A three-phase mixing nozzle special for phosphate rock flotation and a method of using the same

The three-phase mixing nozzle enables instantaneous and uniform mixing and rapid activation of reagents in phosphate rock flotation, solving problems such as uneven local reagent concentration and collector failure, improving flotation recovery rate and production stability, and reducing reagent consumption and energy consumption.

CN123149071APending Publication Date: 2026-11-24HUBEI EZHONG ECOLOGICAL ENG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611384727.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing phosphate rock flotation technologies suffer from problems such as delayed reagent diffusion, uneven local concentration, premature hydrolysis and ineffectiveness of collectors, poor activation effect of frothers, low mixing efficiency, and poor stability of flotation indicators, making it difficult to guarantee production stability.

Method used

A three-phase mixing nozzle specifically designed for phosphate rock flotation is used. Through multi-stage shearing, turbulent disturbance, and high-speed impact within the nozzle, instantaneous uniform mixing of the gas-liquid-solid three-phase media and rapid activation of reagents are achieved, eliminating the need for a pre-stirring tank and relying on fluid power to replace mechanical stirring.

Benefits of technology

The effective utilization rate of reagents is increased by 15%~25%, the flotation recovery rate is steadily increased by 2.8%~3.5%, the reagent consumption cost is significantly reduced, the production stability and process adaptability are greatly improved, and the equipment cost and energy consumption are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149071A_ABST
    Figure CN123149071A_ABST
Patent Text Reader

Abstract

This invention discloses a three-phase mixing nozzle for phosphate rock flotation and its usage method, comprising a nozzle shell, a slurry feed channel, a feed assembly, a three-phase mixing chamber, a discharge nozzle, and a PLC control unit. It adopts a fixed-point injection, non-premature contact structural design, achieving instantaneous and uniform mixing of the three-phase media and instantaneous reagent activation through multi-stage shearing, turbulent disturbance, and high-speed impact effects within the three-phase mixing chamber. This solves the technical problems of uneven local reagent concentration, premature collector hydrolysis and ineffectiveness, poor reagent activation, low mixing efficiency, and poor stability of flotation indicators in traditional technologies. The effective utilization rate of reagents can be increased by 15%~25%, and the flotation recovery rate can be stably increased by 2.8%~3.5%. Simultaneously, it simplifies the flotation process, greatly improving the continuity and stability of flotation production. It is adaptable to phosphate rock flotation operations of different grades, concentrations, and degrees of mudding, exhibiting high versatility and industrial adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of phosphate rock flotation technology, specifically relating to a three-phase mixing nozzle for phosphate rock flotation and its usage method. Background Technology

[0002] Phosphate flotation is a core process for upgrading and reducing impurities in low-grade phosphate rock and lean phosphate rock, and for recovering effective phosphate minerals. The uniformity of mixing flotation reagents with the slurry and the sufficiency of reagent activation directly determine the grade of phosphate concentrate, the flotation recovery rate of phosphate minerals, and the cost of mineral processing. It is a key factor restricting the stability and economy of the phosphate flotation process. Currently, the domestic phosphate flotation industry generally adopts the reagent mixing process of "direct injection through pipeline + mechanical stirring in a mixing tank". Specifically, flotation reagents such as collectors and frothers are directly added to the slurry in the flotation cell or pre-mixing tank through independent pipelines. The mixing, dispersion, and activation of reagents are achieved by the mechanical stirring action of the stirring paddle.

[0003] For example, Chinese invention patent CN117753565A, published on March 26, 2024, discloses a micro-nano bubble enhanced flotation device and method for fine-grained collophane. The technical solution is as follows: (1) nano bubble water is produced by a micro-nano bubble generator; (2) after grinding the collophane raw ore, magnesium-removed concentrate is obtained by reverse flotation; (3) the magnesium-removed concentrate is fed into a spiral sluice to obtain gravity concentrate and gravity tailings respectively; (4) the gravity tailings sample is placed in a stirring tank and nano bubble water is added to adjust the slurry to obtain slurry; (5) phosphoric acid and a dealuminizing collector are added in sequence to adjust the slurry; (6) the gravity tailings flotation adopts a "one roughing and one cleaning" process flow. The flotation index shows that, under the same reagent system, the nano bubble water flotation method significantly accelerates the flotation rate of collophane heavy tailings compared with conventional water flotation, and improves the phosphorus grade and recovery rate of the concentrate.

[0004] As can be seen from the above patents, although the patents utilize nanobubble water flotation to significantly accelerate the flotation rate of collophane tailings and improve the phosphorus grade and recovery rate of the concentrate, the existing technology has the following shortcomings: 1. Direct addition of flotation reagents results in a significant diffusion lag effect, preventing them from uniformly dispersing throughout the pulp system within a short time. This easily leads to concentration stratification issues, such as excessively high reagent concentrations in some areas and insufficient reagent concentrations in larger areas. It also causes premature hydrolysis and oxidation of the collector, significantly reducing the utilization rate of effective reagents. At the same time, the frother cannot fully contact and integrate with the pulp and collector, resulting in slow foaming rate, uneven bubble size, poor bubble stability, and low effective foaming rate. Consequently, it cannot provide a stable foam carrier for the adsorption and flotation of mineral particles, directly reducing the flotation separation effect. 2. The activation effect of traditional processes depends entirely on the static residence time of the slurry in the mixing tank. The process has weak anti-interference ability and extremely poor adaptability to operating conditions. In actual production, fluctuations in raw ore grade, sudden changes in slurry flow rate, changes in slurry concentration, and increased ore mudification will all directly change the activation time and mixing uniformity of the reagents. Insufficient or over-activation of reagents will frequently occur, ultimately leading to significant fluctuations in the grade and recovery rate of flotation concentrate, making it difficult to guarantee production stability. Therefore, there is an urgent need for a new type of mixing device and process that can achieve precise mixing and instantaneous activation of reagents and adapt to complex working conditions, in order to solve the technical problems of uneven local concentration of reagents, premature hydrolysis and failure of collectors, poor activation effect of reagents, low mixing efficiency and poor stability of flotation indicators in the existing technology. Summary of the Invention

[0005] The purpose of this invention is to provide a three-phase mixing nozzle for phosphate rock flotation and its application method, overcoming the shortcomings of existing phosphate rock flotation reagent mixing technology, such as reagent diffusion lag, uneven local concentration, premature hydrolysis and failure of collectors, poor activation effect of frothers, large reagent consumption, and large fluctuations in flotation indicators. Relying on the hydrodynamic effect of the dedicated three-phase mixing nozzle, instantaneous mixing and rapid activation of slurry, collectors, and frothers are achieved, effectively improving reagent utilization, reducing production energy consumption and reagent costs, stabilizing various flotation indicators, and improving the adaptability of process conditions.

[0006] The technical solution of the present invention is as follows: A three-phase mixing nozzle for phosphate rock flotation is detachably and sealedly installed on the end pipeline of the phosphate rock flotation system for conveying slurry to the flotation cell. It is used to realize instantaneous mixing of gas-liquid-solid three phases and efficient activation of reagents. The nozzle includes a nozzle shell, a slurry feed channel, a feed assembly, a three-phase mixing chamber, a discharge nozzle, and a PLC control unit. The slurry feed channel is coaxially fixed inside the nozzle housing from the top to the bottom. The top of the slurry feed channel is sealed and connected to the front slurry conveying pipeline to form a high-speed slurry conveying channel. The slurry can flow into the internal cavity of the nozzle at high speed along the slurry feed channel. The feeding assembly includes six symmetrically arranged, independent, and non-interconnected collector feed lines, frother feed lines, and air inlet pipes. Each collector feed line, frother feed line, and air inlet pipe independently penetrates the side wall of the nozzle housing and is sealed. The outlet ends of each collector feed line, frother feed line, and air inlet pipe are independently connected to the interior of the three-phase mixing chamber and are not connected to the main slurry pipeline or come into contact with the slurry before the slurry enters the three-phase mixing chamber. This achieves independent, precise, and targeted supply of the two flotation reagents and gas, fundamentally preventing premature hydrolysis and failure of the reagents. The three-phase mixing chamber is a sealed cavity formed inside the nozzle housing and is connected to the slurry feed channel and the discharge injection port at the top and bottom respectively. The three-phase mixing chamber integrates a turbulent shearing structure, which can generate high-intensity shearing, tearing, impact and turbulent disturbance on the high-speed flowing solid phase of slurry, liquid phase of reagent and gas phase, providing fluid dynamic support for the mixing of three-phase media and the activation of reagent. The discharge nozzle is fixedly located at the center of the bottom end of the nozzle housing and is connected to the internal cavity of the rear flotation cell. The three-phase material, after being mixed and activated in the three-phase mixing chamber, can be sprayed at high speed into the flotation cell through the discharge nozzle to carry out the separation operation.

[0007] Optionally, the turbulent shearing structure includes multiple levels of staggered and uniformly arranged turbulence teeth and an integrally formed shearing ridge. The multiple levels of turbulence teeth are staggered and distributed on the inner wall of the three-phase mixing cavity, and the shearing ridge is integrally protruded on the fluid flow path in the center of the three-phase mixing cavity. It can perform multi-stage crushing, fine tearing and shearing on the high-speed mineral slurry solid phase, reagent liquid phase and gas phase respectively, which can greatly improve the mixing uniformity of the three-phase medium.

[0008] Optionally, the discharge ends of the collector feed pipe and the frother feed pipe are both inclined toward the mainstream flow direction of the slurry in the three-phase mixing chamber, and the angle between the inclination direction and the slurry flow direction is controlled at 30°~60° to ensure that the agent can be instantly integrated into the high-speed slurry fluid after being sprayed, and to prevent agent retention, accumulation, and deviation. The discharge end of the air inlet pipe is pointed to the tangent direction of the inner wall of the three-phase mixing chamber, so as to ensure that the low-pressure micro-air transported by the air inlet pipe forms turbulence in the three-phase mixing chamber, which facilitates the full and instantaneous mixing of the three-phase media and the efficient activation of the agent in the three-phase mixing chamber.

[0009] Optionally, the slurry feed channel, three-phase mixing chamber, and discharge nozzle adopt an integrated coaxial structure design, and the flow orifice is formed sequentially along the slurry flow direction as a constriction section, throat section, and diffusion section that are close to the Venturi tube structure, which further improves the slurry fluid velocity and shear strength, and ensures the mixing and activation effect of the three-phase medium.

[0010] Optionally, the nozzle further includes a PLC control unit, which is fixedly mounted on the outer wall of the nozzle housing. The collector feed line, foaming agent feed line, and air inlet line are each independently connected to a precision metering pump, and the injection pressure and injection flow rate can be adjusted accordingly. The PLC control unit is electrically connected to and controls the precision metering pump.

[0011] This invention also provides a method for using a three-phase mixing nozzle specifically for phosphate rock flotation, comprising the following steps: S1 Installation and Connection: The three-phase mixing nozzle is sealed and fixedly installed at the end of the slurry conveying pipeline and the front end of the flotation cell feed; the collector feed pipeline, frother feed pipeline and air inlet pipeline are independently connected to the precision metering and delivery pump to realize the quantitative, independent and controllable supply of the two reagents and gases. S2 high-speed slurry conveying: The slurry flows at high speed through the slurry feed channel via the conveying pipeline and continuously enters the three-phase mixing chamber. The high-speed flowing slurry forms a high-intensity turbulent and high-shear fluid in the three-phase mixing chamber. S3 reagent and air precision injection: The PLC control unit, through an independent precision metering pump, injects quantitative collector, frother, and low-pressure trace air directly into the three-phase mixing chamber through corresponding feed pipelines according to the process conditions of slurry pressure 0.2~0.4 MPa, reagent injection pressure 0.3~0.5 MPa, and air inlet pressure 0.03~0.08 MPa. The two reagents do not come into contact with the slurry in advance, completely avoiding the problems of premature hydrolysis and failure of the reagents. S4 Three-Phase Instantaneous Mixing and Activation: High-speed moving solid particles of slurry, liquid collector, liquid frother, and gaseous air are mixed in a closed space within a three-phase mixing chamber. Relying on the shearing force, impact force, and turbulent disturbance effect generated by the high-speed fluid motion, turbulent shear structure, and air turbulence, the three-phase media are rapidly broken, torn, and dispersed, achieving instantaneous uniform mixing of gas, liquid, and solid phases. At the same time, the reagents are rapidly activated within 5~50 ms with the help of high-intensity fluid dynamics, which promotes the rapid and uniform adsorption of the collector on the surface of the effective mineral particles of phosphate rock, and the rapid generation of micro flotation bubbles with uniform particle size and strong stability by the frother. S5 injection flotation: The three-phase mixture that has been mixed and activated by reagents is injected at high speed into the flotation cell through the discharge nozzle at the bottom of the nozzle, and directly enters the subsequent flotation separation process without the need for mechanical stirring and premixing.

[0012] Optionally, in step S2, the flow velocity of the slurry flowing through the three-phase mixing chamber is stably controlled at 2.5~4 m / s. By utilizing the negative pressure and strong shearing effect generated by the high-speed fluid, the mixing efficiency of the three-phase medium and the activation effect of the reagent are maximized.

[0013] Optionally, in step S3, the supply quantity and supply rate of the collector, frother, and low-pressure trace air are adaptively adjusted by the PLC control unit based on the real-time slurry concentration, slurry flow rate, and raw ore grade parameters to achieve precise quantitative supply and eliminate reagent waste from the source.

[0014] The beneficial effects of this invention are: The present application discloses a three-phase mixing nozzle for phosphate rock flotation and its application method, which has the following beneficial effects: 1. This invention employs a three-phase mixing nozzle with a fixed-point injection structure and no premature contact, completely solving the problem of collector hydrolysis failure caused by premature mixing of reagents into the slurry in traditional technologies. Simultaneously, through multi-stage shearing, turbulent disturbance, and high-speed impact within the three-phase mixing chamber, instantaneous and uniform mixing of the three-phase media across the entire domain is achieved. Fluid shearing power completely replaces the traditional mechanical stirring mixing mode, enabling instantaneous reagent activation. This completely overcomes the technical challenges of uneven local reagent concentration, premature collector hydrolysis failure, poor reagent activation effect, low mixing efficiency, and poor stability of flotation indicators in traditional technologies. It significantly shortens the reagent activation response time, increases reagent utilization by 15%~25%, and stably increases flotation recovery by 2.8%~3.5%, significantly reducing flotation reagent consumption costs, minimizing resource waste, and effectively improving phosphate rock flotation recovery and concentrate grade. 2. This invention completely eliminates the pre-mixing process of reagents in the pre-mixing tank, streamlining the flotation process and reducing the purchase, operation, and maintenance costs of mixing equipment. Simultaneously, it eliminates the dependence of reagent activation effects on the residence time in the mixing tank, effectively offsetting the negative impacts of fluctuations in slurry flow, concentration, and raw ore grade, greatly improving the continuity and stability of flotation production. Furthermore, it features a compact structure, convenient installation, wear and corrosion resistance, and strong adaptability to various operating conditions. It can be adapted to phosphate rock flotation operations of different grades, concentrations, and degrees of mudding, exhibiting high versatility and industrial compatibility, making it easy to promote and apply on a large scale. Simultaneously, it achieves multiple technical effects such as improved quality, stable production, reduced consumption, and reduced costs.

[0015] This application employs a three-phase mixing nozzle with a fixed-point injection structure and no premature contact. Through multi-stage shearing, turbulent disturbance, and high-speed impact within the three-phase mixing chamber, it achieves instantaneous and uniform mixing of the three-phase media and instantaneous activation of the reagents. This solves the technical problems of uneven local reagent concentration, premature hydrolysis and failure of the collector, poor reagent activation effect, low mixing efficiency, and poor stability of flotation indicators in traditional technologies. It significantly shortens the reagent activation response time, increases the effective utilization rate of reagents by 15%~25%, and steadily increases the flotation recovery rate by 2.8%~3.5%, effectively improving the phosphate rock flotation recovery rate and concentrate grade. At the same time, it simplifies the flotation process, effectively offsetting the negative impacts of fluctuations in pulp flow rate, concentration, and raw ore grade, greatly improving the continuity and stability of flotation production. It is adaptable to phosphate rock flotation operations of different grades, concentrations, and degrees of mudding, and has high versatility and industrial adaptability. Attached Figure Description

[0016] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings in the following description are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.

[0017] The structures, proportions, sizes, etc. illustrated in this specification are only for the purpose of assisting those skilled in the art in understanding and reading the content disclosed herein, and are not intended to limit the conditions under which the present invention can be implemented. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportions, or adjustments to the size, without affecting the effects and objectives that the present invention can produce, should still fall within the scope of the technical content disclosed in the present invention.

[0018] Figure 1 This is a front view structural diagram of the present invention; Figure 2 This is a top view of the feeding assembly of the present invention; The figure shows: 1. Nozzle housing; 2. Slurry feed channel; 3. Feed assembly; 31. Collector feed pipeline; 32. Foaming agent feed pipeline; 33. Air inlet pipeline; 4. Three-phase mixing chamber; 5. Discharge nozzle; 6. PLC control unit. Detailed Implementation

[0019] The present invention will be further described below with reference to the embodiments, but the scope of protection of the present invention is not limited to the following embodiments.

[0020] Unless otherwise specified, the reagents and materials described in the following examples are commercially available.

[0021] Unless otherwise specified, the "parts" mentioned in the embodiments of the present invention refer to parts by mass, and the "%" refers to a percentage by mass.

[0022] Example 1 This embodiment provides a three-phase mixing nozzle specifically for phosphate rock flotation. It is mainly used in the entire process of phosphate rock flotation, including forward and reverse flotation, roughing, cleaning, and scavenging. It is suitable for the instantaneous mixing of the solid phase of the slurry, the liquid phase of the collector, the liquid phase of the frother, and the gas phase of air during the phosphate rock flotation process, as well as the rapid activation of reagents. The three-phase mixing nozzle includes a nozzle housing 1, a slurry feed channel 2, a feed assembly 3, a three-phase mixing chamber 4, a discharge nozzle 5, and a PLC control unit 6. The three-phase mixing nozzle is detachably and sealedly installed on the end pipeline of the phosphate rock flotation system, which transports the slurry to the flotation cell. It is used to achieve instantaneous mixing of gas, liquid and solid phases and efficient activation of reagents. The nozzle is made of high wear-resistant and corrosion-resistant stainless steel to adapt to the complex working conditions of high-speed slurry scouring and reagent corrosion. The nozzle can adopt a flange quick-release structure for easy maintenance and replacement of internal shear components. The slurry feed channel 2 is coaxially fixed inside the nozzle housing 1 from the top to the bottom. The top of the slurry feed channel 2 is sealed and connected to the front-end slurry conveying pipeline. The diameter of the slurry feed channel 2 matches the diameter of the front-end slurry conveying pipeline, which can achieve seamless sealing and eliminate slurry leakage and pressure relief problems. The slurry can flow into the nozzle cavity at high speed along the slurry feed channel 2 to form a high-speed slurry conveying channel. The feeding assembly 3 includes six symmetrically arranged, independent, and non-connected collector feed pipes 31, frother feed pipes 32, and air inlet pipes 33. Each of these pipes independently penetrates the side wall of the nozzle housing 1 and is sealed to ensure that there is no cross-contamination or interference between them, thus preventing premature reaction of the reagents and flocculation failure. The outlet ends of the collector feed pipes 31, frother feed pipes 32, and air inlet pipes 33 are all independently connected to the interior of the three-phase mixing chamber 4 and are not connected to the main slurry pipeline or come into contact with the slurry before the slurry enters the three-phase mixing chamber 4. This achieves independent, precise, and targeted supply of the two flotation reagents and the gas, thus preventing premature hydrolysis and failure of the reagents from the source. It should be noted that the air inlet pipe 33 is used to deliver low-pressure micro-air into the three-phase mixing chamber 4. An external low-pressure micro-air pipeline can introduce low-pressure micro-air into the three-phase mixing chamber 4 to enhance the pre-foaming effect of the foaming agent. It should be noted that the feed assembly 3 ensures that the feed pipelines of the collector, frother and low-pressure trace air do not intersect. The reagents, namely the collector and frother, do not come into contact with the slurry in advance throughout the process, ensuring that the three-phase media only come into contact with each other inside the three-phase mixing chamber 4 at the last moment. The three-phase mixing chamber 4 is a sealed cavity formed inside the nozzle housing 1 and is connected to the slurry feed channel 2 and the discharge nozzle 5 at the top and bottom respectively. The slurry can enter the three-phase mixing chamber 4 through the slurry feed channel 2. The three-phase mixing chamber 4 integrates a turbulent shearing structure, which can generate high-intensity shearing, tearing, impact and turbulent disturbance on the high-speed flowing solid phase of slurry, liquid phase of reagent and gas phase. This allows the three-phase medium of solid particles of slurry, liquid phase of collector, liquid phase of foaming agent and low-pressure trace air gas phase to be broken, torn and mixed instantly in the sealed cavity of the three-phase mixing chamber 4. This enables the rapid adsorption of collector and mineral particles and rapid foaming and activation of foaming agent, providing fluid dynamic support for the mixing of three-phase medium and activation of reagent. The discharge nozzle 5 is fixedly located at the center of the bottom end of the nozzle housing 1 and is connected to the internal cavity of the rear flotation cell. The three-phase material, after being mixed and activated in the three-phase mixing chamber 4, can be sprayed into the flotation cell at high speed through the discharge nozzle 5 to carry out the separation operation. The PLC control unit 6 is fixedly installed on the outer wall of the nozzle housing 1. The collector feed pipe 31, the frother feed pipe 32 and the air inlet pipe 33 are independently connected to the precision metering pump, which can respectively adjust the injection pressure and injection flow rate of the collector, the frother and the low-pressure micro air. The PLC control unit 6 is electrically connected to and controls the precision metering pump. The precision metering pump is linked with the slurry flow signal. When the slurry flow changes, the dosage of the collector and the frother and the gas flow rate of the low-pressure micro air are adjusted synchronously.

[0023] Example 2 Based on Embodiment 1, this embodiment further defines the feeding assembly 3, the three-phase mixing chamber 4, and the nozzle as a whole.

[0024] In the feeding assembly 3, the outlet ends of the collector feed pipe 31 and the frother feed pipe 32 are inclined towards the mainstream flow direction of the slurry in the three-phase mixing chamber 4, and the angle between the inclined direction and the slurry flow direction is controlled at 30°~60°. This ensures that the reagent can be instantly integrated into the high-speed slurry fluid after being sprayed, and prevents the reagent from stagnating, accumulating, or deviating. The optimal angle is when the reagent spray direction is at a 45° angle to the slurry flow direction, which takes into account both mixing efficiency and reagent dispersion effect. The outlet end of the air inlet pipe 33 in the feeding assembly 3 points to the tangent direction of the inner wall of the three-phase mixing chamber 4, so as to ensure that the low-pressure micro-air transported by the air inlet pipe 33 forms turbulence in the three-phase mixing chamber 4, which facilitates the full and instantaneous mixing of the three-phase media in the three-phase mixing chamber 4 and the efficient activation of the reagent. The turbulent shearing structure in the three-phase mixing chamber 4 includes multi-level staggered and uniformly arranged turbulence teeth and an integrally formed shearing ridge. The multi-level turbulence teeth are staggered and distributed on the inner sidewall of the three-phase mixing chamber 4, and the shearing ridge is integrally protruded on the fluid flow path in the center of the three-phase mixing chamber 4. After the slurry enters the three-phase mixing chamber 4 through the slurry feed channel 2, the multi-level turbulence teeth and shearing ridge can respectively crush, finely tear and shear the high-speed slurry solid phase, reagent liquid phase and gas phase, which greatly improves the mixing uniformity of the three-phase media in the three-phase mixing chamber 4. The nozzle adopts an integrated coaxial molding structure, that is, the slurry feed channel 2, the three-phase mixing chamber 4, and the discharge nozzle 5 are designed as an integrated coaxial structure. The flow orifice forms a constriction section, a throat section, and a diffusion section that are close to the Venturi tube structure along the slurry flow direction. The slurry further improves the slurry fluid velocity and shear strength by passing through the slurry feed channel 2, the three-phase mixing chamber 4, and the discharge nozzle 5 that are close to the Venturi tube structure, thus ensuring the mixing and activation effect of the three-phase medium. It should be noted that the discharge nozzle 5 adopts a gradually expanding jet outlet, and the gas-liquid-solid three-phase material that has been mixed and activated is sprayed out at high speed and directly injected into the lower part of the slurry surface in the flotation cell; the outlet is treated with anti-clogging chamfering to reduce the deposition of coarse phosphate ore particles that block the nozzle channel; the outlet can be fitted with different diameter bushings to adapt to different slurry processing conditions.

[0025] Example 3 Based on Embodiments 1 and 2, this embodiment provides a method for using a three-phase mixing nozzle specifically for phosphate rock flotation, including the following steps: S1 Installation and Connection: The three-phase mixing nozzle is sealed and fixedly installed at the end of the slurry conveying pipeline and the front end of the flotation cell feed; the collector feed pipeline, frother feed pipeline and air inlet pipeline are independently connected to the precision metering and delivery pump to realize the quantitative, independent and controllable supply of the two reagents and gases. S2 high-speed slurry conveying: The slurry flows at high speed through the slurry feed channel via the conveying pipeline and continuously enters the three-phase mixing chamber. The high-speed flowing slurry forms a high-intensity turbulent and high-shear fluid in the three-phase mixing chamber. It should be noted that the pressure of the slurry entering the nozzle is maintained at 0.2~0.4 MPa to ensure sufficient fluid shear strength inside the three-phase mixing chamber; the slurry concentration is adapted to the conventional range of 20%~35% for flotation processes. S3 reagent and air precision injection: The PLC control unit, through an independent precision metering pump, injects quantitative collector, frother, and low-pressure trace air directly into the three-phase mixing chamber through corresponding feed pipelines according to the process conditions of slurry pressure 0.2~0.4 MPa, reagent injection pressure 0.3~0.5 MPa, and air inlet pressure 0.03~0.08 MPa. The two reagents do not come into contact with the slurry in advance, completely avoiding the problems of premature hydrolysis and failure of the reagents. It should be noted that the reagent injection pressure is 0.05~0.1 MPa higher than the slurry pressure inside the three-phase mixing chamber to ensure that the reagent can be injected into the mainstream of the high-speed slurry and to avoid reagent backflow clogging the reagent nozzle; the inlet pressure of the low-pressure micro-air is maintained at 0.03~0.08 MPa, and the small amount of air is used for pre-foaming to avoid excessive air causing the flotation cell foam to run out of control. S4 Three-Phase Instantaneous Mixing and Activation: High-speed moving solid particles of slurry, liquid collector, liquid frother, and gaseous air are mixed in a closed space within a three-phase mixing chamber. Relying on the shearing force, impact force, and turbulent disturbance effect generated by the high-speed fluid motion, turbulent shear structure, and air turbulence, the three-phase media are rapidly broken, torn, and dispersed, achieving instantaneous uniform mixing of gas, liquid, and solid phases. At the same time, the reagents are rapidly activated within 5~50 ms with the help of high-intensity fluid dynamics, which promotes the rapid and uniform adsorption of the collector on the surface of the effective mineral particles of phosphate rock, and the rapid generation of micro flotation bubbles with uniform particle size and strong stability by the frother. It should be noted that the contact activation time between the reagent and the slurry in the three-phase mixing chamber is controlled at 5~50 ms to achieve instantaneous activation without prolonged residence. S5 injection flotation: The three-phase mixture that has been mixed and activated by reagents is injected at high speed into the flotation cell through the discharge nozzle at the bottom of the nozzle, and directly enters the subsequent flotation separation process without the need for mechanical stirring and premixing.

[0026] In step S2, during the high-speed transport of the slurry, the flow velocity of the slurry through the three-phase mixing chamber is stably controlled at 2.5~4 m / s. By utilizing the negative pressure and strong shearing effect generated by the high-speed fluid, the mixing efficiency of the three-phase medium and the activation effect of the reagent are maximized.

[0027] In step S3, the precise injection of reagents and air involves the supply of collectors, frothers, and low-pressure trace amounts of air. The supply quantity and rate of these substances are adaptively adjusted by a PLC control unit based on real-time slurry concentration, slurry flow rate, and raw ore grade parameters. This ensures precise quantitative supply and eliminates reagent waste at the source.

[0028] Comparative Example At a flotation production site for low-grade phosphate rock, the traditional direct reagent addition + pre-stirring process is used, and the separation operation is carried out according to conventional flotation process parameters.

[0029] Example 4 In this embodiment, at the comparative low-grade phosphate rock flotation production site, the pre-mixing process of the reagent in the pre-stirring tank is eliminated. The three-phase mixing nozzles of Embodiments 1 and 2 are used, and the usage method is the same as in Embodiment 3. The difference is that the pressure of the slurry entering the nozzle is 0.2 MPa, the flow velocity of the slurry flowing through the three-phase mixing chamber 4 is stably controlled at 2.5 m / s, the reagent injection pressure is 0.3 MPa, and the inlet pressure of the low-pressure micro-air is 0.03 MPa. The fully mixed and activated three-phase mixture is injected into the flotation cell at high speed through the discharge nozzle 5, and the separation operation is carried out according to the conventional flotation process parameters.

[0030] The application results of this embodiment show that, compared with the comparative example, the present invention can reduce the overall consumption of collectors and frothers by 15%, increase the effective utilization rate of reagents by 15%, and solve the problems of excessive addition and waste of reagents; the fluctuation range of phosphate concentrate grade is significantly reduced, the production stability is significantly improved, and the flotation recovery rate is steadily increased by 2.8%; at the same time, the operation of the stirring equipment is eliminated, the overall energy consumption of the production line is reduced by 16%, the equipment operation and maintenance costs are significantly reduced, and the overall effect of improving quality and reducing consumption, stabilizing production and increasing efficiency is quite significant.

[0031] Example 5 The usage method of this embodiment is the same as that of embodiment four, except that: the pressure of the slurry entering the nozzle is 0.3 MPa, the flow rate of the slurry flowing through the three-phase mixing chamber 4 is stably controlled at the optimal flow rate of 3.2 m / s; the reagent injection pressure is 0.4 MPa, the inlet pressure of the low-pressure micro-air is 0.05 MPa, and the fully mixed and activated three-phase mixture is injected into the flotation cell at high speed through the discharge nozzle 5, and the separation operation is carried out according to the conventional flotation process parameters.

[0032] The application results of this embodiment show that, compared with the comparative example, the present invention can reduce the combined consumption of collectors and frothers by 25%, increase the effective utilization rate of reagents by 25%, and solve the problems of excessive addition and waste of reagents; the fluctuation range of phosphate concentrate grade is significantly reduced, the production stability is significantly improved, and the flotation recovery rate is steadily increased by 3.5%; at the same time, the operation of the stirring equipment is eliminated, the overall energy consumption of the production line is reduced by 20%, the equipment operation and maintenance costs are significantly reduced, and the overall effect of improving quality and reducing consumption, stabilizing production and increasing efficiency is extremely significant.

[0033] Example 6 The usage method of this embodiment is the same as that of embodiment four, except that: the pressure of the slurry entering the nozzle is 0.4 MPa, the flow velocity of the slurry flowing through the three-phase mixing chamber 4 is stably controlled at 4 m / s; the reagent injection pressure is 0.45 MPa, and the air intake pressure of the low-pressure micro-air is 0.08 MPa.

[0034] The application results of this embodiment show that, compared with the comparative example, the present invention can reduce the combined consumption of collectors and frothers by 20%, increase the effective utilization rate of reagents by 20%, and solve the problems of excessive addition and waste of reagents; the fluctuation range of phosphate concentrate grade is significantly reduced, the production stability is significantly improved, and the flotation recovery rate is steadily increased by 3.1%; at the same time, the operation of the stirring equipment is eliminated, the overall energy consumption of the production line is reduced by 18%, the equipment operation and maintenance costs are significantly reduced, and the overall effect of improving quality and reducing consumption, stabilizing production and increasing efficiency is significant.

[0035] The metrics for the examples and comparative examples are shown in Table 1.

[0036] Table 1 Comparison of Indicators between Examples and Comparative Examples

[0037] By comparing the metrics of the examples with those of the comparative examples, the following conclusions can be drawn: 1. After adopting the three-phase mixing nozzle of this application, compared with the comparative examples of the prior art, the effective utilization rate of reagents in Examples 4, 5, and 6 increased by 15%, 25%, and 20%, respectively; the flotation recovery rate was steadily increased by 2.8%, 3.5%, and 3.1%, respectively; and the overall energy consumption of the production line was reduced by 16%, 20%, and 18%. The overall effect of improving quality, reducing consumption, stabilizing production, and increasing efficiency is significant. 2. When the pressure of the slurry entering the nozzle is 0.3 MPa, the flow velocity of the slurry flowing through the three-phase mixing chamber is stably controlled at the optimal flow velocity of 3.2 m / s; the reagent injection pressure is 0.4 MPa, and the inlet pressure of the low-pressure trace air is 0.05 MPa, which are the optimal process conditions. The effective utilization rate of reagents is increased by 25%, the flotation recovery rate is stably increased by 3.5%, and the overall energy consumption of the production line is reduced by 20%. The equipment operation and maintenance costs are significantly reduced, and the overall effect of improving quality, reducing consumption, stabilizing production and increasing efficiency is extremely significant.

[0038] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A three-phase mixing nozzle specifically for phosphate rock flotation, characterized in that, The nozzle is detachably and sealedly installed on the end pipeline of the phosphate rock flotation system for conveying slurry to the flotation cell, and is used to realize instantaneous mixing of gas-liquid-solid three phases and efficient activation of reagents. The nozzle includes a nozzle shell (1), a slurry feed channel (2), a feed assembly (3), a three-phase mixing chamber (4), a discharge injection port (5), and a PLC control unit (6). The slurry feeding channel (2) is coaxially fixed inside the nozzle housing (1) from the top to the middle bottom. The top of the slurry feeding channel (2) is sealed and connected to the front slurry conveying pipeline to form a high-speed slurry conveying channel. The slurry can flow into the nozzle cavity at high speed along the slurry feeding channel (2). The feeding assembly (3) includes six collector feed pipes (31), frother feed pipes (32) and air inlet pipes (33) that are symmetrically opened, independent of each other, and not connected to each other. The collector feed pipes (31), frother feed pipes (32) and air inlet pipes (33) are independently opened through the side wall of the nozzle housing (1) and are sealed. The discharge ends of the collector feed pipes (31), frother feed pipes (32) and air inlet pipes (33) are independently connected to the interior of the three-phase mixing chamber (4) and are not connected to the main slurry pipeline or in contact with the slurry before the slurry enters the three-phase mixing chamber (4), so as to realize the independent, precise and fixed-point supply of the two flotation reagents and the gas, and avoid the premature hydrolysis and failure of the reagents from the source. The three-phase mixing chamber (4) is a sealed cavity formed inside the nozzle housing (1) and is connected to the slurry feed channel (2) and the discharge injection port (5) respectively. The three-phase mixing chamber (4) integrates a turbulent shearing structure, which can generate high-intensity shearing, tearing, impact and turbulent disturbance on the high-speed flowing solid phase of slurry, liquid phase of reagent and gas phase, providing fluid dynamic support for the mixing of three-phase media and the activation of reagent; The discharge nozzle (5) is fixedly located at the center of the bottom end of the nozzle housing (1) and is connected to the internal cavity of the rear flotation cell. The three-phase material, after being mixed and activated in the three-phase mixing chamber (4), can be sprayed into the flotation cell at high speed through the discharge nozzle (5) to carry out the separation operation.

2. The three-phase mixing nozzle for phosphate rock flotation according to claim 1, characterized in that, The turbulent shearing structure includes multiple levels of staggered and uniformly arranged turbulence teeth and an integrally formed shearing ridge. The multiple levels of turbulence teeth are staggered and distributed on the inner sidewall of the three-phase mixing cavity (4). The shearing ridge is integrally protruded on the fluid flow path in the center of the three-phase mixing cavity (4). It can perform multi-level crushing, fine tearing and shearing on the high-speed slurry solid phase, reagent liquid phase and gas phase respectively, which greatly improves the mixing uniformity of the three-phase medium.

3. The three-phase mixing nozzle for phosphate rock flotation according to claim 1, characterized in that, The discharge ends of the collector feed pipe (31) and the foaming agent feed pipe (32) are inclined toward the mainstream flow direction of the slurry in the three-phase mixing chamber (4), and the angle between the inclined direction and the slurry flow direction is controlled at 30°~60° to ensure that the agent can be instantly integrated into the high-speed slurry fluid after being sprayed out, and to prevent the agent from being stuck, accumulating, or deviating. The discharge end of the air inlet pipe (33) points to the tangential direction of the inner wall of the three-phase mixing chamber (4) to ensure that the low-pressure micro-air transported by the air inlet pipe (33) forms turbulence in the three-phase mixing chamber (4), which facilitates the full and instantaneous mixing of the three-phase media in the three-phase mixing chamber (4) and the efficient activation of the agent.

4. The three-phase mixing nozzle for phosphate rock flotation according to claim 1, characterized in that, The slurry feed channel (2), three-phase mixing chamber (4), and discharge nozzle (5) adopt an integrated coaxial structure design, and the flow orifice forms a constriction section, throat section and diffusion section that are close to the Venturi tube structure along the slurry flow direction, which further improves the slurry fluid velocity and shear strength, and ensures the three-phase medium mixing and activation effect.

5. A three-phase mixing nozzle for phosphate rock flotation according to claim 1, characterized in that, The nozzle also includes a PLC control unit (6), which is fixedly installed on the outer wall of the nozzle housing (1). The collector feed pipe (31), the foaming agent feed pipe (32) and the air inlet pipe (33) are independently connected to the precision metering pump, and the injection pressure and injection flow rate can be adjusted accordingly. The PLC control unit (6) is electrically connected to and controls the precision metering pump.

6. A method for using a three-phase mixing nozzle specifically for phosphate rock flotation, characterized in that, Includes the following steps: S1 Installation and Connection: Seal and fix the three-phase mixing nozzle at the end of the slurry conveying pipeline and the front end of the flotation cell feed; independently connect the collector feed pipeline, frother feed pipeline and air inlet pipeline to the precision metering and conveying pump; S2 high-speed slurry conveying: The slurry flows at high speed through the slurry feed channel via the conveying pipeline and continuously enters the three-phase mixing chamber. The high-speed flowing slurry forms a high-intensity turbulent and high-shear fluid in the three-phase mixing chamber. S3 Precision Injection of Reagents and Air: The PLC control unit, through an independent precision metering pump, injects quantitative collectors, frothers, and low-pressure trace amounts of air directly into the three-phase mixing chamber through the corresponding feed pipelines, according to the process conditions of slurry pressure 0.2~0.4 MPa, reagent injection pressure 0.3~0.5 MPa, and air inlet pressure 0.03~0.08 MPa. S4 Three-Phase Instantaneous Mixing and Activation: High-speed moving solid particles of slurry, liquid collector, liquid foaming agent, and gaseous air are rapidly broken up, torn apart, and dispersed in a three-phase mixing chamber by relying on the shear force, impact force, and turbulent disturbance effect generated by the high-speed fluid motion, turbulent shear structure, and air turbulence; at the same time, the agent is rapidly activated within 5~50 ms with the help of high-intensity fluid dynamics. S5 injection flotation: The three-phase mixture that has been mixed and activated by reagents is injected at high speed into the flotation cell through the discharge nozzle at the bottom of the nozzle, and directly enters the subsequent flotation separation process without the need for mechanical stirring and premixing.

7. The method of using the three-phase mixing nozzle for phosphate rock flotation according to claim 6, characterized in that, In step S2, the flow velocity of the slurry flowing through the three-phase mixing chamber is stably controlled at 2.5~4 m / s.

8. The method of using the three-phase mixing nozzle for phosphate rock flotation according to claim 6, characterized in that, In step S3, the supply quantity and supply rate of the collector, frother, and low-pressure trace air are adaptively adjusted by the PLC control unit based on the real-time slurry concentration, slurry flow rate, and raw ore grade parameters to achieve precise quantitative supply.

Citation Information

Patent Citations

  • Micro-nano bubble reinforced fine-particle collophanite flotation device and method

    CN117753565A