具有疏水疏油性表面的板材及其加工方法
By forming a grid-shaped micron-scale microstructure on the substrate surface and coating it with a low surface energy chemical modification coating, the problem of oily materials adhering and accumulating on the equipment surface is solved, achieving the effects of hydrophobic and oleophobic properties of the equipment and reducing maintenance costs.
Patent Information
- Application Number
- CN202611573295.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-12
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, oily materials tend to adhere to and accumulate on equipment surfaces, leading to reduced material conveying efficiency and equipment blockage. Furthermore, existing coating and chemical cleaning methods suffer from coating wear, peeling, and high maintenance costs.
A regular grid-shaped microstructure is formed on the surface of the substrate and coated with a low surface energy chemical modification coating. The adhesion of water droplets and oil droplets is reduced by combining laser etching and chemical modification coating. The process flow is to first laser process and then coat the coating.
This achieves hydrophobic and oleophobic properties on the equipment surface, reducing liquid adhesion and coating peeling, lowering maintenance costs and equipment downtime, and increasing the service life of the equipment.
Smart Images

Figure CN123149140A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of surface treatment technology, specifically to a sheet material with a hydrophobic and oleophobic surface and its processing method. Background Technology
[0002] In chemical production, wastewater treatment, and kitchen waste disposal, equipment components such as conveying pipelines, hoppers, and agitator blades frequently come into contact with edible oil, lubricating oil, and other oily liquids. When oily materials spread, adhere, and accumulate on the equipment surface, they can easily reduce material conveying efficiency and, in severe cases, cause blockages in pipelines or devices, requiring frequent shutdowns for cleaning and maintenance.
[0003] To reduce the adhesion and accumulation of oily materials on equipment surfaces, existing methods typically involve coating the equipment surfaces with low surface energy materials such as Teflon; or, after adhesion or blockage occurs, using chemical reagents to clean the equipment.
[0004] However, the Teflon coating currently in use will experience wear, partial peeling, or performance degradation when subjected to liquid rinsing, friction, and repeated cleaning; while frequent chemical cleaning will increase manpower input, equipment downtime, and maintenance costs. Summary of the Invention
[0005] The purpose of this invention is to provide a sheet material with a hydrophobic and oleophobic surface to solve the problems mentioned in the background art.
[0006] This invention provides a sheet material with a hydrophobic and oleophobic surface, comprising: The substrate has a microstructure on one side surface. The microstructure includes a plurality of first grooves uniformly arranged along the length direction of the substrate and a plurality of second grooves uniformly arranged along the width direction of the substrate. The first grooves and the second grooves are rectangular and have the same size. The depth of the grooves is greater than the width of the grooves, and the distance between two adjacent first grooves is the same as the distance between two adjacent second grooves. One side surface of the substrate, each side of the first groove and the second groove are coated with a low surface energy chemically modified coating, and the thickness of the chemically modified coating is less than 1 / 2 of the groove width.
[0007] In one feasible approach, the chemically modified coating is made of nanoscale silica modified with siloxane or fluorosilane.
[0008] In one feasible approach, the chemically modified coating is made of fluorosilane-modified nanoscale silicon dioxide.
[0009] In one feasible solution, the depths of the first groove and the second groove are 50 μm to 100 μm.
[0010] In one feasible approach, both the first groove and the second groove are formed by pulsed laser scanning etching.
[0011] This invention also provides a method for processing a sheet material with a hydrophobic and oleophobic surface, comprising the following steps: S1 Cleaning the substrate; S2 uses a laser to scan and etch the surface of the substrate to form the first groove and the second groove; S3 The substrate is allowed to cool naturally to room temperature and the surface of the substrate is cleaned. S4. Apply a chemical modification coating to the surface of the substrate and to each side of the first groove and the second groove; S5 cures the chemically modified coating.
[0012] In one feasible scheme, in step S2, a MOPA single-mode pulsed laser with a wavelength of 1064nm is used to scan and etch the substrate. The average power during scanning is 200~300W, the pulse width is 10~20ns, and the single pulse energy is 0.1~0.4mJ. The laser field lens of the laser processing system is selected from F110, F160 or F254, and the diameter of the laser focusing spot is 20~80μm.
[0013] In one feasible solution, the distance between two adjacent grooves is 1.2 to 1.6 times the diameter of the laser focusing spot, and the width of the groove is 0.8 to 1.0 times the diameter of the laser focusing spot.
[0014] In one feasible approach, in step S5, the curing method for the chemically modified coating is either heat curing or natural air drying curing.
[0015] In one feasible approach, when using heat curing, the curing temperature is 70~90℃ and the curing time is 1~2 hours.
[0016] Compared with the prior art, the present invention has the following beneficial effects: 1. Two sets of intersecting continuous grooves form a regular grid-like microstructure on the surface of the substrate. This, combined with a low surface energy chemically modified coating, reduces the actual contact and adhesion of water and oil droplets to the substrate surface, resulting in a material surface with both good hydrophobic and oleophobic properties. This invention provides a sheet material with a hydrophobic and oleophobic surface, suitable for equipment components such as pipes, hoppers, and blades. Through the grid-like continuous grooves and chemically modified coating, it achieves both low adhesion of water and oil liquids and ease of process implementation.
[0017] 2. By controlling the thermal effect of laser processing through short pulses, small spot size and multiple scans, the formed grooves are kept to a small size and clear boundary. While achieving hydrophobic and oleophobic effects, the tendency of low surface tension oil to enter the microstructure and spread continuously is reduced.
[0018] 3. The process flow of laser processing, cooling, and then coating and curing a chemical modification coating is adopted. Compared with the processing method of coating a chemical modification coating first and then laser scanning processing, it can avoid the direct ablation of the chemical modification coating by laser, and the process steps are fewer, which is convenient to implement on the surface of equipment such as pipes, hoppers and blades.
[0019] 4. The combination of micron-level microstructures and chemically modified coatings can improve the hydrophobic and oleophobic properties of the material surface under relatively thin chemically modified coating conditions, which is beneficial to reducing the amount of low surface energy chemically modified materials used.
[0020] 5. The gas retained in the groove helps maintain a low contact state between water droplets and oil droplets. The depth of the groove can also provide some shielding for the chemically modified coating in the groove area, thereby reducing the problem of coating peeling caused by direct liquid scouring. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 This is a schematic diagram of a sheet material with a hydrophobic and oleophobic surface according to Embodiment 1 of the present invention; Figure 2 This is a partial cross-sectional view of the plate material in Embodiment 1 of the present invention; Figure 3 This is a schematic diagram of the processing flow of the sheet metal in Embodiment 2 of the present invention; Figure 4 This is a schematic diagram of the laser scanning path in Embodiment 2 of the present invention.
[0023] Numbering on the map: 100, Substrate; 110, First groove; 120, Second groove; 130, Chemically modified coating. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0026] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection, an electrical connection, or a communication connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise explicitly limited. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0027] The technical solution of the present invention will be described in detail below with reference to specific embodiments. These specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described again in some embodiments.
[0028] As described in the background section of this application, in order to reduce the adhesion and accumulation of oily materials on the surface of equipment, existing methods typically involve coating the surface of equipment with low surface energy materials such as Teflon; or, after adhesion or blockage occurs, using chemical reagents to clean the equipment.
[0029] The inventors of this application have discovered that currently used Teflon coatings can experience wear, localized peeling, or performance degradation when subjected to liquid rinsing, friction, and repeated cleaning; while frequent chemical cleaning increases manpower input, equipment downtime, and maintenance costs.
[0030] To address the aforementioned problems, the inventors of this application have proposed a technical solution, the specific embodiments of which are as follows: Example 1 Figure 1 This is a schematic diagram of a sheet material with a hydrophobic and oleophobic surface according to Embodiment 1 of the present invention. Figure 2 This is a partial cross-sectional view of the plate material in Embodiment 1 of the present invention.
[0031] like Figure 1 and Figure 2 As shown, the sheet material with a hydrophobic and oleophobic surface in this embodiment includes: a substrate 100.
[0032] The substrate 100 is a thin steel plate, such as a 2mm thick 304 stainless steel plate. A microstructure is provided on one side surface of the substrate 100. This microstructure includes a plurality of first grooves 110 extending along the length of the substrate 100 and a plurality of second grooves 120 extending along the width of the substrate 100. The plurality of first grooves 110 are equally spaced, and the distance between any two adjacent first grooves 110 is the same. The plurality of second grooves 120 are also equally spaced, and the distance between any two adjacent second grooves 120 is also the same. Furthermore, the distance between two adjacent first grooves 110 is the same as the distance between two adjacent second grooves 120.
[0033] The grooves (first groove 110 and second groove 120) are rectangular, with a depth greater than the width, and the first groove 110 and second groove 120 are the same size. The first groove 110 and second groove 120 form a regular grid-like microstructure on one side surface of the substrate 100. It should be noted that the grooves on the surface of the substrate 100 can also be arranged in triangular, concentric circular, or star-shaped patterns.
[0034] A low surface energy chemically modified coating 130 is uniformly coated on one side surface of the substrate 100 (the surface having the microstructure), and on each side of the first groove 110 and the second groove 120. The thickness of the chemically modified coating 130 is less than 1 / 2 of the width of the groove (the first groove and the second groove), that is, the chemically modified coating 130 will not fill the groove after it is applied.
[0035] Optionally, in this embodiment, the chemically modified coating 130 of the plate with a hydrophobic and oleophobic surface is made of one of nano-sized silica modified with siloxane or fluorosilane.
[0036] Furthermore, in this embodiment, the chemically modified coating 130 of the plate with a hydrophobic and oleophobic surface is made of fluorosilane-modified nano-sized silicon dioxide.
[0037] Optionally, in this embodiment, the first groove 110 and the second groove 120 on the substrate 100 of the plate with a hydrophobic and oleophobic surface are both formed by pulsed laser scanning etching.
[0038] Optionally, in this embodiment, the plate material with a hydrophobic and oleophobic surface has the same depth for the first groove 110 and the second groove 120, the depth of the groove is between 50μm and 100μm, and the width of the groove (the first groove 110 and the second groove 120) is less than the depth of the groove.
[0039] Example 2 The present invention also provides a method for processing a sheet material having a hydrophobic and oleophobic surface.
[0040] Figure 3 This is a schematic diagram of the processing flow of the sheet metal in Embodiment 2 of the present invention. Figure 4 This is a schematic diagram of the laser scanning path in Embodiment 2 of the present invention.
[0041] like Figure 3 and Figure 4 As shown, the processing method of the sheet material with a hydrophobic and oleophobic surface in this embodiment includes the following steps: S1 Clean the substrate.
[0042] If the substrate is a 2mm thick 304 stainless steel sheet, clean the surface of the stainless steel sheet to remove stains and keep the surface clean. Removing surface contaminants helps the substrate absorb laser light evenly, improving the uniformity of subsequent laser engraving.
[0043] S2 uses a laser to scan and etch the surface of the substrate to form the first and second grooves of the microstructure.
[0044] The cleaned 304 stainless steel plate is placed in the laser processing position, and the surface of the stainless steel plate is scanned and etched by laser to form a grid-shaped groove microstructure on the surface of the stainless steel plate. The depth of the groove is 50~100μm.
[0045] Specifically, a MOPA single-mode pulsed laser with a wavelength of 1064nm was used to scan and etch the surface of the stainless steel plate. A single-mode pulsed laser with an average power of 200~300W was selected, with a pulse width of about 13ns and a single pulse energy of about 0.17mJ. An F160 laser field lens was used to control the diameter of the laser focusing spot to about 50μm. The laser scanning etching speed was about 4m / s, and each groove was scanned 2~3 times.
[0046] like Figure 4 As shown, the laser performs multiple reciprocating grid-shaped scanning etchings on the surface of the stainless steel plate. The laser scanning interval is about 70μm (1.2 to 1.6 times the diameter of the laser focusing spot). That is, the distance between two adjacent grooves (the first groove and the second groove) is about 70μm, and the width of the grooves (the first groove and the second groove) is about 45μm.
[0047] In this embodiment, a single-mode pulsed laser is used for scanning etching to ensure the effective drilling depth of the laser focal point. Using a short-pulse laser minimizes thermal effects during drilling, increasing the drilling depth while minimizing the hole diameter. Multiple scans at lower power also reduce thermal effects during laser processing and improve the precision of the microstructure. While using a high-power, high-energy pulsed laser would increase processing speed, it would exacerbate the thermal melting phenomenon on the substrate surface, reducing the precision of the microstructure and hindering the improvement of oleophobic properties. Because oil droplets have low surface tension, the microstructure needs to be relatively fine to prevent oil inflow; therefore, controlling the laser spot size and thermal effects during processing is crucial. Of course, the above laser processing parameters can be adjusted appropriately based on the flatness, cleanliness, thermal conductivity, and laser absorption rate of the substrate surface.
[0048] S3 The substrate is allowed to cool naturally to room temperature and its surface is cleaned.
[0049] After laser processing is completed, allow the substrate (304 stainless steel plate) to cool naturally for a period of time until the stainless steel plate is completely cooled.
[0050] After laser processing, the 304 stainless steel plate is allowed to cool naturally for a period of time. Once the stainless steel plate has completely cooled, the surface of the substrate is cleaned with high-pressure gas to remove the slag and dust formed by laser ablation, and then a chemical modification coating is applied. The process sequence of first performing laser microstructure processing and then applying the chemical modification coating is adopted because if the chemical coating is applied first, the laser focus point will burn away the already formed chemical coating during laser scanning.
[0051] S4. A chemically modified coating is applied to one side surface of the substrate and each side of the first and second grooves.
[0052] After the substrate has completely cooled, a nano-sized silica coating modified with siloxane or fluorosilane is uniformly applied to one side surface of the substrate, as well as the bottom and sides of the grooves (first groove and second groove).
[0053] The thickness of the chemically modified coating is in the micrometer range, approximately 10 μm to 20 μm. This chemically modified coating is used to reduce the surface energy of the substrate (stainless steel plate). In this embodiment, micrometer-level microstructures are first processed on the surface of the stainless steel plate, and then chemical modification is performed on the surface of the microstructures. By combining the microstructures with the low surface energy chemically modified coating, the oleophobic properties of the substrate surface are improved.
[0054] S5 cures the chemically modified coating.
[0055] After the chemically modified coating is applied, it is allowed to fully cure, so that the chemically modified coating adheres firmly to the surface of the substrate.
[0056] Specifically, the curing method for chemically modified coatings can be either heat curing or natural air drying curing.
[0057] When using heat curing, the curing temperature should be controlled at 70-90℃ and the curing time at 1-2 hours; when using natural air drying curing, the curing time is 1-2 days, and the specific time depends on the weather conditions.
[0058] The curing process allows the chemically modified coating to adhere more firmly to the surface of the substrate (304 stainless steel plate), reduces the surface energy of the substrate, and makes the surface chemically modified coating less susceptible to being washed off by external liquids, thereby improving its service life.
[0059] The sheet material of this invention, after the above treatment, forms a surface combining a grid-shaped continuous groove microstructure with a low surface energy chemical modification coating on the surface of the substrate (304 stainless steel sheet). This treatment suppresses the wetting, spreading, adhesion, and retention of water and oil droplets on the surface, thereby obtaining a material surface with both hydrophobic and oleophobic properties. Under favorable process parameters, superhydrophobic and superoleophobic effects can be achieved.
[0060] In this invention, unless otherwise explicitly specified and limited, the first feature being "on" or "below" the second feature can mean that the first feature and the second feature are in direct contact, or that the first feature and the second feature are in indirect contact through an intermediate medium.
[0061] Furthermore, "above," "on top of," and "above" the first feature in relation to the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. Similarly, "below," "under," and "beneath" the first feature in relation to the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0062] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A sheet material with a hydrophobic and oleophobic surface, characterized in that, include: The substrate has a microstructure on one side surface. The microstructure includes a plurality of first grooves uniformly arranged along the length direction of the substrate and a plurality of second grooves uniformly arranged along the width direction of the substrate. The first grooves and the second grooves are rectangular and have the same size. The depth of the grooves is greater than the width of the grooves, and the distance between two adjacent first grooves is the same as the distance between two adjacent second grooves. One side surface of the substrate, each side of the first groove and the second groove are coated with a low surface energy chemically modified coating, and the thickness of the chemically modified coating is less than 1 / 2 of the groove width.
2. The sheet material with a hydrophobic and oleophobic surface according to claim 1, characterized in that, The chemically modified coating is made of nanoscale silicon dioxide modified with siloxane or fluorosilane.
3. The sheet material with a hydrophobic and oleophobic surface according to claim 2, characterized in that, The chemically modified coating is made of fluorosilane-modified nano-sized silicon dioxide.
4. The sheet material with a hydrophobic and oleophobic surface according to claim 1, characterized in that, The depths of the first groove and the second groove are 50 μm to 100 μm.
5. The sheet material with a hydrophobic and oleophobic surface according to claim 1, characterized in that, Both the first groove and the second groove are formed by pulsed laser scanning etching.
6. A method for processing a sheet material having a hydrophobic and oleophobic surface as described in claim 1, characterized in that, Includes the following steps: S1 Cleaning the substrate; S2 uses a laser to scan and etch the surface of the substrate to form the first groove and the second groove; S3 The substrate is allowed to cool naturally to room temperature and the surface of the substrate is cleaned. S4. Apply a chemical modification coating to the surface of the substrate and to each side of the first groove and the second groove; S5 cures the chemically modified coating.
7. The processing method for a sheet material with a hydrophobic and oleophobic surface according to claim 6, characterized in that, In step S2, a MOPA single-mode pulsed laser with a wavelength of 1064nm is used to scan and etch the substrate. The average power during scanning is 200~300W, the pulse width is 10~20ns, and the single pulse energy is 0.1~0.4mJ. The laser field lens of the laser processing system is selected from F110, F160 or F254, and the diameter of the laser focusing spot is 20~80μm.
8. The sheet material with a hydrophobic and oleophobic surface according to claim 7, characterized in that, The distance between two adjacent grooves is 1.2 to 1.6 times the diameter of the laser focusing spot, and the width of the groove is 0.8 to 1.0 times the diameter of the laser focusing spot.
9. The sheet material with a hydrophobic and oleophobic surface according to claim 6, characterized in that, In step S5, the curing method for the chemically modified coating is either heat curing or natural air drying curing.
10. The sheet material with a hydrophobic and oleophobic surface according to claim 9, characterized in that, When using heat curing, the curing temperature is 70~90℃ and the curing time is 1~2 hours.