High peel strength pet film, preparation process and coating equipment thereof

By using an incremental temperature gradient drying process and a specific component coating slurry, the problem of uneven drying of PET film coatings was solved, peel strength was improved and production efficiency was increased, achieving efficient and uniform coating distribution.

CN123149133APending Publication Date: 2026-11-24JIANGSU SHUANGXING COLOR PLASTIC NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510666970.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-22
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The uneven drying rate of existing PET film coatings leads to uneven adhesive migration, reduced peel strength, easy cracking or warping of the coating, and low oven utilization, which affects production capacity.

Method used

An incremental temperature gradient drying process is adopted, which involves gradually increasing the temperature in multiple temperature zones. Combined with functional coating slurry with specific components, a slot die and a multi-temperature zone oven are used to control the temperature and coating accuracy, suppress binder migration, and ensure uniform coating distribution.

Benefits of technology

It significantly improves the peel strength between PET film and functional coating, ensures coating composition uniformity, increases oven utilization, shortens drying time, and meets the requirements of high peel strength and high-efficiency production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a process for preparing high-peel-strength PET films, characterized by the following steps: applying a functional coating slurry to the surface of a PET substrate; employing an incremental temperature gradient drying process, with the oven divided into at least four temperature zones, the temperature gradually increasing from 50-70℃ to 100-120℃, and the dwell time in each zone being 5-15 seconds; after drying, cooling and shaping, and then winding. This invention significantly improves peel strength and avoids coating defects by extending the constant-speed drying section to inhibit binder migration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer material processing technology, and in particular to a high peel strength PET film, its preparation process and coating equipment. Background Technology

[0002] PET film is widely used in packaging, electronics, and optics due to its excellent mechanical strength, chemical resistance, transparency, and dimensional stability. In the production of functional PET films, it is often necessary to coat their surface with functional coatings such as adhesives, conductive layers, and optical coatings. The peel strength between the coating and the substrate is a key indicator determining the film's performance. Existing technologies suffer from the following problems: Uneven drying rate: Traditional processes use constant temperature or simple segmented temperature control, causing the binder within the coating to migrate to the surface due to capillary action, resulting in uneven distribution between layers and decreased peel strength. Coating defects: Premature solvent evaporation at high temperatures can easily lead to coating cracking, warping, or blistering. Low process efficiency: Traditional "low-high-low" temperature parameters result in insufficient oven utilization, prolonged drying time, and reduced production capacity. Summary of the Invention

[0003] The purpose of this invention is to provide a high peel strength PET film, its preparation process, and its coating equipment. Specifically, by optimizing the drying process through incremental temperature gradient design, the following objectives are achieved: to improve the peel strength between the PET film and the functional coating (≥3.0N / 25mm); to inhibit adhesive migration and ensure uniform distribution of coating components; to improve oven utilization and shorten drying time; and to be compatible with multiple functional coatings (conductive, optical, adhesive, etc.).

[0004] To achieve the above objectives, the present invention provides the following technical solution:

[0005] A process for preparing a high-peel-strength PET film, characterized by comprising the following steps:

[0006] The functional coating paste is applied to the surface of the PET substrate; incremental temperature gradient drying is adopted, the oven is divided into at least four temperature zones, the temperature is gradually increased from 50-70℃ to 100-120℃, and the dwell time in each temperature zone is 5-15 seconds; after drying, it is cooled and shaped and then rolled up.

[0007] The present invention further provides that the heating rate of the incremental temperature gradient is 5-15℃ / temperature zone.

[0008] The present invention further provides that the temperature of the constant speed drying section is 80-100℃, accounting for 50-70% of the total length of the drying oven.

[0009] The present invention further provides that the functional coating slurry comprises the following components and mass percentages:

[0010] 10-20% waterborne polyurethane (PU);

[0011] 5-10% conductive agent;

[0012] Sodium carboxymethyl cellulose (CMC) 0.5-1.5%;

[0013] Solvent 70-85%;

[0014] Additives: 0.3-1.0%.

[0015] In a further embodiment of the present invention, the conductive agent is silver nanowire with a diameter of 30-50 nm and an aspect ratio of >1000.

[0016] The present invention further specifies that the coating speed is 10-20 m / min and the wet film thickness is 50-80 μm.

[0017] The present invention further provides that the peel force of the coating after drying is ≥3.0N / 25mm.

[0018] The present invention further provides that the PET substrate has a thickness of 10-50 μm, and the surface is corona treated, with a surface tension ≥50 mN / m.

[0019] The present invention also provides a high peel strength PET film, characterized in that, prepared by the above-mentioned process, the peel strength between the coating and the substrate is ≥3.0N / 25mm, and the difference in adhesive content between the upper and lower layers of the coating is <0.2%.

[0020] The present invention also provides a coating device for the aforementioned preparation process, comprising: a slit coating die with a coating accuracy error of <±2%; a multi-temperature zone oven with 4-6 temperature zones and a temperature control accuracy of ±1℃; and a cooling roller system with a surface temperature of 20-25℃.

[0021] The beneficial effects of this invention are:

[0022] This invention suppresses binder migration by extending the constant-speed drying section, significantly improving peel strength and avoiding coating defects. Detailed Implementation

[0023] The following will describe the implementation of this application in detail with reference to the embodiments, so that the implementation process of how this application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0024] This invention provides a process for preparing PET film with high peel strength, characterized by comprising the following steps:

[0025] The functional coating paste is applied to the surface of the PET substrate; incremental temperature gradient drying is adopted, the oven is divided into at least four temperature zones, the temperature is gradually increased from 50-70℃ to 100-120℃, and the dwell time in each temperature zone is 5-15 seconds; after drying, it is cooled and shaped and then rolled up.

[0026] The present invention further provides that the heating rate of the incremental temperature gradient is 5-15℃ / temperature zone.

[0027] The present invention further provides that the temperature of the constant speed drying section is 80-100℃, accounting for 50-70% of the total length of the drying oven.

[0028] The present invention further provides that the functional coating slurry comprises the following components and mass percentages:

[0029] 10-20% waterborne polyurethane (PU);

[0030] 5-10% conductive agent;

[0031] Sodium carboxymethyl cellulose (CMC) 0.5-1.5%;

[0032] Solvent 70-85%;

[0033] Additives: 0.3-1.0%.

[0034] In a further embodiment of the present invention, the conductive agent is silver nanowire with a diameter of 30-50 nm and an aspect ratio of >1000.

[0035] The present invention further specifies that the coating speed is 10-20 m / min and the wet film thickness is 50-80 μm.

[0036] The present invention further provides that the peel force of the coating after drying is ≥3.0N / 25mm.

[0037] The present invention further provides that the PET substrate has a thickness of 10-50 μm, and the surface is corona treated, with a surface tension ≥50 mN / m.

[0038] The present invention also provides a high peel strength PET film, characterized in that, prepared by the above-mentioned process, the peel strength between the coating and the substrate is ≥3.0N / 25mm, and the difference in adhesive content between the upper and lower layers of the coating is <0.2%.

[0039] The present invention also provides a coating device for the aforementioned preparation process, comprising: a slit coating die with a coating accuracy error of <±2%; a multi-temperature zone oven with 4-6 temperature zones and a temperature control accuracy of ±1℃; and a cooling roller system with a surface temperature of 20-25℃.

[0040] Example 1: High peel strength conductive PET film

[0041] formula:

[0042] AgNWs 8%, PU 15%, CMC 1%, deionized water 70%, ethanol 6%, defoamer 0.2%, wetting agent 0.3%.

[0043] Process parameters:

[0044] Coating speed 15m / min, wet film thickness 60μm;

[0045] Oven temperature gradient: 60℃→80℃→100℃→120℃, four temperature zones, each zone lasting 10 seconds;

[0046] The coating thickness after drying is 25μm.

[0047] Test results:

[0048] Peel force: 3.8N / 25mm;

[0049] Sheet resistance: 8.5Ω / sq;

[0050] Light transmittance: 87%;

[0051] Thermogravimetric analysis showed that the difference in binder content between the upper and lower layers was <0.1%.

[0052] Example 2: High weather-resistant adhesive PET film

[0053] formula:

[0054] PU 18%, nano SiO2 2%, CMC 1.2%, deionized water balance.

[0055] Process parameters:

[0056] Oven temperature gradient: 60℃→80℃→100℃→110℃, five temperature zones, each zone lasting 12 seconds.

[0057] Test results:

[0058] Peel force: 4.2N / 25mm;

[0059] Resistance to damp heat (85℃ / 85%RH, 240h): Peel strength retention rate >90%.

[0060] Example 3: High-transmittance anti-reflective PET film

[0061] 1. Formula:

[0062] The formula consists of 6% nano-silica (SiO2), 12% waterborne polyurethane (PU), 1% sodium carboxymethyl cellulose (CMC), 75% deionized water, 5% isopropanol, 0.5% leveling agent, and 0.5% ultraviolet absorber.

[0063] 2. Process parameters:

[0064] Coating speed 18m / min, wet film thickness 55μm;

[0065] Oven temperature gradient: 55℃→75℃→95℃→115℃, four temperature zones, each zone held for 8 seconds;

[0066] The coating thickness after drying is 28μm.

[0067] 3. Test Results:

[0068] Peel force: 3.5N / 25mm;

[0069] Light transmittance: 92% (visible light band 400-700nm);

[0070] Reflectivity: <1.5% (wavelength 550nm);

[0071] Weather resistance (QUV 1000 hours): Light transmittance decreases by <2%, and the coating shows no cracking;

[0072] Thermogravimetric analysis showed that the difference in binder content between the upper and lower layers was <0.15%.

[0073] This embodiment targets optical applications. By adding nano-silica to construct a micro / nano structure layer and combining it with an incremental temperature gradient drying process, the interfacial reflectivity is effectively reduced and the light transmittance is improved. The peel strength between the coating and the substrate meets the high peel strength requirement (≥3.0N / 25mm), and the adhesive distribution is excellent, satisfying the long-term stability requirements of the optical thin film.

[0074] In summary, the present invention, by extending the constant-speed drying section, inhibits binder migration, significantly improves peel strength, and avoids coating defects.

[0075] If certain terms are used in the specification and claims to refer to specific components, those skilled in the art will understand that hardware manufacturers may use different names to refer to the same component. This specification and claims do not distinguish components based on differences in name, but rather on differences in function. The term "comprising" as used throughout the specification and claims is an open-ended term and should be interpreted as "comprising but not limited to." "Approximately" means that within an acceptable margin of error, those skilled in the art can solve the technical problem and substantially achieve the technical effect within a certain margin of error.

[0076] It should be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a product or system comprising a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a product or system. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the product or system that includes that element.

[0077] The foregoing description illustrates and describes several preferred embodiments of the present invention. However, as previously stated, it should be understood that the present invention is not limited to the forms disclosed herein and should not be construed as excluding other embodiments. It can be used in various other combinations, modifications, and environments, and can be altered within the scope of the inventive concept by means of the foregoing teachings or techniques or knowledge in related fields. Any modifications and variations made by those skilled in the art that do not depart from the spirit and scope of the present invention should be within the protection scope of the appended claims.

Claims

1. A process for preparing a PET film with high peel strength, characterized in that, Includes the following steps: The functional coating paste is applied to the surface of the PET substrate; incremental temperature gradient drying is adopted, the oven is divided into at least four temperature zones, the temperature is gradually increased from 50-70℃ to 100-120℃, and the dwell time in each temperature zone is 5-15 seconds; after drying, it is cooled and shaped and then rolled up.

2. The process for preparing a high peel strength PET film according to claim 1, characterized in that, The heating rate of the incremental temperature gradient is 5-15℃ / temperature zone.

3. The process for preparing a high-peel-strength PET film according to claim 1, characterized in that, The constant-speed drying section has a temperature of 80-100℃ and accounts for 50-70% of the total length of the oven.

4. The process for preparing a high-peel-strength PET film according to claim 1, characterized in that, The functional coating slurry comprises the following components and mass percentages: 10-20% waterborne polyurethane (PU); 5-10% conductive agent; Sodium carboxymethyl cellulose (CMC) 0.5-1.5%; Solvent 70-85%; Additives: 0.3-1.0%.

5. The process for preparing a high peel strength PET film according to claim 4, characterized in that, The conductive agent is silver nanowires with a diameter of 30-50 nm and an aspect ratio of >1000.

6. The process for preparing a high peel strength PET film according to claim 1, characterized in that, The coating speed is 10-20 m / min, and the wet film thickness is 50-80 μm.

7. The process for preparing a high peel strength PET film according to claim 1, characterized in that, The peel strength of the dried coating is ≥3.0N / 25mm.

8. The process for preparing a high-peel-strength PET film according to claim 1, characterized in that, The PET substrate has a thickness of 10-50 μm, and its surface is corona treated with a surface tension ≥50 mN / m.

9. A high peel strength PET film, characterized in that, The preparation process according to any one of claims 1-8 has a peel force between the coating and the substrate ≥3.0N / 25mm, and the difference in adhesive content between the upper and lower layers of the coating is <0.2%.

10. A coating apparatus for preparing the preparation process according to any one of claims 1-8, comprising: Slit coating die head, coating accuracy error < ±2%; Multi-temperature zone oven, with 4-6 temperature zones and a temperature control accuracy of ±1℃; Cooling roller system, surface temperature 20-25℃.