Air conditioner fin high lubrication function coating aluminum foil precision coating process

By employing a multi-stage convection oven drying process and chemical cross-linking technology, the thermodynamic incompatibility problem of air conditioner coatings during the drying and film formation process was solved. This ensured the stability of the hydrophilicity and lubrication properties of the air conditioner heat sink coating, avoided surface agglomeration and penetration defects, and improved long-term service performance.

CN123149136APending Publication Date: 2026-11-24JIANGSU ALCHA ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611378846.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing hydrophilic coatings for air conditioners exhibit thermodynamic incompatibility in their multiphase systems during the drying and film-forming process. Hydrophobic lubricating components are prone to Oswald curing and migration to the coating surface, leading to macroscopic wax precipitation and loss of hydrophilicity. Meanwhile, conventional rapid heating curing processes cause premature gelation and skin formation on the coating surface, hindering the drainage of internal moisture, resulting in water boiling and penetrating pinhole defects. Furthermore, small molecule lubricants are easily dissolved and lost under long-term condensation.

Method used

A multi-stage convection oven drying process is adopted, which uses ammonia flash evaporation and competitive chelation reaction to delay exhaust to form a latent system. Combined with the competitive chelation of acetylacetone and tetravalent zirconium ions, the crosslinking reaction is delayed. Then, asynchronous covalent crosslinking and lubricant chemical anchoring are carried out to construct an interpenetrating polymer network, which fixes oxidized polyethylene wax particles inside the polymer matrix to ensure the hydrophilicity and lubrication properties of the coating.

Benefits of technology

This invention achieves coupling of hydrodynamic parameters and coordination chemical reaction kinetics in the coating of air conditioner heat sink, prevents aggregation on the surface of hydrophobic wax layer, eliminates penetrating pinhole defects, maintains the hydrophilic condensation drainage function of the coating, and improves long-term lubrication durability and reduces dynamic frictional resistance through chemical anchoring structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149136A_ABST
    Figure CN123149136A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal surface treatment technology and discloses a precision coating process for aluminum foil with a high lubricity function for air conditioner heat sinks. The process includes: preparing a coating solution containing polyacrylic acid, aliphatic waterborne epoxy resin, zirconium carbonate ammonium, acetylacetone, ammonia, N,N-dimethylethanolamine, polytetrahydrofuran ether diol, and oxidized polyethylene wax microemulsion; applying the coating solution to the pretreated aluminum foil surface; and passing the aluminum foil through a multi-stage convection oven for gradient curing: in zone one, high-speed ammonia flash evaporation triggers the dissociation of zirconium carbonate ammonium and delayed crosslinking and degassing via competitive chelation by acetylacetone; in zone two, acetylacetone volatilization dechelates the chelation, zirconium ions crosslink with polyacrylic acid, and physically lock the polyethylene wax particles; in zones three and four, covalent crosslinking and chemical anchoring of polytetrahydrofuran ether diol occur; and finally, cooling and winding. This invention eliminates pinholes caused by boiling water in the coating film, prevents surface wax precipitation to maintain hydrophilicity, and improves lubrication durability against water erosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal surface treatment technology, specifically to a precision coating process for aluminum foil with high lubrication function for air conditioner heat sinks. Background Technology

[0002] Modern air conditioner heat sinks require high-speed stamping during manufacturing, which places demands on the stamping lubrication performance of the hydrophilic aluminum foil surface coating. Currently, industrial production typically uses polyacrylic acid as the main resin, combined with crosslinking agents such as water-based epoxy resin and polyethylene wax microemulsion as lubricating agents to formulate water-based coatings. These coatings are then applied to the surface of the aluminum foil substrate using a roller coating process and subsequently crosslinked into a film through high-temperature convection baking.

[0003] To meet the drag reduction requirements of high-speed stamping dies, conventional processes often increase the content of hydrophobic wax components in the coating formulation. However, due to the significant thermodynamic polarity difference between the hydrophilic polyacrylic matrix and the hydrophobic polyethylene wax, the moisture in the coating evaporates rapidly during oven drying, resulting in a low-viscosity state before cross-linking and curing. At this time, driven by changes in the system's surface free energy, the hydrophobic wax particles easily migrate to the gas-liquid interface and aggregate and precipitate on the coating surface. The resulting hydrophobic wax layer covers the underlying polar groups, causing the finished aluminum foil to lose its original hydrophilic and water-repellent properties.

[0004] In actual production control, attempting to accelerate polymer crosslinking by directly increasing the temperature or airflow rate during the initial drying stage of the oven, in order to prematurely solidify the matrix and limit the migration of wax particles, will lead to mass transfer resistance problems. Excessively rapid surface crosslinking reactions cause premature gelation and skin formation on the coating surface, blocking the fluid venting channels within the coating film. Residual moisture that has not been dried in the underlying layer expands and vaporizes upon heating, and the vapor pressure forcibly breaks through the surface skin, generating numerous boiling bubbles and penetrating pinhole defects on the coating surface, thus damaging the integrity and smoothness of the coating.

[0005] In addition, some technical solutions improve stamping friction resistance by adding free liquid small-molecule polyether lubricants to the coating. These lubricants exist in the cross-linked network in the form of physical blends. During the long-term operation of air conditioning equipment, the condensate on the surface of the heat sink will continuously wash the coating, causing the unfixed hydrophilic small-molecule lubricants to be continuously extracted and washed away, resulting in a gradual decline in the long-term lubrication performance of the coating. Summary of the Invention

[0006] The technical problem solved by this invention is that existing hydrophilic coatings for air conditioners have thermodynamic incompatibility in the multiphase system during the drying and film formation process. The hydrophobic lubricating components are prone to Oswald curing and migration and aggregation to the coating surface, resulting in macroscopic wax precipitation and loss of hydrophilicity. At the same time, conventional rapid heating curing process causes premature gelation and skin formation on the coating surface, which hinders the drainage of internal moisture, causes water boiling and penetrating pinhole defects, and small molecule lubricants are easily dissolved and lost under long-term condensation.

[0007] To address the above problems, the present invention provides the following technical solution: This invention provides a precision coating process for aluminum foil with high lubricity function for air conditioner heat sinks, employing the following technical solution: A precision coating process for high-lubricity aluminum foil coating on air conditioner heat sinks includes the following steps: A coating solution comprising an aqueous polyacrylic acid solution, an aliphatic waterborne epoxy resin, ammonium zirconium carbonate, acetylacetone, ammonia, N,N-dimethylethanolamine, polytetrahydrofuran ether diol, oxidized polyethylene wax microemulsion, and deionized water is prepared. During preparation, the aqueous polyacrylic acid solution and the aliphatic waterborne epoxy resin are mixed, and ammonia is added to adjust the pH of the system to alkaline. Then, ammonium zirconium carbonate and acetylacetone are added to form a latent system, and the remaining components are added and mixed thoroughly to obtain the coating solution. A three-roller coating machine is used to apply the coating liquid to the surface of the degreased and passivated aluminum foil. The aluminum foil is continuously passed through multiple convection ovens, sequentially experiencing: The temperature in one zone of the multi-section convection oven is set to 80 to 95°C, and the convection hot air velocity is 20 to 30 m / s. The temperature in the second zone of the multi-section convection oven is set at 110 to 130°C, and the convection hot air velocity is set at 10 to 18 m / s. The temperature in zones three and four of the multi-section convection oven is set to 160 to 220°C, and the hot air velocity is 5 to 10 m / s. The aluminum foil is wound up under tension after exiting the multi-section convection oven.

[0008] By adopting the above technical solution, the following technical effects are achieved: This process couples fluid dynamics parameters with coordination chemical reaction kinetics, realizing a rheological phase change locking mechanism in a multi-stage convection drying process. The reaction mechanism is explained step-by-step according to the curing process stages as follows: The first step involves flash evaporation of ammonia and competitive chelation followed by delayed exhaust. Aluminum foil enters Zone 1, where an ambient temperature of 80-95°C and high-speed convective hot air at 20-30 m / s break the mass transfer boundary layer at the gas-liquid interface of the coating, causing flash evaporation of ammonia on the coating surface. This results in a sharp drop in the system's pH, disrupting the thermodynamic equilibrium of ammonium zirconium carbonate and causing it to dissociate and release tetravalent zirconium ions. At this point, pre-placed acetylacetone preferentially binds to and occupies the coordination sites of the tetravalent zirconium ions due to its bidentate coordination structure, undergoing a competitive chelation reaction to generate a temporary complex and release protons. The formation of this temporary complex delays the crosslinking process between the tetravalent zirconium ions and the carboxyl groups of polyacrylic acid, inhibiting early gelation on the coating surface and maintaining microscopic fluid open channels within the coating. Deep moisture diffuses out to the gas-liquid interface through the concentration gradient, eliminating boiling bubbles and penetrating pinhole defects caused by thermal vaporization of moisture.

[0009] The second step involves the dissociation of the complex and the locking of the rheological phase transition. As the coating progresses to zone two, the moisture is largely eliminated, and acetylacetone evaporates rapidly upon heating, dissolving the temporary competitive coordination. The exposed tetravalent zirconium ions immediately undergo polydentate coordination crosslinking with the carboxyl groups on the polyacrylic acid molecular chains, forming a crosslinked network. The apparent viscosity of the coating system increases nonlinearly with the advancement of the crosslinking reaction, rapidly surpassing the rheological gel point. The dense three-dimensional coordination network generates corresponding physical steric hindrance, blocking the mass transfer path of the oxidized polyethylene wax particles outward, fixing the oxidized polyethylene wax particles within the polymer matrix, and preventing Oswald curing and surface aggregation of the polyethylene wax. No continuous hydrophobic wax layer is formed on the surface; the polar hydrophilic groups of the polyacrylic acid are orderly arranged at the contact surface, maintaining the macroscopic hydrophilic and water-repellent function of the finished coating.

[0010] The third step involves asynchronous covalent crosslinking and lubricant chemical anchoring. As the coating progresses to zones three and four, the high-boiling-point N,N-dimethylethanolamine slowly volatilizes, catalyzing the ring-opening esterification reaction between the epoxy groups of the aliphatic waterborne epoxy resin and the residual carboxyl groups of polyacrylic acid. The newly formed covalent network intertwines with the previously constructed zirconium ion coordination network, forming an interpenetrating polymer network. The terminal hydroxyl groups of the polytetrahydrofuran ether diol within the system form coordination bonds and hydrogen bonds with the empty orbitals of zirconium ions and the polar groups of the network. The polytetrahydrofuran ether diol is chemically anchored to the polymer network, and the flexible polyether segments accumulate on the coating surface, providing a hydrodynamic lubricating film. This anchoring structure resists phase migration and dissolution extraction of small-molecule lubricants under long-term external water erosion. When the coating is subjected to extreme pressure loads of impact friction, elastic deformation occurs, and the internally embedded oxidized polyethylene wax solid particles are exposed in situ, providing boundary lubrication. The dual load-bearing structure of hydrodynamic lubrication and solid boundary lubrication synergistically reduces dynamic frictional resistance.

[0011] Preferably, the coating liquid is made from raw materials comprising the following parts by weight: An aqueous solution of polyacrylic acid, in parts by weight of effective solids, is 40.0 to 60.0 parts. Aliphatic waterborne epoxy resin, 10.0 to 20.0 parts by weight of effective solid content; ammonium zirconium carbonate, based on effective solid content by mass, is 2.0 to 6.0 parts; Polytetrahydrofuran ether diol, based on effective solid content, 3.0 to 8.0 parts by weight; Oxidized polyethylene wax microemulsion, 5.0 to 12.0 parts by weight of effective solid content; Ammonia water, with a mass fraction of 20% to 25%, or 5.0 to 10.0 parts by actual physical mass; Acetylacetone, 1.0 to 4.0 parts by actual physical mass; N,N-Dimethylethanolamine, 2.0 to 5.0 parts by actual physical mass; Deionized water, by actual physical mass parts, 30.0 to 50.0 parts.

[0012] By employing the above technical solution, a specific mass ratio defines the thermodynamic compatibility boundary of the multi-component system. The mass percentage range of acetylacetone ensures that the system has a sufficient amount of bidentate chelating ligands during decomplexation, allowing the time window of the kinetic delay phase to match the time required for fluid physical degassing.

[0013] Preferably, the coating liquid is made from raw materials comprising the following parts by weight: 50.0 parts by weight of polyacrylic acid aqueous solution, based on effective solid content; Aliphatic waterborne epoxy resin, based on effective solid content by weight, 15.0 parts; ammonium zirconium carbonate, based on effective solid content by mass, 4.0 parts; Polytetrahydrofuran ether diol, based on effective solid content by weight, 5.5 parts; Oxidized polyethylene wax microemulsion, based on effective solid content by weight, 8.5 parts; Ammonia solution, with a mass fraction of 22.5%, is 7.5 parts by actual physical mass. Acetylacetone, 2.5 parts by actual physical mass; N,N-Dimethylethanolamine, 3.5 parts by actual physical mass; Deionized water, 40.0 parts by actual physical mass.

[0014] By adopting the above technical solution, a precise point ratio provides a balanced activation energy benchmark. Excessive waterborne epoxy resin excessively consumes free carboxyl groups, leading to a decrease in hydrophilicity, while excessive polyethylene wax exceeds the retention limit of the coordination network's steric hindrance, causing secondary precipitation. This ratio effectively balances the coating's hydrophilicity and anti-friction and wear properties.

[0015] Preferably, the number-average molecular weight of the polyacrylic acid aqueous solution is between 30,000 and 50,000, and the polyacrylic acid aqueous solution is prepared by the following steps: Under constant temperature conditions of heating in a water bath at 80 to 85°C, an initiator solution prepared by dissolving acrylic acid aqueous solution and ammonium persulfate is simultaneously added dropwise to deionized water that has been deoxygenated by purging with nitrogen. The dropping rate is controlled so that the dropping process is completed within 2.5 to 3.5 hours. Subsequently, the system temperature is raised to 90 to 95°C and the reaction is maintained for 1.5 to 2.0 hours.

[0016] By employing the above technical solution, the isothermal dripping and heat preservation curing processes control the free radical polymerization rate, ensuring that the final polymer molecular weight distribution is concentrated within the target range. Polyacrylic acid molecular chains with a molecular weight between 30,000 and 50,000 exhibit a suitable extended conformation in the room-temperature coating solution to guarantee coating leveling, while simultaneously providing a three-dimensional steric hindrance framework with sufficient mesh strength during crosslinking.

[0017] Preferably, the aliphatic waterborne epoxy resin is sorbitol polyglycidyl ether.

[0018] By employing the above technical solution, sorbitol polyglycidyl ether possesses a multifunctional structure, serving as a crosslinking bridge to connect residual carboxyl groups of polyacrylic acid during the covalent crosslinking stage in the high-temperature region. The high-density aliphatic ether bond architecture enhances the structural compactness of the crosslinking network while maintaining the flexible deformation capability of the coating substrate.

[0019] Preferably, the number average molecular weight of polytetrahydrofuran ether diol is between 1,000 and 2,000.

[0020] By employing the above technical solution, the defined molecular chain segment lengths balance the fluidity of the liquid at room temperature with the entanglement between polymer chains. After undergoing single-end chemical anchoring, the remaining flexible long chains of polyether molecules within the specified molecular weight range still possess sufficient degrees of freedom to extend at the frictional solid-liquid interface, forming a smooth and continuous drag-reducing fluid film.

[0021] Preferably, in the step of preparing the coating solution comprising an aqueous polyacrylic acid solution, an aliphatic waterborne epoxy resin, ammonium zirconium carbonate, acetylacetone, ammonia, N,N-dimethylethanolamine, polytetrahydrofuran ether glycol, oxidized polyethylene wax microemulsion, and deionized water, the preparation specifically includes: mixing the aqueous polyacrylic acid solution and the aliphatic waterborne epoxy resin, adding ammonia to adjust the pH of the system to alkaline, then adding ammonium zirconium carbonate and acetylacetone to form a latent system, and finally adding the remaining components and mixing thoroughly to obtain the coating solution. Aqueous polyacrylic acid, aliphatic waterborne epoxy resin and deionized water were mixed in a stirred tank. Ammonia was slowly added dropwise at 20 to 30°C to adjust and stabilize the pH of the system between 9.5 and 10.5. Slowly add an aqueous solution of zirconium carbonate to the adjusted high pH system and stir, then add acetylacetone and continue stirring; N,N-dimethylethanolamine, polytetrahydrofuran ether diol, and oxidized polyethylene wax microemulsion were added sequentially and dispersed at high speed at 800 to 1200 rpm for 30 to 45 minutes, followed by filtration to obtain the coating solution.

[0022] By adopting the above technical solution, the feeding sequence is standardized to eliminate early side reactions between components. First, a strongly alkaline buffer system is established to maintain the complexed stability of ammonium zirconium carbonate, and then acetylacetone is introduced for uniform dispersion. This feeding sequence prevents the inorganic crosslinking agent from prematurely releasing polyvalent metal ions, which could cause local flocculation of the polymer emulsion, thus ensuring the long-term storage stability of the functional coating.

[0023] Preferably, the step of applying the coating liquid to the surface of the degreased and passivated aluminum foil using a three-roll coater specifically includes: Adjust the gap between the coating rollers of the three-roll coating machine to control the dry film coating weight at 1.5 g / m². 2 Up to 2.5g / m 2 between.

[0024] By adopting the above technical solution, the dry film thickness of the coating is controlled. This thickness range ensures that the coating has a matching thermal conductivity during the heat treatment process, avoiding both excessively thick film layers that accumulate internal stress and cause brittle cracking, and excessively thin film layers that cannot accommodate oxidized polyethylene wax particles, leading to microscopic coating failure.

[0025] Preferably, in a multi-stage convection oven: The residence time of the aluminum foil in one zone of the multi-section convection oven is 1.5 to 3.0 seconds; The residence time of the aluminum foil in the second zone of the multi-section convection oven is 3.0 to 5.0 seconds; The total residence time in the three and four zones of the multi-section convection oven is 8.0 to 15.0 s.

[0026] By adopting the above technical solution, the transmission parameters of the physical equipment are matched to the activation energy accumulation requirements of the chemical reaction. The short-duration thermal shock in Zone 1 distinguishes the deammoniation and degassing process from the gelation process, and the step-wise extended residence time in subsequent temperature zones promotes the complete completion of the thermosetting esterification reaction, preventing insufficient crosslinking from causing hydration and expansion of the film layer.

[0027] Preferably, the step of winding the aluminum foil under tension after it exits the multi-segment convection oven specifically includes: After the aluminum foil exits the multi-section convection oven, it is cooled to below 40°C within 2 seconds by a cold air array at a temperature of 15 to 25°C, and then wound up under a tension of 150 to 250N.

[0028] By employing the above technical solution, the rapid convection of cold air with a large temperature difference terminates the thermal motion of the polymer chain segments inside the coating, causing the coating film in a rubbery state to undergo an instantaneous glass transition. Constant tension controls the tight stacking of the roll material, and this cold-state winding combination prevents thermal adhesion between coating layers, ensuring the geometric integrity of the surface lubrication structure.

[0029] This invention provides a precision coating process for aluminum foil with a high lubricity function for air conditioner heat sinks. It offers the following advantages: 1. This invention promotes the rapid evaporation of ammonia on the coating surface by setting high wind speed and high temperature conditions in the first zone of the convection oven, which triggers the dissociation of ammonium zirconium carbonate. At the same time, the acetylacetone in the formula competes with the dissociated tetravalent zirconium ions for chelation, which delays the crosslinking reaction between zirconium ions and polyacrylic acid. This method maintains the internal fluid mass transfer channel in the early stage of coating drying, allowing deep moisture to diffuse outward and be discharged smoothly, preventing premature skinning of the coating surface and internal moisture boiling, and eliminating through-hole defects on the surface of the finished product.

[0030] 2. This invention utilizes the property of acetylacetone volatilizing and releasing the coordination effect when heated in the second zone of the oven, so that tetravalent zirconium ions and polyacrylic acid molecular chains can quickly coordinate and crosslink, resulting in a nonlinear increase in the apparent viscosity of the coating film. The crosslinked network formed by curing blocks the migration path of oxidized polyethylene wax particles to the coating surface through physical steric hindrance, fixing them inside the polymer matrix. This rheological phase change locking process avoids the formation of a continuous hydrophobic wax layer on the surface, allowing the hydrophilic groups of polyacrylic acid to be normally arranged at the contact surface, thus ensuring the initial hydrophilic properties of the coating.

[0031] 3. In the high-temperature region, this invention constructs an interpenetrating network through covalent cross-linking of epoxy resin and polyacrylic acid, and chemically anchors polytetrahydrofuran ether diol to zirconium ions through terminal hydroxyl groups. Under frictional pressure, the polyether segments enriched on the surface provide fluid lubrication, while the internally fixed polyethylene wax microparticles are exposed to provide boundary lubrication. The two work together to reduce the dynamic coefficient of friction. In addition, the chemically anchored structure effectively resists the leaching and extraction of small molecule lubricants by air conditioning condensate, improving the lubrication durability of the coating during long-term service. Attached Figure Description

[0032] Figure 1 This is a comparison curve of the dynamic changes in the energy storage modulus of the coating liquids in Example 2 and Comparative Example 2 under isothermal time scanning. Figure 2 This is a line graph comparing the dynamic changes of pH on the coating surface during the film-forming and drying process of Example 2 and Comparative Example 3 of the present invention. Detailed Implementation

[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings, preparation examples, embodiments, comparative examples, and test examples. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] Preparation Example 1: This preparation example provides a method for preparing a low molecular weight and low solid content aqueous solution of polyacrylic acid (PAA) (denoted as PAA-1). To obtain a lower molecular weight, a higher polymerization temperature and a higher proportion of initiator are used, including the following steps: (1) Preparation and heating: Add 310.0g of deionized water to a four-necked flask equipped with a mechanical stirrer, reflux condenser, double dropping funnel and thermometer, start stirring, and purge with 99.9% pure nitrogen for 20 minutes to remove oxygen. Then heat the system in a water bath and keep it at 85°C.

[0035] (2) Preparation of initiator: Weigh 3.75g of ammonium persulfate (APS, which is 1.5% of the mass of acrylic acid monomer), dissolve it completely in 75.0g of deionized water, and prepare an initiator solution.

[0036] (3) Monomer preparation and addition: Weigh 250.0g of acrylic acid (AA) monomer and mix it evenly with 376.25g of deionized water. Under constant temperature of 85℃ and stirring at 150rpm, simultaneously add the acrylic acid aqueous solution and initiator solution to the flask using a double dropping funnel. Control the dropping rate so that the dropping process is completed within 2.5h.

[0037] (4) Heat preservation and ripening: After the addition is complete, the system temperature is raised to 95°C and the reaction is kept at this temperature for 1.5 hours to fully consume the residual monomer.

[0038] (5) Cooling and discharging: Stop heating and wait for the system to cool down naturally to below 40°C before filtering and discharging through a 200-mesh filter.

[0039] Material accounting: The total feed amount is 1015.0g, of which the total effective solids are 253.75g. The resulting transparent polyacrylic acid aqueous solution PAA-1 has a solids content of approximately 25.0% and a determined number-average molecular weight (Mn) of approximately 30,000.

[0040] Preparation Example 2: This preparation example provides a method for preparing a polyacrylic acid (PAA) aqueous solution (denoted as PAA-2) with a medium molecular weight and optimal solid content, supported by preferred parameters, and includes the following steps: (1) Preparing the base and raising the temperature: Add 280.0g of deionized water to the above four-necked flask, purge with nitrogen to remove oxygen for 25min, and then heat in a water bath to keep the system at a constant temperature of 82℃.

[0041] (2) Preparation of initiator: Weigh 3.0g of ammonium persulfate (APS, which is 1.0% of the mass of acrylic acid monomer), dissolve it completely in 70.0g of deionized water, and prepare an initiator solution.

[0042] (3) Monomer preparation and addition: Weigh 300.0g of acrylic acid (AA) monomer and mix it evenly with 357.0g of deionized water. Under constant temperature of 82℃ and stirring at 180rpm, simultaneously add the acrylic acid aqueous solution and the initiator solution. The addition process should be completed within 3.0h.

[0043] (4) Heat preservation and ripening: After the addition is complete, the temperature is raised to 92℃ and the reaction is kept at this temperature for 1.7h.

[0044] (5) Cooling and discharging: Cool down to below 40℃ and filter and discharge.

[0045] Material accounting: The total feed amount is 1010.0g, of which the total effective solids are 303.0g. The resulting polyacrylic acid aqueous solution PAA-2 has a solids content of approximately 30.0%, and the determined number average molecular weight (Mn) is approximately 40000.

[0046] Preparation Example 3: This preparation example provides a method for preparing a high molecular weight and high solids content aqueous solution of polyacrylic acid (PAA) (denoted as PAA-3). To obtain a higher molecular weight, a lower polymerization temperature and a lower proportion of initiator are used, including the following steps: (1) Preparing the base and raising the temperature: Add 260.0g of deionized water to the above four-necked flask, purge with nitrogen to remove oxygen for 30 minutes, and then heat in a water bath to keep the system at a constant temperature of 80℃.

[0047] (2) Preparation of initiator: Weigh 1.75g ​​of ammonium persulfate (APS, which is 0.5% of the mass of acrylic acid monomer), dissolve it completely in 65.0g of deionized water, and prepare an initiator solution.

[0048] (3) Monomer preparation and addition: Weigh 350.0g of acrylic acid (AA) monomer and mix it evenly with 328.25g of deionized water. Under constant temperature of 80℃ and stirring at 200rpm, simultaneously add the acrylic acid aqueous solution and the initiator solution. The addition process should be completed within 3.5h.

[0049] (4) Heat preservation and ripening: After the addition is complete, the temperature is raised to 90℃ and the reaction is kept at this temperature for 2.0h.

[0050] (5) Cooling and discharging: Cool down to below 40℃ and filter and discharge.

[0051] Material accounting: The total feed amount is 1005.0g, of which the total effective solids amount is 351.75g. The resulting polyacrylic acid aqueous solution PAA-3 has a solids content of approximately 35.0%, and the determined number average molecular weight (Mn) is approximately 50,000.

[0052] Example 1: This embodiment provides a precision coating process for high-lubricity aluminum foil coating on air conditioner heat sinks, including the following steps: Formulation instructions: Resin and microemulsion components (PAA, waterborne epoxy, ZAC, PTMEG, PE wax) are based on effective solids content by mass; ammonia, DMEA, ACAC, and deionized water are based on actual physical mass. The process includes the following steps: (1) Strong alkali pretreatment: Add 40.0 parts of the PAA-1 aqueous solution obtained in Preparation Example 1, 10.0 parts of aliphatic waterborne epoxy resin (sorbitol polyglycidyl ether, EEW=160) and 30.0 parts of deionized water to a stirred tank. Under stirring at 200 rpm and 20°C, slowly add 5.0 parts of ammonia water (20% by mass) to adjust and stabilize the pH of the system at 9.5, and maintain stirring for 15 min.

[0053] (2) Establishment of the latent system: In the above high pH system, 2.0 parts of zirconium carbonate (ZAC) aqueous solution were slowly added and stirred for 10 min; then 1.0 parts of acetylacetone (ACAC, providing a sufficient molar ratio of competing chelating groups) were added and stirred for another 10 min to form a temporary complex equilibrium.

[0054] (3) Compounding and homogenization: 2.0 parts of N,N-dimethylethanolamine (DMEA), 3.0 parts of polytetrahydrofuran ether diol (PTMEG, Mn=1000) and 5.0 parts of oxidized polyethylene wax microemulsion were added sequentially. The mixture was dispersed at 800 rpm for 30 min and then filtered through a 200-mesh filtration to obtain the coating solution.

[0055] (4) Substrate coating: The coating liquid is applied to the surface of the degreased and passivated aluminum foil using a three-roll coater. The gap between the coating rollers is adjusted to control the dry film coating weight at 1.5 g / m². 2 .

[0056] (5) Gradient phase change curing: Zone 1: Set temperature 80℃, convective hot air velocity 20m / s, aluminum foil residence time 1.5s (triggering ammonia flash evaporation and ACAC delayed exhaust).

[0057] Zone 2: Set temperature 110℃, convective hot air velocity 10m / s, aluminum foil residence time 3.0s (ACAC volatilization dechelation, triggering Zr)4+ (Rapid cross-linking and physical locking).

[0058] Zone 3: Set temperature 160℃, hot air velocity 5m / s; Zone 4: Set temperature 190℃, hot air velocity 5m / s. The total residence time of the aluminum foil in Zones 3 and 4 is 8.0s.

[0059] (6) Cooling and winding: After exiting the oven, the temperature is cooled to below 40°C within 2 seconds by a 15°C cold air array, and then wound up under a tension of 150N.

[0060] Example 2: This embodiment provides a precision coating process for high-lubricity aluminum foil coating on air conditioner heat sinks, including the following steps: (1) Strong alkali pretreatment: 50.0 parts of the PAA-2 aqueous solution obtained in Preparation Example 2, 15.0 parts of aliphatic waterborne epoxy resin and 40.0 parts of deionized water were added to a stirred tank. Under stirring at 250 rpm and 25°C, 7.5 parts of ammonia water (mass fraction 22.5%) were slowly added dropwise to adjust and stabilize the pH of the system at 10.0, and stirring was maintained for 18 min.

[0061] (2) Establishment of the latent system: In the above system, 4.0 parts of zirconium carbonate (ZAC) were slowly added and stirred for 12 min; then 2.5 parts of acetylacetone (ACAC) were added and stirred for another 12 min.

[0062] (3) Compounding and homogenization: 3.5 parts DMEA, 5.5 parts PTMEG (Mn=1500) and 8.5 parts oxidized polyethylene wax microemulsion were added sequentially. The mixture was dispersed at 1000 rpm for 40 minutes and filtered through a 250-mesh filter to obtain the coating solution.

[0063] (4) Substrate coating: A three-roller coater is used for coating, and the dry film coating weight is controlled at 2.0 g / m². 2 .

[0064] (5) Gradient phase change curing: Zone 1: Set temperature 87℃, convection hot air velocity 25m / s, aluminum foil residence time 2.2s.

[0065] Zone 2: Set temperature 120℃, convection hot air velocity 14m / s, aluminum foil residence time 4.0s.

[0066] Zone 3: Set temperature 175℃, wind speed 7.5m / s; Zone 4: Set temperature 205℃, wind speed 7.5m / s. The total dwell time in Zones 3 and 4 is 11.5s.

[0067] (6) Cooling and winding: The temperature is rapidly cooled to below 40°C by a 20°C cold air array and then wound up under a tension of 200N.

[0068] Example 3: This embodiment provides a precision coating process for high-lubricity aluminum foil coating on air conditioner heat sinks. The metrological standards are the same as in Embodiment 1, and the process includes the following steps: (1) Strong alkali pretreatment: 60.0 parts of the PAA-3 aqueous solution obtained in Preparation Example 3, 20.0 parts of aliphatic waterborne epoxy resin and 50.0 parts of deionized water were added to a stirred tank. Under stirring at 300 rpm and 30°C, 10.0 parts of ammonia water (25% by mass) were slowly added dropwise to adjust and stabilize the pH of the system at 10.5, and stirring was maintained for 20 min.

[0069] (2) Establishment of the latent system: In the above system, 6.0 parts of zirconium carbonate (ZAC) were slowly added and stirred for 15 min; then 4.0 parts of acetylacetone (ACAC) were added and stirred for another 15 min.

[0070] (3) Compounding and homogenization: 5.0 parts DMEA, 8.0 parts PTMEG (Mn=2000) and 12.0 parts oxidized polyethylene wax microemulsion were added sequentially. The mixture was dispersed at 1200 rpm for 45 min and filtered through a 300 mesh to obtain the coating solution.

[0071] (4) Substrate coating: A three-roller coater is used for coating, and the dry film coating weight is controlled at 2.5 g / m². 2 .

[0072] (5) Gradient phase change curing: Zone 1: Set temperature 95℃, convection hot air velocity 30m / s, aluminum foil residence time 3.0s.

[0073] Zone 2: Set temperature 130℃, convection hot air velocity 18m / s, aluminum foil dwell time 5.0s.

[0074] Zone 3: Set temperature 190℃, wind speed 10m / s; Zone 4: Set temperature 220℃, wind speed 10m / s. Total dwell time in Zones 3 and 4 is 15.0s.

[0075] (6) Cooling and winding: The temperature is rapidly cooled to below 40°C by a 25°C cold air array and then wound up under a tension of 250N.

[0076] Comparative Example 1: Compared to Example 2, the differences are as follows: no zirconium carbonate (ZAC), no acetylacetone (ACAC), and no latent catalytic base N,N-dimethylethanolamine (DMEA) were added to the formulation; the coating solution was adjusted solely by ammonia. The high-temperature, extremely high-velocity setting in Zone 1 was eliminated, and a conventional low-velocity drying process with a gradual temperature increase of 120℃-200℃ was directly adopted. All other parameters remained the same.

[0077] Comparative Example 2: The difference from Example 2 is that the competitive chelating delay agent acetylacetone (ACAC) was not added to the formulation. Everything else is the same.

[0078] Comparative Example 3: Compared to Example 2, the difference lies in the following: the formula is exactly the same (containing ZAC and ACAC), but the process parameters are changed. The high temperature and extremely high wind speed in Zone 1 (87°C, 25m / s) are eliminated, and instead, conventional gradual heating and low wind speed drying at 120°C-200°C is used. Everything else is the same.

[0079] Comparative Example 4: The difference from Example 2 is that the inorganic-organic hybrid crosslinking agent, zirconium carbonate (ZAC), was not added to the formulation. Everything else is the same.

[0080] Test Example 1: Turn on the rotary rheometer with a forced convection temperature control system, select a parallel plate measurement system with a diameter of 25 mm, and complete the instrument initialization and zero-gap calibration.

[0081] Preheat the temperature control system to 25°C. Use a pipette to take 1.0 mL of the coating sample from Example 2 and Comparative Example 2, place it in the center of the lower measuring plate, lower the upper measuring plate to a test gap of 1.0 mm, and scrape off any excess sample that overflows from the edges.

[0082] The rheometer was set to time-scan test mode, a constant oscillating strain of 1% was applied within the linear viscoelastic region of the sample, and the angular frequency was set to 10 rad / s.

[0083] The instant the time-scan program is initiated, the rapid heating module of the temperature control system is triggered, causing the sample ambient temperature to jump from 25°C to 85°C at a rate of 20°C / s and remain constant, simulating the thermal shock process of coated aluminum foil entering zone one of the oven. During the test, the edges of the measuring plate are kept open to allow volatile components within the system to escape freely.

[0084] The instrument continuously collects and records data points on the changes in the system's storage modulus G' and apparent viscosity over time at a set sampling frequency.

[0085] The data collection stopped after 15 seconds of testing, and the raw data was exported for processing and analysis.

[0086] Table 1. Rheological dynamic data of the coatings in Example 2 and Comparative Example 2 under isothermal time scanning at 85°C. in conclusion: Based on the data in Table 1 and the corresponding... Figure 1 In Comparative Example 2, the storage modulus G' of the coating system surged from 87.42 Pa to 12540.35 Pa within 1.5 s to 2.8 s after the start of the isothermal scanning, while the apparent viscosity simultaneously exhibited a nonlinear jump spanning two orders of magnitude (e.g., Figure 1 (The very early steep rise is shown by the black dashed line). Rheological data confirm that in the system without added acetylacetone, with the evaporation of ammonia and the decrease in pH caused by the temperature jump, the tetravalent zirconium ions released by the dissociation of ammonium zirconium carbonate directly coordinate and crosslink with the carboxyl groups of the polyacrylic acid molecular chain, and the coating film undergoes surface gelation in less than 3 seconds. This overly rapid crosslinking reaction will block the deep liquid phase mass transfer channels in the macroscopic process, causing the unevaporated solvent at the bottom layer to boil violently when heated in the subsequent high-temperature zone.

[0087] In Example 2, the storage modulus G' of the coating system remained in the low range of 18.24 Pa to 45.62 Pa within the first 5.7 s after heating, and the apparent viscosity did not show a step change. The system only exhibited a rheological gel point mutation between 7.1 s and 8.5 s, with the storage modulus jumping to 8950.41 Pa (as shown in the image). Figure 1 (The hysteresis and subsequent surge characteristics are shown by the solid black line). The rheological hysteresis phenomenon in Example 2 demonstrates that acetylacetone introduced into the formulation preferentially occupies the coordination orbitals of zirconium ions through a bidentate chelate structure, inhibiting the early reaction between zirconium ions and polyacrylic acid carboxyl groups. The temporarily formed zirconium-acetylacetone complex introduces a clear time delay in the crosslinking network construction process, maintaining the fluid open channels of the coating film in the first zone of the oven. After moisture is discharged through this microchannel, as acetylacetone evaporates upon heating, releasing the coordination binding, the system resumes normal ionic crosslinking and completes the rheological phase transition lock-in. Rheological dynamic monitoring data verifies the intervention effect of the acetylacetone competitive chelation mechanism on the phase transition process from a chemical kinetic perspective.

[0088] Test Example 2: The microfluidic dynamics test platform with a forced convection environment cavity was activated, the built-in airflow distribution component was adjusted, and the surface-view in-situ pH microelectrode system was connected and calibrated.

[0089] The environmental chambers were set to the operating conditions of Example 2 (temperature 87°C, surface horizontal wind speed 25 m / s) and Comparative Example 3 (temperature 120°C, surface horizontal wind speed 2 m / s, simulating a conventional low wind speed heating oven).

[0090] A coating with an initial wet film thickness of approximately 15 μm was prepared on the surface of a standard aluminum foil substrate using a wire bar coater, and the substrate was immediately transferred to a vacuum adsorption platform in the ambient chamber.

[0091] The planar test end of the in-situ pH microelectrode is lowered vertically so that it just contacts the wet film surface without damaging it, so that the liquid phase on the coating surface and the electrode sensing film form a continuous electrical circuit.

[0092] The environmental chamber is closed and the data acquisition module is started simultaneously. The dynamic changes of the surface pH value during the coating drying process are continuously recorded at a sampling interval of 0.5s.

[0093] When the system detects that the pH value on the coating surface has steadily dropped below 7.0 or the fluctuation range is less than 0.1 for 20 consecutive seconds, data acquisition is stopped, the electrode is cleaned, and the next set of data is recorded.

[0094] Table 2. Dynamic pH monitoring data of the coating surface in Example 2 and Comparative Example 3 in conclusion: Based on the monitoring data in Table 2 and the corresponding Figure 2 Specific fluid dynamic interventions clearly triggered the deammoniation reaction process. The horizontal axis of the graph represents the test time (range 0 to 10.5 s), and the vertical axis represents the real-time pH value of the coating surface (range 5.5 to 10.5). A legend is provided in the blank area at the upper right of the graph to indicate different operating conditions.

[0095] In Comparative Example 3, the coating system, under conventional low-wind-rate heating and drying processes (as shown by the black dashed line in the figure, representing the descent trajectory at 120℃ and 2m / s), although the ambient temperature reached 120℃, had a relatively thick gas-phase mass transfer boundary layer at the gas-liquid interface due to the surface convective wind speed of only 2m / s. The volatilization rate of ammonia molecules was limited by the diffusion resistance within the boundary layer, resulting in a very gentle, approximately linear descent characteristic on the curve. The surface pH value only dropped to 6.89 after 10.0s of testing. In a strongly alkaline environment lasting more than 8s, the zirconium ammonium carbonate complex in the formulation remained stable and could not dissociate to provide crosslinking points. At this time, the polyethylene wax particles inside the coating underwent Oswald ripening driven by thermodynamics and migrated to the surface, inevitably producing macroscopic wax precipitation defects.

[0096] Under high-velocity hydrodynamic conditions of 87°C and 25 m / s (as shown by the solid black line in the figure), the extremely high convective wind speed completely disrupted the mass transfer boundary layer at the gas-liquid interface, significantly reducing gas-phase mass transfer resistance. The ammonia on the surface flashed, propelling the system rapidly towards the deammoniation reaction, with its descent trajectory exhibiting a steep, step-like drop. The surface pH value plummeted from 10.02 to 6.84 within 1.5 seconds, rapidly crossing the black dotted line in the figure (the horizontal reference line at pH=7.0 on the vertical axis, used to visually indicate the critical pH point for the rapid dissociation of ammonium zirconium carbonate).

[0097] This sudden drop in pH, triggered by abrupt changes in external fluid physical parameters, disrupts the thermodynamic equilibrium of ammonium zirconium carbonate, forcing the complexed ions to rapidly dissociate within 1 to 2 seconds and release polyvalent zirconium ions, which are then taken over by acetylacetone to enter the delayed cross-linking process. Table 2 data and Figure 2 The interplay of the broken-line characteristics confirms the necessary correlation between high wind speed process parameters and decomplexation reactions, proving that the process can trigger a rheological phase change locking mechanism at a specific point.

[0098] Test Example 3: The coated aluminum foil samples prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were cut into square specimens with a size of 15cm × 15cm, and three parallel test specimens were prepared for each group.

[0099] A 0.5% (w / w) aqueous solution of methylene blue was prepared as a penetrating colorant, and a small amount of nonionic surfactant was added to reduce surface tension and ensure that it could fully wet the coating surface.

[0100] Place the aluminum foil sample flat on the test platform, use a soft brush to evenly coat the prepared methylene blue solution onto the coating surface to completely cover it, and let it stand and soak for 3 minutes at room temperature.

[0101] After settling, the sample is rinsed under running deionized water to remove excess colorant adhering to the surface. If the coating has penetrating or deep pinhole defects, the colorant will penetrate and accumulate at the micropores of the defects, resulting in color.

[0102] Use lint-free paper to blot away any residual moisture on the sample surface, then place it on a test bench with a standard D65 light source.

[0103] A grid test template with a standard 10cm x 10cm cutout area was placed over the center area of ​​the sample. Using an industrial inspection magnifying glass with 10x magnification, the number of tiny blue dot defects within each grid area was counted.

[0104] Record the number of defects for each parallel sample and calculate the average value as the macroscopic pinhole density of the sample group.

[0105] Table 3. Statistical data on macroscopic pinhole density on the surface of coated aluminum foil for each group. in conclusion: According to the data in Table 3, the coated aluminum foil of Comparative Example 2 showed dense colored pinholes on its surface, with an average pinhole density of 386 pinholes / 100cm². 2 The coating's density was severely compromised. Analysis of reaction kinetics and mass transfer mechanisms revealed that Comparative Example 2's formulation lacked acetylacetone, a competing chelating agent. When the coated aluminum foil entered zone one of the oven, set to extremely high wind speed and temperature, the ammonia on the coating surface flashed, causing a sharp drop in surface pH. The ammonium zirconium carbonate in the system rapidly dissociated, releasing tetravalent zirconium ions that directly and rapidly coordinated with the carboxyl groups on the polyacrylic acid molecular chains. This excessively rapid local reaction resulted in the formation of a dense cross-linked skin on the coating surface within 1 to 2 seconds. The coating system itself contained more than 50% water by volume. When the aluminum foil with the surface skin continued to operate in subsequent temperature zones with even higher temperatures, the unevaporated water deep within the coating vaporized, causing a sharp increase in internal vapor pressure.

[0106] When the vapor pressure exceeds the structural yield strength of the surface cross-linked skin, water vapor forcibly breaks through the film and escapes, leaving a large number of unhealable bubble rupture channels on the macroscopic morphology of the coating, namely the penetrating pinhole defects counted in macroscopic inspection. The pinhole density of Examples 1 to 3 remained at an extremely low level, indicating that the internal moisture was released smoothly. The acetylacetone introduced into the formulation preferentially forms a temporary chelate with tetravalent zirconium ions at the moment of deamination in Zone 1, forcibly delaying the construction of the polyacrylic acid cross-linked network at the chemical level. No early closure occurred on the coating surface, and the system maintained open fluid channels at the microscale for several seconds. The internal moisture diffused to the gas-liquid interface through the concentration gradient and was smoothly discharged. After the moisture was drained, the acetylacetone evaporated upon heating, releasing the complexation effect, and the system underwent deep cross-linking and locking. Comparative Examples 1, 3, and 4 did not experience rapid cross-linking in Zone 1, and the moisture venting channels were not blocked, therefore no severe boiling pinhole defects occurred. Test data demonstrate the essential role of acetylacetone in inhibiting early surface gelation and eliminating the contradiction between fluid mass transfer and chemical reaction rate.

[0107] Test Example 4: Set the environmental constant temperature and humidity chamber parameters to 25℃ and 50% relative humidity, turn on the standard optical contact angle measuring instrument system and perform horizontal calibration of the reference platform.

[0108] Cut aluminum foil products from Examples 1 to 3 and Comparative Examples 1 to 4 to a size of 5cm × 5cm. Wipe the surface of the sample with anhydrous ethanol and dry it with nitrogen to remove environmental dust adhering to the surface.

[0109] Lay the sample flat and fix it on the stage of the contact angle measuring instrument, and adjust the camera focus to make the sample surface clear.

[0110] Use a high-precision micro-syringe to draw up deionized water, suspend it on the sample surface, and drop a water droplet with a volume of 2.0 μL.

[0111] Three seconds after the water droplet detaches from the needle and contacts the coating surface, the CCD camera system is triggered to capture a static profile image of the droplet's side cross-section.

[0112] Import the test software, use the Laplace-Young equation to fit the droplet edge profile, and calculate the static contact angle between the droplet and the coating surface.

[0113] Repeat the above steps for five different random regions of each sample and take the arithmetic mean of the measurement results.

[0114] Table 4. Initial static water contact angle test data of each group of coated aluminum foil surfaces in conclusion: According to the data in Table 4, the initial water contact angles of the aluminum foil surfaces in Comparative Example 1 and Comparative Example 3 reached 78.5° and 82.6°, respectively, exhibiting hydrophobic characteristics. Thermodynamic and mass transfer mechanism analysis revealed that the polyacrylic acid matrix contains polar hydrophilic groups, while the polyethylene wax exhibits a non-polar hydrophobic state. In the uniform temperature baking process of Comparative Example 1 and the conventional temperature-raising drying process of Comparative Example 3, the coating system experienced a relatively long low-viscosity liquid phase period due to the limitation of solvent evaporation rate. Driven by the thermodynamic reduction of the system's surface free energy, the internal polyethylene wax particles underwent Oswald ripening, migrating to the gas-liquid interface through unclosed fluid mass transfer pathways and agglomerating and precipitating on the surface. The precipitated wax layer covered the underlying polymer network, hindering the exposure of the polar carboxyl groups of polyacrylic acid to the surface, resulting in the overall loss of hydrophilicity in the coating. In Comparative Example 2, due to the absence of acetylacetone in the formulation, although instantaneous cross-linking occurred in Zone 1, limiting the macroscopic migration of wax particles, a large number of penetrating boiling pinholes were generated on the surface (as confirmed by Test Example 3), which damaged the smoothness of the coating and exposed the internal hydrophobic components, resulting in increased surface roughness and an abnormal increase in the contact angle to 24.3°.

[0115] In Comparative Example 4, due to the absence of the inorganic crosslinking agent ammonium zirconium carbonate in the formulation, even with high-speed physical intervention in Zone 1 causing deamination and a decrease in pH, the system relied solely on the conformational coiling resulting from the protonation of the polyacrylic acid molecular chains, which could not provide sufficient structural network strength. This physical steric hindrance could not completely restrict the thermal motion of the wax particles kinetically, and some wax particles remained enriched on the surface, with the contact angle increasing to 65.2°. The contact angle measurements of the coating surfaces in Examples 1 to 3 ranged from 6.2° to 8.1°, exhibiting a hydrophilic state. Combining the high-speed hydrodynamic triggering mechanism with the ammonium zirconium carbonate crosslinking system, the coating caused a nonlinear jump in the apparent rheological viscosity of the system through the ionic coordination network formed by zirconium ions and polyacrylic acid. The steric barrier generated by the three-dimensional crosslinking network cut off the mass transfer path of the hydrophobic particles at the microscopic level, forcibly fixing the polyethylene wax inside the matrix. No continuous hydrophobic wax layer was formed on the surface, and the hydrophilic groups of polyacrylic acid were arranged on the coating surface. Test data validated the effectiveness of the phase change locking process in suppressing the separation of multiphase systems and maintaining the polarity of functional coatings.

[0116] Test Example 5: Turn on the reciprocating friction and wear testing machine, preheat the sensor controller, and perform zero-point calibration. Use 6mm diameter GCr15 bearing steel balls as the mating contact components to simulate the metal material of high-speed stamping dies.

[0117] The aluminum foil samples prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were cut into strips of 30 mm × 100 mm, flattened, and fixed on the horizontal stage of the testing machine.

[0118] The paired steel ball was fixed to the end of the loading link and lowered vertically until it contacted the coating surface. A constant normal load of 3.0 N was set to simulate the extreme pressure conditions during the stamping process.

[0119] The reciprocating sliding stroke for the friction test was set to 20 mm, the sliding speed was set to 15 mm / s, and the ambient temperature was maintained at 25℃.

[0120] The test is started, and the device’s built-in two-dimensional force sensor continuously records the normal force and tangential friction force of the friction pair during the sliding process. The test lasts for 50 cycles.

[0121] Extract the dynamic curve of the friction coefficient recorded by the testing software, discard the data from the first 5 cycles of the break-in period, and calculate the average value of the data from the subsequent steady-state sliding stage. Repeat the test on three different regions for each group of samples and take the final arithmetic mean.

[0122] Table 5. Initial dynamic friction coefficient test data for each group of coated aluminum foils in conclusion: According to the data in Table 5, the initial dynamic friction coefficient of Comparative Example 2 reached 0.154. Analysis of the results from Test Example 3 shows that the lack of acetylacetone in Comparative Example 2 led to rapid gelation of the coating surface, and the vaporization of internal moisture broke through the film layer, creating penetrating pinholes. These defects damaged the integrity of the coating and increased surface roughness. During extreme pressure sliding, the paired steel ball mechanically meshed with the micro-protrusions on the rough surface, exacerbating the ploughing effect and generating high frictional resistance. The dynamic friction coefficients of Comparative Example 1 and Comparative Example 3 were 0.086 and 0.081, respectively. In both sets of conventional drying processes, polyethylene wax particles migrated and precipitated on the coating surface. Although a wax layer existed on the surface, under a point contact load of 3.0 N, the rigid precipitated wax layer was prone to brittle fracture, and the detached solid wear debris rolled between the interfaces, affecting the drag reduction effect. The initial dynamic friction coefficient of Comparative Example 4 was 0.073. Due to the lack of ammonium zirconium carbonate, the polyethylene wax could not be firmly locked in, and the polyether lubricant lacked the underlying chemical anchoring support, so it could not form a stable and continuous fluid lubrication film at the friction interface, thus the drag reduction effect was limited.

[0123] The coefficients of dynamic friction in Examples 1 to 3 ranged from 0.031 to 0.042. Under the influence of the formulation and process, the examples utilized the ionic crosslinking of ammonium zirconium carbonate to construct a three-dimensional network, fixing polyethylene wax microparticles within the coating film and preventing surface aggregation. In the formulation, polytetrahydrofuran ether diol, influenced by the concentration gradient, enriched on the coating surface, forming flexible polyether segments. In the initial sliding phase of the mating components, the surface polyether long chains provided a hydrodynamic lubricating film, reducing the initial mechanical engagement force. With continued extreme pressure loading, the aluminum foil coating matrix underwent elastic deformation, exposing the polyethylene wax particles embedded within the network to the contact surface. The polyethylene wax underwent microplastic rheology under frictional heat, providing boundary lubrication. The friction interface of the examples exhibited a dual-load-bearing structure of fluid lubrication and solid boundary lubrication, which reduced surface spalling and maintained low tangential shear forces. Test data verified the tribological synergistic effect generated by the multi-component layered distribution achieved through rheological control.

[0124] Test Example 6: The aluminum foil samples prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were cut into standard sizes of 50 mm × 150 mm, and the initial mass of the samples before rinsing was weighed and recorded using a precision analytical balance.

[0125] Turn on the water tank flushing device with a constant temperature circulation system and inject deionized water into the tank. Use the heating module to keep the water temperature constant at 35°C to simulate the condensate temperature of an air conditioner during operation, and adjust the water pump speed to keep the water flow rate at the flushing pipe outlet at 2.5L / min.

[0126] The cut aluminum foil sample is fixed on a test bracket at a 45° angle to the horizontal plane. The position of the spray nozzle is adjusted so that the continuous water flow is evenly sprayed on the coating surface area.

[0127] Maintain continuous water flow for 72 hours. Replace the deionized water in the tank every 12 hours during the test to prevent the accumulation of dissolved substances from affecting the extraction concentration gradient.

[0128] After the rinsing time is over, remove the aluminum foil sample, use absorbent paper to dry the residual water droplets on the surface, and then place it in a 60℃ forced-air drying oven to dry at a constant temperature for 2 hours until constant weight.

[0129] After the sample was cooled to room temperature, the dynamic friction coefficient of the scouring area was re-determined on a reciprocating friction and wear tester according to the method and parameter conditions of Test Example 5, and the increase in friction coefficient before and after scouring was calculated and compared.

[0130] Table 6. Test data of dynamic friction coefficient of each group of coated aluminum foil before and after water rinsing in conclusion: According to the data in Table 6, after 72 hours of water rinsing, the coefficient of dynamic friction of the coating sample in Comparative Example 4 increased from the initial 0.073 to 0.134, an increase of 83.56%. Comparative Example 4 did not contain ammonium zirconium carbonate, and the system lacked coordination centers for polyvalent inorganic metal ions. Polytetrahydrofuran ether glycol, as a small-molecule fluid lubricant, was physically blended and dispersed in the polyacrylic acid matrix network. Under continuous water rinsing, the hydrophilic ether bonds on the polytetrahydrofuran ether glycol molecular chains caused solvation in the aqueous phase. Due to the lack of chemical bonding, the physically blended polyether molecules diffused to the gas-liquid interface of the coating and were extracted and eluted by the water flow. The loss of the surface hydrodynamic lubricating film led to direct contact between the mating parts and the hard substrate of the coating, resulting in a significant increase in the coefficient of friction.

[0131] In Examples 1 to 3, the coefficients of kinetic friction after rinsing remained at 0.041, 0.035, and 0.046, respectively, with increases controlled within 12.90%. Ammonium zirconium carbonate was added to the formulations of these examples. After the dissociation of tetravalent zirconium ions, the empty orbitals of the zirconium ions form coordination and hydrogen bonds with the terminal hydroxyl groups of polytetrahydrofuran ether diol. The polyether molecules are chemically anchored to a polymer network interwoven with ionic coordination and epoxy covalent bonds. This single- or double-ended anchoring structure allows the flexible segments of the polyether to extend at the contact interface to provide fluid lubrication, while resisting phase migration and dissolution extraction processes during external fluid rinsing.

[0132] After rinsing, the dynamic friction coefficients of the samples in Comparative Examples 1 and 3 reached 0.112 and 0.108, respectively. In both groups of samples, polyethylene wax precipitated onto the surface. The precipitated continuous wax layer lacked a molecular-level entanglement transition zone with the underlying matrix resin, resulting in weak interfacial adhesion. Under continuous fluid shear force, some brittle wax layers underwent microscopic peeling, altering the surface microstructure and roughness of the coating, and consequently increasing the sliding friction resistance. The test data demonstrate the chemical anchoring effect of the multi-metal coordination network on the small-molecule lubricant, proving the necessity of this structural design for maintaining a durable lubricated state on the coating surface.

Claims

1. A precise coating process for high lubrication function coating of an air conditioner fin aluminum foil, characterized in that, Includes the following steps: A coating solution comprising an aqueous polyacrylic acid solution, an aliphatic waterborne epoxy resin, ammonium zirconium carbonate, acetylacetone, ammonia, N,N-dimethylethanolamine, polytetrahydrofuran ether diol, oxidized polyethylene wax microemulsion, and deionized water is prepared. During preparation, the aqueous polyacrylic acid solution and the aliphatic waterborne epoxy resin are mixed, and ammonia is added to adjust the pH of the system to alkaline. Then, ammonium zirconium carbonate and acetylacetone are added to form a latent system, and the remaining components are added and mixed thoroughly to obtain the coating solution. A three-roller coating machine is used to apply the coating liquid to the surface of the degreased and passivated aluminum foil. The aluminum foil is continuously passed through multiple convection ovens, sequentially experiencing: The temperature in one zone of the multi-section convection oven is set to 80 to 95°C, and the convection hot air velocity is 20 to 30 m / s. The temperature in the second zone of the multi-section convection oven is set at 110 to 130°C, and the convection hot air velocity is set at 10 to 18 m / s. The temperature in zones three and four of the multi-section convection oven is set to 160 to 220°C, and the hot air velocity is 5 to 10 m / s. The aluminum foil is wound up under tension after exiting the multi-section convection oven.

2. The process for precision coating of high lubricity functional coating on fin of air conditioner using aluminum foil as claimed in claim 1, wherein The coating solution is made from raw materials comprising the following parts by weight: An aqueous solution of polyacrylic acid, in parts by weight of effective solids, is 40.0 to 60.0 parts. Aliphatic waterborne epoxy resin, 10.0 to 20.0 parts by weight of effective solid content; ammonium zirconium carbonate, based on effective solid content by mass, is 2.0 to 6.0 parts; Polytetrahydrofuran ether diol, based on effective solid content, 3.0 to 8.0 parts by weight; Oxidized polyethylene wax microemulsion, 5.0 to 12.0 parts by weight of effective solid content; Ammonia water, with a mass fraction of 20% to 25%, or 5.0 to 10.0 parts by actual physical mass; Acetylacetone, 1.0 to 4.0 parts by actual physical mass; N,N-Dimethylethanolamine, 2.0 to 5.0 parts by actual physical mass; Deionized water, by actual physical mass parts, 30.0 to 50.0 parts.

3. The process for precision coating of high lubricity functional coating on fin stock of an air conditioner using aluminum foil as claimed in claim 2, wherein the process is characterized by the steps of: The coating solution is made from raw materials comprising the following parts by weight: 50.0 parts by weight of polyacrylic acid aqueous solution, based on effective solid content; Aliphatic waterborne epoxy resin, based on effective solid content by weight, 15.0 parts; ammonium zirconium carbonate, based on effective solid content by mass, 4.0 parts; Polytetrahydrofuran ether diol, based on effective solid content by weight, 5.5 parts; Oxidized polyethylene wax microemulsion, based on effective solid content by weight, 8.5 parts; Ammonia solution, with a mass fraction of 22.5%, is 7.5 parts by actual physical mass. Acetylacetone, 2.5 parts by actual physical mass; N,N-Dimethylethanolamine, 3.5 parts by actual physical mass; Deionized water, 40.0 parts by actual physical mass.

4. The process for precision coating of high lubricity functional coating of aluminum foil for fins of an air conditioner as claimed in claim 1 wherein, The number-average molecular weight of the polyacrylic acid aqueous solution is between 30,000 and 50,000. This polyacrylic acid aqueous solution is prepared by the following steps: Under constant temperature conditions of heating in a water bath at 80 to 85°C, an initiator solution prepared by dissolving acrylic acid aqueous solution and ammonium persulfate is simultaneously added dropwise to deionized water that has been deoxygenated by purging with nitrogen. The dropping rate is controlled so that the dropping process is completed within 2.5 to 3.5 hours. Subsequently, the system temperature is raised to 90 to 95°C and the reaction is maintained for 1.5 to 2.0 hours.

5. The process for precision coating of high lubricity functional coating of aluminum foil for air conditioner fins as claimed in claim 1 wherein, The aliphatic waterborne epoxy resin is sorbitol polyglycidyl ether.

6. The process for precision coating of high lubricity functional coating of aluminum foil for air conditioner fins as claimed in claim 1 wherein, The number average molecular weight of polytetrahydrofuran ether diol is between 1,000 and 2,000.

7. The process as claimed in claim 1, wherein the process is used for the high lubricity functional coating of the aluminum foil for the fin of the air conditioner, characterized in that, In the preparation of the coating solution comprising an aqueous polyacrylic acid solution, an aliphatic waterborne epoxy resin, ammonium zirconium carbonate, acetylacetone, ammonia, N,N-dimethylethanolamine, polytetrahydrofuran ether glycol, oxidized polyethylene wax microemulsion, and deionized water, the steps include: mixing the aqueous polyacrylic acid solution and the aliphatic waterborne epoxy resin, adding ammonia to adjust the pH of the system to alkaline, then adding ammonium zirconium carbonate and acetylacetone to form a latent system, and finally adding the remaining components and mixing thoroughly to obtain the coating solution. Specifically, the steps include: Aqueous polyacrylic acid, aliphatic waterborne epoxy resin and deionized water were mixed in a stirred tank. Ammonia was slowly added dropwise at 20 to 30°C to adjust and stabilize the pH of the system between 9.5 and 10.

5. Slowly add an aqueous solution of zirconium carbonate to the adjusted high pH system and stir, then add acetylacetone and continue stirring; N,N-dimethylethanolamine, polytetrahydrofuran ether diol, and oxidized polyethylene wax microemulsion were added sequentially and dispersed at high speed at 800 to 1200 rpm for 30 to 45 minutes, followed by filtration to obtain the coating solution.

8. The process as claimed in claim 1, wherein the process is used for the high lubricity functional coating of the aluminum foil for the fin of the air conditioner, characterized in that, The step of applying the coating liquid to the surface of the degreased and passivated aluminum foil using a three-roll coating machine specifically includes: The three-roll coater is adjusted to have a gap between the coating rolls to control the dry film coating weight between 1.5 g / m 2 and 2.5 g / m 2 .

9. The precision coating process for high-lubricity functional coated aluminum foil for air conditioner heat sinks according to claim 1, characterized in that, In a multi-stage convection oven: The residence time of the aluminum foil in one zone of the multi-section convection oven is 1.5 to 3.0 seconds; The residence time of the aluminum foil in the second zone of the multi-section convection oven is 3.0 to 5.0 seconds; The total residence time in the three and four zones of the multi-section convection oven is 8.0 to 15.0 s.

10. The process of claim 1, wherein the process is a precision coating process for high lubricity functional coating of an aluminum foil for an air conditioner fin. The step of winding the aluminum foil under tension after it exits the multi-section convection oven specifically includes: After the aluminum foil exits the multi-section convection oven, it is cooled to below 40°C within 2 seconds by a cold air array at a temperature of 15 to 25°C, and then wound up under a tension of 150 to 250N.