In-line polymerization integrated nanocoating coating method for tpu / pet film

By employing an online polymerization-integrated nanocoating method, the problems of nanofiller sedimentation, coating pre-crosslinking, and thermal shrinkage deformation have been solved, achieving efficient and stable multifunctional coating formation suitable for TPU/PET films.

CN123149134APending Publication Date: 2026-11-24NALIN NANO TECH NANTONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611554973.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing coating processes, nanofillers are prone to sedimentation and aggregation, coatings are prone to pre-crosslinking or gelation during storage and transportation, multi-layer functional coatings require multiple coating and drying processes, and traditional high thermosetting temperatures lead to thermal shrinkage and deformation of TPU substrates, resulting in low production efficiency and poor interlayer adhesion.

Method used

An online polymerization integrated nano-coating method is adopted, which involves low-temperature plasma pretreatment, online dynamic mixing of multi-component coatings, and photo-thermal synergistic curing to form an integrated nano-composite coating. This avoids the problem of coating storage stability, realizes multi-functional coating with a single coating, and reduces the curing temperature to protect the TPU substrate.

Benefits of technology

It ensures uniformity of coating composition and surface quality, improves production stability and efficiency, prevents thermal shrinkage of TPU substrate, enhances interlayer adhesion, and broadens the application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149134A_ABST
    Figure CN123149134A_ABST
Patent Text Reader

Abstract

This invention discloses an online polymerization integrated nano-coating method for TPU / PET films, comprising: substrate unwinding and pretreatment: unwinding a TPU or PET film roll and subjecting the substrate surface to low-temperature plasma treatment; online dynamic mixing of multi-component coatings: supplying A-component, B-component, and nanofiller dispersions through three independent liquid supply systems to form a polymerizable nanocomposite precursor; online polymerization coating: continuously coating the polymerization precursor mixture onto the substrate surface through a precision coating head to form a uniform wet film; online photo-thermal synergistic curing: sequentially passing the coated substrate through an ultraviolet curing zone and a hot air micro-curing zone to achieve rapid cross-linking polymerization and post-curing of the coating, forming an integrated nanocomposite coating; cooling and winding: cooling the cured composite film with a cooling roller and then winding it up under constant tension to obtain the finished roll. This invention achieves integrated molding of functional layers, and is particularly suitable for temperature-sensitive TPU films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional film surface coating technology, specifically a method for online polymerization integrated nano-coating on TPU / PET films. Background Technology

[0002] Thermoplastic polyurethane (TPU) film and polyethylene terephthalate (PET) film are the two major substrates in the field of functional films. TPU film has excellent elasticity, abrasion resistance, and weather resistance, and is widely used in automotive paint protection films (car covers); PET film has high transparency, high strength, and dimensional stability, and is widely used in building insulation films, electronic screen protectors, etc. In order to endow the substrate surface with special functions (such as self-healing, scratch resistance, fingerprint resistance, hydrophobicity, oleophobicity, etc.), it is necessary to coat the film surface with a nano-functional coating.

[0003] Existing coating processes typically employ pre-polymerized nano-coatings, which are applied to the substrate surface via a coating head and then dried and cured in an oven. However, this traditional process has the following problems: First, nanofillers are prone to sedimentation and aggregation in the coating, resulting in particles or uneven haze on the coating surface; second, the coating may undergo pre-crosslinking or gelation during storage and transportation, affecting coating stability; third, multilayer functional coatings require multiple coating and drying processes, resulting in low production efficiency and poor interlayer adhesion; fourth, for TPU films, the traditional thermosetting process has a high temperature (>120℃), which easily leads to thermal shrinkage and deformation of the TPU substrate.

[0004] Therefore, to solve the above problems, an online polymerization integrated nano-coating method for coating TPU / PET films is provided. Summary of the Invention

[0005] To address the aforementioned problems in the prior art, this invention provides an online polymerization integrated nano-coating method for TPU / PET films, which avoids the problem of coating storage stability and achieves integrated molding of functional layers, and is particularly suitable for temperature-sensitive TPU films.

[0006] The technical solution to achieve the above objectives is: A method for applying an integrated, online polymerized nanocoating to TPU / PET films includes: Step S1, Substrate unwinding and pretreatment: Unwind the TPU film or PET film roll and perform low-temperature plasma treatment on the substrate surface; Step S2, online dynamic mixing of multi-component coatings: Component A, Component B and nanofiller dispersions are delivered through three independent liquid supply systems, and after precise metering by metering pumps, they are mixed uniformly online to form a polymerizable nanocomposite precursor; Step S3, online polymerization coating: The polymerization precursor mixture obtained in step S2 is continuously coated onto the substrate surface after step S1 through a precision coating head to form a uniform wet film. Step S4, online photo-thermal synergistic curing: The coated substrate is passed sequentially through the ultraviolet curing zone and the hot air micro-curing zone to achieve rapid cross-linking polymerization and post-curing of the coating, forming an integrated nanocomposite coating; Step S5, Cooling and winding: After the cured composite film is cooled by cooling rollers, it is wound up under constant tension to obtain the finished roll material.

[0007] Preferably, in step S1, low-temperature atmospheric pressure plasma treatment is used, with a treatment power of 500-2000W and a treatment speed of 5-30m / min, and the surface energy of the substrate after treatment is ≥52dyn / cm. The pretreatment equipment is set 1 to 3 m in front of the coating station, and the distance between the plasma electrode and the substrate surface is 5 to 20 mm.

[0008] Preferably, in step S2, component A comprises acrylate monomers or oligomers, a photoinitiator, and a leveling agent; Component B contains a crosslinking agent and an adhesion promoter; The nanofiller dispersion contains one or more of the following: surface-modified nano silica, nano alumina, or nano titanium dioxide; The mass ratio of component A to component B is 100:2 to 15, and the amount of nanofiller dispersion added is 5 to 30% of the mass of component A.

[0009] Preferably, in step S2, the acrylate monomer or oligomer of component A is one or more of polyurethane acrylate, epoxy acrylate or polyester acrylate, with a functionality of 2 to 6; the photoinitiator is one or more of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone or diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

[0010] Preferably, in step S2, the preparation method of the nanofiller dispersion is as follows: The nanofiller and silane coupling agent were ultrasonically dispersed in an ethanol / water mixed solvent at a mass ratio of 100:3-10 for 2-4 hours. After centrifugation, washing, and drying, the mixture was redispersed in acrylate monomers to obtain a dispersion with a solid content of 20-50%. Mixing is performed using a static mixer or a dynamic mixing head. The mixer length is 100–500 mm, the number of mixing units is 10–30, and the mixing pressure is 0.2–1.0 MPa.

[0011] Preferably, in step S3, the coating head is a slit coating head or a concave coating head, and the wet film thickness is 10-100 μm. The distance between the coating head and the substrate surface is 0.5–2 mm; The temperature of the coating liquid is controlled at 25-40℃, and the substrate tension is 50-200N during coating.

[0012] Preferably, in step S4, the UV curing area is irradiated with an LED-UV (ultraviolet light-emitting diode) lamp with a wavelength of 365nm or 395nm and an energy density of 800~2000mJ / cm². The UV curing area is protected by nitrogen gas with an oxygen concentration ≤200ppm. The temperature of the hot air micro-curing zone is 60-90℃, the processing time is 30-120 seconds, the hot air velocity is 1-5m / s, and the airflow direction is perpendicular to the substrate running direction. A transition zone is set between the UV curing zone and the hot air micro-curing zone. The length of the transition zone is 0.5 to 2 m, and the temperature is room temperature to 40°C.

[0013] Preferably, an online stretching and shaping step is included between step S4 and step S5: the cured film is stretched longitudinally and / or laterally by a stretching ratio of 1.1 to 1.5 times, and then heat-set at 80 to 120°C for 5 to 30 seconds, followed by cooling to room temperature.

[0014] Preferably, in step S5, the surface temperature of the cooling roller is 10-30℃, the winding tension is 80-300N, the winding speed is synchronized with the coating speed, and the error is ≤±0.5m / min.

[0015] Compared with the prior art, the beneficial effects of the present invention are: This invention fundamentally avoids the problem of sedimentation and agglomeration of nanofillers during coating storage. The filler is mixed with other components just before coating, ensuring the uniformity of coating composition and high surface quality, and eliminating defects such as uneven particle size and haze. This invention solves the risk of pre-crosslinking or gelation of coatings due to storage and transportation, and improves the stability and reliability of the production process because the coatings do not require long-term storage and can be used immediately after mixing. This invention enables the formation of a multifunctional integrated coating with a single coating, or the coating of a composite functional layer in one step by adjusting the mixed components, eliminating the need for multiple coating and drying processes, significantly improving production efficiency, and avoiding interlayer adhesion problems caused by multiple interface treatments. This invention employs a gentle online curing method, such as UV curing or low-temperature thermal curing, with a curing temperature far lower than the traditional process of over 120°C. This effectively prevents thermal shrinkage and deformation of the temperature-sensitive thermoplastic polyurethane (TPU) substrate, and broadens the application range of the process in high-end TPU film materials. Attached Figure Description

[0016] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings: Figure 1 This is a flowchart of the online polymerization integrated nano-coating method for applying the present invention to TPU / PET films. Detailed Implementation

[0017] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0018] like Figure 1 As shown, the method for applying an integrated online polymerized nano-coating to TPU / PET films includes: Step S1, Substrate Unwinding and Pretreatment: Unwind the TPU film or PET film roll and perform low-temperature plasma treatment on the substrate surface to improve the substrate surface energy and coating adhesion.

[0019] In this embodiment, low-temperature atmospheric pressure plasma treatment is used, with a treatment power of 500-2000W and a treatment speed of 5-30m / min. The surface energy of the substrate after treatment is ≥52dyn / cm. The working gas is nitrogen or a mixture of argon and air. The pretreatment equipment is set 1 to 3 m in front of the coating station, and the distance between the plasma electrode and the substrate surface is 5 to 20 mm.

[0020] By adopting the above technical solution, atmospheric pressure plasma treatment does not require vacuum equipment, is suitable for continuous production lines, and can effectively remove low molecular weight substances from the surface and introduce polar groups.

[0021] Step S2, online dynamic mixing of multi-component coatings: Component A, Component B and nanofiller dispersions are delivered through three independent liquid supply systems, and after precise metering by a metering pump, they are mixed uniformly online to form a polymerizable nanocomposite precursor.

[0022] In the examples, component A comprises acrylate monomers or oligomers, a photoinitiator, and a leveling agent; Component B contains a crosslinking agent and an adhesion promoter; The nanofiller dispersion contains one or more of the following: surface-modified nano silica, nano alumina, or nano titanium dioxide; The mass ratio of component A to component B is 100:2 to 15, and the amount of nanofiller dispersion added is 5 to 30% of the mass of component A.

[0023] In the examples, the acrylate monomers or oligomers of component A are one or more of polyurethane acrylate, epoxy acrylate, or polyester acrylate, with a functionality of 2 to 6; the photoinitiator is one or more of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, or diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

[0024] By employing the above technical solutions, high-functionality oligomers impart high crosslinking density and hardness to the coating, while the multi-component photoinitiator system ensures simultaneous curing of the deep and surface layers during UV curing. The amount of nanofiller added can be adjusted online to meet different functional requirements (high hardness, scratch resistance, self-healing, etc.).

[0025] In this embodiment, the preparation method of the nanofiller dispersion is as follows: The nanofiller and silane coupling agent were ultrasonically dispersed in an ethanol / water mixed solvent at a mass ratio of 100:3-10 for 2-4 hours. After centrifugation, washing, and drying, the mixture was redispersed in acrylate monomers to obtain a dispersion with a solid content of 20-50%. Mixing is performed using a static mixer or a dynamic mixing head. The mixer length is 100–500 mm, the number of mixing units is 10–30, and the mixing pressure is 0.2–1.0 MPa.

[0026] By adopting the above technical solution, the silane coupling agent modifies the surface of the nanofiller, improves its compatibility with the acrylate matrix, and avoids secondary agglomeration after online mixing.

[0027] Step S3, online polymerization coating: The polymerization precursor mixture obtained in step S2 is continuously coated onto the surface of the substrate treated in step S1 through a precision coating head to form a uniform wet film.

[0028] In the embodiments, the coating head is a slot coating head or a concave coating head, and the wet film thickness is 10-100 μm; The distance between the coating head and the substrate surface is 0.5–2 mm; The temperature of the coating liquid is controlled at 25-40℃, and the substrate tension is 50-200N during coating.

[0029] Step S4, online photo-thermal synergistic curing: The coated substrate is passed sequentially through the ultraviolet curing zone and the hot air micro-curing zone to achieve rapid cross-linking polymerization and post-curing of the coating, forming an integrated nanocomposite coating.

[0030] In the embodiment, the UV curing area is irradiated with LED-UV lamps with a wavelength of 365nm or 395nm and an energy density of 800-2000mJ / cm². The UV curing area is protected by nitrogen gas with an oxygen concentration of ≤200ppm. The number of LED-UV lamps is 2-6, arranged along the running direction of the substrate, and the power of each lamp is 8-20W / cm². The temperature of the hot air micro-curing zone is 60-90℃ (preferably 70-80℃), the processing time is 30-120 seconds (preferably 60-90 seconds), the hot air velocity is 1-5m / s, and the airflow direction is perpendicular to the substrate running direction. A transition zone is set between the UV curing zone and the hot air micro-curing zone. The length of the transition zone is 0.5 to 2 m, and the temperature is room temperature to 40°C.

[0031] By employing the above technical solutions, nitrogen protection suppresses the oxygen inhibition effect, ensuring complete surface curing, improving coating hardness and scratch resistance. Segmented irradiation by multiple LED-UV lamps controls curing heat release, preventing substrate overheating and deformation. Mild post-curing promotes the reaction between the crosslinking agent and the hydroxyl and carboxyl groups on the substrate surface, forming chemical bonds and significantly improving coating adhesion (reaching grade 0 using the cross-cut adhesion test). Rapid cooling in the cooling section prevents sticking during winding.

[0032] In this embodiment, an online stretching and shaping step is included between step S4 and step S5: the cured film is stretched longitudinally and / or laterally at a stretching ratio of 1.1 to 1.5 times, and then heat-set at 80 to 120°C for 5 to 30 seconds, followed by cooling to room temperature. Specifically, the cured film is stretched at a ratio of 1.1 to 1.5 times in a longitudinal stretching machine and at a ratio of 1.0 to 1.2 times in a transverse stretching machine at a stretching temperature of 80 to 100°C, and then heat-set (100 to 120°C, 10 to 30 seconds) and cooled.

[0033] By adopting the above technical solution, biaxial stretching can improve the orientation consistency between the coating and the substrate, reduce internal stress, and is suitable for PET substrates with high requirements for dimensional stability.

[0034] Step S5, Cooling and winding: After the cured composite film is cooled by cooling rollers, it is wound up under constant tension to obtain the finished roll material.

[0035] In this embodiment, the surface temperature of the cooling roller is 10–30°C, the winding tension is 80–300 N, the winding speed is synchronized with the coating speed, and the error is ≤ ±0.5 m / min.

[0036] In the embodiments, the thickness of the integrated nanocomposite coating is 5-40 μm, the coating hardness is ≥2H (pencil hardness), the adhesion is ≤1 grade (100-cross test), no cracks appear when the elongation at break on TPU substrate is ≥200%, and no cracks appear when folded on PET substrate. The coating has both hardness and flexibility, adapting to the high elongation characteristics of TPU film and the bending characteristics of PET film.

[0037] By adopting the above technical solutions, this process achieves online integration of "mixing-coating-curing," with each component of the coating mixed only seconds in advance, completely avoiding agglomeration and pre-crosslinking issues during storage. Low-temperature plasma pretreatment significantly improves the adhesion between the substrate and the coating. Photo-thermal synergistic curing utilizes rapid UV curing to avoid heat accumulation damage to the TPM substrate, while gentle post-heat treatment perfects the crosslinking density and nanofiller arrangement, forming a high-quality coating.

[0038] The present invention will be further described in detail below with reference to specific embodiments:

[0039] Example 1 An online polymerization integrated nanocoating method for coating TPU / PET films is used to prepare a high-hardness scratch-resistant coating on the surface of a TPU film (150 μm thick, 1200 mm wide).

[0040] Step S1, Substrate Unwinding and Pretreatment: The TPU film roll is mounted on the unwinder 1 and pulled at a speed of 20m / min. After passing through the plasma treatment zone 2, low-temperature atmospheric pressure plasma (power 1200W, nitrogen flow rate 50L / min, air flow rate 5L / min) is used, and the surface energy of the TPU is increased from 38dyn / cm to 56dyn / cm.

[0041] Step S2, Online Dynamic Mixing of Multi-Component Coatings: A component supply system 3 (containing 75 kg of polyurethane acrylate oligomer (functionality 4), 4 kg of 1-hydroxycyclohexylphenyl ketone (photoinitiator 184), 20 kg of isobornyl acrylate (reactive diluent), and 1 kg of leveling agent BYK-333); a component supply system 4 (containing 8 kg of trimethylolpropane triacrylate (crosslinking agent) and 2 kg of silane coupling agent KH560); and a nanofiller dispersion supply system 5 (containing 15 kg of surface-modified nano-silica (40 nm particle size, 30% solid content acrylate dispersion)). These components are respectively pumped by metering pump 6 at a flow rate ratio of A:B:nano-dispersion = 100:10:15 to a static mixer 7 (containing 6 mixing elements) and mixed online at 25°C to obtain a polymerization precursor mixture.

[0042] Step S3, Online Polymerization and Coating: The mixture is immediately delivered to the slit coating head 8 (coating gap 80μm) and coated on the TPM membrane surface, with a wet film thickness of 75μm and a coating width of 1150mm.

[0043] Step S4, Online Photo-Thermal Co-curing: After coating, the film enters the UV curing zone 9, which is protected by nitrogen (oxygen concentration 150ppm). Four LED-UV lamps (wavelength 395nm, single lamp power 12W / cm², total energy density approximately 1500mJ / cm²) are used for 5 seconds of irradiation, allowing the acrylate to rapidly crosslink and cure. It then enters the hot air micro-curing zone 10 (temperature 75℃, wind speed 10m / s, length 4m, processing time approximately 12 seconds) to promote the reaction between the crosslinking agent and silane coupling agent and the TPU surface-active groups. After exiting the curing zone, it is cooled to 25℃ by cooling rollers 11 (temperature 10℃).

[0044] Step S5, Cooling and Rewinding: After online thickness gauge and CCD defect detection, the rewinding machine 12 rewinds the product to obtain the finished product.

[0045] Coating performance testing: Coating thickness approximately 8μm, pencil hardness 3H, adhesion grade 0 (cross-cut test, 100% no peeling), haze 1.2%, light transmittance 91%. After stretching the coating film by 200%, the coating showed no cracks or peeling. No visible scratches were observed after steel wool abrasion (1kg load, 10 cycles).

[0046] Example 2 The difference from Example 1 is as follows: the substrate is a PET film (100 μm thick, 1500 mm wide), and the coating speed is 30 m / min. Component A is replaced with an epoxy acrylate oligomer (functionality 6), and the amount of nanofiller added is 25% of the mass of component A (a mixture of nano-alumina and nano-titanium dioxide). The coating thickness is 12 μm, the hardness is 4H, the adhesion is grade 0, and the coating shows no cracks after the PET film is folded 180°.

[0047] Example 3 The difference from Example 1 is the addition of an online stretching and setting step. After curing, the film enters a longitudinal stretching machine (stretch ratio 1.2 times, temperature 85°C) and a transverse stretching machine (stretch ratio 1.05 times, temperature 90°C), and is then heat-set at 110°C for 20 seconds. The coating surface is smoother, the haze decreases from 1.2% to 0.9%, and the dimensional heat shrinkage rate (150°C, 30 minutes) decreases from 0.8% to 0.3%.

[0048] Comparative Example 1 (Offline Premixed Coating) The same coating formulation as in Example 1 was used, but A, B, and nanofillers were pre-mixed in a mixing tank for 2 hours and left to stand for 24 hours before use. The coating process was the same (using the same equipment). Results: Slight flocculation occurred in the coating, and visible microparticles appeared on the surface of the coating after coating. The haze increased to 3.5%, the adhesion decreased to level 2 (partial peeling), and the hardness decreased to 2H.

[0049] Comparative Example 2 (Single UV Curing) The difference from Example 1 is that the hot air micro-curing zone was omitted, and only UV curing (with the same energy) was used. The initial coating hardness was 2H, and the adhesion was grade 2 (edge ​​peeling in the cross-cut adhesion test). After aging the coating film at 80°C for 72 hours, the adhesion dropped to grade 3, and the coating edges began to peel. This indicates that post-heat curing is crucial for chemical bonding and aging resistance.

[0050] Implementation Principles The online polymerization integrated method of this invention completes the polymerization reaction instantaneously from the storage tank to the coating head, completely avoiding problems such as agglomeration, sedimentation, and pre-crosslinking of nano-coatings during storage and transportation. Its core technology lies in: ① Plasma activation of the substrate introduces polar groups (-OH, -COOH, etc.), providing reaction sites for subsequent chemical bonding; ② Online dynamic mixing of multi-component materials ensures that the polymerization precursor is fresh and uniform; ③ Photo-thermal synergistic curing: UV light rapidly initiates cross-linking of acrylate to form a framework, and thermal curing promotes the chemical bonding of cross-linking agents and coupling agents with the substrate surface. At the same time, the nanofillers are more firmly anchored after micro-movement in the thermal field. ④ The entire process is carried out under low tension and low temperature to protect the heat sensitivity of the TPU / PET substrate. This process is particularly suitable for the continuous production of high-value-added functional films, and the coating performance is superior to the traditional offline premixing + single oven curing process.

[0051] Finally, it should be noted that the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for online polymerization and integrated nano-coating on TPU / PET films, characterized in that, include: Step S1, Substrate unwinding and pretreatment: Unwind the TPU film or PET film roll and perform low-temperature plasma treatment on the substrate surface; Step S2, online dynamic mixing of multi-component coatings: Component A, Component B and nanofiller dispersions are delivered through three independent liquid supply systems, and after precise metering by metering pumps, they are mixed uniformly online to form a polymerizable nanocomposite precursor; Step S3, online polymerization coating: The polymerization precursor mixture obtained in step S2 is continuously coated onto the substrate surface after step S1 through a precision coating head to form a uniform wet film. Step S4, online photo-thermal synergistic curing: The coated substrate is passed sequentially through the ultraviolet curing zone and the hot air micro-curing zone to achieve rapid cross-linking polymerization and post-curing of the coating, forming an integrated nanocomposite coating; Step S5, Cooling and winding: After the cured composite film is cooled by cooling rollers, it is wound up under constant tension to obtain the finished roll material.

2. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S1, low-temperature atmospheric pressure plasma treatment is used, with a treatment power of 500-2000W and a treatment speed of 5-30m / min. The surface energy of the substrate after treatment is ≥52dyn / cm. The pretreatment equipment is set 1 to 3 m in front of the coating station, and the distance between the plasma electrode and the substrate surface is 5 to 20 mm.

3. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S2, component A contains acrylate monomers or oligomers, photoinitiators, and leveling agents; Component B contains a crosslinking agent and an adhesion promoter; The nanofiller dispersion contains one or more of the following: surface-modified nano silica, nano alumina, or nano titanium dioxide; The mass ratio of component A to component B is 100:2 to 15, and the amount of nanofiller dispersion added is 5 to 30% of the mass of component A.

4. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S2, the acrylate monomers or oligomers of component A are one or more of polyurethane acrylate, epoxy acrylate, or polyester acrylate, with a functionality of 2 to 6; the photoinitiator is one or more of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, or diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide.

5. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S2, the preparation method of the nanofiller dispersion is as follows: The nanofiller and silane coupling agent were ultrasonically dispersed in an ethanol / water mixed solvent at a mass ratio of 100:3-10 for 2-4 hours. After centrifugation, washing, and drying, the mixture was redispersed in acrylate monomers to obtain a dispersion with a solid content of 20-50%. Mixing is performed using a static mixer or a dynamic mixing head. The mixer length is 100–500 mm, the number of mixing units is 10–30, and the mixing pressure is 0.2–1.0 MPa.

6. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S3, the coating head is a slot coating head or a concave coating head, and the wet film thickness is 10-100 μm. The distance between the coating head and the substrate surface is 0.5–2 mm; The temperature of the coating liquid is controlled at 25-40℃, and the substrate tension is 50-200N during coating.

7. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S4, the UV curing area is irradiated with an LED-UV lamp with a wavelength of 365nm or 395nm and an energy density of 800~2000mJ / cm². The UV curing area is protected by nitrogen gas with an oxygen concentration ≤200ppm. The temperature of the hot air micro-curing zone is 60-90℃, the processing time is 30-120 seconds, the hot air velocity is 1-5m / s, and the airflow direction is perpendicular to the substrate running direction. A transition zone is set between the UV curing zone and the hot air micro-curing zone. The length of the transition zone is 0.5 to 2 m, and the temperature is room temperature to 40°C.

8. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, Between steps S4 and S5, there is also an online stretching and shaping step: the cured film is stretched longitudinally and / or laterally by a stretching ratio of 1.1 to 1.5 times, and then heat-set at 80 to 120°C for 5 to 30 seconds, followed by cooling to room temperature.

9. The method for online polymerization and integrated nano-coating on TPU / PET films according to claim 1, characterized in that, In step S5, the surface temperature of the cooling roller is 10-30℃, the winding tension is 80-300N, the winding speed is synchronized with the coating speed, and the error is ≤±0.5m / min.