A method for separating complex tungsten-tin mixed concentrate and recovering associated resources

By employing a fine classification and multi-step sorting method, the problems of mineral separation and associated resource recovery in tungsten-tin mixed concentrate were solved, achieving efficient separation of tungsten-tin minerals and comprehensive recovery of associated resources, thereby improving resource utilization.

CN123149053APending Publication Date: 2026-11-24广西桂华成有限责任公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611405336.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently separating and recovering tungsten and tin minerals and associated resources, especially elements such as copper, silver, sulfur, and iron, from mixed tungsten and tin concentrates. Traditional processes result in some valuable elements being unavailable for valuation and utilization, thus reducing the overall utilization level of mineral resources.

Method used

A combined approach of fine classification, targeted grinding, flotation, magnetic separation, and gravity separation is adopted. Fine-grained materials are pre-separated by 0.10mm classification, followed by copper-sulfur mixed flotation, weak magnetic separation, scheelite stepwise pre-enrichment, deep quality improvement and impurity reduction, and multi-gradient strong magnetic separation. This enables the stepwise recovery of scheelite, wolframite, and cassiterite, and also comprehensively recovers associated resources such as copper, silver, sulfur, and iron.

Benefits of technology

It improves the separation efficiency of tungsten-tin mixed concentrate and the recovery rate of associated resources, obtaining high-grade scheelite, wolframite and tin concentrate, while also improving the comprehensive utilization level of copper, silver, sulfur and iron resources, and achieving stable recovery of tungsten and tin resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149053A_ABST
    Figure CN123149053A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of non-ferrous metal mineral processing technology and discloses a method for separating complex tungsten-tin mixed concentrates and recovering associated resources. The method includes fine classification and coarse-grained targeted grinding, copper-sulfur mixed flotation, copper-sulfur separation, weak magnetic iron removal, scheelite staged pre-enrichment, deep upgrading and impurity reduction of scheelite rough concentrate, gravity concentration and enrichment of the upgraded scavenging tailings followed by regrinding and re-dispersion, and multi-gradient strong magnetic separation of scheelite flotation tailings. The copper-sulfur mixed concentrate is separated to obtain copper-silver concentrate and sulfur concentrate; scheelite staged pre-enrichment and deep upgrading and impurity reduction yield scheelite concentrate; and multi-gradient strong magnetic separation yields wolframite concentrate and tin concentrate. This invention can reduce over-grinding and mud formation of tungsten and tin minerals, reduce the intermingling of tungsten and tin concentrates, and achieve comprehensive recovery of tungsten, tin, copper, silver, sulfur, and iron.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of non-ferrous metal mineral processing technology, specifically relating to a method for separating complex tungsten-tin mixed concentrates and recovering associated resources. Background Technology

[0002] Tungsten and tin are both important strategic mineral resources with significant applications in modern equipment manufacturing, electronics, and new energy. Because tungsten and tin minerals have similar specific gravities, they tend to co-accumulate during ore beneficiation, forming mixed tungsten-tin concentrates.

[0003] Currently, in the process of tungsten-tin resource development, the tungsten-tin mixed concentrate obtained after gravity separation usually still contains a certain amount of associated valuable elements such as copper, sulfur, silver, and iron. Due to the low content of these associated elements and their complex symbiotic relationship with tungsten-tin minerals, traditional processes are unable to achieve simultaneous and efficient recovery, resulting in some valuable elements being unable to be valued and utilized, thus reducing the comprehensive utilization level of mineral resources.

[0004] Existing technologies for processing tungsten-tin mixed concentrates mainly include combined flotation-magnetic separation and combined flotation-gravity separation processes. However, due to the wide particle size distribution of tungsten-tin minerals, the strong brittleness of some minerals, and the presence of a certain proportion of liberated minerals in the fine-grained fraction, the liberated fine-grained tungsten-tin minerals are prone to sludge formation due to repeated grinding when using uniform grinding across the entire particle size. Furthermore, scheelite, wolframite, and cassiterite share similar physicochemical properties and exhibit fine-grained intergrowth and inclusion phenomena, making it difficult to simultaneously achieve optimal concentrate grade and recovery rate for each mineral using a single separation method.

[0005] In addition, existing processes typically involve uniform grinding of all materials without fully considering the differences in the degree of liberation of minerals of different particle sizes. This can easily lead to repeated grinding of already liberated minerals, resulting in the loss of tungsten and tin minerals through mud formation. On the other hand, for intermediate products or tailings containing coarse-grained tungsten-tin intergrowths, traditional processes lack effective secondary recovery measures, further reducing the recovery rate of tungsten and tin resources.

[0006] Therefore, it is necessary to develop a beneficiation method that can reduce over-grinding and mudding, enhance tungsten-tin separation, and take into account the recovery of associated resources such as copper, silver, sulfur, and iron in complex tungsten-tin mixed concentrates, which are characterized by complex mineral composition, close intergrowth, and difficulty in the comprehensive recovery of multiple valuable elements. Summary of the Invention

[0007] The purpose of this invention is to provide a method for separating complex tungsten-tin mixed concentrates and recovering associated resources. Through fine classification, targeted grinding, and the synergistic effect of flotation, magnetic separation and gravity separation, the method achieves the stepwise recovery of scheelite, wolframite and cassiterite, and comprehensively recovers associated resources such as copper, silver, sulfur and iron.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A method for separating complex tungsten-tin mixed concentrate and recovering associated resources, wherein the complex tungsten-tin mixed concentrate contains scheelite, wolframite, and cassiterite, and is associated with copper sulfide minerals, silver-bearing sulfide minerals, pyrite, and magnetic iron minerals, comprising the following steps: (1) According to the 0.10mm classification, only the +0.10mm product is ground to the -0.075mm particle size content of 45% to 65%, and then combined with the -0.10mm product as flotation feed; (2) The flotation feed is subjected to copper-sulfur mixed flotation to obtain copper-sulfur mixed concentrate and copper-sulfur flotation tailings; (3) The copper-sulfur mixed concentrate is subjected to copper-sulfur separation to obtain copper-silver concentrate and sulfur concentrate; (4) The copper-sulfur flotation tailings are subjected to weak magnetic separation to obtain iron concentrate and weak magnetic tailings; (5) The weak magnetic tailings are subjected to scheelite stepwise pre-enrichment to obtain scheelite rough concentrate and scheelite flotation tailings; (6) Deeply upgrade and reduce impurities in the scheelite rough concentrate to obtain scheelite concentrate and upgraded scavenging tailings; (7) The upgraded scavenging tailings are enriched by gravity separation to obtain gravity concentrate and gravity tailings. The gravity concentrate is returned to fine classification, wherein the +0.10mm portion enters targeted grinding, the -0.10mm portion is directly merged with the grinding product and enters subsequent beneficiation, and the gravity tailings are discharged. (8) The scheelite flotation tailings are subjected to multi-gradient strong magnetic separation to obtain scheelite concentrate and tin concentrate.

[0009] The complex tungsten-tin mixed concentrate described in this invention refers to a tungsten-tin mixed concentrate containing scheelite, wolframite, and cassiterite, and associated with one or more of copper sulfide minerals, silver-bearing sulfide minerals, pyrite, and magnetic iron minerals. For mixed concentrates containing scheelite, wolframite, and cassiterite, and simultaneously associated with copper, silver, sulfur, and magnetic iron minerals, this invention achieves the stepwise enrichment and recovery of each valuable mineral through the sequential synergistic action of flotation, weak magnetic separation, scheelite flotation, gravity separation, and strong magnetic separation.

[0010] Preferably, in step (1), a 0.10mm sieve is used for fine classification, and the product over the +0.10mm sieve is subjected to targeted grinding so that the content of -0.075mm particles in the ground product is 45% to 65%. The ground product is then combined with the product under the -0.10mm sieve as flotation feed. By pre-separating the -0.10mm fine particles, the tungsten-tin minerals that have already been fully liberated do not undergo repeated grinding, and only the coarse particles are moderately ground, thereby reducing the over-grinding and mudding of tungsten-tin minerals caused by uniform grinding of all particle sizes.

[0011] Preferably, in step (2), the copper-sulfur mixed flotation includes roughing, cleaning and scavenging, with the middlings from the cleaned ore and the scavenged concentrate being returned to the previous stage of operation in sequence.

[0012] Preferably, the copper-sulfur mixed flotation specifically includes: performing copper-sulfur mixed flotation roughing on the flotation feed to obtain copper-sulfur mixed flotation rough concentrate and copper-sulfur mixed flotation roughing tailings; performing copper-sulfur mixed flotation rough concentrate for 1 to 3 cleaning processes to obtain copper-sulfur mixed concentrate and cleaned middlings, with the cleaned middlings being returned to the previous stage of operation; and performing copper-sulfur mixed flotation roughing tailings for 1 to 3 scavenging processes to obtain copper-sulfur flotation tailings and scavenged concentrate, with the scavenged concentrate being returned to the previous stage of operation.

[0013] Preferably, in step (3), the copper-sulfur mixed concentrate is subjected to copper-sulfur separation using a sulfur-suppressing and copper-floating method to obtain copper-silver concentrate and sulfur concentrate. The copper-sulfur separation includes one roughing separation, two to four copper-floating cleaning separations, and one to three scavenging separations. The middlings from the copper-floating cleaning separation and the scavenging separation concentrate are returned to the previous stage of operation in sequence.

[0014] Preferably, the sulfur mineral inhibitor used in the copper-sulfur separation is selected from one or more of calcium hypochlorite, sodium humate, and lime.

[0015] Preferably, in step (4), the weak magnetic separation includes one coarse selection and one to two fine selections, with a magnetic field strength of 0.05 to 0.30 T.

[0016] Preferably, in step (5), the scheelite cascade pre-enrichment includes one pre-enrichment roughing, one to three pre-enrichment cleaning, and one to three pre-enrichment scavenging. The middlings from the pre-enrichment cleaning and the pre-enrichment scavenging concentrate are returned to the pre-enrichment roughing operation.

[0017] Preferably, the scheelite collector used in the scheelite stepwise pre-enrichment is selected from one or more of oxidized paraffin soap, modified fatty acids, oleamide, modified hydroxamic acid, and alkyl phosphate; the modifier used is selected from one or more of sodium carbonate, sodium hydroxide, water glass, aluminum sulfate, and sodium hexametaphosphate.

[0018] Preferably, the scheelite collector is composed of oxidized paraffin soap, modified fatty acid and alkyl phosphate in a mass ratio of 2:1:1.

[0019] Preferably, the pre-enrichment roughing reagent system for the scheelite stepwise pre-enrichment is as follows: sodium carbonate 1200-2000 g / t, water glass 5000-6000 g / t, and scheelite collector 500-650 g / t.

[0020] Preferably, in step (6), the scheelite concentrate is concentrated to a pulp concentration of not less than 55% and then subjected to deep upgrading and impurity reduction. High-concentration stirring is used to enhance the flotation separation between scheelite and wolframite, cassiterite and gangue minerals.

[0021] Preferably, the deep upgrading and impurity reduction includes one upgrading roughing, three to five upgrading cleaning, and one to two upgrading scavenging, with the middlings from the upgrading cleaning and the concentrate from the upgrading scavenging being returned to the previous stage of operation in sequence.

[0022] Preferably, the inhibitor used in the deep quality improvement and impurity reduction is selected from one or more of water glass, salt-modified water glass, aluminum sulfate, sodium carboxymethyl cellulose, tannin, starch, and dextrin.

[0023] Preferably, the reagent system for deep quality improvement and impurity reduction is as follows: 250-300 g / t of scheelite collector and 7500-8000 g / t of water glass.

[0024] Preferably, in step (7), the gravity enrichment adopts shaking table gravity separation, so that the coarse tungsten-tin intergrowth minerals in the scavenging tailings enter the gravity concentrate; the gravity concentrate is returned to the fine classification operation in step (1), so that the tungsten-tin intergrowth minerals that are not fully liberated re-enter the regrinding and re-selection process, and the gravity tailings are discharged.

[0025] Preferably, in step (8), the multi-gradient strong magnetic separation includes one roughing, two cleaning and one scavenging; the magnetic field strengths of the roughing, the first cleaning, the second cleaning and the scavenging are 1.0T, 0.8T, 0.6T and 1.3T respectively, and the middlings of the strong magnetic cleaning and the concentrate of the strong magnetic scavenging are combined and returned to the strong magnetic roughing operation.

[0026] Preferably, the magnetic field strength of the multi-gradient strong magnetic separation is 0.5 to 2.0 T.

[0027] The present invention describes a process of concentrating scheelite rough concentrate to a pulp concentration of not less than 55%, primarily used in the high-concentration reagent preparation stage of the scheelite rough concentrate. During this stage, scheelite collectors and inhibitors are added and thoroughly stirred to ensure the reagents fully interact with the surfaces of scheelite, wolframite, cassiterite, and gangue minerals. After high-concentration preparation, the pulp is adjusted to a concentration suitable for aeration and froth separation in the flotation equipment for upgrading roughing and subsequent cleaning and scavenging operations. The stated pulp concentration of not less than 55% does not imply that this solids concentration must be maintained throughout the entire flotation process.

[0028] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. This invention performs fine classification on tungsten-tin mixed concentrate, pre-separating the -0.10mm fine-grained product so that the fully liberated tungsten-tin minerals do not undergo repeated grinding. Only the +0.10mm coarse-grained product is ground to a -0.075mm particle size content of 45% to 65%, thereby reducing the over-grinding and mudding of fine-grained tungsten-tin minerals caused by uniform grinding of all particle sizes, which is beneficial to stabilizing subsequent flotation and magnetic separation indicators.

[0029] 2. This invention removes the interference of sulfide minerals on the separation of tungsten and tin through copper-sulfur mixed flotation, and further separates copper and sulfur in the copper-sulfur mixed concentrate to obtain copper-silver concentrate and sulfur concentrate, thereby improving the comprehensive utilization level of associated copper, silver and sulfur resources.

[0030] 3. This invention employs a tiered pre-enrichment and deep upgrading and impurity reduction process for scheelite. First, pre-enrichment flotation is used to remove silicate gangue with significant differences in floatability and obtain scheelite rough concentrate. Then, high-concentration deep upgrading and impurity reduction is used to further suppress wolframite, cassiterite, and calcium-containing gangue to obtain low-tin, high-grade scheelite concentrate.

[0031] 4. This invention utilizes the magnetic differences between wolframite and cassiterite, employing a multi-gradient strong magnetic separation method: wolframite is enriched under a high roughing magnetic field strength, and then the finer magnetic field strength is successively reduced to obtain high-quality wolframite concentrate, while the scavenger magnetic field strength is increased to reduce the WO3 content in the tin concentrate; the middlings from the strong magnetic fine separation and the scavenger concentrate are returned to the strong magnetic roughing operation, thereby reducing the Sn content in the wolframite concentrate and the WO3 content in the tin concentrate, and reducing the interconjugation of tungsten and tin.

[0032] 5. This invention uses gravity separation to enrich coarse-grained tungsten-tin intergrowth minerals in the upgrading and scavenging tailings, and returns the gravity separation concentrate to the fine classification operation for regrinding and re-selection, thereby reducing the loss of tungsten-tin intergrowth minerals with the upgrading tailings and improving the overall recovery rate of tungsten and tin.

[0033] 6. This invention, through a combined process of flotation, magnetic separation, and gravity separation, can obtain copper-silver concentrate with a Cu grade of not less than 18%, an Ag content of not less than 1000 g / t, and a Cu recovery rate of not less than 90%, as well as sulfur concentrate with a S grade of not less than 35%; the WO3 grade of both scheelite and wolframite concentrates is not less than 70%, and the combined WO3 recovery rate of both is not less than 97%; the Sn grade of tin concentrate is not less than 45%, and the Sn recovery rate is not less than 98%, thus achieving comprehensive recovery of tungsten, tin, copper, silver, sulfur, and iron resources. Attached Figure Description

[0034] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0035] Figure 1 This is a process flow diagram of the method for separating complex tungsten-tin mixed concentrate and recovering associated resources according to the present invention. Detailed Implementation

[0036] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0037] Unless otherwise specified, the proportions, contents and amounts described in the embodiments of the present invention are all by mass; the amount of reagents used is all by the amount added per ton of dry ore.

[0038] The main reagents used in this embodiment are as follows: Butyl xanthate: Sodium salt of O-dithiocarbonate; Z200: Ethylthiocarbamate, i.e., ethylthiocarbamate-O-isopropyl ester; CY composite scheelite collector: This is a commercial composite collector. Its main effective components include oxidized paraffin soap, modified fatty acids, and alkyl phosphate esters, with a mass ratio of 2:1:1. Among them, oxidized paraffin soap is a mixed collector with C12-C32 fatty acid salts as the main components, modified fatty acids are modified products of C16-C18 unsaturated fatty acids as the main components, and alkyl phosphate esters are aliphatic alkyl phosphate ester collecting components.

[0039] Pinol oil (2# oil, CAS No. 8002-09-3); 733 Scheelite Collector: A commercially available scheelite flotation collector, whose main active ingredients are fatty acids or modified fatty acid collecting components; P86: Tributyl phosphate cassiterite flotation aid collector. Example 1

[0040] This embodiment uses a complex tungsten-tin mixed concentrate obtained from gravity separation at a beneficiation plant in Guangxi as the processing target.

[0041] The ore sample has a WO3 grade of 35.52%, a Sn grade of 15.31%, a Cu grade of 0.24%, a S grade of 3.42%, and a silver content of 32 g / t. The tungsten minerals are mainly wolframite and scheelite, in a ratio of approximately 2:3; the tin mineral is mainly cassiterite; sulfur mainly exists in the form of pyrite, with a small amount of magnetic iron minerals; silver is mainly found in sulfide minerals; and the gangue minerals are mainly quartz, calcite, garnet, and fluorite.

[0042] like Figure 1 As shown, the specific steps include: (1) Fine classification of complex tungsten-tin mixed concentrate is carried out with 0.10 mm as the classification particle size. The product on the +0.10 mm screen is targeted grinding so that the content of -0.075 mm particle size in the grinding product reaches 55%. The grinding product and the product under the -0.10 mm screen are then combined as flotation feed.

[0043] (2) Copper-sulfur mixed flotation is carried out on the flotation feed. 150 g / t of copper sulfate, 200 g / t of butyl xanthate and 20 g / t of No. 2 oil are added to the flotation feed in sequence. The stirring time of each reagent is 3 min. Mixed flotation roughing is carried out under the condition of 45% pulp concentration for 3 min to obtain copper-sulfur mixed flotation rough concentrate and copper-sulfur mixed flotation roughing tailings. The copper-sulfur mixed flotation rough concentrate is subjected to 3 blank cleanings for 3 min each to obtain copper-sulfur mixed concentrate. The copper-sulfur mixed flotation roughing tailings are subjected to 2 scavengings. In scavenging 1, 40 g / t of butyl xanthate and 10 g / t of No. 2 oil are added in sequence and stirred for 3 min each. The flotation time is 2 min. In scavenging 2, 30 g / t of butyl xanthate and 5 g / t of No. 2 oil are added in sequence and stirred for 3 min each. The flotation time is 1.5 min to obtain copper-sulfur flotation tailings and mixed flotation scavenging concentrate. The mixed flotation scavenging concentrate is returned to the previous operation.

[0044] (3) Copper-sulfur separation is performed on the copper-sulfur mixed concentrate. 500 g / t of calcium hypochlorite, 800 g / t of sodium humate, and 30 g / t of Z200 are added sequentially to the copper-sulfur mixed concentrate and stirred for 3 min. Copper-sulfur separation roughing is performed under a pulp concentration of 35% for 3 min to obtain copper rough concentrate and copper-sulfur separation roughing tailings. The copper rough concentrate is then subjected to four cleaning processes: Cleaning 1: 200 g / t of calcium hypochlorite and 200 g / t of sodium humate are added sequentially and stirred for 3 min, with a flotation time of 2.5 min. Cleaning 2: 100 g / t of calcium hypochlorite and 80 g / t of sodium humate are added sequentially and stirred for 3 min, with a flotation time of 2 min. Cleaning 3: 50 g / t of calcium hypochlorite and 40 g / t of sodium humate are added sequentially and stirred for 3 min, with a flotation time of 2 min. Cleaning 4: ... 50 g / t of calcium hypochlorite and 40 g / t of sodium humate were added sequentially, stirred for 3 min each, and floated for 2 min to obtain a copper-silver concentrate with a yield of 1.01%, a Cu grade of 22.45%, a Cu recovery rate of 94.48%, and an Ag content of 2680 g / t. The middlings were returned to the previous stage of the process. The copper-sulfur separation tailings were subjected to two scavenging processes, with Z200 dosages of 6 g / t and 4 g / t respectively, stirred for 3 min each time, and floated for 2 min and 1.5 min respectively, to obtain a sulfur concentrate with a yield of 8.00% and a S grade of 36.77%. The scavenged concentrate was returned to the previous stage of the process.

[0045] (4) The copper-sulfur flotation tailings were subjected to weak magnetic separation. A process of one roughing and one cleaning was adopted. The magnetic field strength of the weak magnetic roughing was 0.20T and the magnetic field strength of the weak magnetic cleaning was 0.15T, and an iron concentrate with a yield of 0.84% ​​and a TFe grade of 65.58% was obtained. The tailings from the weak magnetic roughing and the middlings from the weak magnetic cleaning were combined and fed into a thickener for concentration, which was used as weak magnetic tailings.

[0046] (5) The weakly magnetic tailings were subjected to scheelite cascade pre-enrichment. The pre-enrichment process consisted of one pre-enrichment roughing, two pre-enrichment cleaning, and three pre-enrichment scavenging. In the roughing process, 2000 g / t of sodium carbonate, 6000 g / t of water glass, and 650 g / t of scheelite collector CY (the mass ratio of oxidized paraffin soap, modified fatty acid, and alkyl phosphate in CY was 2:1:1) were added sequentially and stirred for 3 min. The roughing pulp was then floated for 3 min at a pH of 10.20. In scavenging processes 1, 2, and 3, 80 g / t, 60 g / t, and 40 g / t of CY were added, respectively, and stirred for 3 min. The floatation times were 2 min, 2 min, and 1.5 min, respectively. Both cleaning processes used blank cleaning and the floatation time was 2 min. Scavenging rough concentrate and scheelite flotation tailings were obtained. The middlings from the pre-enrichment cleaning and the pre-enrichment scavenging concentrate were combined and returned to the pre-enrichment roughing operation.

[0047] (6) Deeply upgrade and reduce impurities in scheelite rough concentrate. After concentrating the scheelite rough concentrate to a pulp concentration of 55%, it is fed into an upgraded and heated mixing tank. At 80℃, 300g / t of scheelite collector CY is added and stirred for 5 minutes. Then, 8000g / t of water glass is added and stirred for 60 minutes. This mixture is then fed into a normal-temperature flotation cell, where water is added to adjust the pulp concentration to 30%. Upgrading roughing is carried out at a pulp pH of 10.80 to obtain upgraded scheelite rough concentrate and tailings. The upgraded scheelite rough concentrate is then subjected to five blank cleaning cycles to obtain scheelite concentrate with a yield of 29.45%, a WO3 grade of 71.98%, a Sn content of 0.03%, and a WO3 recovery rate of 59.68%. The middlings from the upgrading cleaning are returned to the previous stage of the process. The upgraded scheelite tailings are then subjected to two upgrading scavenging cycles: 50g / t of CY is added in upgrading scavenging cycle 1, and CY is added in upgrading scavenging cycle 2. 40g / t, to obtain upgraded scavenging tailings, and upgraded scavenging concentrate is returned to the previous stage operation in sequence.

[0048] (7) The scavenging tailings are subjected to shaking table gravity separation to obtain gravity concentrate and gravity tailings. The gravity tailings are discharged into the tailings pond. The gravity concentrate is returned to the fine classification operation in step (1) for regrinding and re-selection, so that the tungsten-tin intergrowth minerals that are not fully liberated in the gravity concentrate can re-enter the subsequent beneficiation process.

[0049] (8) The scheelite flotation tailings were separated by multi-gradient high-intensity magnetic separation. The process consisted of one roughing, two cleaning, and one scavenging. The magnetic field strengths for the roughing, first cleaning, second cleaning, and scavenging were 1.0T, 0.8T, 0.6T, and 1.3T, respectively. This yielded scheelite concentrate with a yield of 19.04%, a WO3 grade of 71.43%, a WO3 recovery rate of 38.29%, and a Sn content of 0.14%, as well as tin concentrate with a yield of 28.78%, a Sn grade of 52.36%, and a Sn recovery rate of 98.43%. The middlings from the high-intensity magnetic cleaning and the high-intensity magnetic scavenging concentrate were combined and returned to the high-intensity magnetic roughing operation.

[0050] When the above-mentioned complex tungsten-tin mixed concentrate is processed using the method of the present invention, the combined WO3 recovery rate of scheelite and wolframite concentrate is 97.97%, the Sn recovery rate of tin concentrate is 98.43%, and copper-silver concentrate, sulfur concentrate and iron concentrate are obtained at the same time, realizing the separation of tungsten and tin and the comprehensive recovery of associated resources. Example 2

[0051] This embodiment uses a complex tungsten-tin mixed concentrate obtained from gravity separation at a beneficiation plant in Guangdong as the processing target.

[0052] The ore sample has a WO3 grade of 38.52%, a Sn grade of 13.88%, a Cu grade of 0.45%, a S grade of 2.88%, and a silver content of 38 g / t. The tungsten minerals are mainly wolframite and scheelite, which together account for over 98% of the tungsten minerals; the tin mineral is mainly cassiterite; sulfur mainly exists in the form of pyrite, with a small amount of magnetic iron minerals; silver is mainly hosted in sulfide minerals; and the gangue minerals are mainly garnet, feldspar, calcite, and quartz.

[0053] like Figure 1 As shown, the specific steps include: (1) Fine classification of complex tungsten-tin mixed concentrate is carried out with 0.10 mm as the classification particle size. The product on the +0.10 mm screen is targeted grinding so that the content of -0.075 mm particle size in the grinding product reaches 55%. The grinding product and the product under the -0.10 mm screen are then combined as flotation feed.

[0054] (2) Copper-sulfur mixed flotation is carried out on the flotation feed. 200 g / t of copper sulfate, 200 g / t of butyl xanthate and 20 g / t of No. 2 oil are added to the flotation feed in sequence. The stirring time of each reagent is 3 min. Mixed flotation roughing is carried out under the condition of 45% pulp concentration for 3 min to obtain copper-sulfur mixed flotation rough concentrate and copper-sulfur mixed flotation roughing tailings. The copper-sulfur mixed flotation rough concentrate is subjected to 3 blank cleanings for 3 min each to obtain copper-sulfur mixed concentrate. The copper-sulfur mixed flotation roughing tailings are subjected to 2 scavengings. In scavenging 1, 50 g / t of butyl xanthate and 10 g / t of No. 2 oil are added in sequence and stirred for 3 min each. The flotation time is 2 min. In scavenging 2, 30 g / t of butyl xanthate and 5 g / t of No. 2 oil are added in sequence and stirred for 3 min each. The flotation time is 1.5 min to obtain copper-sulfur flotation tailings and mixed flotation scavenging concentrate. The mixed flotation scavenging concentrate is returned to the previous operation in sequence.

[0055] (3) Copper-sulfur separation is performed on the copper-sulfur mixed concentrate. 500 g / t of calcium hypochlorite, 800 g / t of sodium humate, and 35 g / t of Z200 are added sequentially to the copper-sulfur mixed concentrate. The mixture is stirred for 3 minutes each time, and roughing is performed under a pulp concentration of 35%, with a flotation time of 3 minutes, yielding a copper rough concentrate and copper-sulfur separation tailings. The copper rough concentrate is then subjected to four cleaning processes. For cleaning process 1, 200 g / t of calcium hypochlorite and 200 g / t of sodium humate are added sequentially, stirred for 3 minutes each time, and the flotation time is 2.5 minutes. For cleaning process 2, 100 g / t of calcium hypochlorite and 80 g / t of sodium humate are added sequentially, stirred for 3 minutes each time, and the flotation time is 2 minutes. For cleaning process 3, 50 g / t of calcium hypochlorite and 40 g / t of sodium humate are added sequentially, stirred for 3 minutes each time, and the flotation time is 2 minutes. 4. Add 50 g / t of calcium hypochlorite and 40 g / t of sodium humate sequentially, stir for 3 min each, and separate for 2 min to obtain a copper-silver concentrate with a yield of 2.10%, a Cu grade of 20.73%, a Cu recovery rate of 96.74%, and an Ag content of 1652 g / t. The middlings are returned to the previous stage of operation. The copper-sulfur separation tailings are subjected to two scavenging processes, with Z200 dosages of 6 g / t and 4 g / t respectively, stirring for 3 min each time, and flotation times of 2 min and 1.5 min respectively, to obtain a sulfur concentrate with a yield of 5.80% and a S grade of 35.34%. The scavenged concentrate is returned to the previous stage of operation.

[0056] (4) The copper-sulfur flotation tailings were subjected to weak magnetic separation. A process of one roughing and one cleaning was adopted. The magnetic field strength of the weak magnetic roughing was 0.20T and the magnetic field strength of the weak magnetic cleaning was 0.15T, and an iron concentrate with a yield of 0.84% ​​and a TFe grade of 65.02% was obtained. The tailings of the weak magnetic roughing and the middlings of the weak magnetic cleaning were combined and fed into a thickener for concentration, which was used as weak magnetic tailings.

[0057] (5) The weakly magnetic tailings were subjected to scheelite cascade pre-enrichment. The pre-enrichment process consisted of one pre-enrichment roughing, two pre-enrichment cleaning, and three pre-enrichment scavenging. In the roughing process, 1200 g / t of sodium carbonate, 5000 g / t of water glass, and 500 g / t of scheelite collector CY (the mass ratio of oxidized paraffin soap, modified fatty acid, and alkyl phosphate in CY was 2:1:1) were added sequentially and stirred for 3 min. The roughing pulp was then floated for 3 min at a pH of 10.20. In scavenging processes 1, 2, and 3, 60 g / t, 40 g / t, and 30 g / t of CY were added respectively and stirred for 3 min. The floatation times were 2 min, 2 min, and 1.5 min respectively. The two cleaning processes were both blank cleaning with a floatation time of 2 min each. Scavenging rough concentrate and scheelite flotation tailings were obtained. The middlings from the pre-enrichment cleaning and the pre-enrichment scavenging concentrate were combined and returned to the pre-enrichment roughing operation.

[0058] (6) Deeply upgrade and reduce impurities in scheelite rough concentrate. After concentrating the scheelite rough concentrate to a pulp concentration of 55%, it is fed into an upgraded and heated mixing tank. Under conditions of 80℃, 250g / t of scheelite collector CY is added and stirred for 5 minutes. Then, 7500g / t of water glass is added and stirred for 60 minutes. This mixture is then fed into a normal-temperature flotation cell, and water is added to adjust the pulp concentration to 30%. Upgrading roughing is carried out under pulp pH conditions of 10.80 to obtain upgraded scheelite rough concentrate and scheelite roughing tailings. The upgraded scheelite rough concentrate is then subjected to five blank cleaning cycles to obtain scheelite concentrate with a yield of 16.05%, WO3 grade of 72.73%, Sn content of 0.02%, and WO3 recovery rate of 30.30%. The middlings from the upgrading cleaning are returned to the previous stage of operation. The scheelite roughing tailings are then subjected to two upgrading scavenging cycles: 45g / t of CY is added in upgrading scavenging cycle 1, and CY is added in upgrading scavenging cycle 2. 30g / t, to obtain upgraded scavenging tailings, and upgraded scavenging concentrate is returned to the previous stage operation in sequence.

[0059] (7) The scavenging tailings are subjected to shaking table gravity separation to obtain gravity concentrate and gravity tailings. The gravity tailings are discharged into the tailings pond. The gravity concentrate is returned to the fine classification operation in step (1) for regrinding and re-selection, so that the tungsten-tin intergrowth minerals that are not fully liberated in the gravity concentrate can re-enter the subsequent beneficiation process.

[0060] (8) The scheelite flotation tailings were separated by multi-gradient high-intensity magnetic separation. The process consisted of one roughing, two cleaning, and one scavenging. The magnetic field strengths for the roughing, first cleaning, second cleaning, and scavenging were 1.0T, 0.8T, 0.6T, and 1.3T, respectively. This yielded scheelite concentrate with a yield of 37.04%, a WO3 grade of 70.88%, a WO3 recovery rate of 68.16%, and a Sn content of 0.11%, as well as tin concentrate with a yield of 24.898%, a Sn grade of 55.02%, and a Sn recovery rate of 98.66%. The middlings from the high-intensity magnetic separation and the high-intensity magnetic scavenging concentrate were combined and returned to the high-intensity magnetic roughing operation.

[0061] When the above-mentioned complex tungsten-tin mixed concentrate is processed using the method of the present invention, the combined WO3 recovery rate of scheelite and wolframite concentrate is 98.46%, the Sn recovery rate of tin concentrate is 98.66%, and copper-silver concentrate, sulfur concentrate and iron concentrate are obtained at the same time, indicating that the method of the present invention can be applied to complex tungsten-tin mixed concentrate from different sources.

[0062] Comparative Example 1 The ore sample used in this comparative example is the same as that in Example 1. This comparative example does not employ 0.10mm pre-classification and coarse-grained targeted grinding; instead, all complex tungsten-tin mixed concentrates are uniformly ground to a -0.075mm particle size content of 65%. Furthermore, this comparative example differs from Example 1 in some copper-sulfur separation reagent formulations and scheelite collectors. Therefore, this comparative example is used to evaluate the overall beneficiation indicators of the control process, and the differences in indicators are not attributed solely to the grinding method.

[0063] (1) All complex tungsten-tin mixed concentrates are uniformly ground so that the content of -0.075mm particle size in the grinding product reaches 65%, and the resulting grinding product is used as flotation feed.

[0064] (2) Add 150g / t of copper sulfate, 200g / t of butyl xanthate and 20g / t of No. 2 oil to the flotation feed for copper-sulfur mixed flotation roughing to obtain copper-sulfur mixed flotation rough concentrate and copper-sulfur mixed flotation roughing tailings; perform three blank cleanings on the copper-sulfur mixed flotation rough concentrate to obtain copper-sulfur mixed concentrate; perform two scavengings on the copper-sulfur mixed flotation roughing tailings, adding 40g / t of butyl xanthate and 10g / t of No. 2 oil to scavenging 1 and adding 30g / t of butyl xanthate and 5g / t of No. 2 oil to scavenging 2 to obtain copper-sulfur flotation tailings and mixed flotation scavenging concentrate, and return the mixed flotation scavenging concentrate to the previous operation in sequence.

[0065] (3) Add 500 g / t of calcium hypochlorite and 300 g / t of sodium humate to the copper-sulfur mixed concentrate for rough separation of copper and sulfur; perform four fine separations on the resulting copper concentrate: for fine separation 1, add 300 g / t of calcium hypochlorite and 100 g / t of sodium humate; for fine separation 2, add 200 g / t of calcium hypochlorite and 80 g / t of sodium humate; for fine separation 3, add 150 g / t of calcium hypochlorite and 60 g / t of sodium humate. 4. Add 100 g / t of calcium hypochlorite and 50 g / t of sodium humate to obtain a copper-silver concentrate with a yield of 0.97%, a Cu grade of 22.19%, a Cu recovery rate of 89.68%, and an Ag content of 2691 g / t. Then, perform two scavenging processes on the copper-sulfur separation roughing tailings, with Z200 dosages of 6 g / t and 4 g / t respectively, to obtain a sulfur concentrate with a yield of 7.88% and a S grade of 36.99%.

[0066] (4) The copper-sulfur flotation tailings were subjected to one roughing and one cleaning weak magnetic separation. The magnetic field strength of the roughing was 0.20T and the magnetic field strength of the cleaning was 0.15T, to obtain an iron concentrate with a yield of 0.80% and a TFe grade of 65.72%.

[0067] (5) The weak magnetic tailings were subjected to scheelite pre-enrichment flotation, which consisted of one roughing, two cleaning and three scavenging processes. Sodium carbonate 2000g / t, water glass 6000g / t and scheelite collector 733 650g / t were added during the roughing process. 733 80g / t, 60g / t and 40g / t were added during the three scavenging processes, respectively, to obtain scheelite rough concentrate and scheelite flotation tailings.

[0068] (6) The scheelite rough concentrate was concentrated to a pulp mass concentration of 55%, and scheelite collector 733 300g / t and water glass 8000g / t were added for upgrading roughing. The resulting upgraded rough concentrate was subjected to 5 blank cleanings to obtain scheelite concentrate with a yield of 27.60%, WO3 grade of 71.25%, Sn content of 0.15%, and WO3 recovery rate of 55.36%. The upgraded roughing tailings were subjected to 2 scavengings, with 733 50g / t and 40g / t added respectively to obtain upgraded scavenging tailings.

[0069] (7) The tailings of the scavenging process are subjected to shaking table gravity separation. The gravity separation concentrate is returned to the unified grinding operation for regrinding and re-separation, and the gravity separation tailings are discharged.

[0070] (8) The scheelite flotation tailings were subjected to multi-gradient strong magnetic separation, including one roughing, two cleaning and one scavenging. The magnetic field strengths of the roughing, the first cleaning, the second cleaning and the scavenging were 1.0T, 0.8T, 0.6T and 1.3T respectively, to obtain scheelite concentrate with a yield of 18.06%, WO3 grade of 69.87%, WO3 recovery rate of 35.53% and Sn content of 0.26%, and tin concentrate with a yield of 27.81%, Sn grade of 50.62% and Sn recovery rate of 91.95%.

[0071] Using the above-described control process to process the ore sample from Example 1, the overall WO3 recovery rate of scheelite and wolframite concentrate was 90.89%, a decrease of 7.08 percentage points compared to Example 1; the Sn recovery rate of tin concentrate was 91.95%, a decrease of 6.48 percentage points compared to Example 1. The overall tungsten-tin separation index of the control process was lower than that of Example 1.

[0072] Comparative Example 2 The ore samples used in this comparative example are the same as those in Example 1. This control process eliminates the shaking table gravity separation enrichment of the upgraded scavenging tailings and the return of the gravity concentrate to regrinding and re-concentration; simultaneously, its scheelite collector and some copper-sulfur separation reagent formulations differ from those in Example 1. Therefore, this comparative example is used to illustrate the overall indicators of the control process, including the elimination of gravity separation return, and does not attribute the differences in indicators solely to the technical condition of eliminating gravity separation return.

[0073] (1) Fine classification is carried out with 0.10mm as the grading particle size. The product over the +0.10mm screen is targeted grinding so that the content of -0.075mm particle size in the grinding product reaches 55%, and then it is combined with the product under the -0.10mm screen as flotation feed.

[0074] (2) Add 150g / t of copper sulfate, 200g / t of butyl xanthate and 20g / t of No. 2 oil to the flotation feed for copper-sulfur mixed flotation roughing; perform three blank cleanings on the mixed flotation rough concentrate; perform two scavengings on the mixed flotation roughing tailings, adding 40g / t of butyl xanthate and 10g / t of No. 2 oil to scavenging 1, and adding 30g / t of butyl xanthate and 5g / t of No. 2 oil to scavenging 2.

[0075] (3) Add 500 g / t of calcium hypochlorite and 800 g / t of sodium humate to the copper-sulfur mixed concentrate for copper-sulfur separation roughing; the obtained copper rough concentrate is subjected to 4 cleaning processes. In cleaning process 1, 200 g / t of calcium hypochlorite and 200 g / t of sodium humate are added. In cleaning process 2, 100 g / t of calcium hypochlorite and 80 g / t of sodium humate are added. In cleaning processes 3 and 4, 50 g / t of calcium hypochlorite and 40 g / t of sodium humate are added respectively to obtain copper-silver concentrate with a yield of 1.01%, a Cu grade of 21.98%, a Cu recovery rate of 92.50%, and an Ag content of 2682 g / t. The copper-sulfur separation roughing tailings are scavenged twice to obtain sulfur concentrate with a yield of 7.97% and a S grade of 36.45%.

[0076] (4) The copper-sulfur flotation tailings were subjected to one roughing and one cleaning weak magnetic separation. The magnetic field strength of the roughing was 0.20T and the magnetic field strength of the cleaning was 0.15T, to obtain an iron concentrate with a yield of 0.82% and a TFe grade of 65.51%.

[0077] (5) The weak magnetic tailings were subjected to scheelite pre-enrichment flotation, which consisted of one roughing, two cleaning and three scavenging processes. Sodium carbonate 2000g / t, water glass 6000g / t and scheelite collector 733 650g / t were added during the roughing process. 733 80g / t, 60g / t and 40g / t were added during the three scavenging processes, respectively, to obtain scheelite rough concentrate and scheelite flotation tailings.

[0078] (6) The scheelite rough concentrate was concentrated to a pulp mass concentration of 55%, and scheelite collector 733 300g / t and water glass 8000g / t were added for upgrading roughing. The resulting upgraded rough concentrate was subjected to 5 blank cleanings to obtain scheelite concentrate with a yield of 28.15%, WO3 grade of 71.77%, Sn content of 0.12%, and WO3 recovery rate of 56.88%. The upgraded roughing tailings were subjected to 2 scavengings, with 733 50g / t and 40g / t added respectively to obtain upgraded scavenging tailings.

[0079] (7) The upgraded scavenging tailings are directly discharged as the final tailings, without further shaking table gravity separation enrichment, and without setting up a gravity separation concentrate return to regrinding and re-selection process.

[0080] (8) The scheelite flotation tailings were subjected to multi-gradient strong magnetic separation by one roughing, two cleaning and one scavenging. The magnetic field strengths of the roughing, first cleaning, second cleaning and scavenging were 1.0T, 0.8T, 0.6T and 1.3T respectively, to obtain scheelite concentrate with a yield of 17.04%, WO3 grade of 71.62%, WO3 recovery rate of 34.36% and Sn content of 0.14%, and tin concentrate with a yield of 26.43%, Sn grade of 52.66% and Sn recovery rate of 90.89%.

[0081] Using the control process described above to process the ore samples from Example 1, the WO3 recovery rate of scheelite concentrate decreased by 2.80 percentage points compared to Example 1, the WO3 recovery rate of wolframite concentrate decreased by 3.93 percentage points compared to Example 1, and the Sn recovery rate of tin concentrate decreased by 7.54 percentage points compared to Example 1. These results indicate that when the control process does not include the gravity separation enrichment and return grinding / re-separation stages for the scavenging tailings, the overall tungsten and tin recovery indicators are lower than those of Example 1. Given the differences in collectors and some reagent formulations between the two processes, these differences are not solely attributable to the elimination of the gravity separation and return process.

[0082] Comparative Example 3 The mineral samples used in this comparative example are the same as those in Example 1. The main difference from Example 1 is that the weak magnetic tailings do not employ the scheelite stepwise pre-enrichment, deep upgrading and impurity reduction of scheelite rough concentrate, and multi-gradient strong magnetic separation process for scheelite flotation tailings. Instead, a mixed flotation process of black and white tungsten and tungsten tailings flotation with tin is used.

[0083] (1) Process the mineral sample according to steps (1) to (4) of Example 1 to obtain weak magnetic tailings.

[0084] (2) The weak magnetic tailings were subjected to mixed flotation roughing with black and white tungsten. Sodium carbonate 1000g / t, water glass 1000g / t and benzohydroxyxamic acid 600g / t were added to obtain mixed flotation rough concentrate and mixed flotation roughing tailings with black and white tungsten.

[0085] (3) The mixed tungsten concentrate was subjected to four cleaning processes. Cleaning 1 involved adding 300 g / t of water glass and 200 g / t of aluminum sulfate; Cleaning 2 involved adding 200 g / t of water glass and 150 g / t of aluminum sulfate; Cleaning 3 involved adding 100 g / t of water glass and 50 g / t of aluminum sulfate; and Cleaning 4 involved blank cleaning. The tailings from the mixed tungsten concentrate roughing were subjected to two scavenging processes, with 60 g / t and 30 g / t of benzoyl hydroxamic acid added respectively. A mixed tungsten concentrate with a yield of 52.02%, a WO3 grade of 61.39%, a Sn content of 5.78%, and a WO3 recovery rate of 89.91%, as well as the mixed tungsten tailings, were obtained.

[0086] (4) The black and white tungsten mixed flotation tailings are subjected to cassiterite flotation roughing by adding 1500g / t hydrochloric acid, 800g / t lead nitrate, 500g / t styrene phosphonic acid and 30g / t P86 to obtain cassiterite flotation rough concentrate and cassiterite flotation roughing tailings.

[0087] (5) The cassiterite flotation rough concentrate is cleaned three times. In the first clean, 100 g / t of water glass and 50 g / t of aluminum sulfate are added. In the second clean, 80 g / t of water glass and 40 g / t of aluminum sulfate are added. In the third clean, 100 g / t of water glass and 30 g / t of aluminum sulfate are added. The cassiterite flotation rough tailings are scavenged twice. In the first scavenging, 100 g / t of styrene phosphonic acid and 10 g / t of P86 are added. In the second scavenging, 80 g / t of styrene phosphonic acid and 5 g / t of P86 are added. A tin concentrate with a yield of 26.60%, a Sn grade of 45.21%, and a Sn recovery rate of 78.55% and tin flotation tailings are obtained. The tin flotation tailings are discharged.

[0088] The combined WO3 grade of the scheelite and wolframite concentrates obtained in Example 1, weighted by their respective yields, was approximately 71.76%. The WO3 grade of the mixed scheelite and wolframite concentrate obtained in this comparative example was 61.39%, a decrease of approximately 10.37 percentage points, while the Sn content increased to 5.78%. The Sn grade of the tin concentrate in this comparative example decreased by 7.15 percentage points compared to Example 1, and the WO3 recovery rate of the tungsten concentrate and the Sn recovery rate of the tin concentrate decreased by 8.06 percentage points and 19.88 percentage points, respectively. These results indicate that conventional mixed flotation of scheelite and wolframite, followed by tungsten tailings flotation for tin, suffers from problems such as high tungsten-tin intermingling content, low concentrate quality, and significant loss of tungsten and tin resources.

[0089] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. All equivalent substitutions, modifications, or improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for separating complex tungsten-tin mixed concentrate and recovering associated resources, wherein the complex tungsten-tin mixed concentrate contains scheelite, wolframite, and cassiterite, and is associated with copper sulfide minerals, silver-bearing sulfide minerals, pyrite, and magnetic iron minerals, characterized in that, Includes the following steps: (1) According to the 0.10mm classification, only the +0.10mm product is ground to the -0.075mm particle size content of 45% to 65%, and then combined with the -0.10mm product as flotation feed; (2) The flotation feed is subjected to copper-sulfur mixed flotation to obtain copper-sulfur mixed concentrate and copper-sulfur flotation tailings; (3) The copper-sulfur mixed concentrate is subjected to copper-sulfur separation to obtain copper-silver concentrate and sulfur concentrate; (4) The copper-sulfur flotation tailings are subjected to weak magnetic separation to obtain iron concentrate and weak magnetic tailings; (5) The weak magnetic tailings are subjected to scheelite stepwise pre-enrichment to obtain scheelite rough concentrate and scheelite flotation tailings; (6) Deeply upgrade and reduce impurities in the scheelite rough concentrate to obtain scheelite concentrate and upgraded scavenging tailings; (7) The upgraded scavenging tailings are enriched by gravity separation to obtain gravity concentrate and gravity tailings. The gravity concentrate is returned to the 0.10mm classification operation in step (1) for regrinding and re-selection, and the gravity tailings are discharged. (8) The scheelite flotation tailings are subjected to multi-gradient strong magnetic separation to obtain scheelite concentrate and tin concentrate.

2. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (2), the copper-sulfur mixed flotation includes one mixed flotation roughing, one to three mixed flotation cleaning, and one to three mixed flotation scavenging. The middlings from the mixed flotation cleaning and the mixed flotation scavenging concentrate are returned to the previous stage of operation in sequence.

3. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (3), the obtained copper-sulfur mixed concentrate is subjected to copper-sulfur separation by a sulfur-suppressing and copper-floating method to obtain copper-silver concentrate and sulfur concentrate; the copper-sulfur separation includes one separation roughing, two to four copper-floating cleaning and one to three separation scavenging, and the copper-floating cleaning middlings and the separation scavenging concentrate are returned to the previous stage operation in sequence; the sulfur mineral inhibitor used in the copper-sulfur separation is selected from one or more of calcium hypochlorite, sodium humate and lime.

4. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (4), the weak magnetic separation includes one coarse separation and one to two fine separations, with a magnetic field strength of 0.05 to 0.30T.

5. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (5), the scheelite step-by-step pre-enrichment includes one pre-enrichment roughing, one to three pre-enrichment cleaning, and one to three pre-enrichment scavenging. The middlings from the pre-enrichment cleaning and the pre-enrichment scavenging concentrate are returned to the pre-enrichment roughing operation. The scheelite collector used in the scheelite step-by-step pre-enrichment is selected from one or more of oxidized paraffin soap, modified fatty acids, oleamide, modified hydroxamic acid, and alkyl phosphates. The modifier used is selected from one or more of sodium carbonate, sodium hydroxide, water glass, aluminum sulfate, and sodium hexametaphosphate.

6. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 5, characterized in that, In step (6), the scheelite rough concentrate is concentrated to a pulp mass concentration of not less than 55% and then subjected to deep upgrading and impurity reduction. The deep upgrading and impurity reduction includes one upgrading roughing, three to five upgrading cleaning and one to two upgrading scavenging. The middlings from the upgrading cleaning and the scavenging concentrate are returned to the previous stage of operation in sequence. The inhibitors used in the deep upgrading and impurity reduction are selected from one or more of water glass, salt-modified water glass, aluminum sulfate, sodium carboxymethyl cellulose, tannin, starch and dextrin.

7. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (7), the gravity enrichment adopts shaking table gravity separation, so that the coarse tungsten-tin intergrowth minerals in the upgraded scavenging tailings enter the gravity concentrate; the gravity concentrate is returned to fine classification, of which the +0.10mm part enters targeted grinding, and the -0.10mm part is directly merged with the grinding product and enters the subsequent beneficiation.

8. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 1, characterized in that, In step (8), the multi-gradient strong magnetic separation includes one roughing, two cleaning and one scavenging; the magnetic field strengths of the roughing, the first cleaning, the second cleaning and the scavenging are 1.0T, 0.8T, 0.6T and 1.3T respectively, and the middlings of the strong magnetic cleaning and the concentrate of the strong magnetic scavenging are combined and returned to the roughing operation.

9. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 5, characterized in that, The scheelite collector is composed of oxidized paraffin soap, modified fatty acid, and alkyl phosphate in a mass ratio of 2:1:

1.

10. The method for separating complex tungsten-tin mixed concentrates and recovering associated resources according to claim 6, characterized in that, In step (5), the pre-enrichment roughing reagent system is: sodium carbonate 1200-2000 g / t, water glass 5000-6000 g / t and scheelite collector 500-650 g / t; in step (6), the quality-enhancing roughing reagent system for deep quality improvement and impurity reduction is: scheelite collector 250-300 g / t and water glass 7500-8000 g / t.