Auxiliary collector for coarse-grained ilmenite flotation and application thereof
By combining higher alcohols, fatty acids, and alkyl hydroxamic acids with benzoyl hydroxamic acid, the problems of insufficient selectivity and collectability in the flotation of coarse-grained ilmenite were solved, the recovery rate was improved, and the amount of reagents used was reduced, achieving an environmentally friendly and efficient flotation effect.
Patent Information
- Application Number
- CN202611622971.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-24
AI Technical Summary
Existing collectors lack selectivity and collectivity in the flotation of coarse-grained ilmenite, resulting in low recovery rates, and traditional reagents pose environmental pollution risks.
An auxiliary collector using a combination of higher alcohols, fatty acids, and alkyl hydroxamic acids with benzohydroxyxamic acid can improve the collection effect of benzohydroxyxamic acid through synergistic effects and reduce the amount of reagent used.
It significantly improves the recovery rate and selectivity of coarse-grained ilmenite, reduces reagent usage, and decreases the risk of environmental pollution.
Smart Images

Figure CN123149063A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of mineral flotation separation technology in mineral processing engineering, specifically relating to an auxiliary collector for coarse-grained ilmenite flotation and its application. Background Technology
[0002] my country possesses abundant titanium resources, but most are associated ore deposits, primarily existing as rock-type vanadium-titanium magnetite. Ilmenite is accompanied by numerous gangue minerals such as pyroxene and feldspar, resulting in a complex mineral composition. Because these gangue minerals share similar surface properties with ilmenite, flotation reagents struggle to effectively separate the ilmenite. Furthermore, coarse-grained ilmenite, due to its large mass and relatively low surface energy, is prone to detachment during flotation, leading to generally low recovery rates. The selectivity and collecting properties of collectors remain key bottlenecks limiting improvements in the flotation performance of coarse-grained ilmenite.
[0003] Currently, commonly used collectors for ilmenite flotation include fatty acids, hydroxamic acids, arsenoic acids, and phosphonic acids. Among these, traditional fatty acid collectors (such as oleic acid) have strong collecting ability but poor selectivity and are easily affected by unavoidable ions and gangue minerals in the pulp. Phosphonic acid collectors (such as styrenephosphonic acid) and arsenoic acid collectors (such as benzylarsenoic acid) have good selectivity but are generally highly toxic, polluting the aquatic environment. Hydroxamic acid collectors (such as benzylhydroxamic acid) have excellent selectivity and are widely recognized in oxidative ore flotation practice, but their collecting ability is relatively poor. Against this backdrop, developing an auxiliary collector that combines the selectivity of hydroxamic acid collectors with high-efficiency collecting performance tailored to the characteristics of coarse-grained ilmenite is crucial for improving the recovery rate of coarse-grained minerals. Summary of the Invention
[0004] To address and improve upon the deficiencies and shortcomings of reagents in the flotation of coarse-grained ilmenite, the present invention aims to provide an auxiliary collector that can be used in combination with benzo[a]hydroxyxamic acid. This auxiliary collector utilizes the synergistic effect between the collectors to enhance the collection efficiency of benzo[a]hydroxyxamic acid on coarse-grained ilmenite and reduce the dosage of benzo[a]hydroxyxamic acid. Furthermore, the present invention provides an application of this auxiliary collector in the flotation of coarse-grained ilmenite. By combining the auxiliary collector with benzo[a]hydroxyxamic acid, the selective collection ability for ilmenite is improved, thereby enhancing the flotation performance of coarse-grained ilmenite.
[0005] To achieve the above technical objectives, this invention provides an auxiliary collector for the flotation of coarse-grained ilmenite and its application. The basic concept of the technical solution is as follows: An auxiliary collector for the flotation of coarse-grained ilmenite, wherein the auxiliary collector is an oily mixture of higher alcohols, fatty acids and alkyl hydroxyxamic acids in a certain mass ratio.
[0006] Furthermore, the higher alcohol is one or more of n-hexanol, n-heptanol, n-octanol, sec-hexanol, sec-heptanol, sec-octanol, 1,2-hexanediol, 1,2-heptanediol, and 1,2-octanediol mixed in any proportion; the fatty acid is one or more of oleic acid, linoleic acid, and palmitoleic acid mixed in any proportion; and the alkyl hydroxyoxime acid is an alkyl hydroxyoxime acid with 5 to 9 carbon atoms.
[0007] Furthermore, the mass ratio of higher alcohols, fatty acids, and alkyl hydroxyxamic acids in the auxiliary collector is 1:(0.2-0.5):(0.2-0.5).
[0008] An application of the above-mentioned auxiliary collector for the flotation of coarse-grained ilmenite involves combining the auxiliary collector with benzo[a]hydroxyxamic acid for the flotation of coarse-grained ilmenite.
[0009] The process includes the following steps: A 30% (w / w) slurry is prepared by mixing coarse-grained ilmenite feed material with water; sodium carbonate is added as a pH adjuster to adjust the slurry pH to 7.5–8.0, and the mixture is stirred for 5 minutes; 300–400 g / t of lead nitrate activator is added, and the mixture is stirred for 5 minutes; 800–1500 g / t of benzoyl hydroxamic acid collector is added, and the mixture is stirred for 5 minutes; 80–150 g / t of auxiliary collector is added, and the mixture is stirred for 5 minutes; after slurry conditioning, ilmenite roughing is performed, followed by three cleaning operations on the rough concentrate obtained from the roughing operation, and a scavenging operation on the tailings from the roughing operation. A closed-circuit flotation process is used, with middlings returned sequentially to obtain titanium concentrate and tailings.
[0010] Furthermore, the particle size distribution of the coarse-grained ilmenite feed material is as follows: +0.25mm content ≤ 5%, -0.25 +0.075mm content 70% to 75%.
[0011] Furthermore, the amounts of the auxiliary collector and the benzohydroxyxamic acid collector are in a mass ratio of 1:(10-20).
[0012] Furthermore, in the three-stage purification process, 200g / t to 400g / t of water glass is added in the first purification stage, 50g / t to 100g / t of water glass is added in the second purification stage, and no chemicals are added in the third purification stage.
[0013] Furthermore, in a single scavenging operation, the pulp pH is 7.5–8.0, and 150 g / t–200 g / t of lead nitrate activator, 400 g / t–750 g / t of benzohydroxyxamic acid collector, and 40 g / t–75 g / t of auxiliary collector are added.
[0014] Compared with existing technologies, the beneficial effects of this technical solution are: In this invention, benzohydroxyxamic acid is a chelating collector. Its oxime group can chelate with active metal ions on the surface of ilmenite, exhibiting high selectivity for ilmenite. However, due to the strong hydrophilic groups in the benzohydroxyxamic acid molecule and insufficient overall hydrophobicity, its collecting ability for ilmenite is relatively weak. By combining higher alcohols, fatty acids, and alkyl hydroxyxamic acids as auxiliary collectors with benzohydroxyxamic acid, the fatty acids and alkyl hydroxyxamic acids can synergistically adsorb onto the ilmenite surface, increasing the thickness of the hydrophobic layer. The higher alcohols are directionally adsorbed at the gas-liquid interface, forming stable and appropriately sized bubbles. Some alcohol molecules intersect between the hydroxyxamic acid and fatty acid components, enhancing the interaction strength between the hydrophobic ilmenite particles and the bubbles. Therefore, the auxiliary collector improves the solid-liquid-gas three-phase interaction effect of benzohydroxyxamic acid in the collection of ilmenite, enhances the collection effect of benzohydroxyxamic acid on coarse-grained ilmenite, and significantly reduces its reagent dosage. Attached Figure Description
[0015] Figure 1 This is a flowchart illustrating the application of an auxiliary collector in the flotation of coarse-grained ilmenite according to the present invention. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0017] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; the reagents and materials described are commercially available unless otherwise specified.
[0018] Example 1 This embodiment provides an auxiliary collector for the flotation of coarse-grained ilmenite and its application. The ilmenite feed material is taken from a strong magnetic concentrate from a beneficiation plant in the Panxi region. Elemental chemical analysis shows a TiO2 grade of 16.83%. Particle size analysis shows that the raw material contains 3.42% +0.25mm particles and 73.71% -0.25mm to +0.075mm particles. Liberation analysis shows that the total content of ilmenite monomers and rich intergrowths is 91.76%. The gangue minerals are mainly pyroxene, feldspar, olivine, and chlorite.
[0019] In this embodiment, the mass ratio of n-octanol: oleic acid: C7-9 hydroxamic acid in the auxiliary collector is 1:0.5:0.5.
[0020] Application of an auxiliary collector in the flotation of coarse-grained ilmenite, such as Figure 1The process includes the following steps: A 30% (w / w) slurry is prepared by mixing coarse-grained ilmenite feed material with water. Sodium carbonate pH adjuster is added to maintain the slurry pH at 7.5–8.0, and the mixture is stirred for 5 minutes. 300 g / t of lead nitrate activator is added, and the mixture is stirred for 5 minutes. 1000 g / t of benzoyl hydroxamic acid collector is added, and the mixture is stirred for 5 minutes. 100 g / t of auxiliary collector is added, and the mixture is stirred for 5 minutes. After slurry conditioning, ilmenite roughing is performed. The rough concentrate obtained from the roughing is further treated with three cleaning operations. The tailings from the roughing are treated with one scavenging operation. Closed-circuit flotation (mid-ore returned sequentially) yields titanium concentrate and tailings. 400 g / t of water glass is added in the first cleaning operation, 100 g / t of water glass is added in the second cleaning operation, and no reagent is added in the third cleaning operation. In one of the flotation processes, the pulp pH was 7.5–8.0, and 150 g / t of lead nitrate activator, 500 g / t of benzohydroxyxamic acid collector, and 50 g / t of auxiliary collector were added. The titanium concentrate obtained by flotation had a TiO2 grade of 47.12% and a recovery rate of 82.56%.
[0021] Example 2 Compared with Example 1, the mass ratio of the auxiliary collector 2-octanol: oleic acid or linoleic acid: C5-9 hydroxamic acid was 1:0.5:0.2, and other conditions remained unchanged. After flotation separation, the titanium concentrate TiO2 grade was 47.41% and the recovery rate was 81.87%.
[0022] Example 3 This embodiment provides an auxiliary collector for the flotation of coarse-grained ilmenite and its application. The ilmenite feed material is taken from a strong magnetic concentrate from a beneficiation plant in the Panxi region. Elemental chemical analysis shows a TiO2 grade of 18.46%. Particle size analysis shows that the raw material contains 3.75% +0.25mm particles and 72.43% -0.25mm to +0.075mm particles. Liberation analysis shows that the total content of ilmenite monomers and rich intergrowths is 90.96%. The gangue minerals are mainly pyroxene, feldspar, olivine, and chlorite.
[0023] The mass ratio of the auxiliary collector 1,2-octanediol:palmitoic acid:C7-9-hydroxyoxime acid used in this embodiment is 1:0.5:0.5.
[0024] An auxiliary collector for the flotation of coarse-grained ilmenite includes the following steps: The coarse-grained ilmenite feed material is mixed with water to prepare a slurry with a mass concentration of 30%. Sodium carbonate pH adjuster is added to maintain the slurry pH at 7.5–8.0, and the mixture is stirred for 5 minutes. 400 g / t of lead nitrate activator is added, and the mixture is stirred for 5 minutes. 1200 g / t of benzoyl hydroxamic acid collector is added, and the mixture is stirred for 5 minutes. 100 g / t of auxiliary collector is added, and the mixture is stirred for 5 minutes. After slurry conditioning, ilmenite roughing is performed. The rough concentrate obtained from the roughing is further treated with three cleaning operations, and the tailings from the roughing are treated with one scavenging operation. Closed-circuit flotation (mid-ore returned sequentially) yields titanium concentrate and tailings. 300 g / t of water glass is added for the first cleaning operation, 100 g / t of water glass is added for the second cleaning operation, and no reagent is added for the third cleaning operation. In one of the flotation processes, the pulp pH was 7.5–8.0, and 200 g / t of lead nitrate activator, 600 g / t of benzohydroxyxamic acid collector, and 50 g / t of auxiliary collector were added. The resulting titanium concentrate (TiO2) had a grade of 47.68% and a recovery rate of 83.98%.
[0025] Example 4 Compared with Example 3, the mass ratio of the auxiliary collector 2-octanol: palmitoleic acid: C5-9 hydroxamic acid was 1:0.3:0.5, and other conditions remained unchanged. After flotation separation, the titanium concentrate TiO2 grade was 47.53% and the recovery rate was 84.10%.
[0026] Example 5 This embodiment provides an auxiliary collector for the flotation of coarse-grained ilmenite and its application. The ilmenite feed material is taken from a strong magnetic concentrate from a beneficiation plant in the Panxi region. Elemental chemical analysis shows a TiO2 grade of 20.67%. Particle size analysis shows that the content of +0.25mm particles in the raw material is 2.42%, and the content of -0.25mm to +0.075mm particles is 74.69%. Liberation analysis shows that the total content of ilmenite monomers and rich intergrowths is 93.26%. The gangue minerals are mainly pyroxene, feldspar, olivine, and chlorite.
[0027] In this embodiment, the mass ratio of the auxiliary collector n-heptanol: oleic acid: C7-9 hydroxyoxime acid is 1:0.5:0.2.
[0028] An auxiliary collector for coarse-grained ilmenite flotation is disclosed, comprising the following steps: A 30% (w / w) slurry is prepared by mixing coarse-grained ilmenite feed material with water. Sodium carbonate pH adjuster is added to maintain the slurry pH at 7.5–8.0, and the mixture is stirred for 5 minutes. 400 g / t of lead nitrate activator is added, and the mixture is stirred for 5 minutes. 1500 g / t of benzoyl oxime collector is added, and the mixture is stirred for 5 minutes. 80 g / t of auxiliary collector is added, and the mixture is stirred for 5 minutes. After slurry conditioning, ilmenite roughing is performed. The rough concentrate obtained from the roughing is further treated with three cleaning operations, and the tailings from the roughing are treated with one scavenging operation. Closed-circuit flotation (mid-ore returned sequentially) yields titanium concentrate and tailings. 200 g / t of water glass is added for the first cleaning operation, 50 g / t for the second cleaning operation, and no reagent is added for the third cleaning operation. In one of the flotation processes, the pulp pH was 7.5–8.0, and 200 g / t of lead nitrate activator, 750 g / t of benzohydroxyxamic acid collector, and 40 g / t of auxiliary collector were added. The titanium concentrate obtained by flotation had a TiO2 grade of 47.61% and a recovery rate of 84.37%.
[0029] Example 6 Compared with Example 5, the mass ratio of the auxiliary collector n-hexanol:linoleic acid:C5-9 hydroxamic acid was 1:0.5:0.5, and other conditions remained unchanged. After flotation separation, the titanium concentrate TiO2 grade was 47.40%, and the recovery rate was 84.64%.
[0030] Comparative Example 1 Compared with Example 1, no auxiliary collector was added, but 100 g / t of No. 2 oil frother was added, while the dosage of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate TiO2 grade was 47.05%, and the recovery rate was 65.45%.
[0031] Comparative Example 2 Compared to Example 1, no auxiliary collector was added, but 60 g / t of No. 2 oil frother was added, and the amount of benzoyl hydroxamic acid collector was increased to 1500 g / t. In the single scavenging operation, the amount of benzoyl hydroxamic acid collector was increased to 750 g / t, while the amounts of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate obtained had a TiO2 grade of 47.32% and a recovery rate of 81.24%.
[0032] Comparative Example 3 Compared with Example 3, no auxiliary collector was added, but 100 g / t of No. 2 oil frother was added, while the dosage of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate TiO2 grade was 47.14%, and the recovery rate was 72.57%.
[0033] Comparative Example 4 Compared to Example 3, no auxiliary collector was added, but 60 g / t of No. 2 oil frother was added, and the amount of benzoyl oxime collector was increased to 1800 g / t. In the single scavenging operation, the amount of benzoyl oxime collector was increased to 900 g / t, while the amounts of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate obtained had a TiO2 grade of 47.49% and a recovery rate of 83.78%.
[0034] Comparative Example 5 Compared with Example 5, no auxiliary collector was added, but 80 g / t of No. 2 oil frother was added, while the dosage of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate obtained had a TiO2 grade of 47.21% and a recovery rate of 73.58%.
[0035] Comparative Example 6 Compared to Example 5, no auxiliary collector was added, but 60 g / t of No. 2 oil frother was added, and the amount of benzoyl oxime collector was increased to 2000 g / t. In the single scavenging operation, the amount of benzoyl oxime collector was increased to 1000 g / t, while the amounts of other reagents and process conditions remained unchanged. After flotation separation, the titanium concentrate obtained had a TiO2 grade of 47.38% and a recovery rate of 84.13%.
Claims
1. A coarse fraction ilmenite flotation auxiliary collector, characterized in that, The auxiliary collector is an oily mixture of higher alcohols, fatty acids, and alkyl hydroxyxamic acids in a certain mass ratio.
2. The auxiliary collector for flotation of coarse-grained ilmenite according to claim 1, characterized in that, The higher alcohols are one or more of n-hexanol, n-heptanol, n-octanol, sec-hexanol, sec-heptanol, sec-octanol, 1,2-hexanediol, 1,2-heptanediol, and 1,2-octanediol mixed in any proportion; the fatty acids are one or more of oleic acid, linoleic acid, and palmitoleic acid mixed in any proportion; and the alkyl hydroxyoxime acid is an alkyl hydroxyoxime acid with 5 to 9 carbon atoms.
3. The auxiliary collector for flotation of coarse-grained ilmenite according to claim 1, characterized in that, The mass ratio of higher alcohols, fatty acids, and alkyl hydroxyxamic acids in the auxiliary collector is 1:(0.2-0.5):(0.2-0.5).
4. The application of an auxiliary collector for the flotation of coarse-grained ilmenite as described in any one of claims 1-3, characterized in that, The aforementioned auxiliary collector was combined with benzohydroxyxamic acid for the flotation of coarse-grained ilmenite.
5. The application of the auxiliary collector for coarse-grained ilmenite flotation according to claim 4, characterized in that, The process includes the following steps: mixing coarse-grained ilmenite flotation material with water to prepare a slurry with a mass concentration of 30%; adding sodium carbonate as a pH adjuster to adjust the pH of the slurry to 7.5–8.0, and stirring for 5 minutes; adding 300 g / t–400 g / t of lead nitrate activator, and stirring for 5 minutes; adding 800 g / t–1500 g / t of benzohydroxyxamic acid collector, and stirring for 5 minutes; adding 80 g / t–150 g / t of auxiliary collector, and stirring for 5 minutes. After the slurry is prepared, ilmenite roughing is carried out. The rough concentrate obtained from the roughing is further treated with three cleaning operations, and the tailings from the roughing are treated with one scavenging operation. A closed-circuit flotation process is adopted, and the middlings are returned sequentially to obtain titanium concentrate and tailings.
6. The application of the auxiliary collector for the flotation of coarse-grained ilmenite according to claim 5, characterized in that, The particle size distribution of the coarse-grained ilmenite flotation material is as follows: +0.25mm content ≤ 5%, -0.25mm and +0.075mm content 70% to 75%.
7. The application of the auxiliary collector for the flotation of coarse-grained ilmenite according to claim 5, wherein the amount of the auxiliary collector and the benzo[a]hydroxyxamic acid collector is in a mass ratio of 1:(10-20).
8. In the application of the auxiliary collector for coarse-grained ilmenite flotation according to claim 5, in the three cleaning operations, 200g / t to 400g / t of water glass is added in the first cleaning operation, 50g / t to 100g / t of water glass is added in the second cleaning operation, and no reagent is added in the third cleaning operation.
9. The application of the auxiliary collector in the flotation of coarse-grained ilmenite according to claim 5, wherein in a single scavenging operation, the pulp pH is 7.5-8.0, 150g / t-200g / t of lead nitrate activator is added, 400g / t-750g / t of benzohydroxyxamic acid collector is added, and 40g / t-75g / t of auxiliary collector is added.