A processing method for antique and worn-out treatment of a gold product with cinnabar layered and penetrated color

By constructing nanoscale pores on the surface of gold products and using a layered coloring process with natural cinnabar powder and mineral additives, the environmental risks and adhesion problems in the process of aging gold products have been solved, achieving a permanent and firm cinnabar layered effect and the preservation of ancient patterns.

CN123149139APending Publication Date: 2026-11-24HENAN JINJIANG GOLD JEWELRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611403634.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing antiquing techniques for gold products have problems such as high environmental risks, poor adhesion, monotonous color, and easy wear and tear. In addition, traditional methods are corrosive to the gold substrate, which affects the collectible value.

Method used

Low-temperature dust-free softening and activation treatment is used to construct nanoscale micropores on the gold surface. Combined with a water-based mixed slurry of natural cinnabar powder and mineral additives, layered coloring is achieved through capillary sedimentation and surface adsorption effects. Then, a natural sealing system is used to fix the cinnabar layer, and finally, a cold-pressing and polishing process with an agate knife is used to form natural aging marks.

Benefits of technology

It achieves a permanent and firm bond with cinnabar minerals, a natural layered effect, and preserves the ancient patterns and gold quality. It is suitable for high-end collectible intangible cultural heritage goldware and avoids chemical corrosion and the use of toxic substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123149139A_ABST
    Figure CN123149139A_ABST
Patent Text Reader

Abstract

This invention provides a method for creating an antique-looking gold product with cinnabar layered staining, relating to the field of gold product surface treatment technology. The method includes the following steps: S1: Pre-treating the formed gold workpiece; S2: Performing a low-temperature, dust-free softening and activation treatment on the cleaned gold workpiece surface; S3: Preparing a water-based mixed cinnabar slurry using high-purity natural cinnabar ore according to a particle size gradient ratio; S4: Using a wet micro-immersion coating process; S5: Placing the layered colored workpiece horizontally in a dust-free, constant temperature and humidity environment; S6: Using a natural mineral transparent sealing system, performing a low-temperature thin-coat sealing treatment on the cured workpiece; S7: Using an agate knife cold-pressing and polishing process to obtain the antique-looking finished product. This invention utilizes capillary sedimentation and surface adsorption effects to automatically achieve layered coloring with deep grooves and shallow protrusions, eliminating the need for manual color separation and resulting in a natural transition between layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of surface treatment technology for gold products, and in particular to a method for treating gold products with cinnabar layering and patina to create an antique appearance. Background Technology

[0002] In recent years, with the rise of Chinese cultural trends and the revival of intangible cultural heritage crafts, traditional gold craftsmanship has become a core growth driver in the gold consumer market due to its warm and substantial texture, rich cultural connotations, and craftsmanship value. The large-scale application of traditional techniques such as engraving, hammering, filigree, and granulation has greatly enriched the expressive forms of gold products. Antique finishing, as a key process for enhancing the cultural texture and collectible value of traditional gold craftsmanship, imbues gold objects with a sense of age and restores the visual appearance of ancient gold artifacts. It is an indispensable post-processing step for high-end traditional gold jewelry.

[0003] The sulfide blackening process is the most widely used traditional method of antiquing gold. It utilizes soluble sulfides such as sodium sulfide and potassium sulfide to react chemically with the gold surface, generating a black gold sulfide film. This process is simple to operate and inexpensive. However, sulfides are toxic chemicals, and the production process easily releases hydrogen sulfide gas, posing high environmental and occupational health risks. Secondly, the reaction process can cause micro-corrosion to the gold substrate, which can lead to pinholes, pitting, and loosening of the gold surface with long-term use, seriously damaging the collectible value of high-end intangible cultural heritage gold artifacts. Thirdly, the resulting gold sulfide film is only tens of nanometers thick, with weak adhesion, making it extremely easy to wear off during wear. Moreover, the color is monotonous and dull, only presenting a dull gray-black, unable to reproduce the rich color layers of ancient gold artifacts. Another electroplating blackening process has a large difference in the coefficient of thermal expansion between the gold and the gold substrate, making it prone to peeling and flaking under temperature fluctuations and daily wear. In addition, the electroplating process requires the use of strong acids, heavy metal salts, and other chemical reagents, resulting in high costs for waste treatment, and the plating layer changes the pure metallic nature of the gold surface. Summary of the Invention

[0004] The purpose of this invention is to provide a method for treating gold products with cinnabar layering and patina to create an antique appearance, thereby solving the technical problems existing in the prior art.

[0005] To achieve the above-mentioned objectives, the technical solution adopted by this invention is as follows:

[0006] A method for creating an antique-looking gold product with cinnabar layering includes the following steps: S1: The formed gold workpiece is sequentially subjected to neutral ultrasonic degreasing, multi-stage rinsing with pure water, and dust-free constant temperature air drying to remove surface oil and impurities, resulting in a clean gold workpiece; S2: The cleaned gold workpiece surface is subjected to low-temperature dust-free softening and activation treatment to create uniformly distributed nanoscale micro-adsorption pores on the surface, resulting in an activated workpiece; S3: High-purity natural cinnabar is used to prepare a water-based mixed cinnabar slurry containing ultrafine cinnabar powder, fine cinnabar powder, and trace amounts of natural mineral additives according to a particle size gradient ratio; S4: A wet micro-immersion coating process is used to selectively apply the mixed cinnabar slurry to the surface of the gold workpiece. Utilizing capillary sedimentation and surface adsorption effects, the cinnabar powder preferentially accumulates and settles in the grooves and textures of the workpiece, while only a thin layer adheres to the raised gold surface, resulting in layered coloring. Workpiece S5: The layered colored workpiece is placed horizontally in a dust-free, constant temperature and humidity environment and left to stand, allowing the cinnabar mineral particles to continuously penetrate into the microscopic adsorption pores of the gold surface, forming a mechanically interlocked mineral bonding layer, resulting in a cured workpiece; S6: Using a natural mineral transparent sealing system, the cured workpiece is subjected to a low-temperature thin-coat sealing treatment to seal the micropores on the surface of the cinnabar layer and fix the cinnabar mineral particles, resulting in a sealed workpiece; S7: Using an agate knife cold-pressing and polishing process, the relief, main patterns, and flat areas of the workpiece are lightly pressed and brightened to fully preserve the cinnabar red patina deep in the patterns, resulting in an antique-style finished product; wherein, the wet micro-immersion coating process in step S4 uses a combination of flexible wool brush dot application and ultrasonic atomization touch-up coating, first dotting and wetting the engraved grooves, pattern gaps, and pattern dead corners point by point, and then applying a thin atomized coating to the entire surface of the workpiece; the coating amount per unit area is controlled at — The amount of coating applied to the grooved area is 2-3 times that of the raised area on the flat surface; the workpiece temperature is maintained at 20℃-25℃ during the coating process.

[0007] Furthermore, in step S2, the low-temperature dust-free softening and activation treatment is a low-temperature argon plasma activation treatment, with a treatment temperature of 25℃–80℃, a treatment time of 5 min–30 min, a plasma discharge power of 50 W–200 W, and a vacuum degree maintained in the treatment chamber of 10 Pa–100 Pa; the pore size of the nanoscale micro-adsorption pores is 20 nm–200 nm, the pore depth is 50 nm–500 nm, and the surface roughness Ra of the gold after activation is reduced from 0.02. Increased to 0.08 —0.15 .

[0008] Furthermore, in step S3, the median particle size D50 of the ultrafine cinnabar powder is 50nm-200nm, and the median particle size D50 of the fine cinnabar powder is 1. —5 The water-based mixed cinnabar slurry comprises, by weight, 10-20 parts of ultrafine cinnabar powder, 5-10 parts of fine cinnabar powder, 0.5-2 parts of natural mineral additives, and 68-84.5 parts of deionized water.

[0009] Furthermore, the preparation method of the water-based mixed cinnabar slurry is as follows: first, add ultrafine cinnabar powder and natural mineral additives to deionized water, and ultrasonically disperse for 10 min to 20 min; then add fine cinnabar powder and stir at a low speed of 100 r / min to 200 r / min for 5 min to 10 min to form a uniform suspension system.

[0010] Furthermore, in step S5, the ambient temperature is 20℃-30℃, the relative humidity is 40%-60%, and the settling time is 12h-24h; during the settling process, the penetration depth of cinnabar mineral particles into the micropores of the gold surface is 100nm-800nm, and the bonding force between the formed mineral bonding layer and the gold matrix is ​​≥15MPa.

[0011] Furthermore, in step S6, the natural mineral transparent sealing system is an ethanol dispersion of natural shellac and food-grade beeswax in a mass ratio of 3:1 to 5:1, with a solid content of 5% to 10%. The low-temperature thin-coating sealing treatment is carried out at a temperature of 30°C to 50°C, using ultrasonic atomization spraying, with a dry film coating thickness of 1 mm. —5 After spraying, let it stand at 40℃ for 30-60 minutes to allow the sealing layer to fully cure.

[0012] Furthermore, in step S7, the agate knife is made of natural red agate, with a cutting edge radius of 0.5mm-2mm, a cold-pressing polishing pressure of 0.2MPa-0.8MPa, and a feed speed of 5mm / s-20mm / s; after the brightening treatment, the surface roughness Ra of the raised area of ​​the workpiece is ≤0.05. .

[0013] Furthermore, in step S1, the neutral ultrasonic degreasing uses a neutral water-based cleaning agent with a pH of 6.5-7.5, which is a compound of fatty alcohol polyoxyethylene ether and alkyl glycoside in a mass ratio of 2:1; the ultrasonic frequency is 28kHz-40kHz, the treatment temperature is 30℃-50℃, and the treatment time is 3min-10min; the multi-stage pure water rinsing is a two-stage reverse osmosis pure water rinsing 2-3 times, with each rinsing time being 1min-3min; the dust-free constant temperature air drying temperature is 40℃-60℃, the air velocity is 0.5m / s-1.5m / s, and the air drying time is 5min-15min.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] (I) This invention utilizes capillary sedimentation and surface adsorption effects to automatically achieve layered coloring with deep grooves and shallow protrusions. No manual color separation is required, and the layer transition is natural. It perfectly replicates the natural aging traces of ancient gold artifacts formed by long-term use and burial, such as the accumulated color and polished protrusions. The visual effect is superior to the cheap texture of flat coating.

[0016] (ii) This invention constructs nano-adsorption pores on the gold surface through low-temperature micro-activation, allowing cinnabar mineral particles to penetrate into the micro-layer of the gold surface and form a mechanically interlocking bonding layer, thus completely solving the industry pain point of cinnabar being easy to fall off and shed powder, and achieving a permanent and firm antiquing effect.

[0017] (III) This invention adopts a completely green process route of physical activation, mineral coloring and natural sealing. It does not use strong acids, alkalis, heavy metals and toxic sulfides throughout the process. The gold matrix is ​​free from corrosion, gold damage and sand holes. It fully preserves the fine patterns and gold quality of the ancient engraving method. It is suitable for high-end collectible intangible cultural heritage goldware.

[0018] (iv) This invention uses a two-stage compound of ultrafine powder and fine powder cinnabar, combined with the modifying effect of mineral additives, to form a gradient structure from the bottom layer to the surface layer. The color is rich and deep, and the texture is delicate and textured, which is different from the thin and rigid effect of single fine powder flat coating on the market.

[0019] (v) The invention uses natural raw cinnabar, natural mineral additives, and natural shellac and beeswax throughout the process, without any organic glue, chemical pigments, or heavy metals added. Attached Figure Description

[0020] Figure 1 This is a flowchart of a method for treating gold products with cinnabar layering and patina to create an antique appearance, as disclosed in this invention.

[0021] Figure 2 This is a flowchart of step S4 of a method for treating gold products with cinnabar layering and patina to create an antique appearance, as disclosed in this invention. Detailed Implementation

[0022] To make the content of this invention easier to understand, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Identical components are represented by the same reference numerals. It should be noted that the terms "front," "rear," "left," "right," "up," and "down" used in the following description refer to directions in the accompanying drawings, while the terms "inner" and "outer" refer to directions toward or away from the geometric center of a specific component, respectively.

[0023] In the actual production of gold jewelry, the antiquing process is a crucial step in determining the cultural quality and market value of the product. Traditional methods heavily rely on the personal experience and craftsmanship of artisans. Workers need to prepare chemical reagents, control soaking times, and manually polish and color-separate the pieces. This not only results in low production efficiency but also inconsistent finished products, with significant differences in color and depth often appearing even within the same batch. More importantly, the irreversible corrosion of the gold substrate caused by traditional blackening processes makes the antiquing of high-end engraved gold jewelry extremely risky. Once corrosion flaws appear, the entire piece is scrapped, resulting in substantial economic losses.

[0024] Although some companies have attempted to incorporate cinnabar to enrich the aged color palette, they have been limited by technological bottlenecks and have yet to solve the core issues of adhesion and layering effects. The combination of cinnabar and gold remains at a rudimentary stage of "physical bonding," failing to achieve a true "patina" effect. How to make cinnabar firmly "grow" on the gold surface, and how to naturally present an antique texture with varying shades, are long-standing technical challenges that the industry has been unable to overcome.

[0025] In view of this, some embodiments of this specification provide a method for treating gold products with cinnabar layering and patina to create an antique appearance, fundamentally solving the aforementioned industry pain points.

[0026] like Figure 1 As shown, this embodiment provides a method for creating an antique-looking gold product using cinnabar layering and staining, including the following steps:

[0027] S1: The formed gold workpiece is subjected to neutral ultrasonic degreasing, multi-stage rinsing with pure water, and dust-free constant temperature air drying in sequence to remove surface oil and impurities and obtain a clean gold workpiece.

[0028] The neutral ultrasonic degreasing uses a neutral water-based cleaning agent with a pH of 6.5-7.5. The cleaning agent is a compound of fatty alcohol polyoxyethylene ether and alkyl glycoside in a mass ratio of 2:1. It belongs to a non-ionic and amphoteric surfactant compound system, which has strong degreasing ability, low foam, easy rinsing, and is non-toxic and non-corrosive, meeting environmental protection requirements.

[0029] The process parameters for ultrasonic degreasing are: ultrasonic frequency of 28kHz-40kHz, processing temperature of 30℃-50℃, and processing time of 3min-10min. In this embodiment, the preferred ultrasonic frequency is 40kHz, the processing temperature is 40℃, and the processing time is 8min. In specific operation, the parameters are adjusted according to the complexity of the workpiece. The deeper the texture and the more complex the structure, the longer the processing time should be.

[0030] The multi-stage rinsing with pure water consists of two-stage reverse osmosis pure water rinsing 2-3 times, with each rinsing time being 1-3 minutes. Multi-stage rinsing can avoid cleaning agent residue and prevent organic matter from decomposing and carbonizing to contaminate the gold surface during subsequent activation.

[0031] The dust-free constant temperature air drying temperature is 40℃-60℃, the air velocity is 0.5m / s-1.5m / s, and the air drying time is 5min-15min. Horizontal laminar flow air supply is adopted, and the airflow direction is parallel to the workpiece surface to avoid vertical dust settling. After air drying, the workpiece surface should be free of water stains, oil film, and dust. The water film should be fully spread and the contact angle should be less than 5° to meet the surface cleanliness requirements.

[0032] S2: The cleaned gold workpiece surface is subjected to low-temperature dust-free softening and activation treatment to generate uniformly distributed nanoscale micro-adsorption pores on the surface of the gold workpiece, thus obtaining the activated workpiece.

[0033] The low-temperature dust-free softening and activation treatment is a low-temperature argon plasma activation treatment. The basic principle of plasma activation is to introduce high-purity argon gas into a high-vacuum chamber and generate low-temperature plasma through a high-voltage electric field. The high-energy argon ions in the plasma bombard the surface of the gold workpiece with a certain kinetic energy. The energy of the ion bombardment is controlled within a specific range, acting only on the gold surface layer to a depth of a few hundred nanometers. This can break some of the metallic bonds between gold atoms, causing the surface atoms to rearrange and form a uniformly distributed nanoscale pit and pore structure. At the same time, the ion bombardment can remove the extremely thin oxide layer and contaminants on the surface, introduce unsaturated dangling bonds, and significantly improve the surface energy and surface activity.

[0034] The processing temperature is 25℃-80℃, the processing time is 5min-30min, the plasma discharge power is 50W-200W, and the vacuum degree in the processing chamber is maintained at 10Pa-100Pa; in this embodiment, the preferred processing temperature is 75℃, the processing time is 15min, and the plasma discharge power is 120W.

[0035] The pore size of the nanoscale micro-adsorption sites is 20nm-200nm, and the pore depth is 50nm-500nm. After activation, the surface roughness Ra of the gold changes from 0.02... Increased to 0.08 —0.15 This size range perfectly matches the particle size of the subsequent ultrafine cinnabar powder, allowing the ultrafine cinnabar particles to smoothly penetrate into the pores and form a mechanically interlocking anchoring structure. This is the structural basis for the high bonding strength achieved in this invention.

[0036] S3: A water-based mixed cinnabar slurry containing ultrafine cinnabar powder, fine cinnabar powder and trace amounts of natural mineral additives is prepared by using high-purity natural cinnabar ore and according to the particle size gradient ratio.

[0037] Natural cinnabar has a deep, rich red color, stable chemical properties, and excellent light and weather resistance, far superior to chemically synthesized cinnabar, meeting the material standards for ancient gold production.

[0038] The median particle size D50 of the ultrafine cinnabar powder is 50nm-200nm, and the median particle size D50 of the fine cinnabar powder is 1. —5 Among them, nano-sericite powder is a layered silicate mineral with excellent suspension and adhesion, which can improve the dispersion stability of cinnabar slurry, prevent precipitation and stratification, and fill the gaps between cinnabar particles to improve the density of the film. Attapulgite is a one-dimensional nano-mineral with strong adsorption and colloidal properties, which can enhance the adhesion between cinnabar particles and between cinnabar and gold surface. It is also a natural mineral component and does not introduce organic impurities.

[0039] The water-based mixed cinnabar slurry, by weight, comprises: 10-20 parts ultrafine cinnabar powder, 5-10 parts fine cinnabar powder, 0.5-2 parts natural mineral additives, and 68-84.5 parts deionized water; the formula in this embodiment is: 15 parts ultrafine cinnabar powder, 8 parts fine cinnabar powder, 0.5 parts nano-sericite powder, 0.5 parts attapulgite powder, and 76 parts deionized water.

[0040] The water-based mixed cinnabar slurry is prepared as follows: first, add ultrafine cinnabar powder and natural mineral additives to deionized water and ultrasonically disperse for 10-20 minutes; then add fine cinnabar powder and stir at a low speed of 100-200 r / min for 5-10 minutes to form a uniform suspension system; the prepared slurry should be uniform and fine, without obvious agglomerated particles, and should not stratify after standing for 2 hours.

[0041] like Figure 2 As shown, S4: Using a wet micro-immersion coating process, the mixed cinnabar slurry is applied to the surface of the gold workpiece. By utilizing capillary sedimentation and surface adsorption effects, the cinnabar powder is preferentially enriched and settled in the grooves and textures of the workpiece, while only a thin layer is formed on the raised gold surface, resulting in natural light and dark gradations and a layered colored workpiece.

[0042] The described wet micro-immersion coating process employs a combination of flexible wool brush dotting and ultrasonic atomization for touch-up coating. First, the engraved grooves, texture gaps, and hard-to-reach areas are dotted and immersed. In this embodiment, specifically: a fine wool brush with a tip diameter of 0.5mm-2mm is used, dipped in a small amount of mixed cinnabar paste, to dot-paint the engraved grooves, texture gaps, and hard-to-reach areas. During dotting, capillary action is utilized to allow the paste to automatically fill the texture, ensuring sufficient paste in the grooves. The amount of paste on the brush tip is controlled during dotting to prevent paste from overflowing onto raised surfaces. Then, a thin atomized coating is applied to the entire workpiece surface. In this embodiment, an ultrasonic atomizing spray gun with an atomized particle size of 10mm is used. —30 Apply a uniform, thin spray to the entire surface of the workpiece. Atomized spraying forms an extremely thin and uniform wet film, avoiding brush marks and runs. Spray distance: 15cm-20cm; spray pressure: 0.1MPa-0.2MPa; moving speed: 10cm / s-15cm / s; 1-2 coats are sufficient. The coating amount per unit area should be controlled at... — The amount of coating applied to the grooved area should be 2-3 times that of the raised area. If the amount of coating is too low, the color of the groove will be too light and the layering effect will not be obvious. If the amount of coating is too high, the raised surface will be too thick, which will not form a bright gold base and will easily lead to defects such as dripping and cracking. During the coating process, the workpiece temperature should be kept at 20℃-25℃ and the relative humidity of the environment should be about 50% to avoid the rapid evaporation and drying of the slurry and to ensure that the cinnabar particles have enough time to settle and penetrate.

[0043] The principle behind the automatic stratification in this step is as follows: First, the difference in capillary action: the smaller capillary radius and higher capillary pressure in the grooves result in a stronger ability to adsorb and retain the slurry, causing it to spontaneously flow and accumulate towards the grooves. Second, the gravitational settling effect: the slurry on the raised surfaces flows towards the lower areas under the influence of gravity, leaving only a very thin layer on the raised areas. Third, the difference in surface adsorption capacity: the grooves have a larger specific surface area and more micropores, resulting in a stronger physical adsorption capacity for cinnabar particles. These three effects work together to automatically create a natural stratification effect of "deep red veins and lightly dyed raised areas," with a smooth transition and no trace of artificial modification.

[0044] S5: The layered colored workpiece is placed horizontally in a dust-free, constant temperature and humidity environment and left to stand, so that the cinnabar mineral particles continuously penetrate into the micro-adsorption pores of the gold surface, forming a mechanically interlocked mineral bonding layer, and the cured workpiece is obtained.

[0045] The ambient temperature is 20℃-30℃, the relative humidity is 40%-60%, and the settling time is 12h-24h; in this embodiment, the preferred ambient temperature is 25℃, the relative humidity is 50%, and the settling time is 18h; during the settling process, the penetration depth of cinnabar mineral particles into the micropores of the gold surface is 100nm-800nm, and the bonding force between the formed mineral bonding layer and the gold substrate is ≥15MPa, which is higher than that of traditional glue adhesion, truly realizing "penetration" aging rather than "surface coating".

[0046] S6: Using a natural mineral transparent sealing system, the cured workpiece is subjected to a low-temperature thin-coat sealing treatment to block the micropores on the surface of the cinnabar layer and fix the cinnabar mineral particles, resulting in a sealed workpiece.

[0047] The natural mineral transparent sealing system is an ethanol dispersion of natural shellac and edible beeswax in a mass ratio of 3:1 to 5:1, with a solid content of 5% to 10%. In this embodiment, a mass ratio of natural shellac and edible beeswax of 4:1 is preferred, with a solid content of 8%. The low-temperature thin-coating sealing treatment is carried out at a temperature of 30℃ to 50℃, using ultrasonic atomization spraying, with a dry film coating thickness of 1 mm. —5 After spraying, allow the coating to stand at 40℃ for 30-60 minutes to allow the sealing layer to fully cure; in this embodiment, a temperature of 40℃ and a dry film coating thickness of 2 are preferred. Let stand for 45 minutes; the cured sealing layer is colorless and transparent, and will not change the red hue of cinnabar. At the same time, it can effectively seal the surface pores, firmly lock the cinnabar particles inside the film layer, and isolate the erosion of external air, sweat and dust, greatly improving the durability and stain resistance of the finished product.

[0048] S7: Using the cold pressing and polishing process with an agate knife, the relief, main patterns and flat areas of the workpiece are lightly pressed and brightened, preserving the vermilion red stain deep in the pattern, resulting in an antique-style finished product.

[0049] The agate knife is made of natural red agate, with a blade radius of 0.5mm-2mm. The cold-pressing polishing pressure is 0.2MPa-0.8MPa, and the feed speed is 5mm / s-20mm / s. During operation, the knife is used only in a single direction on raised areas, main decorative patterns, and flat, bright surfaces. The pressure causes slight plastic deformation of the gold surface, removing the thin cinnabar layer and sealing layer, revealing the metallic luster of the gold itself. After brightening, the surface roughness Ra of the raised areas of the workpiece is ≤0.05. It restores the warm, matte metallic luster of gold made using ancient methods; the cinnabar layer in the groove area is intact and has a rich and pure color.

[0050] Examples and Performance Tests

[0051] Example 1:

[0052] Processing is performed according to the preferred process parameters of this invention:

[0053] S1: Use a neutral water-based cleaning agent with pH=7, clean with 40kHz ultrasonic waves at 40℃ for 5 minutes, rinse 3 times with secondary pure water, and air dry at 50℃ for 10 minutes.

[0054] S2: Argon plasma activation, vacuum degree 50Pa, power 120W, processing time 15min, temperature ≤60℃;

[0055] S3: Slurry preparation: 15 parts ultrafine cinnabar powder (D50=100nm), fine cinnabar powder (D50=2... 8 parts of nano-sericite, 0.5 parts of attapulgite, 0.5 parts of deionized water, ultrasonically dispersed for 15 minutes and stirred at low speed for 8 minutes;

[0056] S4: Apply in dots to the grooves with a wool brush, then spray thinly across the entire surface with a misting spray gun, with a unit application rate of 1.2 mg / L. ;

[0057] S5: Let stand for 18 hours at 25℃ and 50% RH.

[0058] S6: Shellac:beeswax = 4:1, 8% ethanol dispersion, atomized spraying at 40℃, dry film thickness 2. Curing temperature: 40℃ for 45 minutes;

[0059] S7: Cutting edge radius 1mm, pressure 0.5MPa, feed speed 10mm / s, only highlights raised areas.

[0060] Example 2:

[0061] Adjust the activation parameters, and the rest is the same as in Example 1:

[0062] Low-temperature activation: Argon plasma activation, vacuum degree 80Pa, power 80W, processing time 25min, temperature ≤50℃.

[0063] Comparative Example 1:

[0064] The industry-standard potassium sulfide blackening process is adopted: the workpiece is immersed in a 5g / L potassium sulfide solution for 30 seconds at room temperature, then taken out and rinsed clean. The raised parts are then wiped with a color-wiping cloth to form a black base with a bright gold effect.

[0065] Comparative Example 2:

[0066] Using a common commercial process: mix cinnabar powder and transparent epoxy resin in a 1:1 mass ratio, apply by hand to the surface of the workpiece, let it stand for 24 hours to cure, and then use sandpaper to polish the raised parts to expose the gold surface.

[0067] Comparative Example 3:

[0068] The low-temperature activation step is omitted, and the rest is the same as in Example 1, that is, the same cinnabar paste is directly coated on the clean gold surface, and the subsequent processes are completely identical.

[0069] Performance testing methods and results

[0070] The following performance tests were performed on all samples:

[0071] 1. Adhesion test: The 100-grid test method is used. A 10×10 grid is made on the surface with a 1mm spacing using a cross-cutting knife. 3M tape is then peeled vertically, and the degree of peeling is observed. Grade 0 is no peeling, and Grade 5 is severe peeling.

[0072] 2. Abrasion resistance test: The standard dry rubbing test is adopted. The surface is rubbed repeatedly with a pure cotton cloth at a pressure of 500g. After 500 times, the surface condition is observed and the presence of powder, whitening, or peeling is recorded.

[0073] 3. Sweat resistance test: The sample was soaked in artificial sweat (pH=4.7) at room temperature for 72 hours. After soaking, the color change and peeling were observed. The gold loss rate was calculated by weighing the sample before and after the test.

[0074] 4. Layering effect evaluation: Five senior craftsmen will conduct visual scoring, with a maximum score of 10 points, to evaluate the naturalness of layering, color saturation, and antique texture.

[0075] 5. Evaluation of gold substrate corrosion: The surface morphology of gold before and after treatment was observed using a metallographic microscope, and the gold loss rate was calculated using a precision weighing method.

[0076] The test results are shown in Table (I) below:

[0077] Table (1)

[0078]

[0079] The test results show that:

[0080] The adhesion and wear resistance of the embodiments of the present invention are significantly better than those of traditional processes. The first embodiment achieves a level 0 adhesion and shows no peeling or whitening after 500 dry wiping cycles, completely solving the industry problem of cinnabar easily falling off.

[0081] The gold loss rate of this invention is extremely low, almost negligible, and there are no corrosive pinholes, causing no damage to the gold matrix, which is far superior to the traditional sulfidation process.

[0082] The layering effect of this invention is natural and soft, with a strong antique texture, and its score is significantly higher than that of traditional vulcanization and glue application processes.

[0083] Comparative Example 3, after omitting the activation step, showed a significant decrease in adhesion and exhibited powdering and whitening, proving that low-temperature micro-activation is a key process for improving adhesion.

[0084] In summary, through systematic process innovation, this invention achieves penetrating coloring and natural layering effects of cinnabar minerals without corroding the gold matrix. All performance indicators surpass existing technologies, demonstrating significant technological progress and application value.

[0085] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for creating an antique-looking gold product using cinnabar layering and staining, characterized in that: Includes the following steps: S1: The formed gold workpiece is subjected to neutral ultrasonic degreasing, multi-stage rinsing with pure water, and dust-free constant temperature air drying in sequence to remove surface oil and impurities and obtain a clean gold workpiece. S2: The cleaned gold workpiece surface is subjected to low-temperature dust-free softening and activation treatment to generate uniformly distributed nanoscale micro-adsorption pores on the surface of the gold workpiece, thus obtaining the activated workpiece. S3: A water-based mixed cinnabar slurry containing ultrafine cinnabar powder, fine cinnabar powder and trace amounts of natural mineral additives is prepared by using high-purity natural cinnabar ore and according to the particle size gradient ratio. S4: Using a wet micro-immersion coating process, the mixed cinnabar slurry is selectively applied to the surface of the gold workpiece. Utilizing capillary sedimentation and surface adsorption effects, the cinnabar powder preferentially accumulates and settles in the grooves and textures of the workpiece, while only a thin layer adheres to the raised gold surface, resulting in a layered colored workpiece. S5: The layered colored workpiece is placed horizontally in a dust-free, constant temperature and humidity environment and left to stand, so that the cinnabar mineral particles continuously penetrate into the micro-adsorption pores of the gold surface, forming a mechanically interlocked mineral bonding layer, and the cured workpiece is obtained. S6: Using a natural mineral transparent sealing system, the cured workpiece is subjected to a low-temperature thin-coat sealing treatment to block the micropores on the surface of the cinnabar layer and fix the cinnabar mineral particles, resulting in a sealed workpiece. S7: Using the cold pressing and polishing process with an agate knife, the relief, main patterns and flat areas of the workpiece are lightly pressed and brightened, preserving the vermilion red stain deep in the pattern, resulting in an antique-style finished product. In step S4, the wet micro-immersion coating process employs a combination of flexible wool brush dot application and ultrasonic atomization touch-up coating. First, the engraved grooves, texture gaps, and hard-to-reach areas are dotted and immersed point by point. Then, a thin atomized coating is applied to the entire workpiece surface. The coating amount per unit area is controlled at... — The amount of coating applied to the grooved area is 2-3 times that of the raised area on the flat surface; the workpiece temperature is maintained at 20℃-25℃ during the coating process.

2. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: In step S2, the low-temperature dust-free softening and activation treatment is a low-temperature argon plasma activation treatment. The treatment temperature is 25℃–80℃, the treatment time is 5 min–30 min, the plasma discharge power is 50W–200W, and the vacuum degree in the treatment chamber is maintained at 10 Pa–100 Pa. The pore size of the nanoscale micro-adsorption pores is 20 nm–200 nm, and the pore depth is 50 nm–500 nm. After activation, the surface roughness Ra of the gold is reduced from 0.

02. Increased to 0.08 —0.15 .

3. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: In step S3, the median particle size D50 of the ultrafine cinnabar powder is 50nm-200nm, and the median particle size D50 of the fine cinnabar powder is 1. —5 The water-based mixed cinnabar slurry comprises, by weight, 10-20 parts of ultrafine cinnabar powder, 5-10 parts of fine cinnabar powder, 0.5-2 parts of natural mineral additives, and 68-84.5 parts of deionized water.

4. The method for treating gold products with cinnabar layering and antiquing according to claim 3, characterized in that: The water-based mixed cinnabar slurry is prepared by first adding ultrafine cinnabar powder and natural mineral additives to deionized water and ultrasonically dispersing for 10-20 minutes, then adding fine cinnabar powder and stirring at a low speed of 100-200 r / min for 5-10 minutes to form a uniform suspension system.

5. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: In step S5, the ambient temperature is 20℃-30℃, the relative humidity is 40%-60%, and the settling time is 12h-24h. During the settling process, the penetration depth of cinnabar mineral particles into the micropores of the gold surface is 100nm-800nm, and the bonding force between the formed mineral bonding layer and the gold matrix is ​​≥15MPa.

6. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: In step S6, the natural mineral transparent sealing system is an ethanol dispersion of natural shellac and food-grade beeswax in a mass ratio of 3:1 to 5:1, with a solid content of 5% to 10%. The low-temperature thin-coating sealing treatment is carried out at a temperature of 30°C to 50°C, using ultrasonic atomization spraying, with a dry film coating thickness of 1 mm. —5 After spraying, let it stand at 40℃ for 30-60 minutes to allow the sealing layer to fully cure.

7. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: The agate knife used in step S7 is made of natural red agate, with a cutting edge radius of 0.5mm-2mm. The applied pressure for cold pressing and polishing is 0.2MPa-0.8MPa, and the feed rate is 5mm / s-20mm / s. After the brightening treatment, the surface roughness Ra of the raised area of ​​the workpiece is ≤0.

05. .

8. The method for treating gold products with cinnabar layering and antiquing according to claim 1, characterized in that: In step S1, the neutral ultrasonic degreasing uses a neutral water-based cleaning agent with a pH of 6.5-7.

5. The cleaning agent is a compound of fatty alcohol polyoxyethylene ether and alkyl glycoside in a mass ratio of 2:

1. The ultrasonic frequency is 28kHz-40kHz, the treatment temperature is 30℃-50℃, and the treatment time is 3min-10min. The multi-stage pure water rinsing is a two-stage reverse osmosis pure water rinsing 2-3 times, with each rinsing time being 1min-3min. The dust-free constant temperature air drying temperature is 40℃-60℃, the air velocity is 0.5m / s-1.5m / s, and the air drying time is 5min-15min.