A low alkalinity copper-sulfur separation process for complex polymetallic ore
By preparing a low-alkalinity potential-controlled mineral processing and separation agent, combined with electrochemical control, efficient separation of copper and sulfur in a low-alkalinity environment was achieved, solving the problems of equipment scaling and reduced copper concentrate grade, and improving the selectivity and stability of copper-sulfur separation.
Patent Information
- Application Number
- CN202611358398.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies for copper-sulfur separation suffer from problems such as equipment scaling and reduced copper concentrate grade and recovery rate due to the use of lime in high alkalinity environments. Furthermore, the organic inhibitors have poor selectivity, making it difficult to achieve efficient copper-sulfur separation in low alkalinity environments.
A low-alkalinity potential-controlled beneficiation and separation reagent for polymetallic ores, prepared under specific catalytic systems and heat treatment conditions, is used to construct targeted chelation adsorption capacity through melt polymerization reaction. Combined with in-situ electrochemical regulation by sodium hypochlorite and sodium metabisulfite, precise flotation separation of copper and sulfur is achieved in a low-alkalinity environment.
The method improves the grade and recovery rate of copper concentrate under lime-free conditions, solves the problem of equipment scaling, enhances the selectivity and stability of copper-sulfur separation, and extends the service life of the equipment.
Smart Images

Figure CN123149062A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymetallic mineral processing technology, specifically to a copper-sulfur separation process for complex polymetallic ores with low alkalinity. Background Technology
[0002] Copper is an indispensable strategic resource for national economy and defense. However, with the increasing depletion of high-quality, easily beneficiated copper ore resources, the efficient recovery of refractory polymetallic sulfide ores containing chalcopyrite, iron sulfides, and complex gangue has become a research hotspot in the field of non-ferrous metal beneficiation. In these ores, chalcopyrite is often closely associated with pyrite, pyrrhotite, and easily oxidized marcasite, and is often accompanied by silicate gangue such as talc with high natural floatability, making the flotation separation of copper-sulfur and copper-based heterogeneous minerals extremely difficult.
[0003] Currently, the most commonly used traditional process for copper-sulfur separation in industry is still high-alkali desulfurization technology. This method involves adjusting the pH of the slurry to above 12 by adding large amounts of lime, using the high concentration of calcium ions and the strong alkaline environment to passivate the pyrite. However, this method has significant systemic drawbacks. The use of large amounts of lime causes severe calcium carbonate scaling and caking on the inner walls of industrial pipelines, pumps, valves, and beneficiation equipment, increasing maintenance costs and shortening equipment lifespan. Furthermore, the strong alkaline calcification system can cause the surface of fine-grained chalcopyrite to become hydrophilic, leading to a decrease in copper concentrate grade and recovery rate.
[0004] To reduce reliance on high-alkalinity lime systems, domestic and international engineers have begun exploring copper-sulfur separation in low-alkalinity environments using organic inhibitors or potential modulation techniques. However, existing organic inhibitors generally suffer from poor selectivity and limited functionality. When dealing with complex polymetallic ores rich in easily oxidizable marcasite, easily floatable pyrrhotite, and highly muddy talc, the effects of simple small-molecule chelating agents or single polymers are limited, failing to achieve the dual effects of macromolecular physical coating and chemical chelation passivation. This results in significant entrainment and flotation of pyrite and talc gangue, making it difficult to achieve efficient and precise copper concentrate uptake in low-alkalinity, lime-free environments. Therefore, a low-alkalinity copper-sulfur separation process for complex polymetallic ores is proposed. Summary of the Invention
[0005] The primary objective of this invention is to provide a method for preparing a low-alkalinity potential-controlled flotation separation reagent for complex polymetallic ores. This reagent is obtained through a melt polymerization reaction under specific catalytic systems and heat treatment conditions. This method not only enhances the chemical activity and buffering tolerance of the reagent to the pH of the slurry, but also constructs characteristic groups in its molecular framework that have targeted chelation and adsorption capabilities for the target minerals. This achieves precise and efficient flotation separation of copper and sulfur in a low-alkalinity, lime-free scaling environment. The flotation separation reagent prepared by this invention can effectively eliminate the interference of easily oxidized pyrrhotite, sulfur-rich easily floatable pyrrhotite, and naturally highly floatable talc gangue on chalcopyrite, improving the grade and recovery rate of copper concentrate. Furthermore, the entire process is green, low-toxicity, and environmentally friendly.
[0006] The second objective of this invention is to provide a low-alkalinity potential-controlled mineral processing and separation reagent for complex polymetallic ores, prepared using the method described above. This reagent enables efficient copper-sulfur flotation separation of complex polymetallic ores in a low-alkalinity environment with little or no lime addition, exhibiting good separation selectivity and reagent stability. It effectively eliminates the technical challenges of traditional high-alkalinity sulfur suppression processes, which involve large lime consumption and the negative impact of calcium ions on scaling and corrosion of pipelines and equipment.
[0007] A third objective of this invention is to provide the application of the above-mentioned polymetallic ore beneficiation and separation reagent in the low-alkalinity copper-sulfur flotation separation of complex polymetallic ores.
[0008] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: A method for preparing a low-alkalinity potential-controlled beneficiation and separation reagent for complex polymetallic ores includes the following steps: S1. A mixture of raw materials, modified lignin source, fluxing alkali, and inorganic polysulfide is added, and a modified catalyst is introduced. The mixture is then heated to undergo a melt-catalyzed polymerization reaction to obtain a skeletal intermediate with specific chelating groups. The raw materials include one or more of urea, glycine, sodium persulfate, ammonium cyanate, and isocyanate; the modified lignin source is sodium lignosulfonate. The fluxing alkali includes sodium hydroxide and sodium carbonate; the inorganic polysulfide is sodium polysulfide.
[0009] After the reaction is completed, the mixture is cooled to room temperature, and an appropriate amount of deionized water is added to dissolve the molten product. The solid catalyst is then recovered by filtration through a microporous membrane. The filtrate is concentrated and dried under reduced pressure to obtain the framework intermediate.
[0010] S2. The skeleton intermediate is mixed with dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid to form a multi-metal ore beneficiation and separation agent.
[0011] Preferably, the mass ratio of the mixed raw materials, sodium lignosulfonate, sodium hydroxide, sodium carbonate and sodium polysulfide in S1 is 10-15:8-12:10-35:1-5:3-5.
[0012] Preferably, in S1, the heating method for the melt catalytic polymerization reaction is a segmented stepped heating, and the conditions for the melt catalytic polymerization reaction are to react for 2-6 hours at a first stage temperature of 120-150℃, and then react for 2-8 hours at a second stage temperature of 160-200℃.
[0013] Preferably, in S1, the modified catalyst includes at least one of nano-titanium dioxide supported gold catalyst, activated carbon supported palladium-copper bimetallic catalyst, and magnetic nanocatalyst.
[0014] Preferably, the preparation steps of the nano-titanium dioxide supported gold catalyst are as follows: 10.0 g of titanium dioxide is dispersed in 200 mL of deionized water and magnetically stirred at 500 r / min for 30 min in a constant temperature water bath at 60 °C to form a uniform suspension; 50.8 mL of 0.01 mol / L chloroauric acid solution is added dropwise to the suspension using a pipette; the pH of the mixture is adjusted to a fixed value of 9.0 using a 0.1 mol / L sodium hydroxide solution, and the reaction is carried out under constant temperature and continuous stirring for 4 h.
[0015] After the reaction was completed, the mixture was cooled to 25°C and centrifuged at 4000 r / min. The precipitate was repeatedly washed with deionized water at 50°C until no white precipitate formed after adding 0.1 mol / L silver nitrate solution to the filtrate. The washed solid was placed in an oven and dried at 105°C for 12 h. The dried powder was then transferred to a muffle furnace and calcined at 350°C for 3 h in air at a heating rate of 5°C / min. After cooling to room temperature in the furnace, the powder was ground to obtain a nano-titanium dioxide-supported gold catalyst with a gold loading of 1.0 wt%.
[0016] Preferably, the preparation method of the activated carbon-supported palladium-copper bimetallic catalyst is as follows: 10.0 g of coconut shell activated carbon is added to 100 mL of 30% (v / v) nitric acid solution and refluxed at 80 °C for 4 h; the solution is washed with deionized water until the pH of the washing solution is 7.0, and then dried at 110 °C for 8 h; 0.625 g of palladium chloride is weighed and dissolved in 10.0 mL of 1.0 mol / L hydrochloric acid solution to prepare H2PdCl4 solution; 0.335 g of copper chloride dihydrate is weighed and dissolved in 20 mL of deionized water; the two solutions are mixed and diluted to 50 mL with deionized water.
[0017] 10.0 g of pretreated activated carbon was added to 50 mL of the above mixed solution and ultrasonically dispersed for 30 min. The solution was then sealed at 25 °C and stirred at 300 r / min for 12 h. The impregnated suspension was placed in an ice-water bath at 3 °C, and 40.0 mL of 0.5 mol / L sodium borohydride solution was added dropwise while stirring at 600 r / min. After the addition was complete, the reaction was maintained at 25 °C for 2 h. The reduced catalyst was filtered, washed 5 times with deionized water, and then washed 3 times with anhydrous ethanol. It was then vacuum dried in a vacuum oven at 80 °C for 10 h to obtain an activated carbon-supported palladium-copper bimetallic catalyst with a total metal loading of 5 wt% and a Pd:Cu mass ratio of 3:1.
[0018] Preferably, the magnetic nanocatalyst includes at least one of the following: iron(III) oxide coated titanium dioxide nanoparticles, titanium dioxide nanoparticles, and carbon-cobalt coated iron nanoparticles.
[0019] Preferably, the preparation steps of iron(III) oxide coated titanium dioxide nanoparticles are as follows: 1.0 g of iron(III) oxide powder is weighed and added to a mixture of 300 mL of anhydrous ethanol and 2.0 mL of deionized water, and ultrasonically dispersed for 40 min to form a uniform suspension. 4.0 mL of concentrated ammonia solution with a mass fraction of 25% is added to the suspension, and the mixture is stirred at 400 r / min at 25 °C. 3.0 mL of tetrabutyl titanate is slowly added dropwise at a constant rate of 0.1 mL / min using a variable-speed feed pump. After the addition is complete, the mixture is continuously stirred at 25 °C for 6 h. The precipitate is collected by magnetic separation using an external magnet, washed three times with anhydrous ethanol, and dried at 80 °C for 12 h. The dried solid is placed in a tube furnace, protected with high-purity argon gas (≥99.999%), heated to 450 °C at a heating rate of 2 °C / min, and calcined at this temperature for 2 h to obtain iron(III) oxide coated titanium dioxide nanoparticles with a particle size of 50-80 nm.
[0020] Preferably, the titanium dioxide nanoparticles are P25 type titanium dioxide nanoparticles with a mixed crystal form of anatase and rutile in a mass ratio of 80:20 and a specific surface area of 50 m². 2 / g, with a native average particle size of 21nm.
[0021] Preferably, the preparation steps of carbon-coated iron-cobalt nanoparticles are as follows: 2.38 g of cobalt chloride hexahydrate and 2.70 g of ferric chloride hexahydrate are weighed and dissolved in 100 mL of deionized water, with a Fe:Co molar ratio of 1:1. 9.0 g of glucose is added, and the mixture is stirred for 30 min to form a transparent mixed solution. Concentrated ammonia is added dropwise to adjust the pH to 10.0, resulting in co-precipitation. The mixture is transferred to a 200 mL polytetrafluoroethylene-lined reactor and hydrothermally reacted at 180 °C for 12 h. After the reaction is completed and cooled, the black precursor is obtained by centrifugation, washed three times with deionized water, and dried at 80 °C for 8 h. The dried precursor powder is placed in a tube furnace, and a mixed reducing gas of 5% H2 and 95% Ar (by volume) is introduced. The furnace is heated to 700 °C at a heating rate of 5 °C / min and carbonized under constant temperature reduction and gas permeation for 4 h. The furnace is then cooled to room temperature to obtain carbon-coated iron-cobalt nanoparticles with a particle size of 30-50 nm.
[0022] Preferably, in S2, the mass ratio of the skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid is 1-3:0.5-1:1-5:2-4:1-2.
[0023] A polymetallic ore beneficiation and separation agent is prepared by any of the methods described in the preceding embodiments.
[0024] The above-mentioned polymetallic ore beneficiation and separation reagents are used in the low-alkalinity copper-sulfur flotation separation of complex polymetallic ores.
[0025] Preferably, the method for copper-sulfur flotation separation includes the following steps: S1. A coarse grinding and classification process is performed on the complex polymetallic ore containing chalcopyrite, pyrite, marcasite, pyrrhotite, and talc, and water is added to prepare a copper roughing slurry. By controlling the grinding and classification parameters, the content of particles with a diameter <0.074mm in the copper roughing slurry is made up to 70% to 75%.
[0026] S2. Prepare the slurry by adding polymetallic ore separation reagents as targeted organic inhibitors, a low-alkalinity selective collector, and a frother to the copper roughing slurry. Through a closed-loop cycle of primary roughing, secondary cleaning, and two scavenging processes, the final copper concentrate and copper tailings are obtained. During slurry preparation, a compound in-situ electrochemical regulator consisting of sodium hypochlorite and sodium metabisulfite in a 1:4 mass ratio is added to control the slurry pH to 7.8-8.3. The slurry mass concentration of the copper roughing slurry is controlled at 30%-35%.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. This invention does not use traditional high-calcium strong-alkali reagents in the process, but instead uses an in-situ electrochemical regulator composed of sodium hypochlorite and sodium metabisulfite. The two potential-regulating components work synergistically to change the pulp potential in situ under a slightly alkaline environment of pH 7.8-8.3, promoting shallow oxidation of the surfaces of pyrite, marcasite, and monoclinic pyrrhotite. This widens the difference in surface potential and floatability between chalcopyrite and interfering minerals, achieving efficient flotation separation of low-alkalinity copper and sulfur under lime-free conditions.
[0028] 2. The hydrophilic macromolecular framework of sodium lignin sulfonate introduced into the organic inhibitor molecular condensate is physically covered on the crystal shear plane of natural easily floatable talc gangue to construct a hydrophilic layer. At the same time, high-density sulfur-containing active mercapto bonds and nitrogen atom coordinating chelating groups introduced by the compound modification of dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-(4-imidazolyl)propionic acid are used to chemically passivate the surface of the pyrite minerals that have been slightly oxidized in the slurry in situ. The two-pronged approach eliminates the above-mentioned mixing and flotation interference and improves the grade and recovery rate of copper concentrate.
[0029] 3. The entire process does not require the addition of lime, replacing the traditional high-consumption, high-alkali, and high-calcium desulfurization mode. This not only solves the industry bottleneck of hydrophilic calcification and difficulty in recovery of fine-grained chalcopyrite caused by high-calcium systems, but also avoids the damage to industrial pipelines, pumps, valves, and subsequent dewatering and beneficiation equipment caused by calcium ion scaling, thus extending the service life of production equipment. Attached Figure Description
[0030] Figure 1 This is a flowchart of the low-alkali full-sulfur flotation separation and comprehensive recovery process for complex polymetallic ores according to the present invention. Figure 2 This is a bar chart comparing the copper concentrate indicators of Example 1 and Comparative Example 1 of the present invention. Detailed Implementation
[0031] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions are followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0032] The following information is provided regarding the substances used: Chloroauric acid (HAuCl4·3H2O), CAS 16961-25-4, analytical grade, gold content ≥47.8wt%; Palladium chloride (PdCl2), CAS 7647-10-1, analytical grade, palladium content ≥59.5wt%; Copper chloride dihydrate (CuCl2·2H2O), CAS 10125-13-0, analytical grade, purity ≥99.0wt%; Coconut shell activated carbon with a specific surface area of 1100 m². 2 / g, pore volume 0.75cm 3 / g, particle size 100-200 mesh; ferric oxide powder purity ≥98.0wt%, average particle size 30nm; tetrabutyl titanate, CAS 5593-70-4, analytical grade, purity ≥99.0wt%; cobalt chloride hexahydrate CoCl2·6H2O, CAS 7791-13-1, purity ≥99.0wt%; ferric chloride hexahydrate FeCl3·6H2O, CAS 10025-77-1, purity ≥99.0wt%; glucose C6H 12 O6, CAS 50-99-7, analytical grade. It should also be noted that the metal grade and recovery rate analysis of copper and sulfur concentrates in this scheme were conducted in accordance with national standards GB / T 3884-2012 "Chemical Analysis Methods for Copper Concentrates" and GB / T 2463-2012.
[0033] The first aspect of this invention provides a method for preparing a polymetallic ore beneficiation and separation reagent, comprising the following steps: S1. Mix the raw materials, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide in a certain proportion, add a modified catalyst, and heat to carry out a segmented catalytic polymerization reaction to obtain a framework intermediate. The raw materials include one or more of urea, glycine, sodium persulfate, ammonium cyanate, and isocyanate.
[0034] S2. The skeleton intermediate is modified by mixing and mixing dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate and 2-amino-3-4-imidazolylpropionic acid in a certain proportion to obtain a multi-metal ore beneficiation and separation agent.
[0035] The polymetallic ore beneficiation separation reagent prepared by this invention is used in the mineral processing industry in the form of an aqueous solution with a mass concentration of 1%-5%. For example, it can be prepared into any single value or a range of any two values from 1%, 2%, 3%, 4%, to 5%. In some specific embodiments of this invention, the reagent exhibits excellent water solubility and resistance to water quality fluctuations under normal temperature and pressure conditions.
[0036] In some specific embodiments of the present invention, the mass ratio of the mixed raw materials, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide in S1 is 10-15:8-12:10-35:1-5:3-5. In specific implementations, any ratio or any range of two of the following can be selected, including but not limited to 10:8:10:1:3, 10:12:10:1:5, 10:10:10:5:5, 12:10:20:5:5, 11:9:28:1:3, 15:12:35:2:5, 15:8:20:1:3, and 15:11:30:5:4.
[0037] In some specific embodiments of the present invention, in S1, the catalytic reaction is heated in a segmented, stepped manner, where the material undergoes a segmented, stepped heating melt polymerization reaction. The catalytic reaction conditions are: first, the reaction is carried out at a first-stage heating temperature of 120-150°C for 2-6 hours, and then at a second-stage heating temperature of 160-200°C for 2-8 hours. Using a segmented heating method ensures a more complete in-situ condensation reaction of the polymer and the coordination processes of sulfur bonds and nitrogen atoms, which is beneficial for improving the stability of functional groups and the hydrophilic inhibition efficiency in the final reagent.
[0038] In different implementations, the first stage heating temperature of the catalytic reaction can be any one value or a range of any two values among 120℃, 150℃, 160℃, 170℃, and 180℃, and the reaction time can be any one value or a range of any two values among 2h, 3h, 4h, 5h, and 6h; the second stage heating temperature of the catalytic reaction can be any one value or a range of any two values among 160℃, 180℃, 190℃, and 200℃, and the reaction time can be any one value or a range of any two values among 2h, 3h, 4h, 5h, 6h, 7h, and 8h.
[0039] In some specific embodiments of the present invention, the modified catalyst in S1 includes at least one of the following: a gold catalyst supported on nano-titanium dioxide, a palladium-copper bimetallic catalyst supported on activated carbon, and a magnetic nanocatalyst. Preferably, the magnetic nanocatalyst includes at least one of the following: iron(III) oxide coated titanium dioxide nanoparticles, titanium dioxide nanoparticles, and carbon-cobalt coated iron nanoparticles.
[0040] In some specific embodiments of the present invention, in S2, the mass ratio of the skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid is 1-3:0.5-1:1-5:2-4:1-2. Specifically, ratios can be selected from, but are not limited to, any one or any two of the following: 1:0.5:1:2:1, 1:0.5:1:4:2, 1:1:1:2:1, 1:1:1:3:2, 1:0.5:3:2:1, 1:0.5:5:4:2, 2:1:2:3:1, 2:0.5:5:2:1, 2:1:5:4:2, 3:0.5:3:2:1. This compound modification, through the introduction of sodium mercaptoacetate, enables the agent to have good chemical adsorption and locking ability on the surface of pyrite minerals.
[0041] A second aspect of the present invention provides a polymetallic ore beneficiation and separation agent, prepared using the preparation method of any of the polymetallic ore beneficiation and separation agents described in the foregoing embodiments. This agent exhibits excellent low-alkalinity selective inhibition performance when targeting complex polymetallic ores containing easily floatable talc, marcasite, and pyrrhotite.
[0042] A third aspect of the present invention provides the application of the above-mentioned polymetallic ore beneficiation and separation reagent in the low-alkalinity copper-sulfur flotation separation of complex polymetallic ores.
[0043] In some specific embodiments of the present invention, the method for copper-sulfur flotation separation includes the following steps; see [link to relevant documentation]. Figure 1 And the following specific steps: S1. Grinding and classifying complex polymetallic ores containing chalcopyrite, pyrite, marcasite, pyrrhotite, and talc is performed. The content of particles with a diameter <0.074mm in the grinding product is controlled at 70%-75%. Water is added to prepare a slurry, and the slurry mass concentration is controlled at 30%-35%. At this coarse grinding particle size, the coarser pyrite minerals are partially liberated, while the fine chalcopyrite particles are not over-ground.
[0044] S2. Prepare the slurry by sequentially adding a compound in-situ electrochemical regulator consisting of sodium hypochlorite and sodium metabisulfite in a mass ratio of 1:4, i.e., adding sodium hypochlorite first and then sodium metabisulfite, at a dosage of 200-300 g / t, to control the slurry pH value at a low-alkalinity, slightly alkaline environment of 7.8-8.3. Subsequently, add a polymetallic ore beneficiation and separation agent as a targeted organic inhibitor, along with a low-alkalinity specific copper collector and a frother, pine oil. After one roughing and two scavenging processes, the copper rough concentrate is regrinded using a tower mill ceramic ball mill until the particle size <0.074 mm accounts for more than 98% of the total. After two more cleaning processes, high-grade copper concentrate and copper tailings are finally obtained.
[0045] In some specific embodiments of the present invention, the low-alkalinity specific copper collector in mineral processing includes ethyl thiocyanate, which is insensitive to H+ at low alkalinity, exhibits good chemical stability at pH 8, and can synergistically collect associated gold, silver, and bismuth. The frother, pine oil, commonly known as No. 2 oil, is used at a dosage of 15-25 g / t in the roughing stage.
[0046] Ethylthiocyanate can be prepared according to the following steps: 0.1 mol of sodium isopropyl xanthate is dissolved in 150 mL of anhydrous ethanol. Under ice-water bath conditions, 0.1 mol of ethyl aminoethyl hydrochloride is added dropwise, along with 0.1 mol of sodium carbonate as a deacidifying agent. After the addition is complete, the mixture is heated to 45 °C and refluxed for 8 h. The reaction progress is monitored by thin-layer chromatography, and the reaction endpoint is defined as the complete disappearance of the sodium isopropyl xanthate spot. After the reaction, the inorganic salts are removed by filtration. The filtrate is then subjected to vacuum distillation to remove the ethanol solvent. The residue is purified by column chromatography using a mixture of petroleum ether and ethyl acetate to obtain ethylthiocyanate with a purity ≥95%.
[0047] In some specific embodiments of the present invention, in S2, the dosage of the polymetallic ore separation reagent in the copper roughing process is 100-150 g / t, the dosage of the polymetallic ore separation reagent in the first scavenging process is 30-50 g / t, and the second scavenging process is a blank scavenging process without adding reagents. The dosage of the low-alkalinity specific copper collector in the roughing, scavenging, and scavenging processes is 40-60 g / t, 10 g / t, and 5 g / t, respectively.
[0048] In some specific embodiments of the present invention, the tailings from the secondary copper scavenging process are gravity-fed into the sulfur beneficiation mixing tank as copper tailings. The sulfur beneficiation operation is carried out in a low-alkalinity, copper-free activation system. First, a copper-free combined activator consisting of oxalic acid and ammonium sulfate in a 1:3 mass ratio is added to the sulfur beneficiation mixing tank at a dosage of 400-600 g / t. Then, a low-alkalinity, broad-spectrum active sulfur collector, isobutyl xanthate propylene ester, is added at a dosage of 60-100 g / t, and No. 2 oil at 35 g / t. After stirring, the slurry undergoes segmented early-harvest flotation: the primary sulfur roughing stage is conducted in a separate tank, and high-grade froth is quickly skimmed off as sulfur concentrate one; the tailings from the primary sulfur roughing stage enter the secondary sulfur roughing stage, and the froth from the secondary roughing stage enters the sulfur beneficiation cleaning machine to produce sulfur concentrate two. The tailings from the secondary roughing stage are then subjected to sulfur scavenging, and the scavenging froth is returned to the secondary roughing stage. Finally, sulfur concentrate one and sulfur concentrate two are combined to obtain the total sulfur concentrate, and the sulfur scavenging tailings are used in subsequent iron and tungsten beneficiation operations.
[0049] The following detailed description of some embodiments of the present invention is provided in conjunction with specific examples. Unless otherwise specified, all raw materials used in the embodiments can be purchased commercially. The amounts of reagents added in the embodiments refer to the absolutely effective mass of the reagent relative to the dry ore.
[0050] The raw ore samples processed in the following embodiments and comparative examples of this invention are all complex polymetallic mines in a certain area of Jiangsu Province. Their process mineralogical characteristics are as follows: the grade of the selected raw ore contains approximately 0.85% copper and approximately 15.5% sulfur. The main metallic sulfide minerals in the ore are chalcopyrite, pyrite, pyrrhotite, unstable and easily oxidized marcasite, trace amounts of sphalerite, and arsenopyrite. The gangue minerals are mainly quartz, calcite, garnet, and gangue rich in naturally highly buoyant talc. Grain size analysis of the main minerals in the raw ore shows that chalcopyrite has a fine and difficult-to-liberate particle size, with a micro-particle size <0.04 mm accounting for as high as 34.08%, while the gangue interfering minerals such as pyrite and pyrrhotite have a coarser particle size, mainly concentrated in the 0.08 mm-1.28 mm range, as shown in Table 1.
[0051] Table 1. Results of particle size analysis of major minerals
[0052] Example 1 This embodiment performs low-alkalinity copper-sulfur separation in complex polymetallic ores, specifically including the following steps: 1. Preparation of polymetallic ore beneficiation and separation reagents Urea and glycine were mixed in a 1:1 mass ratio to prepare a mixed raw material. This mixed raw material, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide were then thoroughly mixed in a 10:8:10:1:3 mass ratio. A nano-titanium dioxide-supported gold catalyst was added to the mixture at a rate of 0.5 wt% of the total mixed reagent mass. The material was placed in a reactor for a staged, stepped heating melt polymerization reaction. The reaction was first carried out at 140°C for 3 hours, followed by a further increase to 180°C for 5 hours. After cooling, the skeletal intermediate was collected.
[0053] The above-mentioned skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid were uniformly mixed at room temperature in a mass ratio of 1:0.5:1:2:1 to prepare a polymetallic ore beneficiation and separation reagent. This reagent was then prepared into a 2% (w / w) aqueous solution at room temperature for later use.
[0054] 2. Preparation of mineral processing reagents The copper-selective slurry potential regulator is prepared on-site by diluting and compounding industrial-grade sodium hypochlorite and sodium metabisulfite at a mass ratio of 1:4. The low-alkalinity, specific copper collector is ethyl thiocyanate. The sulfur-selective, copper-free combined activator is prepared on-site by dissolving oxalic acid and ammonium sulfate at a mass ratio of 1:3. The low-alkalinity, active sulfur collector is propylene isobutyl xanthate. The foaming agent is pine oil.
[0055] 3. Closed-circuit operation for copper-sulfur flotation separation First-stage grinding and classification: The complex polymetallic ore, crushed to 0-13mm, is fed into a first-stage closed-circuit ball mill for coarse grinding. The grinding product is classified by a classifying hydrocyclone. The fineness of the grinding product in the overflow of the hydrocyclone is controlled so that the content of particles with a diameter <0.074mm is 70%. The classified sand is returned to the ball mill as return sand for regrinding.
[0056] Copper Concentration Low-Alkalinity Potential Control and Flotation: The overflow slurry from the classifying hydrocyclone is introduced by gravity into the copper concentration mixing tank, and water is added to adjust the slurry concentration to 30%. A prepared sodium hypochlorite and sodium metabisulfite compound potential control agent is added to the copper concentration mixing tank at a dosage of 200 g / t, and a trace amount of sodium carbonate is added simultaneously to adjust and maintain the slurry pH at 7.8. At this time, the platinum electrode potential of the slurry is measured to be stable at +50 mV.
[0057] Copper closed-circuit separation operation: The polymetallic ore separation reagent aqueous solution prepared in step 1 is added to the slurry after slurry conditioning as a targeted inhibitor, with an absolute reagent dosage of 100 g / t, and stirred for 3 min for adsorption; then, 40 g / t of the low-alkalinity specific copper collector ethyl thiocyanate is added, and stirred for 2 min; finally, 15 g / t of the frother pine oil is added; the slurry is flowed to an aerated flotation machine for primary roughing, scraping off the copper rough concentrate froth. The primary roughing underflow slurry sequentially enters the primary scavenging and secondary scavenging stages. In the primary scavenging stage, 10 g / t of ethyl thiocyanate and 5 g / t of pine oil are added; in the secondary scavenging stage, 5 g / t of ethyl thiocyanate is added. The secondary scavenging froth is returned to the primary scavenging stage, and the primary scavenging froth is returned to the primary roughing stage. Finally, the secondary scavenging underflow is used as copper tailings and flows to the sulfur separation mixing tank.
[0058] Copper rough concentrate regrinding: The scraped copper rough concentrate foam is pumped into a 200kW tower mill, where high-alumina ceramic balls are used as the grinding media for fine regrinding. The regrinded product is classified by a classifying hydrocyclone, and the regrinding overflow fineness is controlled so that the content of particles with a diameter <0.074mm reaches 98%, ensuring that the fine chalcopyrite particles are fully liberated. The classified sediment is returned to the tower mill. The regrinding overflow slurry enters the primary cleaning process, where 30g / t of the polymetallic ore beneficiation separation reagent prepared in step 1 is added. The primary cleaning foam flows to the secondary cleaning process, where blank cleaning is performed without adding any reagents. The foam product scraped off from the secondary cleaning process is the final copper concentrate. The primary cleaning tailings are returned to the copper roughing process, and the secondary cleaning tailings are returned to the primary cleaning process.
[0059] Copper tailings staged copper-free activation sulfur beneficiation closed-circuit operation: The secondary scavenging tailings from copper beneficiation are introduced into a sulfur beneficiation mixing tank. 400g / t of a copper-free combined activator is added to the tank to remove the slightly hydrophilic passivation film on the surface of the pyrite. Subsequently, 60g / t of isobutyl xanthate propylene glycol collector and 35g / t of frother pine oil are added. After thorough mixing, the slurry enters the primary sulfur roughing stage. The primary sulfur roughing stage is conducted in a separate tank, where high-grade flotation froth of sulfide ore is rapidly scraped off by adjusting the liquid level, directly used as sulfur concentrate one. The tailings from the primary sulfur roughing stage flow to the secondary sulfur roughing stage. The froth product scraped off from the secondary roughing stage is sent to the sulfur cleaning stage for further cleaning. The final froth produced by the sulfur cleaning stage is used as sulfur concentrate two. The tailings from the secondary roughing stage flow to the sulfur scavenging stage. 30g / t of isobutyl xanthate propylene glycol and 8g / t of pine oil are added to the sulfur scavenging stage. The sulfur scavenging froth is returned to the secondary sulfur roughing stage, and the sulfur cleaning tailings are also returned to the secondary sulfur roughing stage. Sulfur concentrate one and sulfur concentrate two are combined to obtain the final total sulfur concentrate. The sulfur scavenging tailings are discharged by gravity as the final sulfur tailings and used in the subsequent iron and tungsten beneficiation workshop.
[0060] According to sampling and analysis, the copper grade in the copper concentrate obtained by the final closed-circuit test in this embodiment was 23.51%, and the copper recovery rate was 91.55%; the total sulfur grade in the combined total sulfur concentrate was 46.52%, and the total sulfur recovery rate was 94.02%. No obvious talc mudification or calcium scaling was found in the dewatering and recycling system of copper and sulfur tailings.
[0061] Example 2 This embodiment performs low-alkalinity copper-sulfur separation in complex polymetallic ores, specifically including the following steps: 1. Preparation of polymetallic ore beneficiation and separation reagents Urea, glycine, and sodium persulfate were mixed in a mass ratio of 1:0.5:0.2 to prepare a mixed raw material. This mixed raw material, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide were then thoroughly mixed in a mass ratio of 15:12:35:2:5. An activated carbon-supported palladium-copper bimetallic catalyst was added to the mixture at a dosage of 0.4 wt% of the total mixed reagents. The material was placed in a reactor for a staged, stepped heating melt polymerization reaction. The reaction was first carried out at 120°C for 6 hours, followed by a further increase in temperature to 160°C for 8 hours. After cooling, the skeletal intermediate was collected.
[0062] The above-mentioned skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid were uniformly mixed at room temperature in a mass ratio of 2:1:2:3:1 to prepare a polymetallic ore beneficiation and separation reagent. This reagent was then prepared into a 2% (w / w) aqueous solution at room temperature for later use.
[0063] 2. Preparation of mineral processing reagents The copper-selective slurry potential regulator is prepared on-site by diluting and compounding industrial-grade sodium hypochlorite and sodium metabisulfite at a mass ratio of 1:4. The low-alkalinity, specific copper collector is ethyl thiocyanate. The sulfur-selective, copper-free combined activator is prepared on-site by dissolving oxalic acid and ammonium sulfate at a mass ratio of 1:3. The low-alkalinity, active sulfur collector is propylene isobutyl xanthate. The foaming agent is pine oil.
[0064] 3. Closed-circuit operation for copper-sulfur flotation separation First-stage grinding and classification: The complex polymetallic ore, crushed to 0-13mm, is fed into a first-stage closed-circuit ball mill for coarse grinding. The grinding product is classified by a classifying hydrocyclone. The fineness of the grinding product in the overflow of the hydrocyclone is controlled so that the content of particles with a diameter <0.074mm is 75%. The classified sand is returned to the ball mill as return sand for regrinding.
[0065] Copper ore beneficiation with low alkalinity potential control and flotation: The overflow slurry from the classifier hydrocyclone is introduced into the copper beneficiation mixing tank by gravity, and water is added to adjust the slurry mass concentration to 35%. A prepared sodium hypochlorite and sodium metabisulfite compound potential control agent is added to the copper beneficiation mixing tank at a dosage of 300 g / t, and a trace amount of sodium carbonate is added at the same time to adjust and maintain the slurry pH value at 8.3. At this time, the platinum electrode potential of the slurry is measured to be stable at +120 mV.
[0066] Copper closed-circuit separation operation: The polymetallic ore separation reagent aqueous solution prepared in step 1 is added to the slurry after conditioning as a targeted inhibitor, with an absolute reagent dosage of 150 g / t, and stirred for 3 minutes for adsorption. Then, 60 g / t of the low-alkalinity specific copper collector ethyl thiocyanate is added, and the mixture is stirred for 2 minutes. Finally, 25 g / t of the frother pine oil is added. The slurry flows to an aerated flotation machine for primary roughing, scraping off the copper rough concentrate froth. The primary roughing underflow slurry sequentially enters the primary and secondary scavenging stages. In the primary scavenging stage, 10 g / t of ethyl thiocyanate and 5 g / t of pine oil are added, and in the secondary scavenging stage, 5 g / t of ethyl thiocyanate is added. Afterward, the secondary scavenging froth is returned to the primary scavenging stage, and the primary scavenging froth is returned to the primary roughing stage. The secondary scavenging underflow, as copper tailings, flows to the sulfur separation mixing tank.
[0067] Copper rough concentrate regrinding: The scraped copper rough concentrate froth is pumped into a 200kW tower mill, where high-alumina ceramic balls are used as the grinding media for fine regrinding. The regrinded product is classified by a classifying hydrocyclone, controlling the regrinding overflow fineness to ensure that the particle size <0.074mm accounts for 99%, ensuring sufficient liberation of fine chalcopyrite particles. The classified sediment is returned to the tower mill. The regrinding overflow slurry enters the primary cleaning process, where 50g / t of the polymetallic ore separation reagent prepared in step 1 is added. The primary cleaning froth flows to the secondary cleaning process, where blank cleaning is performed without adding any reagents. The froth product scraped from the secondary cleaning process is the final copper concentrate. The primary cleaning tailings are returned to the copper roughing process, and the secondary cleaning tailings are returned to the primary cleaning process.
[0068] Copper tailings staged copper-free activation sulfur beneficiation closed-circuit operation: The copper secondary scavenging tailings are introduced into the sulfur beneficiation mixing tank. 600g / t of copper-free combined activator is added to the tank to peel off the slightly hydrophilic passivation film on the surface of the pyrite. Subsequently, 100g / t of sulfur collector isobutyl xanthate propylene glycol and 35g / t of frother pine oil are added. After thorough mixing, the slurry enters the primary sulfur roughing stage. The primary sulfur roughing stage is in a separate tank, where high-grade flotation froth of sulfide ore is rapidly scraped off by adjusting the liquid level, directly used as sulfur concentrate one. The tailings from the primary sulfur roughing stage flow to the secondary sulfur roughing stage. The froth product scraped off from the secondary roughing stage is sent to the sulfur cleaner for further cleaning. The final froth produced by the sulfur cleaner is used as sulfur concentrate two. The tailings from the secondary roughing stage flow to the sulfur scavenging stage. 40g / t of isobutyl xanthate propylene glycol and 8g / t of pine oil are added to the sulfur scavenging stage. The sulfur scavenging froth is returned to the secondary sulfur roughing stage, and the sulfur cleaner tailings are also returned to the secondary sulfur roughing stage. Sulfur concentrate one and sulfur concentrate two are combined to obtain the final total sulfur concentrate. The sulfur scavenging tailings are discharged by gravity as the final sulfur tailings and used in the subsequent iron and tungsten beneficiation workshop.
[0069] According to the sampling and testing, the copper grade in the copper concentrate obtained by the final closed-circuit test in this embodiment is 23.82%, and the copper recovery rate is 91.12%; the total sulfur grade in the combined total sulfur concentrate is 46.91%, and the total sulfur recovery rate is 94.51%.
[0070] Example 3 This embodiment performs low-alkalinity copper-sulfur separation in complex polymetallic ores, specifically including the following steps: 1. Preparation of polymetallic ore beneficiation and separation reagents Urea, ammonium cyanate, and isocyanate were mixed in a mass ratio of 1:0.5:0.1 to prepare a mixed raw material. This mixed raw material, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide were then thoroughly mixed in a mass ratio of 11:9:28:1:3. A magnetic catalyst, consisting of iron oxide-coated titanium dioxide nanoparticles, was added to the mixture at a dosage of 0.3 wt% of the total mixed reagent mass. The material was placed in a reactor for a staged, stepped heating melt polymerization reaction. The reaction was first carried out at 150°C for 2 hours, followed by a further increase in temperature to 200°C for 3 hours. After cooling, the skeletal intermediate was collected.
[0071] The above-mentioned skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-4-imidazolylpropionic acid were uniformly mixed at room temperature in a mass ratio of 1:1:1:3:2 to prepare a polymetallic ore beneficiation and separation reagent. This reagent was then prepared into a 2% (w / w) aqueous solution at room temperature for later use.
[0072] 2. Preparation of mineral processing reagents The copper-selective slurry potential regulator is prepared on-site by diluting and compounding industrial-grade sodium hypochlorite and sodium metabisulfite at a mass ratio of 1:4. The low-alkalinity, specific copper collector is ethyl thiocyanate. The sulfur-selective, copper-free combined activator is prepared on-site by dissolving oxalic acid and ammonium sulfate at a mass ratio of 1:3. The low-alkalinity, active sulfur collector is propylene isobutyl xanthate. The foaming agent is pine oil.
[0073] 3. Closed-circuit operation for copper-sulfur flotation separation First-stage grinding and classification: The complex polymetallic ore, crushed to 0-13mm, is fed into a first-stage closed-circuit ball mill for coarse grinding. The grinding product is classified by a classifying hydrocyclone. The fineness of the grinding product in the overflow of the hydrocyclone is controlled so that the content of particles with a diameter <0.074mm is 72%. The classified sand is returned to the ball mill as return sand for regrinding.
[0074] Copper Concentration with Low-Alkalinity Potential Control and Flotation: The overflow slurry from the classifying hydrocyclone is introduced by gravity into the copper concentration mixing tank, and water is added to adjust the slurry concentration to 32%. A prepared sodium hypochlorite and sodium metabisulfite compound potential control agent is added to the copper concentration mixing tank at a dosage of 250 g / t, along with a trace amount of sodium carbonate, to adjust and maintain the slurry pH at 8.0. At this point, the platinum electrode potential of the slurry is measured to be stable at +85 mV.
[0075] Copper closed-circuit separation operation: The polymetallic ore separation reagent aqueous solution prepared in step 1 is added to the slurry after conditioning as a targeted inhibitor, with an absolute reagent dosage of 120 g / t, and stirred for 3 minutes for adsorption. Then, 50 g / t of the low-alkalinity specific copper collector ethyl thiocyanate is added, and the mixture is stirred for 2 minutes. Finally, 20 g / t of the frother pine oil is added. The slurry flows to an aerated flotation machine for primary roughing, scraping off the copper rough concentrate froth. The underflow slurry from the primary roughing stage sequentially enters the primary and secondary scavenging stages. In the primary scavenging stage, 10 g / t of ethyl thiocyanate and 5 g / t of pine oil are added as supplementary agents, and in the secondary scavenging stage, 5 g / t of ethyl thiocyanate is added as supplementary agents. The secondary scavenging froth is returned to the primary scavenging stage, and the primary scavenging froth is returned to the primary roughing stage. The secondary scavenging underflow, as copper tailings, flows to the sulfur separation mixing tank.
[0076] Copper rough concentrate regrinding: The scraped copper rough concentrate froth is pumped into a 200kW tower mill, where high-alumina ceramic balls are used as the grinding media for fine regrinding. The regrinded product is classified by a classifying hydrocyclone, controlling the regrinding overflow fineness to ensure that the particle size <0.074mm accounts for 98.5%, ensuring sufficient liberation of fine chalcopyrite particles. The classified sediment is returned to the tower mill. The regrinding overflow slurry enters the primary cleaning process, where 40g / t of the polymetallic ore separation reagent prepared in step 1 is added. The primary cleaning froth flows to the secondary cleaning process, where blank cleaning is performed without adding any reagents. The froth product scraped from the secondary cleaning process is the final copper concentrate. The primary cleaning tailings are returned to the copper roughing process, and the secondary cleaning tailings are returned to the primary cleaning process.
[0077] Copper tailings staged copper-free activation sulfur beneficiation closed-circuit operation: The secondary scavenging tailings from copper beneficiation are introduced into a sulfur beneficiation mixing tank. 500g / t of a copper-free combined activator is added to the tank to remove the slightly hydrophilic passivation film on the surface of the pyrite. Then, 80g / t of isobutyl xanthate propylene glycol collector and 35g / t of pine oil frother are added. After thorough mixing, the slurry enters the primary sulfur roughing stage. The primary sulfur roughing stage is in a separate tank, where high-grade flotation froth of sulfide ore is rapidly scraped off by adjusting the liquid level, directly used as sulfur concentrate one. The tailings from the primary sulfur roughing stage flow to the secondary sulfur roughing stage. The froth product scraped off from the secondary roughing stage is sent to the sulfur cleaning stage for further cleaning. The final froth produced by the sulfur cleaning stage is used as sulfur concentrate two. The tailings from the secondary roughing stage flow to the sulfur scavenging stage. 35g / t of isobutyl xanthate propylene glycol and 8g / t of pine oil are added to the sulfur scavenging stage. The sulfur scavenging froth is returned to the secondary sulfur roughing stage, and the sulfur cleaning tailings are also returned to the secondary sulfur roughing stage. Sulfur concentrate one and sulfur concentrate two are combined to obtain the final total sulfur concentrate. The sulfur scavenging tailings are discharged by gravity as the final sulfur tailings and used in the subsequent iron and tungsten beneficiation workshop.
[0078] According to the sampling and testing, the copper grade in the copper concentrate obtained by the final closed-circuit test in this embodiment is 23.64%, and the copper recovery rate is 91.38%; the total sulfur grade in the combined total sulfur concentrate is 46.73%, and the total sulfur recovery rate is 94.26%.
[0079] Comparative Example 1 The difference between this comparative example and Example 1 is that a traditional strong-alkali, high-calcium process was used to suppress pyrite minerals. The polymetallic ore beneficiation and separation reagents of step 1 of this invention were neither prepared nor added, and no sodium hypochlorite and sodium metabisulfite compound potential regulator was added. Specifically, industrial quicklime was added during slurry preparation in the copper beneficiation mixing tank, with a lime consumption as high as 3 kg / t, raising the slurry pH to 10.5. Conventional butyl xanthate was used as the copper collector at a dosage of 60 g / t.
[0080] In subsequent sulfur beneficiation operations, due to the inhibition of residual high alkali and high concentration of calcium ions, it is necessary to first add 1.5 kg / t of concentrated sulfuric acid to adjust the pH of the slurry to 7.5, and add 200 g / t of copper sulfate pentahydrate, a conventional activator with high pollution, to activate the sulfur zone. The sulfur collector is 300 g / t of butyl xanthate. The remaining grinding and closed-loop circulation connection structure is the same as in Example 1.
[0081] Sampling and analysis revealed that the copper grade in the final copper concentrate obtained from this comparative closed-circuit test was only 18.12%. Due to the intermingling of talc gangue and some fine-grained chalcopyrite inhibited by high calcium, the concentrate grade was significantly reduced. The comparison results with Example 1 are as follows: Figure 2As shown, the copper recovery rate decreased to 85.45%; the sulfur grade in the final sulfur concentrate was 39.20%, and the sulfur recovery rate decreased to 81.33%; at the same time, after one week of trial operation, severe calcium carbonate scaling and caking were observed on the inner walls of the foam tank and return water circulation pipe of the beneficiation machine.
[0082] Comparative Example 2 The difference from Example 2 is that in S1, which is used to prepare polymetallic ore beneficiation and separation reagents, no modified lignin-derived sodium lignin sulfonate was added. The proportions of the remaining components in the raw materials are the same as in Example 2. The subsequent reagent compounding and modification steps and the closed-circuit flotation process parameters for copper and sulfur beneficiation are the same as in Example 2.
[0083] Sampling and analysis revealed that the lack of hydrophilic oligomeric lignin macromolecular segments in the reagent's molecular structure, which could effectively target and physically cover the shear planes of talc gangue crystals, resulted in a large amount of naturally highly floatable talc gangue from the raw ore being mixed with chalcopyrite and floated into the copper concentrate. Consequently, the copper grade in the final copper concentrate decreased to 20.15%, with a copper recovery rate of 90.58%; the total sulfur concentrate index remained largely unchanged. This comparative study demonstrates that the absence of lignin framework segments is insufficient to address the issue of high-mud, high-talc contamination in polymetallic ores while maintaining a high copper concentrate grade.
[0084] Comparative Example 3 The difference from Example 3 is that sodium mercaptoacetate, a functionally modified small molecule containing active sulfur bonds and carboxyl groups, was not added in S2, which is used to prepare polymetallic ore beneficiation and separation reagent. The proportion of intermediate B and other compound components in the raw materials is the same as in Example 3, and the subsequent copper-sulfur separation closed-circuit flotation process parameters are the same as in Example 3.
[0085] Sampling and analysis revealed that the reagent lacked high-density active thiol groups after melt polymerization to specifically anchor and lock onto the surface of slightly oxidized pyrite minerals. This resulted in a significant weakening of the reagent's hydrophilic passivation effect on interfering pyrite minerals such as marcasite and pyrrhotite, leading to the inclusion of some easily floatable pyrite minerals in the copper concentrate. The final copper concentrate had a copper grade of 21.34% and a copper recovery rate of 89.10%. This comparative result demonstrates the contribution of sodium thioglycolate compound modification to improving the selectivity of low-alkali copper-sulfur separation.
[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A process for low alkaline copper-sulphur separation of complex polymetallic ores, characterized by, The beneficiation process is carried out under weakly alkaline conditions without the addition of lime. During slurry preparation, a compound in-situ electrochemical regulator composed of sodium hypochlorite and sodium metabisulfite in a mass ratio of 1:4 is added to the slurry, and a polymetallic ore beneficiation separation agent is added as an inhibitor. The polymetallic ore beneficiation separation agent is prepared by mixing raw materials containing sodium lignosulfonate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate and 2-amino-3-(4-imidazolyl)propionic acid.
2. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 1, characterised in that, The beneficiation steps include: grinding the complex polymetallic ore and adding water to prepare a copper roughing slurry; adding the compound in-situ electrochemical regulator to the copper roughing slurry to adjust the slurry to a pH of 7.8-8.3; adding the polymetallic ore beneficiation separation reagent to the slurry, and adding a low-alkalinity specific copper collector and a frother for flotation; obtaining copper rough concentrate and copper tailings through roughing and scavenging; pumping the copper rough concentrate into a tower mill for fine regrinding; and sending the regrinded product into a cleaning process to finally obtain copper concentrate.
3. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 2, characterised in that, The copper roughing ore pulp contains 70%-75% particles with a diameter <0.074mm, and the pulp mass concentration is 30%-35%.
4. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 2, characterised in that, The polymetallic ore beneficiation and separation agent is prepared by the following steps: S1, mixing the mixed raw materials, sodium lignosulfonate, sodium hydroxide, sodium carbonate and sodium polysulfide in proportion, adding the modified catalyst, and carrying out a segmented step-by-step heating melt catalytic polymerization reaction to obtain the skeleton intermediate; S2. The skeleton intermediate is mixed with dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate and 2-amino-3-(4-imidazolyl)propionic acid for modification to obtain the polymetallic ore beneficiation and separation agent.
5. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 4, characterised in that, In S1, the mass ratio of the mixed raw materials, sodium lignosulfonate, sodium hydroxide, sodium carbonate, and sodium polysulfide is 10-15:8-12:10-35:1-5:3-5; the conditions for the segmented step-heating melt catalytic polymerization reaction are to react for 2-6 hours at a first stage temperature of 120-150℃, and then react for 2-8 hours at a second stage temperature of 160-200℃. In S2, the mass ratio of the skeletal intermediate, dichloroisocyanuric acid, trichloroisocyanuric acid, sodium mercaptoacetate, and 2-amino-3-(4-imidazolyl)propionic acid is 1-3:0.5-1:1-5:2-4:1-2.
6. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 4, characterised in that, The mixed raw materials are one or more of urea, aminoacetic acid, sodium persulfate, ammonium cyanate, and isocyanate.
7. A low alkalinity copper-sulphur separation process for complex polymetallic ores according to claim 4, characterised in that, The modified catalyst includes one of the following: nano-titanium dioxide supported gold catalyst, activated carbon supported palladium-copper bimetallic catalyst, and magnetic nanocatalyst.