A method for preparing a honeycomb type coal gas hydrolysis catalyst
By preparing a honeycomb catalyst, the problems of high pressure drop and low utilization rate of spherical catalysts in blast furnace gas were solved, achieving efficient COS hydrolysis conversion and low-temperature stable operation, which is suitable for large-scale blast furnace gas treatment.
Patent Information
- Application Number
- CN202611403086.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-24
AI Technical Summary
Existing spherical alumina-based catalysts suffer from problems such as high pressure drop, low loading, uneven bed structure, and low utilization rate in the COS hydrolysis desulfurization process of blast furnace gas, making it difficult to meet the requirements of high flow rate and low resistance scenarios.
A honeycomb catalyst preparation method was adopted, which involves kneading, extrusion molding, multi-stage drying and calcination of the support, combined with impregnation of active components and gradient drying, to prepare a sulfur- and oxygen-resistant honeycomb catalyst, ensuring uniform distribution and efficient utilization of active components.
It achieves high COS hydrolysis conversion rate at low temperature, reduces pressure drop, and minimizes activity decay, making it suitable for large-scale industrial processing of blast furnace gas.
Smart Images

Figure CN123149000A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of coal gas purification technology, and more specifically, to a method for preparing a honeycomb coal gas hydrolysis catalyst. Background Technology
[0002] Blast furnace gas, the largest combustible byproduct produced during ironmaking, is mostly used for combustion heating and power generation after dust removal and purification. Its sulfur-containing components are mainly carbonyl sulfide (COS) and hydrogen sulfide (H2S), which are converted into SO2 upon combustion, a significant factor affecting flue gas emission standards. The total sulfur content is typically between 100-200 mg / m³. 3 Between these, weakly polar organic sulfur (COS) accounts for as much as about 70%, and because it is much more difficult to remove than H2S, it has become the core target of blast furnace gas desulfurization processes.
[0003] Currently, mainstream COS removal methods include catalytic hydrolysis, amine absorption, adsorption, hydrogenation reduction, and oxidation. Among these, catalytic hydrolysis, with its advantages of mild reaction conditions, high COS conversion rate, and low operating cost, has become the most promising technology for industrial application. COS hydrolysis catalysts are typically prepared using Al2O3, TiO2, or activated carbon as supports, with alkali metals or alkaline earth metals as active components. These catalysts can efficiently convert COS into easily removable H2S, providing support for subsequent fine desulfurization and ultra-low emissions.
[0004] Currently, the catalysts used for COS hydrolysis desulfurization of blast furnace gas are all spherical alumina-based catalysts. From the perspective of engineering applications, their core shortcomings are concentrated in the dimensions of pressure drop, loading amount, and bed uniformity. Especially in scenarios with high flow rate and low resistance requirements, such as blast furnace gas, the disadvantages are very obvious. The main disadvantages are: (1) High pressure drop, high resistance, and high blower energy consumption. Spherical catalysts are randomly stacked into a bed with point contact between particles, resulting in tortuous flow channels and low porosity (generally 0.35-0.45); honeycomb catalysts have regular channels with straight flow channels and high porosity (0.6-0.75). At the same space velocity, the pressure drop of spherical bed is usually 3-10 times that of honeycomb bed, which leads to a significant increase in blower head requirements, high long-term operating power consumption costs, and even limits the processing capacity of the device. (2) Spherical catalysts are limited by the stacking method, resulting in low effective loading amount in a fixed reactor; the regular structure of honeycomb catalysts can achieve higher specific surface area and volume utilization. (3) The bed is prone to flow deviation and channeling, resulting in low utilization. When spherical particles are randomly stacked, the gaps between the particles are uneven, and the gas can easily short-circuit through the "channels" with low resistance, resulting in insufficient catalyst utilization in some areas and severe overload in other areas. The honeycomb catalyst has regular parallel channels with uniform airflow distribution, which can realize the utilization of the entire cross section of the catalyst at the same space velocity, resulting in more stable conversion rate and easier scale-up to industrial scale.
[0005] Given the current state of the industry, the targeted development of a honeycomb COS hydrolysis catalyst specifically for blast furnace gas can overcome the engineering application limitations of traditional granular catalysts and fill the domestic technological gap in monolithic honeycomb hydrolysis catalytic materials for alumina. This type of novel, well-structured catalyst possesses advantages such as low pressure drop, high mass transfer efficiency, and full utilization of active sites, effectively improving the hydrolysis conversion efficiency of carbonyl sulfur and perfecting the deep treatment technology system for organic sulfur in blast furnace gas. It has significant engineering application value and industrial promotion significance for promoting the efficient utilization of gas resources in the steel industry, achieving synergistic emission reduction of sulfides, and realizing green and low-carbon production. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a honeycomb-type coal gas hydrolysis catalyst. The catalyst obtained by this method exhibits excellent sulfur and oxygen resistance, superior low-temperature catalytic reaction performance, and can stably maintain a high COS hydrolysis conversion efficiency with low activity decay, fully meeting the operating requirements of large-scale industrial blast furnace gas processing units.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A method for preparing a honeycomb-type coal gas hydrolysis catalyst includes the following steps:
[0009] S1. Add carrier powder and organic additives to the kneader, with or without inorganic additives, mix well to obtain mixed dry powder;
[0010] S2. Add water, glycerin and a glue solution containing latex powder, polyvinyl alcohol and polyethylene oxide to the mixed dry powder, and knead, knead and extrude it through a kneader to obtain agglomerated mud.
[0011] S3. After the clumps of mud have cooled and aged, put them into a mud-making machine and knead them repeatedly to even out the moisture and remove air, to obtain aged and kneaded mud.
[0012] S4. After aging and kneading, the clay material is extruded and shaped to obtain an alumina honeycomb carrier.
[0013] S5. After multi-stage drying, the alumina honeycomb carrier is calcined in stages.
[0014] S6. Using at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, and sodium bicarbonate as active components, prepare an active impregnation solution, then immerse the catalyst after one calcination in the active impregnation solution, and age it at room temperature after impregnation.
[0015] S7. The aged green body from step S6 is subjected to gradient drying, and then the dried green body is subjected to secondary calcination in stages to obtain a honeycomb gas hydrolysis catalyst.
[0016] In summary, the present invention has the following beneficial effects:
[0017] The preparation method of the honeycomb coal gas hydrolysis catalyst of the present invention belongs to a new type of fine desulfurization hydrolysis catalyst, which can completely solve the technical problem of high pressure drop of spherical hydrolysis catalyst, and the hydrolysis conversion rate can reach more than 90%. It is suitable for COS hydrolysis treatment in industrial large-scale production scenarios such as blast furnace gas. Attached Figure Description
[0018] Figure 1 The efficiency curve of the catalyst prepared in Example 1 for hydrolyzing COS is shown.
[0019] Figure 2 The graph shows the efficiency curve of the catalyst prepared in Example 2 for hydrolyzing COS.
[0020] Figure 3 The image shows the appearance of the mud obtained after the mixing and agglomeration operation in step (2) of Comparative Example 1.
[0021] Figure 4 The final product appearance drawing is shown in Comparative Example 2. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] The preparation method of the honeycomb coal gas hydrolysis catalyst of the present invention includes the following steps:
[0024] S1. Add carrier powder and organic additives to the kneader, with or without inorganic additives, mix well to obtain mixed dry powder.
[0025] In step S1, the carrier powder is composed of p-alumina, α-alumina, boehmite, and titanium dioxide. The organic excipient is composed of at least one of guar gum, hydroxypropyl methylcellulose, glass fiber, and kapok fiber. The inorganic excipient is attapulgite. The mass ratio of the carrier powder to the organic and inorganic excipients is (95-100):(3.5-4):(0-1).
[0026] S2. Add water, glycerin, and a glue solution containing latex powder, polyvinyl alcohol, and polyethylene oxide to the mixed dry powder, and knead, knead, and extrude using a kneader to obtain agglomerated mud with a moisture content of 28-35 wt%.
[0027] In step S2, the latex powder content in the adhesive solution is 0.2-0.4 wt%, the polyvinyl alcohol content is 3-5 wt%, and the polyethylene oxide content is 0.5-1%. During the kneading and extrusion process, the water, glycerin, and adhesive solution account for 18-25%, 6-10%, and 40-50% of the mass of the mixed dry powder, respectively.
[0028] S3. After the clumps of mud have cooled and aged (21-23℃), put them into a mud-making machine and knead them repeatedly to homogenize the moisture and remove air, to obtain aged and kneaded mud.
[0029] S4. After the aged clay is kneaded, it is extruded into a mold to obtain an alumina honeycomb carrier.
[0030] S5. After multi-stage drying of the alumina honeycomb carrier (in sequence: wet drying oven drying, microwave drying and hot air circulation drying), it is calcined in stages.
[0031] The calcination process is as follows: calcination is carried out in five temperature ranges, in the following order: 0-100℃, heating time 90-100min, holding time 110-125min; 100-200℃, heating time 195-200min, holding time 55-65min; 200-300℃, heating time 145-250min, holding time 85-90min; 300-400℃, heating time 245-250min, holding time 55-60min; 400-500℃, heating time 295-300min, holding time 115-120min.
[0032] S6. Using at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, and sodium bicarbonate as active components, prepare an active impregnation solution with an active component content of 5-30 wt%. Then, immerse the catalyst after one calcination in the active impregnation solution and age it at room temperature after impregnation.
[0033] S7. The aged green body from step S6 is subjected to gradient drying, and then the dried green body is subjected to a second calcination in stages to obtain a honeycomb-type coal gas hydrolysis catalyst. The second calcination adopts a three-stage heating program, specifically: 0-200℃, heating time 195-200min, holding time 115-120min; 200-350℃, heating time 195-200min, holding time 55-60min; 350-450℃, heating time 245-250min, holding time 115-120min.
[0034] In the following examples and comparative examples, α-alumina was purchased from Shijiazhuang Jinghuang Technology Co., Ltd., with a particle size of 0.6 μm; p-alumina was p-alumina fast descaling powder from Zibo Henghuan Aluminum Co., Ltd.; boehmite was purchased from Zibo Henghuan Aluminum Co., Ltd., with product number HHNBS-101; titanium dioxide was denitrification catalytic titanium dioxide from Guangxi Jinmao Titanium Industry Co., Ltd.; guar gum was purchased from Shandong Langcheng Chemical Co., Ltd., with product number 01; hydroxypropyl methylcellulose was purchased from Shandong Heda Co., Ltd., with product number 65HD6000; and glass fiber was purchased from Shanghai Yuanye Biotechnology Co., Ltd., with product number [missing information]. The product is S30527; the kapok fiber was purchased from Shanghai Panda Industrial (Group) Co., Ltd., with a fineness of 1.44 dtex and a length of 26 mm; the attapulgite clay was purchased from Guangdong Haike New Material Technology Co., Ltd., model HY-P1; the latex powder (VAE) was redispersible latex powder purchased from Qingdao Tengyun Chemical Technology Co., Ltd., model 25583-20-4; the polyvinyl alcohol (PVA) was purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number S30196; and the polyethylene oxide (PEO) was purchased from Henan Yaoze Chemical Products Co., Ltd., product number 68441-17-8.
[0035] Example 1
[0036] The honeycomb-type coal gas hydrolysis catalyst in this embodiment is prepared through the following steps:
[0037] (1) Dry powder mixing: α-alumina, ρ-alumina, boehmite, titanium dioxide, guar gum, hydroxypropyl methylcellulose, glass fiber, kapok fiber and attapulgite are weighed in a mass ratio of 5:80:5:5:0.5:3:0.5:0.5:0.5 and placed in a kneader. The mixture is stirred in the forward direction at 25 r / min for 35 min, and then in the reverse direction at 15 r / min for 15 min to obtain mixed dry powder.
[0038] (2) Mixing and agglomerating: Prepare a glue solution containing 0.2wt% latex powder (VAE), 5wt% polyvinyl alcohol (PVA), and 0.5% polyethylene oxide (PEO) (water as solvent). Turn on the water cooling system circulating inside the kneader and set the chiller temperature to 24℃. Add water, glycerin, and glue solution to the mixed dry powder in proportions of 20%, 8%, and 40% of the mass of the mixed dry powder, respectively. First, mix at 18r / min for 40min, and then knead and extrude at 24r / min for 30min to obtain agglomerated mud with a moisture content of 27.3%.
[0039] (3) Aging and kneading: The clump of clay is aged at 20℃ for 12 hours. On the second day, the aged clay is put into a kneading machine and kneaded repeatedly to homogenize the moisture and remove air, resulting in cylindrical clay (diameter 280mm).
[0040] (4) Honeycomb molding: The cylindrical mud material is added to the hydraulic mud mixer and extruded at a rate of 0.12 m / s under 12 MPa to obtain an alumina honeycomb carrier with 40 holes and a size of 100 mm × 100 mm × 300 mm.
[0041] (5) The alumina honeycomb carrier is dried in multiple stages: first, it is dried in a wet drying room to reduce the weight by 11%; then it is dried in microwave to reduce the weight by 16%; finally, it is dried in hot air circulation at 70°C for 48 hours to achieve constant weight.
[0042] (6) Calcination: The multi-stage dried alumina honeycomb carrier is calcined in five temperature ranges (0-100℃, heating time 100min, holding time 120min; 100-200℃, heating time 200min, holding time 60min; 200-300℃, heating time 250min, holding time 90min; 300-400℃, heating time 250min, holding time 60min; 400-500℃, heating time 300min, holding time 120min).
[0043] (7) Impregnation and aging: The catalyst after one calcination is placed in a mixed solution containing 20wt% potassium carbonate and 5wt% potassium hydroxide (as an active impregnation solution) for 30 minutes, and then left to dry and age for 24 hours.
[0044] (8) Drying and secondary calcination: The aged green body is placed on a tunnel dryer for drying; then the dried green body is stacked in a box kiln for calcination (three heating programs are set: 0-200℃, heating time 200min, holding time 120min; 200-350℃, heating time 200min, holding time 60min; 350-450℃, heating time 250min, holding time 120min).
[0045] The activity of the honeycomb gas hydrolysis catalyst prepared in this embodiment is expressed by the COS hydrolysis efficiency. The testing equipment is a GC-7820 gas chromatograph, and the testing conditions are: temperature 60℃, space velocity 1300 h⁻¹. -1 The imported CO content is 200 ppm, N2 content is 54 vol%, CO content is 23 vol%, CO2 content is 19 vol%, O2 content is 1 vol%, and H2O content is 1.5 vol. Figure 1 This is a graph showing the efficiency curve of COS hydrolysis using the catalyst in this experiment. The results show that the hydrolysis efficiency of COS is 90-92% within a reaction time of 1000 min.
[0046] Example 2
[0047] The honeycomb-type coal gas hydrolysis catalyst in this embodiment is prepared through the following steps:
[0048] (1) Dry powder mixing: Weigh α-alumina, ρ-alumina, boehmite, titanium dioxide, hydroxypropyl methylcellulose, glass fiber and kapok fiber in a mass ratio of 3:84:5:4:3:0.5:0.5 and place them in a kneader. Stir in the forward direction at 20 r / min for 40 min and in the reverse direction at 18 r / min for 20 min.
[0049] (2) Mixing and agglomeration: Prepare a glue solution containing 0.3wt% VAE and 4wt% PVA, turn on the water cooling system circulating inside the kneader, set the chiller temperature to 24℃, add water, glycerin and glue solution to the mixed dry powder in proportions of 22%, 7% and 38% of the mass of the mixed dry powder respectively, first mix at 22r / min speed for 45min, then knead and extrude at 20r / min speed for 30min, squeeze out the water to bind the powder, and obtain agglomerate mud with a moisture content of 28%.
[0050] (3) Aging and kneading: The clump of clay is aged overnight at 20°C. The next day, the aged clay is put into a kneading machine and kneaded repeatedly to homogenize the moisture and remove air, resulting in cylindrical clay (280 mm in diameter).
[0051] (4) Honeycomb molding: The cylindrical mud material is added to the hydraulic mud mixer and extruded at a rate of 0.12 m / s under 12 MPa to obtain an alumina honeycomb carrier with 40 holes and a size of 100 mm × 100 mm × 300 mm.
[0052] (5) The alumina honeycomb carrier is dried in multiple stages: the first step is to enter the wet drying room, with a target weight reduction of 12%; the second step is microwave drying, with a target weight reduction of 15%; the third step is to dry with hot air circulation at 70℃ for 48 hours to achieve constant weight.
[0053] (6) Calcination: The alumina honeycomb carrier after multi-stage drying is calcined in five temperature ranges (0-100℃, heating time 100min, holding time 120min; 100-200℃, heating time 200min, holding time 60min; 200-300℃, heating time 250min, holding time 90min; 300-400℃, heating time 250min, holding time 60min; 400-500℃, heating time 300min, holding time 120min).
[0054] (7) Impregnation and aging: The alumina carrier after one calcination is placed in a mixed solution containing 25 wt% potassium carbonate and 3 wt% potassium hydroxide for 20 min, and then left to dry and age for 24 h.
[0055] (8) Drying and secondary calcination: The aged green body is placed on a tunnel dryer for drying; then the dried green body is stacked in a box kiln for calcination (three heating programs are set: 0-200℃, heating time 300min, holding time 120min; 200-350℃, heating time 300min, holding time 90min; 350-450℃, heating time 360min, holding time 120min).
[0056] The activity of the honeycomb gas hydrolysis catalyst prepared in this embodiment is expressed by the COS hydrolysis efficiency. The testing equipment is a GC-7820 gas chromatograph, and the testing conditions are: temperature 60℃, space velocity 1300 h⁻¹. -1 The imported CO content is 200 ppm, N2 content is 54 vol%, CO content is 23 vol%, CO2 content is 19 vol%, O2 content is 1 vol%, and H2O content is 1.5 vol. Figure 2 This is a graph showing the efficiency curve of COS hydrolysis using the catalyst in this experiment. The results show that the hydrolysis efficiency of COS is 91-93% within a reaction time of 1000 min.
[0057] Comparative Example 1
[0058] The procedure is the same as in Example 1, except that in step (1), eight powders, namely ρ-alumina, pseudoboehmite, titanium dioxide, guar gum, glass fiber, kapok fiber and attapulgite, are weighed in a mass ratio of 88:5:5:0.5:0.5:0.5:0.5 and then placed in a kneader.
[0059] HPMC molecular chains are adsorbed onto the surface of ceramic particles through hydrogen bonds, forming a three-dimensional flexible network that "bridges" lean materials (low-plasticity powders such as quartz and alumina) into a whole, increasing the plasticity index from 1-2 to 3-5. However, in this comparative example, because hydroxypropyl methylcellulose was not added during the dry powder mixing stage, even with the addition of a glue solution in step (2) to try to agglomerate the powder, the powder still could not be kneaded into agglomerates and remained entirely loose (see the clay obtained after the kneading and agglomeration operation in step (2) of Comparative Example 1). Figure 3 As shown in the figure, this demonstrates the importance of hydroxypropyl methylcellulose in the powder mixing stage.
[0060] Comparative Example 2
[0061] The operation is carried out according to the steps of Example 2, except that the controlled drying and aging step is cancelled in step (7), and the soaking is directly dried. In step (8), the secondary drying is no longer set with multiple temperature programs, and the drying is carried out at a constant temperature of 65°C.
[0062] The aging treatment following impregnation modification promotes the full penetration and distribution of the active precursor solution within the pores of the honeycomb carrier through capillary diffusion, facilitating uniform loading of the active components. Simultaneously, it allows for the full adsorption and coordination of metal ions with the functional groups on the carrier surface, enhancing binding stability and the dispersibility of the active components. Through the regulation of system complexation and hydrolysis equilibrium, the grain morphology can be refined, the pore structure optimized, and the internal moisture of the preform homogenized, effectively alleviating drying shrinkage stress and preventing cracking, powdering, and segregation of active components in the honeycomb structure. However, in this comparative example, the impregnated sample was not allowed to stand for aging; it was directly dried after impregnation, resulting in severe peeling of the final product (see...). Figure 4 ),not available.
[0063] Example 3
[0064] The procedure is the same as in Example 1, except that step (7) of immersion aging is modified as follows:
[0065] (7.1) Dissolve aluminum lactate and potassium bicarbonate in deionized water to prepare K + Concentration of 0.2 mol / L, Al 3+ A pre-wetting solution with a concentration of 0.05 mol / L was prepared. The carrier after one calcination was completely immersed in the pre-wetting solution and impregnated at 25°C for 10 min. After impregnation, the carrier was filtered out.
[0066] (7.2) Place the carrier obtained in step (7.1) in a closed reaction vessel, introduce CO2 gas into the vessel, control the flow rate to 0.2 L / min, maintain the pressure inside the vessel at 0.3 MPa, and react at 60°C for 40 min; after the reaction is completed, immerse the carrier in 0.2 wt% H3BO3 aqueous solution, soak at 25°C for 20 min, and filter.
[0067] Comparative Example 3
[0068] The procedure is the same as in Example 3, except that step (7.2) is replaced by: directly immersing the carrier obtained by step (7.1) in a 0.2wt% H3BO3 aqueous solution, soaking at 25°C for 20 min, and then filtering.
[0069] The activity of the catalyst prepared in this comparative example was expressed as the COS hydrolysis efficiency. The testing equipment was a GC-7820 gas chromatograph, and the test conditions were: temperature 60℃, space velocity 1300 h⁻¹. -1 The imported COS content is 200 ppm, N2 content is 54 vol%, CO content is 23 vol%, CO2 content is 19 vol%, O2 content is 1 vol%, and H2O content is 1.5 vol%; the hydrolysis efficiency of COS within a reaction time of 1000 min is 72-78%.
[0070] Comparative Example 4
[0071] The procedure is the same as in Example 3, except that step (7.2) is replaced by: placing the carrier obtained in step (7.1) in a closed reaction vessel, introducing CO2 gas into the vessel, controlling the flow rate at 0.2 L / min, maintaining the pressure inside the vessel at 0.3 MPa, reacting at 60°C for 40 min, and filtering after the reaction is completed.
[0072] The activity of the catalyst prepared in this comparative example was expressed as the COS hydrolysis efficiency. The testing equipment was a GC-7820 gas chromatograph, and the test conditions were: temperature 60℃, space velocity 1300 h⁻¹. -1 The imported COS content is 200 ppm, N2 content is 54 vol%, CO content is 23 vol%, CO2 content is 19 vol%, O2 content is 1 vol%, and H2O content is 1.5 vol%; the hydrolysis efficiency of COS within a reaction time of 1000 min is 80-84%.
[0073] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a honeycomb-type coal gas hydrolysis catalyst, characterized in that, Includes the following steps: S1. Add carrier powder and organic additives to the kneader, with or without inorganic additives, mix well to obtain mixed dry powder; S2. Add water, glycerin and a glue solution containing latex powder, polyvinyl alcohol and polyethylene oxide to the mixed dry powder, and knead, knead and extrude it through a kneader to obtain agglomerated mud. S3. After the clumps of mud have cooled and aged, put them into a mud-making machine and knead them repeatedly to even out the moisture and remove air, to obtain aged and kneaded mud. S4. After aging and kneading, the clay material is extruded and shaped to obtain an alumina honeycomb carrier. S5. After multi-stage drying, the alumina honeycomb carrier is calcined in stages. S6. Using at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, sodium carbonate, and sodium bicarbonate as active components, prepare an active impregnation solution, then immerse the catalyst after one calcination in the active impregnation solution, and age it at room temperature after impregnation. S7. The aged green body from step S6 is subjected to gradient drying, and then the dried green body is subjected to secondary calcination in stages to obtain a honeycomb gas hydrolysis catalyst.
2. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S1, the carrier powder is composed of p-alumina, α-alumina, boehmite, and titanium dioxide; the organic excipient is composed of at least one of guar gum, hydroxypropyl methylcellulose, glass fiber, and kapok fiber; and the inorganic excipient is attapulgite.
3. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S1, the mass ratio of carrier powder to organic and inorganic excipients is (95-100):(3.5-4):(0-1).
4. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S2, the latex powder content in the adhesive solution is 0.2-0.4 wt%, the polyvinyl alcohol content is 3-5 wt%, and the polyethylene oxide content is 0.5-1%. During the kneading and extrusion process, the water, glycerin, and adhesive solution account for 18-25%, 6-10%, and 40-50% of the mass of the mixed dry powder, respectively.
5. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S2, the moisture content of the agglomerated mud is 28-35 wt%.
6. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S3, the aging temperature is 21-23℃.
7. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, Step S5, the multi-stage drying process, consists of wet drying oven drying, microwave drying, and hot air circulating drying.
8. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 7, characterized in that, The calcination in step S5 is specifically carried out in five temperature ranges: 0-100℃, heating time 90-100min, holding time 110-125min; 100-200℃, heating time 195-200min, holding time 55-65min; 200-300℃, heating time 145-250min, holding time 85-90min; 300-400℃, heating time 245-250min, holding time 55-60min; 400-500℃, heating time 295-300min, holding time 115-120min.
9. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S6, the content of active components in the active impregnation solution is 5-30 wt%.
10. The method for preparing a honeycomb-type coal gas hydrolysis catalyst according to claim 1, characterized in that, In step S7, the secondary calcination adopts a three-stage heating program, specifically: 0-200℃, heating time 195-200min, holding time 115-120min; 200-350℃, heating time 195-200min, holding time 55-60min; 350-450℃, heating time 245-250min, holding time 115-120min.