A method and apparatus for preparing a yttria composite coating
By simultaneously dispersing yttrium oxide and alumina aerosols online, forming a uniform composite aerosol, and spraying it onto the substrate, the problems of density and mechanical properties of alumina-yttrium oxide composite coatings are solved, and the density and mechanical properties of the coatings are improved.
Patent Information
- Application Number
- CN202611360323.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-24
AI Technical Summary
Existing methods for preparing alumina-yttrium oxide composite coatings suffer from problems such as cracking, phase transformation, and agglomeration caused by high-temperature processes, which affect the coating's density and mechanical properties.
Yttrium oxide and alumina powders are used to form aerosols, and a uniform yttrium oxide-alumina composite aerosol is formed by online synchronous impact dispersion and turbulent shearing. The aerosol is then sprayed onto the substrate to form a composite coating. The particle size ratio and mass ratio are controlled to improve the density and mechanical properties.
This study achieved high density and improved mechanical properties of yttrium oxide composite coatings, avoiding coating cracking and agglomeration formation, and improving the coating's resistance to plasma etching and hardness.
Smart Images

Figure CN123149138A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of yttrium oxide coating preparation, and more specifically to a method and apparatus for preparing a yttrium oxide composite coating. Background Technology
[0002] In semiconductor etching processes, the etching of wafers using fluorine-containing plasma inevitably corrodes other components within the etching atmosphere, reducing their lifespan and contaminating the wafer with etching products. To mitigate this issue, etch-resistant coatings are applied to the surface of these components. Alumina-yttrium oxide composite ceramic coatings are widely used in etch-resistant coatings due to their excellent plasma resistance and relatively economical production cost.
[0003] Currently, alumina-yttrium oxide composite coatings are mainly prepared using thermal spraying and aerosol deposition techniques. Among these, thermal spraying, due to the insolubility of Al₂O₃ and Y₂O₃, allows for the in-situ generation of Y₂O₃ during the spraying process. x Al γ O2 compounds (such as Y2Al5O) 12 Y2O3 (Y4Al2O9, YAlO3) plays a role in dispersion toughening and strengthening of the phase interface, thereby improving the toughness and thermal shock resistance of the coating. However, this method has serious drawbacks: 1. High-temperature processes can easily generate huge thermal stress inside the coating, especially when the thermal expansion coefficients of the coating and the substrate material do not match, which can easily lead to cracking and peeling of the coating; 2. Under high-temperature conditions, Y2O3 materials are prone to adverse phase transformations or gradual performance degradation during thermal cycling, ultimately affecting the long-term reliability of the coating.
[0004] Aerosol deposition technology, performed at room temperature, avoids the aforementioned problems of thermal spraying and offers better coating density. However, its main drawback is that submicron-sized composite powders are prone to agglomeration due to van der Waals forces, forming soft agglomerates. These large agglomerates can deposit within the coating during deposition, causing defects and reducing its density and mechanical properties. Summary of the Invention
[0005] In view of the above-mentioned problems or deficiencies, the present invention aims to provide a method and apparatus for preparing yttrium oxide composite coating, so as to improve the density and mechanical properties of yttrium oxide composite coating.
[0006] A method for preparing a yttrium oxide composite coating includes the following steps:
[0007] S1. Prepare yttrium oxide and alumina powders by mass ratio of (70-95):(5-30), with a particle size ratio of (0.3-0.65):1, wherein the average particle size of yttrium oxide is 0.3-0.5 μm and the average particle size of alumina is 0.8-1 μm;
[0008] S2. Place yttrium oxide and alumina powders in separate aerosol generators to form yttrium oxide aerosol and alumina aerosol, respectively.
[0009] S3. Yttrium oxide aerosol and alumina aerosol are subjected to online synchronous impact dispersion and turbulent shearing to obtain a uniformly mixed yttrium oxide-alumina composite aerosol;
[0010] S4. The yttrium oxide-alumina composite aerosol is sprayed at high speed onto the substrate placed in the deposition chamber to deposit a Y2O3-Al2O3 composite coating; the yttrium oxide-alumina composite aerosol is sprayed onto the substrate placed in the deposition chamber at a speed of 150-500 m / s, and the pressure in the deposition chamber is 10-500 Pa.
[0011] An apparatus for preparing a yttrium oxide composite coating includes a mixing chamber, a yttrium oxide aerosol generator, an alumina aerosol generator, and a deposition unit. A rotating plate is provided within the mixing chamber. The outputs of the yttrium oxide and alumina aerosol generators are connected to the mixing chamber, and the input of the deposition unit is connected to the mixing chamber. The deposition unit includes a deposition chamber containing a nozzle and a substrate stage for fixing the substrate.
[0012] Preferably, in the mixing chamber, the output ends of the yttrium oxide aerosol generator and the alumina aerosol generator are located at the bottom of the mixing chamber and are arranged on both sides of the rotating plate. The rotating plate is located at the center of the bottom of the mixing chamber, and the output end of the mixing chamber is located at the top of the mixing chamber.
[0013] Preferably, as an improvement, the rotational speed of the rotating plate is 200-2000 rpm. The rotational speed is a "process window" that needs to be dynamically adjusted according to factors such as powder characteristics and gas flow rate, rather than a fixed value. The core basis of the rotational speed is to balance the "shear force required for deagglomeration" and "avoiding excessive damage". If the rotational speed is too low, it will not be able to disperse effectively, while if it is too high, the particles may be excessively "damaged" and unable to deposit effectively due to insufficient kinetic energy caused by the small particle size, resulting in a decrease in deposition efficiency. At high rotational speeds, the erosion effect of particles on the baffle and the inner wall of the cavity is significantly enhanced, increasing equipment maintenance costs.
[0014] The internal pressure of the mixing chamber varies according to the carrier gas flow rate, ranging from 5000 to 60000 Pa.
[0015] Preferably, as an improvement, the carrier gas pressure of the yttrium oxide aerosol generator and the alumina aerosol generator is 0.6 MPa.
[0016] Preferably, in the deposition chamber, the nozzle at the inlet is located at the bottom of the deposition chamber, and the substrate stage for fixing the substrate inside the deposition chamber is located at the top of the nozzle.
[0017] Preferably, during use, the two different powders arrive at the mixing chamber at different times due to their different qualities. To ensure the uniformity of the aerosol in the powder feeding pipe, the powder feeding and mixing device should be turned on before starting the spraying. Spray dry for 2-5 minutes until the powder feeding is stable before starting the formal spraying. At this time, the aerosol in the mixing chamber and the powder feeding pipe will be in a uniform state.
[0018] The principles and advantages of this invention are:
[0019] 1. This invention simultaneously delivers separately formed yttrium oxide aerosol and alumina aerosol into a mixing chamber equipped with a rotating plate. When the aerosols impact the rotating plate, they are mechanically broken down, forming well-dispersed, uniformly sized single-particle aerosols, thus avoiding the soft agglomerates present in traditional processes. Simultaneously, the dispersed aerosols are thoroughly mixed under the strong turbulence and shear force generated by the rotating plate, ultimately resulting in a well-defined, uniformly mixed composite aerosol, thereby improving the density and mechanical properties of the coating.
[0020] 2. This scheme controls the particle size ratio of yttrium oxide to alumina within the range of (0.3-0.65):1, with the average particle size of yttrium oxide controlled at 0.3-0.5 μm and the average particle size of alumina controlled at 0.8-1 μm. The synergistic effect produced by this particle size difference is as follows: On the one hand, through the particle size difference between yttrium oxide and alumina, as well as their mass ratio, the two form a balanced filling effect in the coating. Small particles can fill the gaps left after the deposition of large particles, which significantly increases the packing density of the coating and greatly reduces the porosity. On the other hand, controlling the average particle size of alumina to 0.8-1μm ensures that it is not prone to settling or clogging during airflow. At the same time, the kinetic energy of large-diameter Al2O3 particles can reach 2-3 times that of small-diameter Y2O3 particles. When these high-kinetic-energy Al2O3 particles impact the surface of the deposited coating, they generate a stronger impact compaction effect—the "hammering effect"—causing further plastic deformation and re-densification of the deposited layer. In addition, due to the high hardness of Al2O3 particles, fine nanoscale fragments are generated during impact. These fragments can fill the gaps between Y2O3 particles, further enhancing the filling and densification effect.
[0021] 3. This invention controls the mass ratio of yttrium oxide to aluminum oxide at (70-95):(5-30), ensuring excellent plasma etching resistance of the coating while improving its density and hardness. If the Al2O3 addition exceeds 30 wt%, the continuous Y2O3 phase is destroyed, and the overall etching rate of the composite coating increases exponentially, losing its core function as a semiconductor cavity liner. Furthermore, a large number of hard Al2O3 particles impacting the deposited layer can produce a "sandblasting erosion effect," making it difficult for the particles to adhere and even bombarding and peeling off the deposited Y2O3 layer, leading to a sharp decrease in deposition efficiency and even preventing the formation of a continuous coating. If the Al2O3 addition is too low, the hard particles are too sparse in the Y2O3 matrix, with excessively large spacing, allowing dislocations to easily bypass or pass through the gaps, failing to form an effective "dispersion strengthening" effect, resulting in negligible improvement in hardness and toughness. At the same time, the number of large particles that can provide a "hammering" effect per unit volume is too small to form a continuous and effective impact compaction on the underlying Y2O3, and the porosity remains high. Attached Figure Description
[0022] Figure 1 This is a schematic diagram of the structure of the device of the present invention.
[0023] Figure 2 This is a schematic diagram of the mixing chamber.
[0024] Figure 3 The image shows a cross-sectional SEM image of the yttrium oxide-alumina composite ceramic coating in Example 1.
[0025] Figure 4 This is a TEM image of the cross-section of the yttrium oxide-alumina composite ceramic coating in Example 1.
[0026] Figure reference numerals: 1. Yttrium oxide aerosol generator; 2. Aluminum oxide aerosol generator; 3. Powder mixing unit; 4. Deposition chamber; 5. Nozzle; 6. Matrix stage; 7. Yttrium oxide aerosol inlet; 8. Aluminum oxide aerosol inlet; 9. Mixed aerosol outlet; 10. Rotating plate. Detailed Implementation
[0027] The following detailed description illustrates the specific implementation method:
[0028] A method for preparing a yttrium oxide composite coating includes the following steps:
[0029] S1. Prepare yttrium oxide and alumina powders by mass ratio of (70-95):(5-30), with a particle size ratio of (0.3-0.65):1, wherein the average particle size of yttrium oxide is 0.3-0.5μm and the average particle size of alumina is 0.8-1μm.
[0030] S2. Place yttrium oxide and alumina powders in separate aerosol generators to form yttrium oxide aerosol and alumina aerosol, respectively.
[0031] S3. Yttrium oxide aerosol and alumina aerosol are simultaneously transported to the powder mixing unit (mixing chamber) using gas (such as N2, He or clean air) as carriers. They impact the rotating plate, breaking up and dispersing the soft agglomerates. The strong turbulence and shear force generated by the rotating baffles cause the two aerosols to be uniformly mixed in the device, resulting in yttrium oxide-alumina composite aerosol. The gas pressure is 0.3-0.7 MPa and the gas flow rate is 30-120 L / min.
[0032] S4. Yttrium oxide-alumina composite aerosol is sprayed at high speed (speed range 150-500 m / s) onto the substrate placed in the deposition chamber. The high-speed impact of the yttrium oxide-alumina composite aerosol on the substrate causes plastic deformation and breakage. Through mechanical anchoring and interparticle bonding, a Y2O3-Al2O3 composite coating is deposited layer by layer. The pressure in the deposition chamber is 10-500 Pa.
[0033] To achieve the above preparation method, the corresponding preparation apparatus is as follows: Figure 1 , Figure 2 As shown, it specifically includes a yttrium oxide aerosol generator 1, an alumina aerosol generator 2, a powder mixing unit 3, and a deposition unit.
[0034] The powder mixing unit 3 includes a closed cylindrical mixing chamber. A rotating plate 10 is vertically positioned at the center of the circular bottom of the cylindrical mixing chamber. This rotating plate 10 is driven by a speed-regulating motor with a rotation speed of 200-2000 rpm. In this design, the volume of the mixing chamber is 1500 cm³. 3 The rotating plate 10 is 8cm wide and 10cm high. Yttrium oxide aerosol inlets 7 and alumina aerosol inlets 8 are located on the left and right sides near the bottom of the mixing chamber, respectively. A mixed aerosol outlet 9 is located at the top of the mixing chamber. The outputs of the yttrium oxide aerosol generator 1 and the alumina aerosol generator 2 are connected to the yttrium oxide aerosol inlets 7 and 8, respectively.
[0035] The deposition unit includes a deposition chamber 4, which contains a nozzle 5 and a substrate stage 6 for fixing the substrate. The mixed aerosol outlet 9 of the mixing chamber is connected to the nozzle 5 in the deposition chamber 4 via a pipe. The substrate stage 6 fixes the substrate in an inverted position, so that the mixed aerosol outlet 9 is aligned with the substrate from below during deposition. During the spraying process, undeposited powder particles or loose powder with low bonding strength fall off due to gravity, resulting in better coating density and uniformity.
[0036] Example 1
[0037] Experimental parameter settings
[0038] Yttrium oxide aerosol generator: Y2O3 powder, carrier gas is high-purity helium, carrier gas pressure is 0.6 MPa.
[0039] Alumina aerosol generator: Al2O3 powder, carrier gas is high-purity helium, carrier gas pressure is 0.6 MPa.
[0040] Powder mixing device: cavity volume 1500 cm³, rotating baffle diameter 8 cm, height 10 cm, rotation speed 1500 rpm.
[0041] Deposition chamber: vacuum degree 200 Pa, nozzle distance from substrate 15 mm.
[0042] Substrate: Alumina ceramic sheet, size: 30×30×3 mm.
[0043] The specific preparation method of the yttrium oxide composite coating is as follows:
[0044] Yttrium oxide and aluminum oxide were prepared at a mass ratio of 80:20, with a particle size ratio of 1:3. The average particle size of yttrium oxide was 0.3 μm, and the average particle size of aluminum oxide was 0.9 μm.
[0045] Yttrium oxide and aluminum oxide were placed in yttrium oxide and aluminum oxide aerosol generators, respectively, to form yttrium oxide aerosol and aluminum oxide aerosol, respectively.
[0046] Yttrium oxide aerosol and alumina aerosol are simultaneously fed into the mixing chamber and impacted onto a rotating plate, breaking up and dispersing the soft agglomerates. The strong turbulence and shear force generated by the rotating baffles cause the two aerosols to be uniformly mixed in the device, resulting in a yttrium oxide-alumina composite aerosol.
[0047] Yttrium oxide-alumina composite aerosol is sprayed at high speed onto a substrate placed in a deposition chamber. The high-speed impact of the yttrium oxide-alumina composite aerosol on the substrate causes plastic deformation and breakage. Through mechanical anchoring and interparticle bonding, a Y2O3-Al2O3 composite coating is deposited layer by layer.
[0048] Example 2
[0049] This embodiment is basically the same as Embodiment 1, except that: the mass ratio of yttrium oxide to aluminum oxide is 95:5, the particle size ratio of yttrium oxide to aluminum oxide is 0.5:1, wherein the average particle size of yttrium oxide is 0.4 μm, and the average particle size of aluminum oxide is 0.8 μm; and the rotation speed of the rotating plate is adjusted to 800 rpm.
[0050] Comparative Example 1
[0051] Unlike Example 1, Y2O3 and Al2O3 powders were pre-mixed mechanically at a mass ratio of 80:20 and then directly fed into a single aerosol generator for deposition.
[0052] Comparative Example 2
[0053] Unlike Example 1, no Al2O3 powder was added, and a powder mixing unit with a rotating plate was not used.
[0054] Comparative Example 3
[0055] Unlike Example 1, no Al2O3 powder was added.
[0056] Comparative Example 4
[0057] Unlike Example 1, the Y2O3 and Al2O3 powders were mixed in a mass ratio of 60:40.
[0058] Comparative Example 5
[0059] Unlike Example 1, the particle size ratio of Y2O3 and Al2O3 is 1:1, and the average particle size of both is 0.5 μm.
[0060] Comparative Example 6
[0061] Unlike Example 1, the particle size ratio of Y2O3 to Al2O3 is 0.1:1, with Y2O3 having a particle size of 0.4 μm and Al2O3 having a particle size of 4 μm.
[0062] Comparative Example 7
[0063] Unlike Example 1, the particle size ratio of Y2O3 to Al2O3 is 0.5:1, with Y2O3 having a particle size of 3 μm and Al2O3 having a particle size of 6 μm.
[0064] Experimental results
[0065]
[0066] As can be seen from the above embodiments, the present invention first prepares yttrium oxide and alumina powders with specific mass and particle size ratios; then, yttrium oxide and alumina are respectively formed into yttrium oxide aerosol and alumina aerosol; next, the yttrium oxide aerosol and alumina aerosol are subjected to online synchronous impact dispersion and turbulent shearing to avoid soft agglomerates, resulting in a uniformly dispersed yttrium oxide-alumina composite aerosol; finally, the yttrium oxide-alumina composite aerosol is sprayed onto the substrate at a specific azimuth angle. At this point, the initial mass and particle size ratio design significantly reduces porosity during spraying and achieves a hammering effect, depositing and forming a Y2O3-Al2O3 composite coating. Corresponding supporting manufacturing equipment is also provided to ensure the implementation of the multi-physical mechanism synergistic design concept of the present invention, ultimately achieving a significant improvement in the density and mechanical properties of the yttrium oxide composite coating.
Claims
1. A method for preparing a yttrium oxide composite coating, characterized in that, Includes the following steps: S1. Prepare yttrium oxide and alumina powders by mass ratio of (70-95):(5-30), with a particle size ratio of (0.3-0.65):1, wherein the average particle size of yttrium oxide is 0.3-0.5 μm and the average particle size of alumina is 0.8-1 μm; S2. Place yttrium oxide and alumina powders in separate aerosol generators to form yttrium oxide aerosol and alumina aerosol, respectively. S3. Yttrium oxide aerosol and alumina aerosol are subjected to online synchronous impact dispersion and turbulent shearing to obtain a uniformly mixed yttrium oxide-alumina composite aerosol; S4. Spray yttrium oxide-alumina composite aerosol onto the substrate placed in the deposition chamber to deposit a Y2O3-Al2O3 composite coating; the yttrium oxide-alumina composite aerosol is sprayed onto the substrate placed in the deposition chamber at a speed of 150-500 m / s, and the pressure in the deposition chamber is 10-500 Pa.
2. An apparatus for preparing a yttrium oxide composite coating, characterized in that: The preparation method according to claim 1 includes a mixing chamber, a yttrium oxide aerosol generator, an alumina aerosol generator, and a deposition unit; the mixing chamber is provided with a rotating plate, the output ends of the yttrium oxide aerosol generator and the alumina aerosol generator are connected to the mixing chamber, and the input end of the deposition unit is connected to the mixing chamber; The deposition unit includes a deposition chamber, which contains a nozzle and a substrate stage for fixing the substrate.
3. The apparatus for preparing the yttrium oxide composite coating according to claim 2, characterized in that: The output ends of the yttrium oxide aerosol generator and the alumina aerosol generator are located at the bottom of the mixing chamber and are arranged on both sides of the rotating plate. The rotating plate is located at the center of the bottom of the mixing chamber, and the output end of the mixing chamber is located at the top of the mixing chamber.
4. The apparatus for preparing the yttrium oxide composite coating according to claim 2, characterized in that: The rotating plate rotates at a speed of 200-2000 rpm, and the air pressure in the mixing chamber ranges from 5000-60000 Pa.
5. The apparatus for preparing the yttrium oxide composite coating according to claim 2, characterized in that: The deposition chamber has a nozzle at its inlet located at the bottom, and a substrate stage for fixing the substrate inside the deposition chamber located at the top of the nozzle.
6. The apparatus for preparing the yttrium oxide composite coating according to claim 2, characterized in that: The carrier gas pressure of the yttrium oxide aerosol generator and the alumina aerosol generator is 0.6 MPa.