after 30 min with the lamp on, indicating that the removal of tetracycline by this heterojunction is mainly a synergistic process of adsorption and degradation.

[0065] (II) Cyclic Experiment:

[0066] After the first reaction of the MIP-209 Ti / Cu9S5 prepared in Example 1, the solution containing the photocatalyst was centrifuged, and the lower layer material was dried at 60°C for 24 hours. Then it was put back into the reactor for the next photoreaction. Except for the catalyst material, the other reaction conditions were kept the same as the first time. After the second reaction was completed, the above steps were repeated, and a total of five tetracycline degradation experiments were carried out.

[0067] Figure 5 This is a cyclic experimental diagram of the visible light catalytic degradation of tetracycline by MIP-209 Ti / Cu9S5 prepared in Example 1. Figure 5As shown, the degradation efficiency of tetracycline was above 90% in five consecutive experiments, indicating that the photocatalytic degradation activity of MIP-209 Ti / Cu9S5 remained good after five cycles, and the material has good stability.

[0068] The results of the two experiments above show that: with a xenon lamp as the light source and a light intensity of 200 mW / cm², 2 Under visible light (λ>420nm) irradiation, with a catalyst dosage of 0.5 g / L, a tetracycline solution of 20 mg / L, an initial temperature of room temperature (25℃), and a pH of 7, the MIP-209 Ti / Cu9S5 heterojunction photocatalyst achieved a tetracycline degradation rate of 95.23% after 60 minutes. This degradation rate significantly exceeds that of similar photocatalysts. Furthermore, the material exhibits stable photocatalytic performance after multiple reactions, demonstrating its practical application value.

Claims

1. A MIP-209 Ti / Cu9S5 heterojunction photocatalyst, characterized in that: A heterojunction structure is formed by combining MIP-209 Ti and Cu9S5 nanomaterials.

2. A method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst, characterized in that, Includes the following steps: A. Preparation of Cu9S5: Copper acetate monohydrate, thiourea and polyvinylpyrrolidone were added to polyethylene glycol 400 in sequence, stirred evenly and then subjected to hydrothermal reaction. After the reaction was completed, the mixture was cooled to room temperature, filtered and collected, washed and vacuum dried to obtain Cu9S5 nanomaterials. B. Preparation of MIP-209 Ti: 2-nitroterephthalic acid and glacial acetic acid were added to the reactor and stirred at room temperature to form a uniformly dispersed suspension; tetraisopropyl titanate was added to the suspension and stirred to mix the system evenly. Then, a hydrothermal reaction was carried out. After cooling, the mixture was washed and dried to obtain MIP-209 Ti. C. Assembly and preparation of MIP-209 Ti / Cu9S5 heterojunction: The Cu9S5 nanomaterials obtained in step A and the MIP-209 Ti obtained in step B were added to a dispersion medium, ultrasonically dispersed and stirred, and then placed at 20-60℃ for interfacial self-assembly. After the reaction was completed, the solid product was collected by centrifugation, washed and vacuum dried to obtain the MIP-209 Ti / Cu9S5 heterojunction photocatalyst.

3. The method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 2, characterized in that: In step A, the hydrothermal reaction temperature is 120-180℃, and the hydrothermal reaction time is 12-24 hours.

4. The method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 2, characterized in that: In step A, the molar ratio of copper acetate monohydrate to thiourea is 1:0.8-1.5; the number average molecular weight of polyvinylpyrrolidone is 8000; and the mass ratio of polyvinylpyrrolidone to the volume ratio of polyethylene glycol 400 is 0.3-0.5 g:30 mL.

5. The method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 2, characterized in that: In step B, the hydrothermal reaction temperature is 120-150℃, and the hydrothermal reaction time is 30-48 hours.

6. The method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 2, characterized in that: In step B, the molar ratio of 2-nitroterephthalic acid to tetraisopropyl titanate is 2.5-3.5:1; the molar amount of 2-nitroterephthalic acid to the volume ratio of glacial acetic acid is 0.005-0.007 mol:5 mL.

7. The method for preparing a MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 2, characterized in that: In step C, the mass ratio of MIP-209 Ti to Cu9S5 is 3-25:

1.

8. A MIP-209 Ti / Cu9S5 heterojunction photocatalyst, characterized in that: It is prepared by any one of the preparation methods of the MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to any one of claims 2-7.

9. The application of the MIP-209 Ti / Cu9S5 heterojunction photocatalyst as described in claim 1 or 8 in the photocatalytic degradation of organic pollutants in water.

10. The application of the MIP-209 Ti / Cu9S5 heterojunction photocatalyst according to claim 9 in the photocatalytic degradation of organic pollutants in water, wherein the organic pollutants are at least one of antibiotic pollutants, organic dye pollutants, phenolic compounds, and fluorine-containing organic pollutants.